Non-aqueous electrolyte of high-nickel positive electrode lithium ion battery and lithium ion battery containing electrolyte

By using unsaturated phosphorus-containing silicone esters and polycyclic sulfate ester additives in lithium-ion batteries, combined with the non-aqueous electrolyte of lithium hexafluorophosphate, the problems of short cycle life and poor high-temperature storage performance of lithium-ion batteries are solved, and the electrolyte solution is realized The suppression of decomposition and improvement of the thermal stability of the SEI film significantly improve the cycle and storage performance of the battery.

CN118800967APending Publication Date: 2024-10-18CHANGSHU CHANGJI CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411018301.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing lithium-ion batteries have short cycle life, poor high-temperature storage performance, and the electrolyte decomposes under high temperatures and high voltages, causing battery bloating.

Method used

Unsaturated phosphorus-containing silicon-based esters and polycyclic sulfate esters are used as additives, combined with lithium hexafluorophosphate, to form a non-aqueous electrolyte, which is used in high-nickel positive lithium-ion batteries to inhibit electrolyte decomposition and improve the thermal stability of the SEI film.

Benefits of technology

It significantly improves the cycle life and high-temperature storage performance of the battery, suppresses the gas problem caused by the decomposition of electrolyte in the battery under high voltage and high temperature, and improves the cycle and storage performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004966402610000033
    Figure BDA0004966402610000033
  • Figure BDA0004966402610000041
    Figure BDA0004966402610000041
  • Figure BDA0004966402610000042
    Figure BDA0004966402610000042
Patent Text Reader

Abstract

The invention belongs to the technical field of lithium ion batteries, provides a high-nickel positive electrode lithium ion battery non-aqueous electrolyte and a lithium ion battery containing the electrolyte, and solves the problems that the lithium ion battery in the prior art is short in cycle life and poor in high-temperature storage performance, and the electrolyte is decomposed in the high-temperature and high-voltage storage process to cause battery gas expansion. The non-aqueous electrolyte of the high-nickel positive electrode lithium ion battery provided by the invention comprises a lithium salt electrolyte, a non-aqueous solvent, an unsaturated phosphorus-containing silicon-based ester additive and a polycyclic sulfate additive, the invention also provides a technical scheme of a lithium ion battery containing the non-aqueous electrolyte, so that the problems in the prior art are well solved, and the non-aqueous electrolyte can be applied to the field of high-nickel positive electrode lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a high-nickel positive electrode lithium ion battery non-aqueous electrolyte and a lithium ion battery containing the electrolyte. Background Art

[0002] With the development of new energy vehicles, the driving range of vehicles has become one of the most important concerns of most car owners. Therefore, it is particularly urgent to improve the energy density of lithium-ion batteries. High nickel materials, such as (LiNi 0.8 Co 0.1 Mn 0.1 O2, referred to as NCM811), as a positive electrode material, has attracted widespread attention due to its advantages such as high specific capacity and low cost, and has become one of the positive electrode materials with the greatest potential to improve the energy density of lithium-ion batteries.

[0003] Although increasing the cut-off voltage can significantly increase the capacity of the battery, a higher voltage (≥4.4V) will cause the electrolyte to decompose and produce gas, which will deteriorate the battery performance; and high-nickel cathode materials also have problems such as poor structural stability, transition metal ion dissolution, lattice oxygen release, and high residual moisture on the surface of the material, which will affect the storage and cycle performance of the battery. Therefore, the development of high-nickel lithium-ion battery materials with excellent comprehensive performance is of great practical significance to the development of lithium-ion new energy.

[0004] For example, Chinese patent CN111106384B discloses an electrolyte matching a high-nickel positive electrode lithium ion battery, the electrolyte containing a lithium salt, an organic solvent, an additive A and an additive B, wherein the additive A is a borate compound and the additive B is a phosphate compound; the electrolyte is applied to a high-nickel positive electrode lithium ion battery, and its cut-off operating voltage is 4.4 to 4.5 V, the operating temperature can reach 55°C, and it has good high temperature and high pressure cycle resistance; however, the phosphate containing three cyano groups has a large film formation resistance on the positive electrode surface, which is not conducive to low temperature performance, and must be used in combination with an additive that reduces internal resistance. At the same time, the phosphate compound is a high-viscosity liquid or solid, which is difficult to purify and has high production costs. Chinese patent application CN115775908A discloses a high-nickel ternary lithium-ion battery electrolyte and a lithium-ion battery containing the electrolyte. The electrolyte comprises a non-aqueous organic solvent, a lithium salt and an additive. The additive comprises at least one type of low-impedance silicon-containing additive A and one type of silane-based unsaturated positive electrode additive B with higher impedance. The combination of the two types of silicon-containing additives can improve the cycle stability and high and low temperature performance of the battery system and inhibit the DCR growth of the battery during use. However, due to the high film-forming internal resistance of the additive B, it is also necessary to use it in combination with a variety of lithium salts (such as lithium difluorophosphate) that reduce the internal resistance, which increases the difficulty of preparing the electrolyte and increases the cost of use. Summary of the invention

[0005] One of the technical problems to be solved by the present invention is that the lithium ion batteries in the prior art have a short cycle life and poor high-temperature storage performance. The battery has a problem of battery bloating caused by electrolyte decomposition during high-temperature and high-voltage storage. A non-aqueous electrolyte for a high-nickel positive electrode lithium ion battery is provided. The non-aqueous electrolyte can be used in combination with high-nickel materials and has the advantages of long cycle life and good high-temperature storage performance. At the same time, it can also suppress the battery bloating problem caused by electrolyte decomposition during high-voltage and high-temperature storage.

[0006] The second technical problem to be solved by the present invention is to provide a lithium ion battery corresponding to the first technical problem.

[0007] In order to solve one of the above technical problems, the technical solution adopted by the present invention is: to provide a high-nickel positive electrode lithium ion battery non-aqueous electrolyte, the non-aqueous electrolyte comprising a lithium salt electrolyte, a non-aqueous solvent and an additive, wherein the additive includes an unsaturated phosphorus-containing silicon-based ester additive and a polycyclic sulfate ester additive.

[0008] Furthermore, the unsaturated phosphorus-containing silicon-based ester additive has a structure shown in formula (I-1) or (I-2): Wherein, R1 and R2 are independently selected from At least one of a saturated or unsaturated hydrocarbon group, a fluorine-containing hydrocarbon group, and a cyano-containing hydrocarbon group having 1 to 6 carbon atoms; R3 to R 11 At least one selected independently from the group consisting of a saturated or unsaturated hydrocarbon group, a hydrocarbonoxy group, a fluorine-containing hydrocarbon group, and a fluorine-containing hydrocarbonoxy group having 1 to 6 carbon atoms; R 12 At least one selected from saturated or unsaturated alkylene groups and fluorinated alkylene groups having 1 to 6 carbon atoms; n is 0 or 1; and R1 to R 12 There is at least one carbon-carbon unsaturated bond.

[0009] Furthermore, the polycyclic sulfate additives include but are not limited to compounds containing at least two cyclic sulfate structures, wherein the cyclic sulfate structures are selected from at least one of a four-membered ring, a five-membered ring, and a six-membered ring, and the connection between adjacent rings is a linked ring, a spiro ring, or a bridge ring connection.

[0010] Furthermore, the unsaturated phosphorus-containing silicon-based ester additive is selected from at least one of the following structural formulas:

[0011]

[0012]

[0013] Furthermore, the polycyclic sulfate additive is selected from at least one of the following structural formulas:

[0014]

[0015]

[0016] Furthermore, based on the mass of the non-aqueous electrolyte being 100%, the mass proportion of the unsaturated phosphorus-containing silicon-based ester additive in the non-aqueous electrolyte is 0.1-3%, and the mass proportion of the polycyclic sulfate ester additive in the non-aqueous electrolyte is 0.1-5%.

[0017] Furthermore, the lithium salt electrolyte is lithium hexafluorophosphate, and the concentration of the lithium salt electrolyte in the non-aqueous electrolyte is 0.5-1.5 mol / L.

[0018] Furthermore, the non-aqueous electrolyte also contains other additives, and the amount of the other additives accounts for 0.5-5% of the total mass of the non-aqueous electrolyte.

[0019] Furthermore, the other additives are selected from at least one of unsaturated carbonates, halogenated carbonates, sulfates, sulfites, sulfonates, phosphates, phosphites, borates, anhydrides, polynitriles, phosphazenes or lithium salt additives.

[0020] Furthermore, the other additives are selected from vinylene carbonate (VC), vinyl carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), vinyl sulfate (DTD), vinyl sulfite (ES), methylene disulfonate (MMDS), 1,3-propane sultone (PS), 1,3-propylene sultone (PST), tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) phosphite (TMSPi), tris(trimethylsilyl) borate (TMSB), succinic anhydride (SA), succinonitrile (SN), ), adiponitrile (ADN), 1,2-bis(2-cyanoethoxy)ethane (DENE), ethoxypentafluorocyclotriphosphazene (PFPN), lithium difluorophosphate (LiPO2F2), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium bis(oxalatodifluorophosphate) (LiDFBP), lithium tetrafluorooxalatophosphate (LiOTFP), lithium bis(fluorosulfonyl imide) (LiFSI), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI) or lithium 4,5-dicyano-2-trifluoromethyl-imidazole (LiTDI).

[0021] Furthermore, the non-aqueous organic solvent is selected from at least one of carbonate, carboxylic acid ester and ether solvents.

[0022] Further, the non-aqueous organic solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl butyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, phenyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, 2,2,2-trifluoroethyl methyl carbonate, bistrifluoroethyl carbonate, 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl acetate or 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoroethyl ether.

[0023] To solve the second technical problem mentioned above, the technical solution adopted by the present invention is: to provide a lithium-ion battery, which includes a high-nickel positive electrode material, a separator, a negative electrode material and the non-aqueous electrolyte.

[0024] Furthermore, the high nickel positive electrode material is LiNi x Co y M (1-x-y) O2, wherein M is Mn or Al, 0.6≤x≤1, 0≤y≤0.4, 1-xy≥0.

[0025] Furthermore, the negative electrode material includes but is not limited to at least one of carbon material, silicon-carbon composite material or lithium metal.

[0026] The beneficial effects of the present invention are:

[0027] The present invention uses unsaturated phosphorus-containing silicon-based esters and polycyclic sulfates as additives in combination and adds them to a battery with a high-nickel material as the positive electrode material. On the one hand, the unsaturated phosphorus-containing silicon-based ester can form a CEI film containing alkyl phosphorus on the surface of the positive electrode to inhibit the oxidative decomposition of the electrolyte, and the unsaturated silicon-based group can form a SEI film containing Si elements on the surface of the negative electrode to improve the thermal stability of the SEI film, thereby improving the high-temperature cycle performance of the battery; the unsaturated phosphorus-containing silicon-based ester can also eliminate moisture and HF in the electrolyte, further improving the cycle life of the battery. On the other hand, the polycyclic sulfate can form a SEI film rich in inorganic sulfur elements such as Li2SO4 on the negative electrode of the battery, promote the migration of lithium ions, improve the internal resistance, and at the same time inhibit the increase of the internal resistance of the battery, thereby improving the cycle performance of the battery. DETAILED DESCRIPTION

[0028] The technical solution of the present invention is further explained below in conjunction with specific implementation methods, but the following embodiments are only examples for explaining the present application and are not limitations on the content of the present application. Those skilled in the art may make improvements or modifications to the content of the present invention without creative contribution as needed under the guidance of this specification, and all of them fall within the protection scope of the present invention.

[0029] The present application is further described in detail below in conjunction with embodiments.

[0030] [Example 1]

[0031] (1) Preparation of non-aqueous electrolyte

[0032] In a glove box filled with nitrogen or argon with water and oxygen content ≤ 0.1ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 3:4:3. Lithium hexafluorophosphate is added to the prepared non-aqueous solvent, mixed and dissolved thoroughly, and a 1 mol / L lithium hexafluorophosphate solution is prepared.

[0033] Based on 100% of the total mass of the electrolyte, 1% by mass of VC, 2% by mass of FEC, 1% by mass of PS, 1% by mass of the unsaturated phosphorus-containing silicon ester represented by the structure of formula (Ⅰ-1) and 1% by mass of the polycyclic sulfate represented by the structure of (Ⅱ-1) were added to the lithium hexafluorophosphate solution, and the mixture was fully dissolved and mixed to obtain a non-aqueous electrolyte.

[0034] (2) Production of lithium-ion batteries

[0035] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive carbon black, carbon nanotubes, and binder polyvinylidene fluoride (PVDF) are added and dispersed in N-methyl-2-pyrrolidone (NMP) in a mass ratio of 96:1.5:0.5:2, and are fully mixed to obtain a positive electrode slurry; the positive electrode slurry is coated on both sides of an aluminum foil, and after drying, rolling, and cutting, a positive electrode sheet is obtained.

[0036] The negative electrode active material graphite, conductive carbon black, binder sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) are added and dispersed in deionized water in a mass ratio of 96:1:1.5:1.5, and mixed thoroughly to obtain a negative electrode slurry; the negative electrode slurry is coated on both sides of a copper foil, and after drying, rolling and cutting, a negative electrode sheet is obtained.

[0037] The positive electrode sheet, polypropylene porous isolation membrane, and negative electrode sheet are stacked to prepare an electrode assembly, and an ultrasonic spot welder is used to weld aluminum tabs and nickel tabs on the positive and negative electrodes respectively. The electrode assembly is then placed in an aluminum foil bag and fully vacuum dried to obtain a lithium-ion battery dry cell.

[0038] In a glove box filled with nitrogen or argon with water and oxygen contents of ≤0.1ppm, the prepared non-aqueous electrolyte was injected into the fully dried battery cell, and after the injection, the battery cell was sealed and left to stand, formed, aged, sealed again, and divided to obtain the lithium ion battery used in Example 1. The electrochemical performance of the lithium ion battery was tested, and the results are shown in Table 2.

[0039] [Examples 2 to 18]

[0040] The non-aqueous electrolyte was prepared and the lithium-ion battery was manufactured according to the method steps of Example 1, the only difference being the combination and amount of additives in the non-aqueous electrolyte, as shown in Table 1.

[0041] The electrochemical performance of the prepared lithium-ion battery was tested, and the results are shown in Table 2.

[0042] [Comparative Example 1]

[0043] (1) Preparation of non-aqueous electrolyte

[0044] In a glove box filled with nitrogen or argon with water and oxygen content ≤ 0.1ppm, ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) are mixed in a volume ratio of 3:4:3. Lithium hexafluorophosphate is added to the prepared non-aqueous solvent, mixed and dissolved thoroughly, and a 1 mol / L lithium hexafluorophosphate solution is prepared.

[0045] Based on 100% of the total mass of the electrolyte, 1% by mass of VC, 2% by mass of FEC and 1% by mass of PS were added to the lithium hexafluorophosphate solution, and the mixture was fully dissolved and mixed to obtain a non-aqueous electrolyte.

[0046] (2) Production of lithium-ion batteries

[0047] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive carbon black, carbon nanotubes, and binder polyvinylidene fluoride (PVDF) are added and dispersed in N-methyl-2-pyrrolidone (NMP) in a mass ratio of 96:1.5:0.5:2, and are fully mixed to obtain a positive electrode slurry; the positive electrode slurry is coated on both sides of an aluminum foil, and after drying, rolling, and cutting, a positive electrode sheet is obtained.

[0048] The negative electrode active material graphite, conductive carbon black, binder sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) are added and dispersed in deionized water in a mass ratio of 96:1:1.5:1.5, and mixed thoroughly to obtain a negative electrode slurry; the negative electrode slurry is coated on both sides of a copper foil, and after drying, rolling and cutting, a negative electrode sheet is obtained.

[0049] The positive electrode sheet, polypropylene porous isolation membrane, and negative electrode sheet are stacked to prepare an electrode assembly, and an ultrasonic spot welder is used to weld aluminum tabs and nickel tabs on the positive and negative electrodes respectively. The electrode assembly is then placed in an aluminum foil bag and fully vacuum dried to obtain a lithium-ion battery dry cell.

[0050] In a glove box filled with nitrogen or argon with water and oxygen contents of ≤0.1ppm, the prepared non-aqueous electrolyte was injected into the fully dried battery cell, and after the injection, the battery cell was sealed and left to stand, formed, aged, sealed again, and divided to obtain the lithium ion battery used in Comparative Example 1. The electrochemical performance of the lithium ion battery was tested, and the results are shown in Table 2.

[0051] [Comparative Examples 2 to 5]

[0052] The non-aqueous electrolyte was prepared and the lithium-ion battery was manufactured according to the method steps of Comparative Example 1, the only difference being the combination and amount of additives in the non-aqueous electrolyte, as shown in Table 1.

[0053] The electrochemical performance of the prepared lithium-ion battery was tested, and the results are shown in Table 2.

[0054] Table 1 Formula composition and dosage of non-aqueous electrolyte in Examples 1 to 18 and Comparative Examples 1 to 5

[0055]

[0056]

[0057]

[0058] The performance testing method of the lithium-ion battery involved in this application is as follows:

[0059] (1) Normal temperature cycle performance

[0060] At room temperature (25°C), the above-divided lithium-ion battery is charged to 4.5V at 1C constant current, and then discharged to 3V at 1C constant current. The charge and discharge cycle is 800 times, and the discharge capacity retention rate after the 800th cycle is calculated as follows:

[0061] Discharge capacity retention rate (%) = 800th cycle discharge capacity / first cycle discharge capacity × 100%.

[0062] (2) High temperature cycle performance

[0063] At high temperature (45°C), the above-divided lithium-ion battery is charged to 4.5V at 1C constant current, and then discharged to 3V at 1C constant current. The charge and discharge cycle is 400 times, and the discharge capacity retention rate after the 400th cycle is calculated as follows:

[0064] Discharge capacity retention rate (%) = 400th cycle discharge capacity / first cycle discharge capacity × 100%

[0065] (3) High temperature storage performance

[0066] At room temperature (25°C), charge the above-divided lithium-ion battery to 4.5V at 0.5C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 3V at 0.5C constant current, and record the discharge capacity Qt1. Then charge it to 4.5V at 0.5C constant current and constant voltage, measure the initial thickness H1 of the battery, and store it in a 60°C high-temperature oven for 7 days after fully charged. Take it out after 7 days, and measure the thickness H2 of the battery after storage after the battery returns to room temperature. Discharge it to 3V at 0.5C at room temperature, record the discharge capacity Qt2, and finally charge it to 4.5V at 0.5C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 3V at 0.5C constant current, and record the discharge capacity Qt3.

[0067] Capacity retention rate (%) = Qt2 / Qt1×100%

[0068] Capacity recovery rate (%) = Qt3 / Qt1×100%

[0069] Thickness expansion rate (%) = (H2-H1) / H1×100%

[0070] Table 2 Test results of lithium ion battery performance in Examples 1 to 18 and Comparative Examples 1 to 5

[0071]

[0072]

[0073] It can be seen from the test data in Table 2 that after adding unsaturated phosphorus-containing silicon-based ester to the batteries of Comparative Examples 2 and 3, the cycle performance and high-temperature storage performance of the batteries are improved compared with Comparative Example 1, and the flatulence after high-temperature storage is also suppressed. This is because the unsaturated phosphorus-containing silicon-based ester can eliminate trace amounts of HF and water in the electrolyte, and can form a film on the positive and negative electrodes, inhibiting the decomposition of the electrolyte, thereby improving the performance of the battery.

[0074] In the batteries of Comparative Examples 4 and 5, after adding polycyclic sulfate, the various performances of the batteries are significantly improved compared with those of Comparative Example 1. This is attributed to the fact that polycyclic sulfate forms a film at the negative electrode, preventing the reduction and decomposition of the electrolyte at the negative electrode, reducing the film formation internal resistance of the negative electrode, and inhibiting the increase of the internal resistance of the battery during the cycle, thereby improving the cycle and storage performance of the battery.

[0075] In the batteries of Examples 1 to 18, after the unsaturated phosphorus-containing silicon-based ester and the polycyclic sulfate are added at the same time, the two additives work together to exert their respective advantages. Compared with the addition of unsaturated silicon-based phosphate or polycyclic sulfate alone, the room temperature cycle, high temperature cycle and high temperature storage performance of the battery are further improved, and the flatulence after high temperature storage is also further suppressed, achieving good technical effects.

Claims

1. A non-aqueous electrolyte for a high-nickel positive electrode lithium-ion battery, the non-aqueous electrolyte comprising a lithium salt electrolyte, a non-aqueous solvent and an additive, characterized in that: The additives include unsaturated phosphorus-containing silicon-based ester additives and polycyclic sulfate ester additives.

2. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The unsaturated phosphorus-containing silicon-based ester additive has a structure shown in formula (I-1) or (I-2): Wherein, R1 and R2 are independently selected from At least one of a saturated or unsaturated hydrocarbon group, a fluorine-containing hydrocarbon group, and a cyano-containing hydrocarbon group having 1 to 6 carbon atoms; R3 to R 11 At least one selected independently from the group consisting of a saturated or unsaturated hydrocarbon group, a hydrocarbonoxy group, a fluorine-containing hydrocarbon group, and a fluorine-containing hydrocarbonoxy group having 1 to 6 carbon atoms; R 12 At least one selected from saturated or unsaturated alkylene groups and fluorinated alkylene groups having 1 to 6 carbon atoms; n is 0 or 1; and R1 to R 12 There is at least one carbon-carbon unsaturated bond.

3. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The polycyclic sulfate additives include but are not limited to compounds containing at least two cyclic sulfate structures, wherein the cyclic sulfate structures are selected from at least one of a four-membered ring, a five-membered ring, and a six-membered ring, and the connection between adjacent rings is a linked ring, a spiro ring, or a bridge ring connection.

4. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 2, characterized in that: The unsaturated phosphorus-containing silicon-based ester additive is selected from at least one of the following structural formulas:

5. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 3, characterized in that: The polycyclic sulfate additive is selected from at least one of the following structural formulas:

6. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: Taking the mass of the non-aqueous electrolyte as 100%, the mass proportion of the unsaturated phosphorus-containing silicon-based ester additive in the non-aqueous electrolyte is 0.1-3%, and the mass proportion of the polycyclic sulfate ester additive in the non-aqueous electrolyte is 0.1-5%.

7. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The lithium salt electrolyte is lithium hexafluorophosphate, and the concentration of the lithium salt electrolyte in the non-aqueous electrolyte is 0.5-1.5 mol / L; the non-aqueous electrolyte also contains other additives, and the amount of the other additives is 0.5-5% of the total mass of the non-aqueous electrolyte, and the other additives are selected from at least one of unsaturated carbonates, halogenated carbonates, sulfates, sulfites, sulfonates, phosphates, phosphites, borates, anhydrides, polynitriles, phosphazenes or lithium salt additives.

8. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 7, characterized in that: The other additives are selected from vinylene carbonate (VC), vinyl carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), vinyl sulfate (DTD), vinyl sulfite (ES), methylene disulfonate (MMDS), 1,3-propane sultone (PS), 1,3-propylene sultone (PST), tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) phosphite (TMSPi), tris(trimethylsilyl) borate (TMSB), succinic anhydride (SA), succinonitrile (SN), hexane At least one of dinitrile (ADN), 1,2-bis(2-cyanoethoxy)ethane (DENE), ethoxypentafluorocyclotriphosphazene (PFPN), lithium difluorophosphate (LiPO2F2), lithium tetrafluoroborate (LiBF4), lithium bis(oxalatoborate) (LiBOB), lithium difluorooxalatoborate (LiODFB), lithium bis(oxalatodifluorophosphate) (LiDFBP), lithium tetrafluorooxalatophosphate (LiOTFP), lithium bis(fluorosulfonyl imide) (LiFSI), lithium bis(trifluoromethylsulfonyl imide) (LiTFSI) or lithium 4,5-dicyano-2-trifluoromethyl-imidazole (LiTDI).

9. The high nickel positive electrode lithium ion battery non-aqueous electrolyte according to claim 1, characterized in that: The non-aqueous organic solvent is selected from at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, methyl butyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, phenyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, 2,2,2-trifluoroethyl methyl carbonate, bistrifluoroethyl carbonate, 2,2,2-trifluoroethyl acetate, 2,2-difluoroethyl acetate or 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoroethyl ether.

10. A lithium ion battery comprising a high nickel positive electrode material, a separator, a negative electrode material and the non-aqueous electrolyte according to any one of claims 1 to 9, characterized in that: The high nickel cathode material is LiNi x Co y M (1-x-y) O2, wherein M is Mn or Al, 0.6≤x≤1, 0≤y≤0.4, 1-xy≥0; the negative electrode material includes but is not limited to at least one of a carbon material, a silicon-carbon composite material or lithium metal.