Positive electrode active material, method for producing positive electrode active material, and lithium ion secondary battery

By optimizing the chemical composition and particle size of the cathode active material and combining it with ion exchange technology, Li-containing oxide particles with an O2-type structure are formed, which solves the problem of insufficient capacity of the existing cathode active material and realizes high-capacity lithium ion diodes. Secondary battery performance.

CN118800902APending Publication Date: 2024-10-18TOYOTA JIDOSHA KK
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410419297.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-09
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

There is room for improvement in capacity of existing cathode active materials having an O2 type structure.

Method used

Li-containing oxide particles are used, the chemical composition of which is LiaNabMnx-pNiy-qCoz-rMp+q+rO2, the particle size D50 is 0 μm to 3.0 μm, and the D90 is 2.0 μm to 6.0 μm, and the I2/ I1 ≤ 0.5, the Na ions of the Na oxide are exchanged for Li through ion exchange, forming a cathode active material with an O2 type structure.

Benefits of technology

Significantly improves the capacity of the positive active material and ensures efficient lithium-ion secondary battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800902A_ABST
    Figure CN118800902A_ABST
Patent Text Reader

Abstract

The invention relates to a positive electrode active material, a method for manufacturing the positive electrode active material, and a lithium ion secondary battery. Disclosed is a positive electrode active material having an O2-type structure and having a large capacity. The positive electrode active material of the present disclosure contains an oxide containing Li. The Li-containing oxide particles have an O2-type structure and have a prescribed chemical composition. The Li-containing oxide particles have a particle diameter D50 of more than 0 [mu] m and 3.0 [mu] m or less, and the Li-containing oxide particles have a particle diameter D90 of 2.0 [mu] m or more and 6.0 [mu] m or less. The X-ray diffraction pattern of the Li-containing oxide particles satisfies 0 < = I2 / I1 < = 0.5. Wherein I1 is the X-ray diffraction peak intensity from the (002) plane of the O2 type structure, and I2 is the X-ray diffraction peak intensity from the (003) plane of the O3 type structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application discloses a positive electrode active material, a method for producing the positive electrode active material, and a lithium ion secondary battery. Background Art

[0002] As a positive electrode active material, a positive electrode active material having an O2 type structure is known. As disclosed in Patent Document 1, a positive electrode active material having an O2 type structure is obtained by ion-exchanging at least a portion of Na in an oxide containing Na having a P2 type structure with Li.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2010-092824 Summary of the invention

[0006] Problems to be solved by the invention

[0007] Conventional positive electrode active materials having an O2 type structure have room for improvement in capacity.

[0008] Means for solving problems

[0009] The present application discloses the following multiple solutions as means for solving the above-mentioned problems.

[0010] <Option 1>

[0011] The positive electrode active material comprises an oxide particle containing Li, wherein the oxide particle containing Li has an O2 type structure, and the oxide particle containing Li has a Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (wherein, 0<a≤1.00, 0≤b<0.01, x+y+z=1 and 0≤p+q+r<0.17, element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.), the particle size D50 of the Li-containing oxide particles is greater than 0μm and less than 3.0μm, the particle size D90 of the Li-containing oxide particles is greater than 2.0μm and less than 6.0μm, the X-ray diffraction pattern of the Li-containing oxide particles satisfies 0≤I2 / I1≤0.5, the I1 is the X-ray diffraction peak intensity from the (002) plane of the O2 type structure, and the I2 is the X-ray diffraction peak intensity from the (003) plane of the O3 type structure.

[0012] <Option 2>

[0013] The positive electrode active material according to claim 1, wherein the particle size D10 of the oxide particles containing Li is greater than 0 μm and 2.0 μm or less.

[0014] <Option 3>

[0015] A method for manufacturing a positive electrode active material, comprising: obtaining precursor particles containing at least one element among Mn, Ni and Co; coating the surface of the precursor particles with a Na source to obtain composite particles; obtaining Na-containing oxide particles having a P2-type structure by subjecting the composite particles to a main calcination; and exchanging Na ions of the Na-containing oxide particles with Li by bringing an ion exchange material into contact with the Na-containing oxide particles to obtain Li-containing oxide particles having an O2-type structure, wherein the main calcination temperature is above 700°C and below 950°C, the particle size D50 of the Na-containing oxide particles is greater than 0 μm and below 3.0 μm, the particle size D90 of the Na-containing oxide particles is above 2.0 μm and below 6.0 μm, the ion exchange temperature is above the melting point of the ion exchange material and below 300°C, and the ion exchange time is above 30 minutes and below 3 hours.

[0016] <Option 4>

[0017] The production method according to claim 3, wherein the particle size D10 of the oxide particles containing Na is greater than 0 μm and less than or equal to 2.0 μm.

[0018] <Option 5>

[0019] A lithium ion secondary battery comprising a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material according to embodiment 1 or 2.

[0020] Effects of the Invention

[0021] The positive electrode active material disclosed in the present invention has an O2 type structure and has a large capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 An example of a process for producing a Li-containing oxide having an O2 type structure is shown.

[0023] Figure 2 An example of the structure of a lithium ion secondary battery is schematically shown.

[0024] Figure 3 The X-ray diffraction pattern of the positive electrode active material of Example 1 is shown.

[0025] Figure 4 X-ray diffraction patterns of the positive electrode active materials of Comparative Examples 1 to 3 are shown.

[0026] Figure 5 X-ray diffraction patterns of the positive electrode active materials of Comparative Examples 4 and 5 are shown.

[0027] Description of Reference Numerals

[0028] 100 Lithium-ion secondary battery

[0029] 10 Positive electrode active material layer

[0030] 20 electrolyte layer

[0031] 30 Negative electrode active material layer

[0032] 40 Positive electrode collector

[0033] 50 Negative electrode collector DETAILED DESCRIPTION

[0034] 1. Positive electrode active material

[0035] A positive electrode active material according to one embodiment includes oxide particles containing Li. The oxide particles containing Li have an O2 type structure. The oxide particles containing Li have a Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (wherein 0<a≤1.00, 0≤b<0.01, x+y+z=1, and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) The particle size D50 of the Li-containing oxide particles is greater than 0μm and less than 3.0μm. The particle size D90 of the Li-containing oxide particles is greater than 2.0μm and less than 6.0μm. The X-ray diffraction pattern of the Li-containing oxide particles satisfies 0≤I2 / I1≤0.5. Wherein, I1 is the X-ray diffraction peak intensity from the (002) plane of the O2 type structure, and I2 is the X-ray diffraction peak intensity from the (003) plane of the O3 type structure.

[0036] 1.1 Crystal structure

[0037] The Li-containing oxide particles according to one embodiment have at least an O2-type structure (belonging to the space group P63mc) as a crystal structure. The Li-containing oxide particles according to one embodiment may have an O2-type structure and a crystal structure other than the O2-type structure. Examples of the crystal structure other than the O2-type structure include a Li-containing oxide particle formed when Li is removed and inserted from the O2-type structure. Type structure (belonging to the space group Cmca), O6 type structure (belonging to the space group R-3m, c-axis length is greater than 2.5nm and less than 3.5nm, typically greater than 2.9nm and less than 3.0nm, which is different from the O3 type structure also belonging to the space group R-3m), etc. However, as described later, the Li-containing oxide particles involved in the embodiment basically do not contain the O3 type structure, or even if they contain it, it is very little. The Li-containing oxide particles involved in one embodiment may have an O2 type structure as the main phase. The Li-containing oxide particles involved in one embodiment may have an O2 type structure and also have In the Li-containing oxide particles according to the embodiment, the crystal structure of the main phase may change depending on the charge and discharge state.

[0038] As described later, Li-containing oxide particles having an O2-type structure are manufactured by exchanging Na ions of Na-containing oxide particles having a P2-type structure for Li. According to the present inventors' understanding, when the particle size of the Na-containing oxide particles is large, Na is likely to remain in the Li-containing oxide particles after ion exchange. On the other hand, when the particle size of the Na-containing oxide particles is small, although Na is difficult to remain, if the ion exchange time is inappropriate, it is also easy to generate an O3-type structure together with the O2-type structure in the Li-containing oxide particles after ion exchange. According to the present inventors' understanding, if the O3-type structure contained in the Li-containing oxide particles is large, the capacity as a positive electrode active material is reduced. In other words, the lower the X-ray diffraction peak from the O3-type structure is relative to the X-ray diffraction peak from the O2-type structure, the more the capacity as a positive electrode active material increases.

[0039] When obtaining an X-ray diffraction pattern of the oxide particles containing Li according to one embodiment, the ratio I2 / I1 of the X-ray diffraction peak intensity I2 from the (003) plane of the O3 type structure to the X-ray diffraction peak intensity I1 from the (002) plane of the O2 type structure is 0.5 or less, which is sufficiently small, so the capacity as a positive electrode active material is large. The X-ray diffraction pattern may satisfy 0≤I2 / I1≤0.4, 0≤I2 / I1≤0.3, 0≤I2 / I1≤0.2, 0≤I2 / I1≤0.1, or I2 / I1=0. In addition, in the present application, "X-ray diffraction pattern of oxide particles containing Li" and "X-ray diffraction peak intensity" refer to products obtained under the following conditions. That is, for oxide particles containing Li, an X-ray diffraction device (Rigaku, fully automatic multi-purpose X-ray diffraction device SmartLab) is used, CuKα is used as a radiation source, and 2θ / θ scanning is performed at a tube voltage of 45 kV, a tube current of 200 mA, a step width of 0.02°, and a scanning speed of 1° / min to obtain an X-ray diffraction pattern. From the X-ray diffraction pattern, the X-ray diffraction peak from the (002) plane of the O2 type structure and the X-ray diffraction peak from the (003) plane of the O3 type structure are determined. After subtracting the value of the background near the peak, the above-mentioned I2 / I1 can be calculated from the intensity of each X-ray diffraction peak. In addition, the position of the X-ray diffraction peak from the (002) plane of the O2 type structure and the position of the X-ray diffraction peak from the (003) plane of the O3 type structure can change according to the Li amount and the transition metal composition.

[0040] 1.2 Chemical composition

[0041] The Li-containing oxide particles according to one embodiment have Li a Na b Mn x-p Ni y-q Co z-r M p+q+rO2 (wherein 0<a≤1.00, 0≤b<0.01, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) A chemical composition represented by. When the oxide particles containing Li have such a chemical composition, it is easy to maintain the O2 type structure. In addition, by making the composition ratio b of Na less than 0.01, the Na remaining in the oxide particles containing Li is sufficiently reduced, and the reversible capacity as a positive electrode active material is increased. In the above chemical composition, a is greater than 0, and can be greater than 0.10, greater than 0.20, greater than 0.30, greater than 0.40, greater than 0.50 or greater than 0.60, and is less than 1.00, and can be less than 0.90, less than 0.80 or less than 0.70. In addition, b is 0.01 or less, and may be 0.00. In addition, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. In addition, y is 0 or more, and may be 0.10 or more, or 0.20 or more, and is 1.00 or less, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. In addition, z is greater than 0, and may be greater than 0.10, greater than 0.20, or greater than 0.30, and is less than 1.00, and may be less than 0.90, less than 0.80, less than 0.70, less than 0.60, less than 0.50, less than 0.40, or less than 0.30. Element M contributes little to charge and discharge. In this regard, in the above-mentioned chemical composition, high capacity is easily ensured by p+q+r being less than 0.17. p+q+r may be less than 0.16, less than 0.15, less than 0.14, less than 0.13, less than 0.12, less than 0.11, or less than 0.10. On the other hand, by including element M, the O2-type structure is easily stabilized. In addition, the presence of element M has no substantial effect on the problem-solving mechanism of the positive active material of the present disclosure. That is, independent of the presence of element M, the reversible capacity as a positive active material can be improved by having less O3-type structure and less residual Na in the oxide particles containing Li. In the above chemical composition, p+q+r is greater than 0, and may be greater than 0.01, greater than 0.02, greater than 0.03, greater than 0.04, greater than 0.05, greater than 0.06, greater than 0.07, greater than 0.08, greater than 0.09, or greater than 0.10. The composition of O is approximately 2, and is not limited to exactly 2.0, but is indefinite.

[0042] 1.3 Particle size

[0043] The particle size D50 of the Li-containing oxide particles involved in one embodiment is greater than 0 μm and less than 3.0 μm, and the particle size D90 is greater than 2.0 μm and less than 6.0 μm. If the Li-containing oxide particles have such D50 and D90, they are likely to become particles with a small amount of Na residue as described above (particles with b in the above chemical composition less than 0.01). The particle size D50 of the Li-containing oxide particles can be greater than 0.2 μm and less than 2.8 μm, greater than 0.4 μm and less than 2.6 μm, greater than 0.6 μm and less than 2.4 μm, greater than 0.8 μm and less than 2.2 μm, or greater than 1.0 μm and less than 2.0 μm. In addition, the particle size D90 of the oxide particles containing Li may be 2.3 μm or more and 5.5 μm or less, 2.5 μm or more and 5.0 μm or less, 2.7 μm or more and 4.5 μm or less, or 2.9 μm or more and 4.0 μm or less. In addition, the particle size D10 of the oxide particles containing Li according to one embodiment may be greater than 0 μm and less than 2.0 μm. The particle size D10 may be 0.1 μm or more and 1.9 μm or less, 0.2 μm or more and 1.8 μm or less, 0.3 μm or more and 1.7 μm or less, 0.4 μm or more and 1.6 μm or less, or 0.5 μm or more and 1.5 μm or less. Furthermore, in the present application, "particle size D50" is the particle size (median diameter) at the 50% cumulative value in the volume-based particle size distribution obtained by the laser diffraction scattering method, "particle size D90" is the particle size at the 90% cumulative value in the volume-based particle size distribution obtained by the laser diffraction scattering method, and "particle size D10" is the particle size at the 10% cumulative value in the volume-based particle size distribution obtained by the laser diffraction scattering method.

[0044] 1.4 Shape

[0045] As described later, Li-containing oxide particles having an O2-type structure can be obtained by replacing Na of Na-containing oxide particles having a P2-type structure with Li. Among them, the P2-type structure is a hexagonal system, the diffusion coefficient of Na ions is large, and it is easy to crystallize and grow in a specific direction. In particular, as a transition metal element constituting the P2-type structure, when at least one of Mn, Ni and Co is included, it is easy to crystallize and grow into a plate in a specific direction. Therefore, the oxide containing Na with a P2-type structure is easy to become a plate-like particle with a large aspect ratio and a crystal growth direction biased in a specific direction. The Li-containing oxide involved in one embodiment can be obtained based on such a plate-like Na-containing oxide particle, or it can be obtained based on the spherical Na-containing oxide particle described later. That is, the shape of the Li-containing oxide can be a plate-like particle or a spherical particle. In the case where the Li-containing oxide is a spherical particle, due to the reduction of the crystallite size, the reaction resistance is reduced, and the diffusion resistance inside the particle is easily reduced. Furthermore, in the case of application to secondary batteries, etc., it is believed that the curvature is reduced due to spheroidization, and the lithium ion conduction resistance is reduced. Thus, for example, the rate characteristics are improved and the reversible capacity is easily increased. Furthermore, in the present application, "spherical particles" means particles with a circularity of 0.80 or more. The circularity of the particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particles is defined as 4πS / L 2 Wherein, S is the orthographic projection area of ​​the particle, and L is the perimeter of the orthographic projection image of the particle. The circularity of the particle can be obtained by observing the appearance of the particle using a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. The circularity of multiple particles can be measured as an average value as described below.

[0046] (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by laser diffraction scattering method.

[0047] (2) For the appearance of the particles whose particle size distribution has been measured, an image is observed using a SEM, TEM, or optical microscope, and 100 particles contained in the image are randomly extracted that have an equivalent circle diameter (the diameter of a circle having the same area as the orthographic projection area of ​​the particle) greater than D10 and less than D90 determined in (1).

[0048] (3) The circularity of each of the 100 extracted particles is calculated by image processing, and the average value thereof is regarded as the "circularity of the particle".

[0049] 1.5 Others

[0050] As described above, the positive electrode active material involved in one embodiment has a large capacity by including the above-mentioned specific Li-containing oxide particles. From the viewpoint of further improving the capacity as a positive electrode active material, with respect to the content of the Li-containing oxide particles contained in the positive electrode active material, the entire positive electrode active material is set to 100 mass%, and can be 50 mass% or more and 100 mass% or less, 60 mass% or more and 100 mass% or less, 70 mass% or more and 100 mass% or less, 80 mass% or more and 100 mass% or less, 90 mass% or more and 100 mass% or less, 95 mass% or more and 100 mass% or less, or 99 mass% or more and 100 mass% or less, and the positive electrode active material can be composed of the above-mentioned specific Li-containing oxide particles.

[0051] 2. Method for producing positive electrode active material

[0052] The Li-containing oxide particles according to the above-mentioned embodiment can be produced by, for example, the following method. Figure 1 As shown, a method for manufacturing a positive electrode active material according to one embodiment includes:

[0053] S1: obtaining precursor particles containing at least one element of Mn, Ni and Co;

[0054] S2: coating the surface of the precursor particles with a Na source to obtain composite particles;

[0055] S3: performing main calcination on the composite particles to obtain oxide particles containing Na and having a P2 type structure; and

[0056] S4: By bringing an ion exchange material into contact with the Na-containing oxide particles, the Na ions of the Na-containing oxide particles are exchanged for Li, thereby obtaining Li-containing oxide particles having an O2 type structure. The main calcination temperature is 700° C. or higher and lower than 950° C., the particle size D50 of the Na-containing oxide particles is greater than 0 μm and lower than 3.0 μm, the particle size D90 of the Na-containing oxide particles is 2.0 μm or higher and lower than 6.0 μm, the ion exchange temperature is higher than the melting point of the ion exchange material and lower than 300° C., and the ion exchange time is 30 minutes or higher and lower than 3 hours.

[0057] 2.1S1

[0058] In S1, precursor particles containing at least one element of Mn, Ni and Co are obtained. The precursor particles may contain at least Mn, and one or both of Ni and Co, and may contain at least Mn, Ni and Co. The precursor particles may be salts containing at least one element of Mn, Ni and Co. For example, the precursor particles may be at least one of carbonates, sulfates, nitrates and acetates. Alternatively, the precursor particles may be compounds other than salts. For example, the precursor particles may be hydroxides. The precursor particles may be water and substances. The precursor particles may be a combination of multiple compounds. There is no particular limitation on the particle size of the precursor particles. In S1, an ion source that can form a precipitate with transition metal ions in an aqueous solution and a transition metal compound containing at least one element of Mn, Ni and Co are used, and a coprecipitation method is used to obtain a precipitate as the above-mentioned precursor particles. "An ion source that can form a precipitate with transition metal ions in an aqueous solution" may be, for example, at least one selected from sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide and sodium oxide. The transition metal compound may be the above-mentioned salt, hydroxide, etc. containing at least one element of Mn, Ni and Co. Specifically, in S1, after the ion source and the transition metal compound are made into solutions respectively, each solution is dripped and mixed, so that a precipitate as a precursor particle can be obtained. At this time, as a solvent, for example, water is used. At this time, as an alkali, various sodium compounds can be used, and in addition, an ammonia solution or the like can be added to adjust the alkalinity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and each aqueous solution is dripped and mixed to obtain spherical precursor particles. Alternatively, the precursor particles can also be obtained by a sol-gel method. In S1, the precursor particles may contain element M. Element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W. These elements M, for example, have the function of stabilizing a P2 type structure and an O2 type structure. The method for obtaining a precursor containing element M is not particularly limited. In the case where the precursor is obtained by the coprecipitation method in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and the respective aqueous solutions are dropped and mixed, thereby obtaining a precursor containing at least one of Mn, Ni and Co and element M. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped during Na-doping calcination in S2 and S3 described later.

[0059] 2.2S2

[0060] In S2, the surface of the precursor particles obtained by S1 is coated with a Na source to obtain composite particles. The Na source can be a salt containing Na such as carbonates and nitrates, or a compound other than salts such as sodium oxide and sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor particles can be determined by adding the portion of Na that disappears during the subsequent firing. In S2, there is no particular limitation on the coverage of the Na source on the surface of the precursor. For example, in S2, the above-mentioned composite particles can be obtained by coating more than 40 area%, more than 50 area%, more than 60 area% or more than 70 area% of the surface of the above-mentioned precursor particles with a Na source. If the coverage of the Na source is small, when the composite particles are fired, on the surface of the composite particles, P2 type crystals are easy to grow in a specific direction, and the oxide containing Na is easy to become plate-like. In the case where the coverage of the Na source is large, when the composite particles are fired, the crystallites of the P2 type crystals are easy to become smaller, and the oxide particles containing Na are easy to become a shape corresponding to the shape of the precursor particles. In S2, the method for coating the surface of the above-mentioned precursor particles with a Na source is not particularly limited. As described above, when more than 40% by area of ​​the surface of the precursor particles are coated with a Na source, as its method, for example, a tumbling flow coating method and a spray drying method can be cited. That is, a coating solution dissolved with a Na source is prepared, and the surface of the precursor particles is contacted with the coating solution, and dried at the same time or after contact. By adjusting the conditions (temperature, time, number of times, etc.) of the coating, more than 40% by area of ​​the surface of the precursor particles can be coated with a Na source. In S2, for the precursor particles, the M source can be coated together with the Na source. For example, in S2, the precursor particles obtained by S1, the Na source and the M source containing the element M are mixed to obtain composite particles. The M source can be, for example, a salt containing the element M such as a carbonate, a sulfate, or a compound other than a salt such as an oxide or a hydroxide.

[0061] 2.3S3

[0062] In S3, the composite particles obtained in S2 are subjected to main calcination to obtain oxide particles containing Na and having a P2 type structure. S3 may include the following S3-1 to S3-3.

[0063] In S3-1, the composite particles are pre-calcined at a temperature of 300°C to less than 700°C for 2 hours to 10 hours. The pre-calcination temperature may be 400°C to less than 700°C, 450°C to less than 700°C, 500°C to less than 700°C, 550°C to less than 700°C, or 550°C to 650°C. In addition, the pre-calcination time may be 2 hours to 8 hours, 3 hours to 8 hours, 4 hours to 8 hours, 5 hours to 8 hours, or 5 hours to 7 hours. There is no particular limitation on the pre-calcination atmosphere, and for example, it may be an oxygen-containing atmosphere.

[0064] In S3-2, following the above-mentioned pre-calcination, the main calcination is performed on the composite particles. The temperature of the main calcination is above 700°C and below 950°C, and can be above 800°C and below 920°C. If the main calcination temperature is too low, the P2 phase is not generated. In addition, if the main calcination temperature is too high, Na is likely to remain after the ion exchange in S4. There is no particular limitation on the heating conditions from the pre-calcination temperature to the main calcination temperature. There is no particular limitation on the main calcination time, for example, it can be above 30 minutes and below 48 hours, above 30 minutes and below 24 hours, above 30 minutes and below 10 hours, or above 30 minutes and below 3 hours. However, the shape of the oxide containing Na can be controlled according to the main calcination time. As described above, in the method disclosed in the present invention, when the coverage of the Na source in the composite particles is 40% by area or more, when the composite particles are calcined, small P2-type crystals are easily formed on their surface. In the method disclosed in the present invention, a P2 type microcrystal is connected to another P2 type microcrystal, and a P2 type crystal is grown along the surface of the particle, so that the shape of the oxide particle containing Na becomes a shape corresponding to the shape of the precursor particle. For example, when the precursor particle is spherical, the oxide particle containing Na may also become spherical. If the main firing time is too short, the generation of the P2 phase becomes insufficient. On the other hand, if the main firing time is too long, the P2 phase grows and becomes a plate-like particle instead of a spherical one. According to the inventors, when the main firing time is more than 30 minutes and less than 3 hours, the oxide particle containing Na tends to become spherical. The oxide particle containing Na obtained after the main firing may have a structure in which a plurality of microcrystals are present on the surface and the microcrystals are connected.

[0065] In S3-3, following the above-mentioned main calcination, the composite particles after the main calcination are rapidly cooled (cooled at a temperature drop rate of 20°C / min or more) from a temperature T1 of more than 200°C to a temperature T2 of less than 100°C. The above-mentioned preliminary calcination and main calcination are performed, for example, in a heating furnace. In step S3-3, for example, after the main calcination of the composite body in a heating furnace, the composite body is cooled to an arbitrary temperature T1 of more than 200°C in the heating furnace. After reaching the temperature T1, the calcined body is taken out of the heating furnace and rapidly cooled outside the furnace to an arbitrary temperature T2 of less than 100°C. Temperature T1 is an arbitrary temperature of more than 200°C, and may also be an arbitrary temperature of more than 250°C. Temperature T2 is an arbitrary temperature of less than 100°C, and may also be an arbitrary temperature of less than 50°C, or may be the cooling end temperature. In the specified temperature range between temperature T1 and temperature T2, moisture easily penetrates into the interlayers of the P2 type structure due to atomic vibration, molecular motion, etc. When the composite particles (Na-containing oxide particles having a P2-type structure) after the main firing are cooled, it is considered that by making the time in the temperature region where moisture easily penetrates into such a region short (i.e., high-speed cooling), the amount of moisture penetrating between the layers of the P2-type structure is reduced. In this regard, in S3-3, when the composite body after the main firing is cooled, it is cooled in a dry atmosphere outside the furnace from an arbitrary temperature T1 above 200°C to an arbitrary temperature T2 below 100°C, so that the cooling rate between the temperature T1 and the temperature T2 becomes high (for example, 20°C / min or more), and moisture becomes difficult to penetrate between the layers of the P2-type structure, and the collapse of the P2-type structure can be suppressed. As a result, Na can be efficiently ion-exchanged for Li in S4, and the amount of residual Na after the ion exchange becomes easy to reduce.

[0066] By using the above method, it is possible to produce oxide particles containing Na having a P2 type structure and a predetermined chemical composition. The oxide particles containing Na may have a structure composed of Na c Mn x-p Ni y-q Co z-r M p+q+rThe chemical composition represented by O2. Wherein, 0.10≤c≤1.00, x+y+z=1 and 0≤p+q+r<0.17. In addition, M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W. In the case where the oxide particles containing Na have such a chemical composition, it is easy to maintain the P2 type structure. In the above chemical composition, c may be greater than 0.10, greater than 0.20, greater than 0.30, greater than 0.40, greater than 0.50 or greater than 0.60, and may be less than 1.00, less than 0.90, less than 0.80 or less than 0.70. For x, y, z, p, q and r, as described above.

[0067] In addition, the Na-containing oxide particles obtained by the above method have a particle size distribution. In the present embodiment, after obtaining Na-containing oxide particles having specified D50 and D90 by airflow classification of the above-mentioned precursor particles, airflow classification of the above-mentioned composite particles, or airflow classification of the Na-containing oxide particles, the Na-containing oxide particles are used in the later-described S4. Thus, Li-containing oxide particles having specified D50 and D90 are obtained. Specifically, the particle size D50 of the Na-containing oxide particles used for S4 is greater than 0 μm and less than 3.0 μm, and the particle size D90 is greater than 2.0 μm and less than 6.0 μm. The particle size D50 may be greater than 0.2 μm and less than 2.8 μm, greater than 0.4 μm and less than 2.6 μm, greater than 0.6 μm and less than 2.4 μm, greater than 0.8 μm and less than 2.2 μm, or greater than 1.0 μm and less than 2.0 μm. In addition, the particle size D90 may be 2.3 μm to 5.5 μm, 2.5 μm to 5.0 μm, 2.7 μm to 4.5 μm, 2.9 μm to 4.0 μm. In addition, the particle size D10 of the oxide particles containing Na may be greater than 0 μm and 2.0 μm or less. The particle size D10 may be 0.1 μm to 1.9 μm, 0.2 μm to 1.8 μm, 0.3 μm to 1.7 μm, 0.4 μm to 1.6 μm, or 0.5 μm to 1.5 μm.

[0068] 2.4S4

[0069] In S4, the Na-containing oxide particles obtained by S3 are contacted with an ion exchange material, thereby exchanging the Na ions of the Na-containing oxide particles for Li, and obtaining Li-containing oxide particles having an O2 type structure. As an ion exchange material, for example, a mixture of lithium halide and other lithium salts (such as a molten salt) can be cited. The lithium halide constituting the molten salt is preferably at least one of lithium chloride, lithium bromide and lithium iodide. The other lithium salts constituting the molten salt are preferably lithium nitrate. By using a molten salt, the melting point is lowered compared to the case where lithium halide or other lithium salts are used alone, and ion exchange at a lower temperature can be performed. The temperature in the ion exchange is above the melting point of the above-mentioned ion exchange material and below 300°C. If the temperature of the ion exchange is too high, it is easy to generate an O3 type structure instead of an O2 type structure as a stable phase. On the other hand, from the viewpoint of making the ion exchange time short, the temperature of the ion exchange is preferably as high a temperature as possible. The ion exchange time is more than 30 minutes and less than 3 hours. If the ion exchange time is too short, the amount of residual Na in the Li-containing oxide particles increases. On the other hand, if the ion exchange time is too long, an O3 type structure and the like are easily generated together with the O2 type structure.

[0070] 3. Lithium-ion secondary battery

[0071] exist Figure 2 The structure of a lithium ion secondary battery according to one embodiment is schematically shown in FIG. Figure 2 As shown, a lithium ion secondary battery 100 according to one embodiment includes a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. The positive electrode active material layer 10 includes the positive electrode active material according to the above-mentioned embodiment. Figure 2 As shown, the lithium ion secondary battery 100 may include a positive electrode current collector 40 and a negative electrode current collector 50. In the lithium ion secondary battery 100, the structure other than the positive electrode active material is the same as in the related art, for example, the structure described in Patent Document 1 (Japanese Patent Application Laid-Open No. 2010-092824) may be adopted.

[0072] Example

[0073] As described above, one embodiment of the positive electrode active material, the method for manufacturing the positive electrode active material, and the lithium ion secondary battery has been described, but the technology disclosed herein can be variously modified beyond the above-mentioned embodiments without departing from the scope of its purpose. The following examples are shown to further illustrate the technology disclosed herein, and the technology disclosed herein is not limited to the following examples.

[0074] 1. Preparation of positive electrode active material

[0075] 1.1 Example 1

[0076] 1.1.1 Preparation of precursor particles

[0077] (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed to a target composition ratio and dissolved in distilled water to a concentration of 1.2 mol / L to obtain a first solution. In addition, Na2CO3 was dissolved in distilled water to a concentration of 1.2 mol / L in another container to obtain a second solution.

[0078] (2) 1000 mL of pure water was placed in a reaction container (with baffles), and 500 mL of the first solution and 500 mL of the second solution were added dropwise at a rate of about 4 mL / min.

[0079] (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product.

[0080] (4) The product is washed with pure water, separated into solid and liquid using a centrifuge, and the precipitate is recovered.

[0081] (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and separated into coarse particles and fine particles by air flow classification. The coarse particles and fine particles are both composite salts containing Mn, Ni and Co. In Example 1, the above-mentioned fine particles were used as precursor particles.

[0082] 1.1.2 Preparation of composite particles

[0083] By mixing the precursor particles and Na2CO3 to form a target composition after sintering as described below, Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O2 is weighed and mixed, thereby coating the surface of the precursor particles with Na2CO3 to obtain composite particles.

[0084] 1.1.3 Calcination of composite particles

[0085] The composite particles were placed in an alumina crucible and fired in an air atmosphere to obtain an oxide containing Na and having a P2 type structure. The firing conditions were as described in the following (1) to (7).

[0086] (1) An alumina crucible containing the above-mentioned composite particles is placed in a heating furnace in an air atmosphere.

[0087] (2) The temperature in the heating furnace was raised from room temperature (25°C) to 600°C over 115 minutes.

[0088] (3) The temperature in the heating furnace is maintained at 600° C. for 360 minutes for preliminary calcination.

[0089] (4) After the pre-sintering, the temperature in the heating furnace was raised from 600°C to 900°C over 60 minutes.

[0090] (5) Maintain the temperature in the heating furnace at 900°C for 60 minutes to perform main sintering.

[0091] (6) After the main firing, the temperature in the heating furnace was lowered from 900°C to 250°C over 130 minutes.

[0092] (7) The alumina crucible was taken out of the heating furnace at 250°C and allowed to cool in a dry atmosphere outside the furnace.

[0093] The calcined product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles A having a P2 type structure. The chemical composition, and particle sizes D10, D50, and D90 of the Na-containing oxide particles A are shown in Table 1 below.

[0094] 1.1.4 Ion exchange

[0095] (1) LiNO 3 and LiCl were weighed in a molar ratio of 50:50, and mixed with the above-mentioned Na-containing oxide particles A in a molar ratio of 10 times the minimum amount of Li required for ion exchange to obtain a mixture.

[0096] (2) Using an alumina crucible, ion exchange was performed in an air atmosphere at 280° C. for 1 hour to obtain a product including oxide particles containing Li.

[0097] (3) The salt remaining in the product is washed with pure water, and solid-liquid separation is performed by vacuum filtration to obtain a precipitate.

[0098] (4) The obtained precipitate was dried at 120° C. overnight to obtain the positive electrode active material according to Example 1.

[0099] 1.2 Comparative Example 1

[0100] 1.2.1 Preparation of precursor particles and composite particles

[0101] In the same manner as in Example 1, precursor particles and composite particles were obtained.

[0102] 1.2.2 Calcination of composite particles

[0103] The composite particles were placed in an alumina crucible and fired in an air atmosphere to obtain oxide particles containing Na and having a P2 type structure. The firing conditions were as described in the following (1) to (7).

[0104] (1) An alumina crucible containing the above-mentioned composite particles is placed in a heating furnace in an air atmosphere.

[0105] (2) The temperature in the heating furnace was raised from room temperature (25°C) to 600°C over 115 minutes.

[0106] (3) The temperature in the heating furnace is maintained at 600° C. for 360 minutes for preliminary calcination.

[0107] (4) After the preliminary firing, the temperature in the heating furnace was raised from 600°C to 950°C over 70 minutes.

[0108] (5) Maintain the temperature in the heating furnace at 950°C for 60 minutes to perform main sintering.

[0109] (6) After the main firing, the temperature in the heating furnace was lowered from 950°C to 250°C over 140 minutes.

[0110] (7) The alumina crucible was taken out of the heating furnace at 250°C and allowed to cool in a dry atmosphere outside the furnace.

[0111] The calcined product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles B having a P2 type structure. The chemical composition, and particle sizes D10, D50, and D90 of the Na-containing oxide particles B are shown in Table 1 below.

[0112] 1.2.3 Ion exchange

[0113] Ion exchange was performed under the same conditions as in Example 1, except that Na-containing oxide particles B were used instead of Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 1.

[0114] 1.3 Comparative Example 2

[0115] 1.3.1 Preparation of precursor particles and composite particles

[0116] In the same manner as in Example 1, precursor particles and composite particles were obtained.

[0117] 1.3.2 Calcination of composite particles

[0118] The composite particles were placed in an alumina crucible and fired in an air atmosphere to obtain an oxide containing Na and having a P2 type structure. The firing conditions were as described in the following (1) to (7).

[0119] (1) An alumina crucible containing the above-mentioned composite particles is placed in a heating furnace in an air atmosphere.

[0120] (2) The temperature in the heating furnace was raised from room temperature (25°C) to 600°C over 115 minutes.

[0121] (3) The temperature in the heating furnace is maintained at 600° C. for 360 minutes for preliminary calcination.

[0122] (4) After the preliminary firing, the temperature in the heating furnace was raised from 600°C to 1000°C over 80 minutes.

[0123] (5) Maintain the temperature in the heating furnace at 1000°C for 60 minutes to perform main sintering.

[0124] (6) After the main firing, the temperature in the heating furnace was lowered from 1000°C to 250°C over 150 minutes.

[0125] (7) The alumina crucible was taken out of the heating furnace at 250°C and allowed to cool in a dry atmosphere outside the furnace.

[0126] The calcined product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles C having a P2 type structure. The chemical composition, and particle sizes D10, D50, and D90 of the Na-containing oxide particles C are shown in Table 1 below.

[0127] 1.3.3 Ion exchange

[0128] Ion exchange was performed under the same conditions as in Example 1, except that Na-containing oxide particles C were used instead of Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 2.

[0129] 1.4 Comparative Example 3

[0130] 1.4.1 Preparation of precursor particles and composite particles

[0131] Precursor particles and composite particles were obtained in the same manner as in Example 1 except that the above-mentioned coarse particles were used as precursor particles.

[0132] 1.4.2 Calcination of composite particles

[0133] The composite particles were placed in an alumina crucible and fired in an air atmosphere to obtain an oxide containing Na and having a P2 type structure. The firing conditions were as described in the following (1) to (7).

[0134] (1) An alumina crucible containing the above-mentioned composite particles is placed in a heating furnace in an air atmosphere.

[0135] (2) The temperature in the heating furnace was raised from room temperature (25°C) to 600°C over 115 minutes.

[0136] (3) The temperature in the heating furnace is maintained at 600° C. for 360 minutes for preliminary calcination.

[0137] (4) After the preliminary firing, the temperature in the heating furnace was raised from 600°C to 1000°C over 80 minutes.

[0138] (5) Maintain the temperature in the heating furnace at 1000° C. for 1440 minutes to perform main sintering.

[0139] (6) After the main firing, the temperature in the heating furnace was lowered from 1000°C to 250°C over 150 minutes.

[0140] (7) The alumina crucible was taken out of the heating furnace at 250°C and allowed to cool in a dry atmosphere outside the furnace.

[0141] The calcined product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles D having a P2 type structure. The chemical composition, and particle sizes D10, D50, and D90 of the Na-containing oxide particles D are shown in Table 1 below.

[0142] 1.4.3 Ion exchange

[0143] Ion exchange was performed under the same conditions as in Example 1, except that Na-containing oxide particles D were used instead of Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 3.

[0144] 1.5 Comparative Example 4

[0145] 1.5.1 Preparation of precursor particles, composite particles and sintering of composite particles

[0146] After obtaining precursor particles and composite particles in the same manner as in Example 1, the composite particles were calcined and pulverized under the same conditions as in Example 1 to obtain Na-containing oxide particles E having a P2-type structure. The chemical composition, and particle sizes D10, D50, and D90 of the Na-containing oxide particles E are shown in Table 1 below.

[0147] 1.5.2 Ion Exchange

[0148] A positive electrode active material according to Comparative Example 4 was obtained by performing ion exchange under the same conditions as in Example 1, except that Na-containing oxide particles E were used instead of Na-containing oxide particles A and the ion exchange time was changed from 1 hour to 3 hours.

[0149] 1.6 Comparative Example 5

[0150] 1.6.1 Preparation of precursor particles, composite particles and sintering of composite particles

[0151] After obtaining precursor particles and composite particles in the same manner as in Comparative Example 3, the composite particles were calcined and pulverized under the same conditions as in Comparative Example 3 to obtain Na-containing oxide particles F having a P2-type structure. The chemical composition, and particle sizes D10, D50, and D90 of the Na-containing oxide particles F are shown in Table 1 below.

[0152] 1.6.2 Ion Exchange

[0153] A positive electrode active material according to Comparative Example 5 was obtained by performing ion exchange under the same conditions as in Example 1, except that Na-containing oxide particles F were used instead of Na-containing oxide particles A and the ion exchange time was changed from 1 hour to 3 hours.

[0154] 2. Evaluation of positive electrode active materials

[0155] 2.1 Elemental analysis

[0156] Elemental analysis was performed on each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5 to determine the chemical composition. The results are shown in Table 2 below.

[0157] 2.2 Particle size distribution determination

[0158] The particle size distribution of each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5 was measured to determine the particle diameters D10, D50, and D90. The results are shown in Table 2 below.

[0159] 2.2 Determination of crystal structure by X-ray diffraction

[0160] For each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5, X-ray diffraction measurement was performed using CuKα as a radiation source to obtain X-ray diffraction patterns. Figures 3 to 5 The X-ray diffraction patterns of Example 1 and Comparative Examples 1 to 5 are shown in FIG. Figures 3 to 5 As shown, it can be seen that the positive electrode active materials of Example 1 and Comparative Examples 1 to 5 all have an O2 type structure. The crystal structure contained in each positive electrode active material of Example 1 and Comparative Examples 1 to 5 and the ratio I2 / I1 of the X-ray diffraction peak intensity I2 from the (003) plane of the O3 type structure and the X-ray diffraction peak intensity I1 from the (002) plane of the O2 type structure are shown in Table 3 below.

[0161] 3. Preparation of battery cells for evaluation

[0162] A coin cell was produced using the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2. The steps for producing the coin cell are as follows.

[0163] (1) The positive electrode active material, acetylene black (AB) as a conductive aid, and polyvinylidene fluoride (PVdF) as a binder are weighed in a mass ratio of positive electrode active material: AB: PVdF = 85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode composite slurry. The positive electrode composite slurry is coated on an aluminum foil and vacuum dried at 120°C overnight to obtain a positive electrode as a laminate of a positive electrode active material layer and a positive electrode collector.

[0164] (2) TDDK-217 (manufactured by Daikin Corporation) was prepared as an electrolyte solution.

[0165] (3) As a negative electrode, a metal lithium foil is prepared.

[0166] (4) Using the positive electrode, electrolyte and negative electrode, a coin battery cell (CR2032) was produced.

[0167] 4. Evaluation of charge and discharge characteristics

[0168] Each coin cell was charged and discharged at 0.1C (1C=220 mA / g) in a constant temperature chamber maintained at 25°C in a voltage range of 2.0 to 4.8V to measure the discharge capacity. The results are shown in Table 3 below.

[0169] 5. Evaluation results

[0170] In the following Table 1, the main calcination temperature, chemical composition, particle size D10, D50 and D90 are shown for each of the Na-containing oxide particles A to F used in Example 1 and Comparative Examples 1 to 5. In addition, in the following Table 2, the ion exchange time, chemical composition, particle size D10, D50 and D90 are shown for each of the positive electrode active materials in Example 1 and Comparative Examples 1 to 5. In addition, in the following Table 3, the crystal structure contained in the positive electrode active material, I2 / I1 determined from the X-ray diffraction pattern, and the discharge capacity of the evaluated battery cell are shown for each of Example 1 and Comparative Examples 1 to 5.

[0171] [Table 1]

[0172] (Table 1

[0173]

[0174] [Table 2]

[0175] (Table 2)

[0176]

[0177] [Table 3]

[0178] (Table 3)

[0179]

[0180] As can be seen from the results shown in Tables 1 to 3, in Comparative Examples 1 to 3, since the main calcination temperature when preparing the Na-containing oxide particles having the P2 type structure was too high, the ion exchange after the main calcination was not sufficiently carried out, and Na remained in the Li-containing oxide particles. Among them, in Comparative Examples 2 and 3, since the particle size of the Na-containing oxide particles after the main calcination was excessively large, the ion exchange was difficult to proceed further, and the amount of residual Na in the Li-containing oxide particles increased. In Comparative Example 5, since the particle size of the Na-containing oxide particles after the main calcination was excessively large, Na remained in the Li-containing oxide particles after the ion exchange even if the ion exchange time was long. In Comparative Example 4, the particle size of the Na-containing oxide particles after the main calcination was small, and on the other hand, since the ion exchange time after the main calcination was too long, the O3 phase was generated in the Li-containing oxide after the ion exchange. Therefore, the Li-containing oxide particles involved in Comparative Examples 1 to 5 have a lower capacity as a positive electrode active material than the Li-containing oxide particles involved in Example 1. On the other hand, the Li-containing oxide particles according to Example 1 have appropriate chemical composition, particle size, and crystal structure, and as a result, have a high capacity as a positive electrode active material.

[0181] 6. Supplement

[0182] Furthermore, in the above-mentioned embodiments, the case where the precursor particles are obtained by the coprecipitation method is illustrated, but the precursor particles can also be obtained by methods other than this. In addition, in the above-mentioned embodiments, the case where the precursor particles and the Na source (Na2CO3) are mixed to obtain composite particles is illustrated, but the composite particles can also be obtained by methods other than this. In addition, in the above-mentioned embodiments, as the oxide containing Na with a P2 type structure and the oxide containing Li with an O2 type structure, an oxide with a prescribed chemical composition is illustrated, but the chemical composition of the oxide containing Na and the oxide containing Li is not limited thereto. For example, the oxide containing Na and the oxide containing Li can also be doped with an element M other than Mn, Ni and Co. For the element M, as described in the embodiment.

[0183] From the above results, it can be said that the Li-containing oxide particles satisfying the following characteristics (1) to (5) have a high capacity as a positive electrode active material.

[0184] (1) The Li-containing oxide particles have an O2 type structure.

[0185] (2) The Li-containing oxide particles have Li a Na b Mn x-p Ni y-q Coz-r M p+q+r O2 (wherein 0<a≤1.00, 0≤b<0.01, x+y+z=1 and 0≤p+q+r<0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W.) The chemical composition represented by the above-mentioned is shown in FIG.

[0186] (3) The particle size D50 of the Li-containing oxide particles is greater than 0 μm and less than 3.0 μm.

[0187] (4) The particle size D90 of the Li-containing oxide particles is 2.0 μm or more and 6.0 μm or less.

[0188] (5) The X-ray diffraction pattern of the Li-containing oxide particles satisfies 0≤I2 / I1≤0.5, wherein I1 is the X-ray diffraction peak intensity from the (002) plane of the O2-type structure, and I2 is the X-ray diffraction peak intensity from the (003) plane of the O3-type structure.

Claims

1. A positive electrode active material comprising Li-containing oxide particles, wherein the Li-containing oxide particles have an O2-type structure, and the Li-containing oxide particles have a Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 represents the chemical composition, where 0<a≤1.00, 0≤b<0.01, x+y+z=1 and 0≤p+q+r<0.17, the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo and W, the particle size D50 of the Li-containing oxide particles is greater than 0μm and less than 3.0μm, the particle size D90 of the Li-containing oxide particles is greater than 2.0μm and less than 6.0μm, the X-ray diffraction pattern of the Li-containing oxide particles satisfies 0≤I2 / I1≤0.5, the I1 is the X-ray diffraction peak intensity from the (002) plane of the O2 type structure, and the I2 is the X-ray diffraction peak intensity from the (003) plane of the O3 type structure.

2. The positive electrode active material according to claim 1, wherein The particle size D10 of the Li-containing oxide particles is greater than 0 μm and less than or equal to 2.0 μm.

3. A method for producing a positive electrode active material, comprising: obtaining precursor particles comprising at least one element of Mn, Ni and Co; The surfaces of the precursor particles are coated with a Na source to obtain composite particles; and the composite particles are subjected to main calcination to obtain oxide particles containing Na and having a P2 type structure; and exchanging Na ions of the Na-containing oxide particles for Li by bringing an ion exchange material into contact with the Na-containing oxide particles, thereby obtaining Li-containing oxide particles having an O2 type structure, wherein the main sintering temperature is greater than 700°C and less than 950°C, the particle size D50 of the Na-containing oxide particles is greater than 0 μm and less than 3.0 μm, the particle size D90 of the Na-containing oxide particles is greater than 2.0 μm and less than 6.0 μm, the ion exchange temperature is greater than the melting point of the ion exchange material and less than 300°C, and the ion exchange time is greater than 30 minutes and less than 3 hours.

4. The manufacturing method according to claim 3, wherein: The particle size D10 of the oxide particles containing Na is greater than 0 μm and less than or equal to 2.0 μm. 5 . A lithium ion secondary battery comprising a positive electrode active material layer, an electrolyte layer and a negative electrode active material layer, wherein the positive electrode active material layer comprises the positive electrode active material according to claim 1 or 2 .