Method for removing lithium metal separated out from negative electrode of pre-lithiated lithium ion battery

By adding lithium iodate or iodine element into the lithium-ion battery electrolyte as a lithium metal remover, combined with a stabilizer, the problem of lithium metal precipitation caused by excessive prelithiation of the negative electrode sheet is solved, and the cycle life and safety of the lithium-ion battery are improved. performance.

CN118800964APending Publication Date: 2024-10-18HEFEI GUOXUAN HIGH TECH POWER ENERGY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410850688.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

During the prelithiation process of existing lithium-ion batteries, it is easy to cause excessive prelithiation of the negative electrode, leading to the precipitation of lithium metal, reducing cycle life and posing safety risks, and there is a lack of effective removal methods.

Method used

The lithium metal remover lithium iodate or iodine is added to the basic electrolyte of a lithium-ion battery to convert the precipitated lithium metal into lithium ions through a spontaneous reaction to achieve recycling. Combined with a stabilizer, the stability of the remover is improved to avoid side effects. reaction.

Benefits of technology

It effectively avoids the precipitation of lithium metal caused by excessive prelithiation of the negative electrode, improves the cycle life and safety performance of lithium-ion batteries, and at the same time improves the first Coulomb efficiency and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004916762260000081
    Figure BDA0004916762260000081
  • Figure BDA0004916762260000091
    Figure BDA0004916762260000091
  • Figure FDA0004916762090000011
    Figure FDA0004916762090000011
Patent Text Reader

Abstract

The invention provides a method for removing lithium metal separated out from a negative electrode of a pre-lithiated lithium ion battery, and belongs to the technical field of lithium ion batteries. The method comprises the following steps: S1, adding a lithium metal remover into a basic electrolyte of the lithium ion battery to form a functionalized electrolyte; wherein the lithium metal remover is selected from lithium iodate and / or iodine elementary substance; s2, the lithium ion battery is charged and discharged, the lithium metal remover in the functionalized electrolyte and lithium metal separated out of the negative electrode of the lithium ion battery are subjected to spontaneous reaction, and the lithium metal separated out of the negative electrode is converted into lithium ions to enter the electrolyte. The method is simple to operate, and can ensure that the electrical performance of the lithium ion battery is improved through a pre-lithiation technology, and meanwhile, the cycle life is prevented from being shortened and even the safety risk is caused by lithium precipitation after excessive pre-lithiation of the negative electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a method for removing lithium metal precipitated from a negative electrode of a pre-lithiated lithium ion battery. Background Art

[0002] During the first charge and discharge process of lithium-ion batteries, the negative electrode consumes a large amount of active lithium due to the formation of a solid electrolyte interface (SEI), resulting in irreversible capacity loss. For example, graphite materials have an initial irreversible capacity loss of about 10%, while for emerging high-capacity silicon-based materials, the initial irreversible capacity loss is as high as 20%. On the other hand, the expansion of the negative electrode and the decomposition of the electrolyte during the cycle will also cause the loss of active lithium. Therefore, the pre-lithiation technology is used to use lithium metal and lithium compounds as external lithium sources, and to supplement additional active lithium in the negative electrode of lithium-ion batteries through chemical and electrochemical driving forces, in order to compensate for the loss of active lithium during SEI formation and the cycle process. This can achieve the following: (1) compensate for the loss of active lithium and improve the initial coulombic efficiency and energy density of the battery; (2) make the negative electrode expand in advance to avoid structural collapse and side reactions due to the large volume change of the negative electrode during subsequent cycle charge and discharge, thereby improving the cycle life of the battery.

[0003] However, if the pre-lithiation is uneven and the pre-lithiation rate is uncontrollable, it is easy to cause excessive pre-lithiation of the negative electrode sheet. Taking lithium metal rolling pre-lithiation as an example, the lithium foil is rolled on the negative electrode sheet, the lithium foil and the negative electrode sheet are short-circuited, and the electrons are spontaneously transferred from the lithium foil to the negative electrode. At the same time, lithium ions are generated and embedded in the negative electrode, that is, the potential difference between the lithium foil and the negative electrode sheet is used as the driving force to consume the lithium foil to achieve pre-lithiation of the negative electrode sheet. This pre-lithiation method is simple to operate and is generally applicable to various negative electrode active materials. However, the consumption rate of lithium foil and lithium ion transfer at different positions of the negative electrode sheet are uncontrollable, resulting in uneven pre-lithiation and uncontrollable pre-lithiation rate, and excessive pre-lithiation occurs. Over-pre-lithiation of negative electrode sheets is prone to lithium precipitation during the charge and discharge process, thereby reducing the cycle life of lithium-ion batteries and even causing safety risks. At present, there is no method that can effectively remove the lithium metal precipitated from the negative electrode. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery, so as to solve the problem in the prior art that excessive pre-lithiation and lithium precipitation on the negative electrode sheet will reduce the cycle life and safety performance of the lithium-ion battery.

[0005] In order to achieve the above object, according to one aspect of the present invention, a method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery is provided, comprising the following steps:

[0006] S1: adding a lithium metal remover to a base electrolyte of a lithium-ion battery to form a functionalized electrolyte; wherein the lithium metal remover is selected from lithium iodate and / or iodine;

[0007] S2: During the charge and discharge process of the lithium-ion battery, the lithium metal remover in the functionalized electrolyte reacts spontaneously with the lithium metal deposited at the negative electrode of the lithium-ion battery, and the lithium metal deposited at the negative electrode is converted into lithium ions and enters the electrolyte.

[0008] In the present invention, lithium metal remover lithium iodate or iodine is added to the electrolyte to spontaneously react with lithium metal produced by lithium precipitation due to excessive pre-lithiation on the negative electrode to generate iodide ions (I – ), iodide ion (I – ) can be oxidized to iodine element (I in solution) at the positive electrode. 3– ), iodine (I 3– ) reacts with lithium metal again to generate iodide ions (I – The method is simple to operate and can ensure that the electrical performance of lithium-ion batteries is improved through pre-lithiation technology while avoiding the reduction of cycle life or even safety risks caused by lithium deposition after excessive pre-lithiation of the negative electrode.

[0009] Furthermore, in step S1, a stabilizer of the first lithium metal remover and a stabilizer of the second lithium metal remover are added to the basic electrolyte of the lithium ion battery to form a functionalized electrolyte;

[0010] The stabilizer of the first lithium metal remover is alkyl-substituted ammonium iodide, and its chemical formula is Formula 1:

[0011]

[0012] In Formula 1, R1 is a C1 alkyl group or a C2 alkyl group, R2 is a C1 alkyl group or a C2 alkyl group, n is an integer between 0 and 2, m is an integer between 0 and 2, and n+m is 1 or 2;

[0013] The stabilizer of the second lithium metal remover is alkyl-substituted ammonium iodide, and its chemical formula is Formula 2:

[0014]

[0015] In formula 2, R1 is a C1 alkyl group or a C2 alkyl group, R2 is a C3-C5 alkyl group, R3 is a C3-C5 alkyl group, x is an integer between 0 and 4, y is an integer between 0 and 4, and x+y is 3 or 4.

[0016] The present invention further adds a stabilizer of the remover to the base electrolyte of the lithium ion battery. Since the lithium metal remover lithium iodate (or iodine element, which is in the solution as I 3– In the process of recycling and removing lithium metal, the electrolyte is I 3– ,I –There are two valence states, and these two valence states will cause side reactions in the electrolyte that affect the electrochemical performance of the lithium ion battery. In order to avoid the above side reactions and ensure that the above two valence states can stably exist in the electrolyte and play their role in removing lithium metal, the present invention adds two different stabilizers to the basic electrolyte. The stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover can respectively react with the generated iodide ions (I – ), iodine (I 3– ) complexation, thereby improving the stability of the lithium metal remover lithium iodate (or iodine element) in the electrolyte, and the above two stabilizers will not react with the components in the electrolyte, and only play the role of complexing and stabilizing the lithium metal remover; for this reason, the present invention selects the following two compounds as stabilizers, and the use of the stabilizer can improve the stability effect of the above two removers to be more conducive to the lithium removal effect.

[0017] Further, the stabilizer of the first lithium metal remover is selected from one or more of methylammonium iodide, methylethylammonium iodide and dimethylammonium iodide.

[0018] Further, the stabilizer of the second lithium metal remover is selected from one or more of ethyltripropylammonium iodide, methylpropyldibutylammonium iodide and tetrapentylammonium iodide.

[0019] The two stabilizers selected in the present invention can form a stable complex with the two iodide ions.

[0020] Furthermore, in step S1, the mass percentage of the lithium metal remover added to the basic electrolyte is 0.5% to 1.5%; preferably, the mass percentage of the lithium metal remover added to the basic electrolyte is 0.7% to 1.2%.

[0021] Furthermore, in step S1, the stabilizer of the first lithium metal remover is added to the basic electrolyte in an amount of 0.5% to 1.7% by mass.

[0022] Furthermore, the stabilizer of the first lithium metal remover is added in an amount of 0.7% to 1.3% by mass in the basic electrolyte.

[0023] Furthermore, in step S1, the stabilizer of the second lithium metal remover is added to the basic electrolyte in an amount of 0.6% to 2.5% by mass.

[0024] Furthermore, the stabilizer of the second lithium metal remover is added in an amount of 0.8% to 2.0% by mass in the basic electrolyte.

[0025] The specific ratio selected in the present invention is related to the content of the lithium metal remover; a certain amount of lithium metal remover will produce two different valence states (I –and I 3– ), in order to complex the two different valence states, the two stabilizer solutions should have a specific and reasonable addition ratio; the above content can improve the stability of the lithium metal remover in the electrolyte.

[0026] Furthermore, in step S1, the total added mass percentage of the lithium metal remover, the stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover in the basic electrolyte is less than or equal to 5%.

[0027] The present invention controls the content of the above three additives within 5%, which does not affect the properties of the electrolyte and can further improve the stability and recycling effect of the lithium metal remover and the effect of removing lithium deposition.

[0028] Furthermore, the negative electrode active material of the lithium-ion battery is selected from one or more of graphite, hard carbon, silicon, silicon oxide, silicon carbide, hard carbon-graphite, silicon-graphite, silicon oxide-graphite and silicon carbide-graphite.

[0029] The lithium removal method of the present invention is more suitable for the pre-lithiation lithium precipitation phenomenon of the above-mentioned negative electrode material.

[0030] Furthermore, in step S1, the solvent of the basic electrolyte includes a carbonate solvent; preferably, the solvent of the basic electrolyte is selected from one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate and diethyl carbonate.

[0031] Furthermore, the lithium salt in the electrolyte is selected from one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium perchlorate.

[0032] Furthermore, the positive electrode active material of the lithium-ion battery is selected from one or more of lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium cobalt oxide, lithium manganese iron phosphate, lithium nickel cobalt aluminum oxide, and lithium nickel manganese oxide.

[0033] The technical solution of the present invention is applied to provide a method for removing lithium from the negative electrode of a lithium ion battery. The method is to add a lithium metal remover, lithium iodate or iodine, to the basic electrolyte. The remover can spontaneously react with the lithium metal produced by lithium precipitation due to excessive pre-lithiation on the negative electrode to generate iodide ions. The iodine ions can be oxidized to iodine on the positive electrode. The iodine continues to react with lithium metal to generate iodide ions, and recycling is achieved. The method of the present invention is simple to operate, and can ensure that the electrical performance of the lithium ion battery is improved by the pre-lithiation technology, while avoiding the reduction of the cycle life or even the safety risk caused by lithium precipitation after excessive pre-lithiation of the negative electrode. DETAILED DESCRIPTION

[0034] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0035] Lithium metal rolling pre-lithiation is to roll lithium foil onto the negative electrode sheet. The lithium foil and the negative electrode sheet are short-circuited, and electrons are spontaneously transferred from the lithium foil to the negative electrode. At the same time, lithium ions are generated and embedded in the negative electrode, that is, the potential difference between the lithium foil and the negative electrode sheet is used as the driving force to consume the lithium foil to achieve pre-lithiation of the negative electrode sheet. This pre-lithiation method is simple to operate and is generally applicable to various negative electrode active materials. However, the consumption rate of lithium foil and lithium ion transfer at different positions of the negative electrode sheet are uncontrollable, resulting in uneven pre-lithiation and uncontrollable pre-lithiation rate, resulting in excessive pre-lithiation. Over-pre-lithiation of negative electrode sheets is prone to precipitating lithium metal during the charge and discharge process, thereby reducing the cycle life of lithium-ion batteries and even causing safety risks.

[0036] In order to improve the cycle life and safety performance of pre-lithiated lithium-ion batteries, the inventors have found through a large number of experimental studies that when lithium metal is deposited during the charge and discharge process of a lithium battery, if the deposited lithium metal can be converted into lithium ions through a chemical reaction in time so that it enters the electrolyte from the surface of the negative electrode sheet, the problem that the lithium metal deposited at the negative electrode affects the battery cycle life and safety risks can be solved; therefore, the present invention innovatively proposes a method for removing the lithium metal deposited at the negative electrode of a pre-lithiated lithium-ion battery, comprising the following steps:

[0037] S1: adding a lithium metal remover to a base electrolyte of a lithium-ion battery to form a functionalized electrolyte; wherein the lithium metal remover is selected from lithium iodate and / or iodine;

[0038] S2: During the charge and discharge process of the lithium-ion battery, the lithium metal remover in the functionalized electrolyte reacts spontaneously with the lithium metal deposited at the negative electrode of the lithium-ion battery, and the lithium metal deposited at the negative electrode is converted into lithium ions and enters the electrolyte.

[0039] In the present invention, lithium metal remover lithium iodate or iodine is added to the electrolyte to spontaneously react with lithium metal produced by lithium precipitation due to excessive pre-lithiation on the negative electrode to generate iodide ions (I – ), iodide ion (I – ) can be oxidized to iodine element (I in solution) at the positive electrode. 3– ), iodine (I 3– ) reacts with lithium metal again to generate iodide ions (I – ), and the reaction formula is as follows. The method is simple to operate, and can ensure that the electrical performance of lithium-ion batteries is improved through pre-lithiation technology, while avoiding the reduction of cycle life and even safety risks caused by lithium precipitation after excessive pre-lithiation of the negative electrode.

[0040] 6Li+IO3 – =I– +3Li2O (Formula-1)

[0041] 2Li+I 3– =2Li + +3I – (Formula-2)

[0042] 2Li + +3I – +2FePO4=2LiFePO4+I 3– (Formula-3)

[0043] In order to ensure the stability of the lithium metal remover in the electrolyte and avoid the side reaction of the added remover which affects the effect of the electrolyte itself, the present invention further adds a stabilizer of the remover to the basic electrolyte of the lithium ion battery. 3– In the process of recycling and removing lithium metal, the electrolyte is I 3– ,I – There are two valence states, and these two valence states will cause side reactions in the electrolyte that affect the electrochemical performance of the lithium ion battery. In order to avoid the above side reactions and ensure that the above two valence states can stably exist in the electrolyte and play their role in removing lithium metal, the present invention adds two different stabilizers to the basic electrolyte. The stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover can respectively react with the generated iodide ions (I – ), iodine (I 3– ) complexation, thereby improving the stability of the lithium metal remover lithium iodate (or iodine element) in the electrolyte, and the above two stabilizers will not react with the components in the electrolyte, and only play the role of complexing and stabilizing the lithium metal remover; for this reason, the present invention selects the following two compounds as stabilizers, and the use of the stabilizer can improve the stability effect of the above two removers to be more conducive to the lithium removal effect.

[0044] The stabilizer of the first lithium metal remover is alkyl-substituted ammonium iodide, and its chemical formula is Formula 1:

[0045]

[0046] In Formula 1, R1 is a C1 alkyl group or a C2 alkyl group, R2 is a C1 alkyl group or a C2 alkyl group, n is an integer between 0 and 2, m is an integer between 0 and 2, and n+m is 1 or 2;

[0047] The stabilizer of the second lithium metal remover is alkyl-substituted ammonium iodide, and its chemical formula is Formula 2:

[0048]

[0049] In formula 2, R1 is a C1 alkyl group or a C2 alkyl group, R2 is a C3-C5 alkyl group, R3 is a C3-C5 alkyl group, x is an integer between 0 and 4, y is an integer between 0 and 4, and x+y is 3 or 4.

[0050] Specifically, the stabilizer of the first lithium metal remover is selected from one or more of methylammonium iodide, methylethylammonium iodide and dimethylammonium iodide; the stabilizer of the second lithium metal remover is selected from one or more of ethyltripropylammonium iodide, methylpropyldibutylammonium iodide and tetrapentylammonium iodide. The inventors have noticed that when the above two specific stabilizers are used, the stabilizing effect on the lithium metal remover is relatively good.

[0051] In order to further ensure the removal effect of the lithium metal remover on the precipitated lithium metal, the present invention sets the added mass percentage of the lithium metal remover in the basic electrolyte to 0.5% to 1.5%. Within this range, any value of 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5% or any range between two values ​​can be used; preferably 0.7% to 1.2%. If the addition amount of the above lithium metal remover is less than 0.5%, the removal effect on the precipitated lithium metal is not good, or if it is greater than 1.5%, the viscosity of the electrolyte will increase and the conductivity of the electrolyte will decrease.

[0052] The above two specific ratios of the two stabilizers used in the present invention are related to the content of the lithium metal remover; specifically, a certain amount of lithium metal remover will produce two different valence states (I – and I 3– ), in order to complex the two different valence states, the two stabilizers should also have a specific and reasonable addition ratio.

[0053] In order to further improve the lithium metal remover in the electrolyte a valence state (I – ) stability, the present invention sets a specific ratio for the amount of stabilizer added; the two are complexed to form a complex with a stable structure; the added mass percentage of the stabilizer of the first lithium metal remover in the basic electrolyte is 0.5% to 1.7%, within this range, any value of 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7% or any range between two values ​​can be used, preferably 0.7% to 1.3%. Beyond the above range, the stabilization effect is not good or the viscosity of the electrolyte is increased and the conductivity of the electrolyte is reduced.

[0054] Similarly, in order to further improve another valence state (I 3–) stability, the present invention sets a specific ratio for the amount of stabilizer added; the two are complexed to form a complex with a stable structure; the added mass percentage of the stabilizer of the second lithium metal remover in the basic electrolyte is 0.6% to 2.5%, within this range, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5% or any range between two values ​​can be used, preferably 0.8% to 2.0%. Beyond the above range, the stabilization effect is not good or the viscosity of the electrolyte is increased and the conductivity of the electrolyte is reduced.

[0055] In order to further improve the stability and recycling effect of the lithium metal remover and the effect of removing lithium precipitation, and at the same time not affect the electrochemical properties of the electrolyte itself, it is necessary to make specific requirements on the amount of the above three external additives; therefore, the total added mass percentage of the lithium metal remover, the stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover added in the method of the present invention in the basic electrolyte is less than or equal to 5%; the ratio can be set to any value of 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5% or any range between the two, and further preferably 1% to 5%, 2% to 5%, 2.5% to 4.5%. When the addition ratio is higher than 5%, the viscosity of the electrolyte will increase and the conductivity of the electrolyte will decrease.

[0056] In order to give full play to the role of the electrolyte in the method of the present invention, the solvent of the basic electrolyte is a carbonate solvent; preferably one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate and diethyl carbonate, wherein the charge and discharge effect is better when multiple compounds are used, for example, a compound of ethylene carbonate, propylene carbonate and ethyl methyl carbonate, or a compound of ethylene carbonate, propylene carbonate, ethyl methyl carbonate and diethyl carbonate.

[0057] The lithium salt in the electrolyte of the present invention is selected from one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium bis(oxalatoborate), lithium difluorooxalatoborate and lithium perchlorate.

[0058] The negative electrode active material of the lithium ion battery of the present invention is selected from one or more of graphite, hard carbon, silicon, silicon oxide, silicon carbide, hard carbon-graphite, silicon-graphite, silicon oxide-graphite and silicon carbide-graphite.

[0059] The positive electrode active material of the lithium ion battery of the present invention is selected from one or more of lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium manganese oxide, lithium cobalt oxide, lithium manganese iron phosphate, lithium nickel cobalt aluminum oxide, and lithium nickel manganese oxide.

[0060] The selection of the electrolyte solvent, negative electrode active material, positive electrode active material and electrolyte of the present invention can be selected by those skilled in the art from the prior art.

[0061] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0062] Example 1

[0063] The graphite negative electrode sheet is pre-lithiated by double-sided rolling using 20μm lithium foil, and then the pre-lithiated graphite negative electrode sheet, lithium iron phosphate positive electrode sheet, and separator are assembled into a bare battery cell using a lamination process. The bare battery cell is encapsulated with an aluminum plastic film and injected with an electrolyte for 48 hours to obtain a pre-lithiated soft-pack battery. Among them, the solvent used in the electrolyte is ethylene carbonate, propylene carbonate, and ethyl methyl carbonate, the lithium salt is lithium hexafluorophosphate, the additive is vinylene carbonate, and the mass percentage of iodine added as a lithium metal remover is 0.7%; the product number is A1.

[0064] Example 2

[0065] The graphite negative electrode sheet is pre-lithiated by double-sided rolling using a 20μm lithium foil, and then the pre-lithiated graphite negative electrode sheet, lithium iron phosphate positive electrode sheet, and separator are assembled into a bare battery cell using a lamination process. The bare battery cell is encapsulated with an aluminum plastic film and injected with an electrolyte for 48 hours to obtain a pre-lithiated soft-pack battery. Among them, the solvents used in the electrolyte are ethylene carbonate, propylene carbonate, and ethyl methyl carbonate, the lithium salt is lithium hexafluorophosphate, the additive is vinylene carbonate, the mass percentage of iodine added as a lithium metal remover is 0.7%, the amount of methyl ammonium iodide (NH3CH3I) added as a stabilizer of the first lithium metal remover is 0.7%, and the mass percentage of ethyl tripropyl ammonium iodide (NC2H5(CH3CH2CH2)3I) added as a stabilizer of the second lithium metal remover is 0.8%, and the product number is A2.

[0066] Example 3

[0067] The silicon oxide-graphite negative electrode sheet was pre-lithiated by double-sided rolling using 20μm lithium foil, and then the pre-lithiated silicon oxide-graphite negative electrode sheet, lithium iron phosphate positive electrode sheet, and separator were assembled into a bare cell using a lamination process. The bare cell was encapsulated with an aluminum-plastic film and injected with electrolyte for 48 hours to obtain a pre-lithiated soft-pack battery. Among them, the solvents used in the electrolyte are ethylene carbonate, propylene carbonate, ethyl methyl carbonate, and diethyl carbonate, the lithium salts are lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalatoborate, the additives are vinylene carbonate, fluoroethylene carbonate, and 1,3-propylene sulfone, the mass percentage of iodine added as the lithium metal remover is 0.5%, the mass percentage of lithium iodate added is 0.5%, the amount of methylethylammonium iodide (NH2CH3C2H5I), the stabilizer of the first lithium metal remover, added in an amount of 1.2%, and the amount of methylpropyldibutylammonium iodide (NCH3CH3CH2CH2(CH3CH2CH2CH2)2I), the stabilizer of the second lithium metal remover, added in an amount of 1.2%, and the product number is A3.

[0068] Example 4

[0069] The silicon carbide-graphite negative electrode sheet was pre-lithiated by double-sided rolling using 20μm lithium foil, and then the pre-lithiated silicon oxide-graphite negative electrode sheet, lithium iron phosphate positive electrode sheet, and separator were assembled into a bare cell using a lamination process. The bare cell was encapsulated with an aluminum-plastic film and injected with electrolyte for 48 hours to obtain a pre-lithiated soft-pack battery. Among them, the solvents used in the electrolyte are ethylene carbonate, propylene carbonate, ethyl methyl carbonate, and diethyl carbonate, the lithium salts are lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, and lithium difluorooxalatoborate, the additives are vinylene carbonate, fluoroethylene carbonate, and 1,3-propylene sulfone, the lithium metal remover lithium iodate added in an amount of 1.2% by mass, the first lithium metal remover stabilizer dimethylammonium iodide (NH2(CH3)2I) added in an amount of 1.3% by mass, the second lithium metal remover stabilizer tetrapentylammonium iodide (N(CH3CH2CH2CH2CH2)4I) added in an amount of 2.0% by mass, and the product number is A4.

[0070] Example 5

[0071] The difference between Example 5 and Example 2 is that the amounts of the lithium metal remover, the stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover added to the electrolyte are 0.5%, 0.5% and 0.6% respectively, and the other processes are the same, numbered A5.

[0072] Example 6

[0073] The difference between Example 6 and Example 2 is that the mass percentage of iodine added as a lithium metal remover is 1.5%, the mass percentage of dimethylammonium iodide (NH2(CH3)2I) added as the stabilizer of the first lithium metal remover is 1.7%, and the mass percentage of ethyltripropylammonium iodide (NC2H5(CH3CH2CH2)3I) added as the stabilizer of the second lithium metal remover is 1.8%. The other processes are the same and are numbered A6.

[0074] Example 7

[0075] The difference between Example 7 and Example 2 is that the mass percentage of iodine added as a lithium metal remover is 1.2%, the mass percentage of dimethylammonium iodide (NH2(CH3)2I) added as the stabilizer of the first lithium metal remover is 1.3%, and the mass percentage of tetrapentylammonium iodide (N(CH3CH2CH2CH2CH2)4I) added as the stabilizer of the second lithium metal remover is 2.5%. The other processes are the same and are numbered A7.

[0076] Comparative Example 8

[0077] The difference between Comparative Example 8 and Example 2 is that the amounts of the lithium metal remover, the stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover added to the electrolyte are 0.4%, 0.4% and 0.5% respectively, and the other processes are the same, numbered A8.

[0078] Comparative Example 9

[0079] The difference between Comparative Example 9 and Example 2 is that the mass percentage of iodine added as a lithium metal remover is 1.6%, the mass percentage of dimethylammonium iodide (NH2(CH3)2I) added as the stabilizer of the first lithium metal remover is 1.8%, and the mass percentage of tetrapentylammonium iodide (N(CH3CH2CH2CH2CH2)4I) added as the stabilizer of the second lithium metal remover is 2.7%. The total addition amount is 6.1%, and the other processes are the same, numbered A9.

[0080] Comparative Example 1

[0081] The difference between Comparative Example 1 and Examples 2-4 is that no lithium metal remover, first stabilizer and second stabilizer are added to the basic electrolyte; other processes are the same: the same pre-lithiation negative electrode sheet, positive electrode sheet and separator are made into the first comparison group of soft-pack batteries according to the same process, corresponding to A2-A4, and the product numbers are B2-B4.

[0082] Comparative Example 2

[0083] The difference between Comparative Example 2 and Examples 2-4 is that no lithium metal remover, first stabilizer and second stabilizer are added to the basic electrolyte, and the negative electrode sheet is not pre-lithiated; other processes are the same: the same positive electrode sheet and separator are used to make the second comparison group of soft-pack batteries according to the same procedure, corresponding to A2-A4, and the product numbers are C2-C4.

[0084] The lithium removal method of the present invention is for pre-lithiation and lithium precipitation of negative electrode materials of lithium ion batteries, such as the graphite negative electrode sheet of Example 2, the silicon oxide-graphite negative electrode sheet of Example 3 and the silicon carbide-graphite negative electrode sheet of Example 4. These three negative electrode materials are respectively subjected to pre-lithiation + lithium removal operation (Examples 2-4), pre-lithiation + no lithium removal operation (Comparative Example 1) and no pre-lithiation operation (Comparative Example 2), and the lithium ion battery products of the above-mentioned embodiments and comparative examples are subjected to performance tests.

[0085] Battery performance test: 3 batteries numbered A1-A9, B2-B4, and C2-C4 were taken for formation and capacity separation, and the first coulombic efficiency of the battery was calculated; a cycle performance test of up to 2000 cycles was carried out, and the results are shown in Table 1.

[0086] Thermal runaway test: 6 batteries numbered A1-A9, B2-B4, and C2-C4 were taken for each cycle for 500 cycles, and then thermal runaway tests were carried out in accordance with GB / T36276-2018. The passing index was no explosion or fire. The passing rate is shown in Table 1.

[0087] Table 1

[0088]

[0089]

[0090] From the test results in Table 1, it can be seen that the first coulombic efficiency and early cycle stability of the batteries of Examples 1-7, Comparative Examples 8-9, and Comparative Example 1, which were pre-lithiated by calendering, were significantly improved compared to the control group of batteries that were not pre-lithiated in Comparative Example 2. However, due to the shortcomings of the calendering pre-lithiation technology, such as uneven pre-lithiation and uncontrollable pre-lithiation rate, it is easy to cause local excessive pre-lithiation of the negative electrode sheet, which in turn leads to lithium deposition and capacity drop during the battery cycle of Comparative Example 1; in addition, lithium deposition can also cause safety hazards and lead to thermal runaway.

[0091] The first coulombic efficiency of the three negative electrode materials of Examples 2-4 of the present invention compared with the three negative electrode materials of graphite, silicon oxide-graphite, and silicon carbide-graphite negative electrode of Comparative Example 2 was improved by 4-5% (comparison of A2 and C2 graphite negative electrodes), 8-9% (comparison of A3 and C3 silicon oxide-graphite negative electrodes), and 7-8% (comparison of A4 and C4 silicon carbide-graphite negative electrodes), respectively. The number of cycles of C2 increased from 900 to 2000, and the number of cycles of C3 increased from 800 to 1500. The cycle stability was all improved by more than 100%, the capacity did not change, and there was no capacity diving phenomenon. All thermal runaways passed. It shows that after the pre-lithiation lithium precipitation + lithium removal operation of the present invention, the electrochemical performance of the lithium-ion battery without pre-lithiation has been significantly improved, and there will be no phenomenon that is not conducive to the electrochemical performance of lithium ions.

[0092] Comparative Example 1 (B2, B3, B4) is a battery with a negative electrode pre-lithiation after calendering. Compared with Comparative Example 2 (C2, C3, C4), the first coulombic efficiency of the negative electrode materials graphite, silicon oxide-graphite, and silicon carbide-graphite negative electrode batteries is increased by 5% (B2 and C2 graphite negative electrode comparison), 9% (B3 and C3 silicon oxide-graphite negative electrode comparison), 8% (B4 and C4 silicon carbide-graphite negative electrode comparison), and the battery capacity retention rate is improved in the early stage of the cycle, but the capacity diving phenomenon occurs during the cycle, and the thermal runaway pass rate is only 2 / 6 to 4 / 6. It shows that the pre-lithiation operation can improve the performance of lithium-ion batteries while also causing the above-mentioned disadvantages.

[0093] By comparing Examples 1-7, Comparative Examples 8-9 and Comparative Example 1, it can be seen that after adding a lithium metal remover to the base electrolyte, the first coulomb efficiency of the present invention remains basically unchanged and a stable cycle can be maintained, which is a relatively good effect; and in terms of the thermal runaway pass rate, Examples 1-4, Examples 5-7, and Comparative Example 9 all pass, indicating that their safety performance is better, while 2 / 6 to 4 / 6 of the batteries in Comparative Example 1 still fail to meet the thermal runaway requirements. The above shows that the lithium removal method of the present invention not only maintains the performance improvement after pre-lithiation, but also solves the defect of easy capacity drop in Comparative Example 1.

[0094] The above experimental results fully verify that the present invention adopts the addition of lithium metal remover lithium iodate and / or iodine to the basic electrolyte, which can remove the lithium metal precipitated on the negative electrode sheet during the cycle due to excessive pre-lithiation, and can ensure the improvement of coulombic efficiency while improving long-term cycle stability and eliminating safety hazards; after further adding the stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover, the coulombic efficiency and thermal runaway can be further improved.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery, characterized in that: The method comprises the following steps: S1: adding a lithium metal remover to a base electrolyte of a lithium-ion battery to form a functionalized electrolyte; wherein the lithium metal remover is selected from lithium iodate and / or iodine; S2: The lithium-ion battery undergoes a charge and discharge process, the lithium metal remover in the functionalized electrolyte and the lithium metal precipitated from the negative electrode of the lithium-ion battery undergo a spontaneous reaction, and the lithium metal precipitated from the negative electrode is converted into lithium ions and enters the electrolyte.

2. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to claim 1, characterized in that: In step S1, a stabilizer of the first lithium metal remover and a stabilizer of the second lithium metal remover are added to the basic electrolyte of the lithium ion battery to form a functionalized electrolyte; The stabilizer of the first lithium metal remover is alkyl-substituted ammonium iodide, and its chemical formula is Formula 1: In formula 1, R 1 is C1 alkyl or C2 alkyl, R 2 is a C1 alkyl group or a C2 alkyl group, and n is an integer between 0 and 2, m is an integer between 0 and 2, and n+m is 1 or 2; The stabilizer of the second lithium metal remover is alkyl-substituted ammonium iodide, and its chemical formula is Formula 2: In formula 2, R 1 is C1 alkyl or C2 alkyl, R 2 is a C3-C5 alkyl group, R 3 is a C3-C5 alkyl group, x is an integer between 0 and 4, y is an integer between 0 and 4, and x+y is 3 or 4.

3. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to claim 2, characterized in that: The stabilizer of the first lithium metal remover is selected from one or more of methylammonium iodide, methylethylammonium iodide and dimethylammonium iodide.

4. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to claim 2 or 3, characterized in that: The stabilizer of the second lithium metal remover is selected from one or more of ethyltripropylammonium iodide, methylpropyldibutylammonium iodide and tetrapentylammonium iodide.

5. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to any one of claims 1 to 4, characterized in that: In step S1, the lithium metal remover is added to the basic electrolyte in an amount of 0.5% to 1.5% by mass; preferably, the lithium metal remover is added to the basic electrolyte in an amount of 0.7% to 1.2% by mass.

6. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to any one of claims 2 to 5, characterized in that: In step S1, the added mass percentage of the stabilizer of the first lithium metal remover in the basic electrolyte is 0.5% to 1.7%; preferably, the added mass percentage of the stabilizer of the first lithium metal remover in the basic electrolyte is 0.7% to 1.3%.

7. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to any one of claims 2 to 6, characterized in that: In step S1, the added mass percentage of the stabilizer of the second lithium metal remover in the basic electrolyte is 0.6% to 2.5%; preferably, the added mass percentage of the stabilizer of the second lithium metal remover in the basic electrolyte is 0.8% to 2.0%.

8. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to any one of claims 2 to 7, characterized in that: In step S1, the total added mass percentage of the lithium metal remover, the stabilizer of the first lithium metal remover and the stabilizer of the second lithium metal remover in the basic electrolyte is less than or equal to 5%.

9. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to any one of claims 2 to 8, characterized in that: The negative electrode active material of the lithium ion battery is selected from one or more of graphite, hard carbon, silicon, silicon oxide, silicon carbide, hard carbon-graphite, silicon-graphite, silicon oxide-graphite and silicon carbide-graphite.

10. The method for removing lithium metal precipitated from the negative electrode of a pre-lithiated lithium-ion battery according to any one of claims 1 to 9, characterized in that: The solvent of the basic electrolyte includes a carbonate solvent; preferably, the solvent of the basic electrolyte is selected from one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate and diethyl carbonate.

Citation Information

Patent Citations

  • Battery electrolyte containing amine iodide additive and preparation method of battery electrolyte

    CN112768768A

  • Isolating membrane and preparation method thereof, secondary battery, battery module, battery pack and electric device

    CN115810863A

  • Electrolyte for improving cycle performance of battery and aqueous zinc ion battery

    CN117059911A

  • Electrolyte for lithium secondary battery

    JP2000058120A