Electrolyte and lithium ion battery
By using electrolyte additives containing F atoms and phenyl ether structure in lithium-ion batteries, a stable LiF SEI film is formed and the conductivity is improved, which solves the problem of SEI film instability caused by volume expansion of silicon-based anode materials and improves Kinetic performance and safety of lithium-ion batteries.
Patent Information
- Application Number
- CN202411067153.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-18
AI Technical Summary
The volume expansion of silicon-based anode materials in lithium-ion batteries causes instability of the SEI film, which affects cycle performance and battery safety. The SEI film formed by existing electrolyte solvents has a high organic component content, resulting in poor kinetic performance.
Use electrolyte additives containing F atoms and phenyl ether structure to reduce LUMO and HOMO energy levels, preferentially form LiF SEI film, improve conductivity and stability, and provide flame retardancy through the cyano carbon-nitrogen triple bond and fluorine group in the cyano group function to enhance battery safety.
It improves the first Coulombic efficiency, cycle performance and rate performance of lithium-ion batteries, improves low temperature and high voltage performance, and enhances the flame retardancy of the electrolyte and battery safety.
Smart Images

Figure CN118800968A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of lithium ion batteries, and in particular relates to an electrolyte and a lithium ion battery. Background Art
[0002] Anode materials with high specific capacity are an important breakthrough in improving the energy density of lithium-ion batteries. Silicon-based materials are considered to be the most likely anode materials to replace graphite because of their high theoretical specific capacity (Si: 4200mAh / g, SiO: 2650mAh / g), suitable discharge potential and relatively abundant reserves in nature. However, there are many problems in the commercial application of single silicon in lithium-ion batteries. First, silicon-based materials as anodes will have volume expansion problems during battery cycles, and may cause the rupture of active particles, pulverization of pole pieces and the shedding of active materials. Secondly, the silicon anode is accompanied by a large volume expansion during the first cycle. Due to the change in silicon volume, the solid electrolyte interface film (SEI) will rupture. The newly exposed silicon on the surface will produce a new SEI film, and at the same time, it will continuously consume lithium ions in the electrolyte, reducing the first coulomb efficiency. More seriously, due to the volume change of the electrode material during the cycle, the SEI film at the silicon anode interface repeatedly grows and ruptures, greatly affecting the cycle stability.
[0003] Due to the volume effect of silicon-based negative electrode materials, it is difficult for silicon-based negative electrodes to form stable solid electrolyte interface films in the electrolyte, and the electrode structure is destroyed during the battery cycle. New solid electrolyte interface films will continue to form on the exposed silicon-based surface, leading to corrosion of the negative electrode material and capacity attenuation.
[0004] Currently, commonly used electrolyte solvents are linear carbonates and cyclic carbonates, such as dimethyl carbonate, ethyl methyl carbonate, ethylene carbonate and propylene carbonate. The SEI film formed by these solvents has a high content of organic components, resulting in poor SEI film stability and lithium-ion battery kinetic performance. Summary of the invention
[0005] In order to solve the technical problem in the above-mentioned prior art that when the electrolyte solvent is linear carbonate and cyclic carbonate, the formed SEI film has a high organic component content, resulting in poor SEI film stability and lithium ion battery kinetic performance, the purpose of the present invention is to provide an electrolyte and a lithium ion battery.
[0006] The present invention provides an electrolyte, wherein the electrolyte comprises an electrolyte additive, and the general structural formula of the electrolyte additive is shown in the following formula (I):
[0007]
[0008] Among them, R 1 ~R 2At least one of them contains F atoms, R 1 is a halogenated hydrocarbon group, R 2 Contains a phenyl ether structure.
[0009] The electrolyte of the present invention includes an electrolyte additive of the above-mentioned general structural formula. In the first aspect, the electrolyte additive can reduce the LUMO energy level, preferentially form a LiF SEI film on the surface of the negative electrode, and the formed LiF interface film has high ion conductivity, which can improve the kinetic performance of the lithium ion battery, thereby improving the rate performance of the lithium ion battery. At the same time, the formed LiF interface film has high stability, which can improve the initial coulomb efficiency and cycle performance of the lithium ion battery; in the second aspect, the electrolyte additive reduces the HOMO energy level, improves the oxidation stability of the electrolyte, and improves the cycle performance under high voltage; in the third aspect, the carboxylate group in the electrolyte additive has a stronger polarity than the carbonate in the prior art, and can provide higher conductivity. , and the viscosity and freezing point are lower, which can be widely used in low temperature fields, and have good effects in solving low temperature charging and improving fast charging; fourthly, the bond energy of the cyano carbon-nitrogen triple bond in the cyano group in the electrolyte additive is very high, not easily oxidized, and has good stability on the positive electrode, and strong oxidation resistance. At the same time, the cyano group has a strong coordination ability, which can be combined with the active sites on the electrode surface (for example, some high-valent metal ions such as nickel, cobalt, manganese, etc.), and play a role in masking these active metal ions on the positive electrode surface, reducing the decomposition of the electrode on the electrolyte, and improving the stability of the lithium ion battery; fifthly, the fluorine group and cyano group in the electrolyte additive have a certain flame retardant effect, which can improve the safety performance of the lithium ion battery. Therefore, the electrolyte additive of the present invention can improve the stability of the SEI film and the kinetic performance of the lithium ion battery, effectively improve the first coulomb efficiency, cycle performance and rate performance of the lithium ion battery, and improve the low temperature and high voltage performance of the electrolyte, while making the electrolyte have a flame retardant effect, and improving the safety performance of the lithium ion battery.
[0010] Preferably, the R 1 As shown in the following formula (II), R 2 As shown in the following formula (III):
[0011]
[0012] Among them, R 3 ~R 18 At least one of them is a F atom or a fluoroalkyl group, and * is a connecting end.
[0013] More preferably, R 3 ~R 9 At least one of them is a F atom or a fluorinated alkyl group.
[0014] Preferably, in the electrolyte, the mass fraction of the electrolyte additive is 3% to 9%.
[0015] In the electrolyte of this solution, the mass fraction of the electrolyte additive is 3% to 9%. The mass fraction of the electrolyte additive within this range can fully realize the above-mentioned technical effects of the electrolyte additive, and can also maintain the appropriate conductivity of the electrolyte at a reasonable cost.
[0016] Preferably, the electrolyte further comprises linear carbonate and cyclic carbonate.
[0017] Preferably, the linear carbonate includes at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and methyl propyl carbonate (MPC).
[0018] Preferably, the cyclic carbonate includes at least one of ethylene carbonate (EC), fluoroethylene carbonate (FEC), and propylene carbonate (PC).
[0019] Preferably, the electrolyte further comprises a sulfur-containing additive and a carbonate additive; in the electrolyte, the mass fraction of the sulfur-containing additive is 1% to 2%, and the mass fraction of the carbonate additive is 0.2% to 0.8%.
[0020] The electrolyte described in this scheme also includes a sulfur-containing additive and a carbonate additive; in the electrolyte, the mass fraction of the sulfur-containing additive is 1% to 2%, and the mass fraction of the carbonate additive is 0.2% to 0.8%; the electrolyte includes a sulfur-containing additive and a carbonate additive, and the mass fractions of the sulfur-containing additive and the carbonate additive are within this range, which can not only form a stable and dense SEI film on the electrode surface, improve the high temperature performance of the electrolyte, inhibit gas expansion and reduce the internal resistance of the battery, but also reduce the content of organic components in the SEI film.
[0021] Preferably, the sulfur-containing additive includes at least one of vinyl sulfate, propylene sulfite, 1,3-propane sultone, and propenyl-1,3-sultone.
[0022] Preferably, the carbonate additive includes at least one of vinylene carbonate and bis(2,2,2-trifluoroethyl) carbonate (TFEC).
[0023] Preferably, the electrolyte further comprises lithium hexafluorophosphate LiPF6 at a concentration of 1.0 to 1.5 mol / L. 6 .
[0024] The present invention also provides a lithium ion battery comprising the electrolyte. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.
[0026] Example 1
[0027] The electrolyte additive of this embodiment is cyano (3-phenoxyphenyl) methyl 2,2-dimethyl-3- (3,3,3-trifluoro-1-propylene-1-yl) cyclopropanecarboxylate, and the structural formula is as follows:
[0028]
[0029] Preparation of electrolyte
[0030] S1. Dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC), and ethylene carbonate (EC) are mixed in a mass ratio of 50:20:10:20, and the mixture is stirred to obtain a first mixture;
[0031] S2. LiPF6 6 Add the first mixture and stir until the mixture is evenly mixed to obtain a second mixture;
[0032] S3. Add electrolyte additive cyano (3-phenoxyphenyl) methyl 2,2-dimethyl-3-(3,3,3-trifluoro-1-propylene-1-yl) cyclopropanecarboxylate, sulfur-containing additive vinyl sulfate (DTD) and carbonate additive vinylene carbonate (VC) to the second mixture and stir, stir and mix to obtain an electrolyte. In the electrolyte of this embodiment, LiPF 6 The concentration is 1 mol / L, the mass fraction of cyano(3-phenoxyphenyl)methyl 2,2-dimethyl-3-(3,3,3-trifluoro-1-propene-1-yl)cyclopropanecarboxylate is 6%, the mass fraction of vinyl sulfate is 1.5%, and the mass fraction of vinylene carbonate is 0.5%.
[0033] Example 2
[0034] The structural formula of the electrolyte additive used in the preparation of the electrolyte in this embodiment is as follows:
[0035] Other than that, the same as in Example 1.
[0036] Example 3
[0037] The structural formula of the electrolyte additive used in the preparation of the electrolyte in this embodiment is as follows:
[0038] Other than that, the same as in Example 1.
[0039] Example 4
[0040] The preparation of the electrolyte in this example is the same as in Example 1, except that the mass fraction of the electrolyte additive cyano(3-phenoxyphenyl)methyl 2,2-dimethyl-3-(3,3,3-trifluoro-1-propene-1-yl)cyclopropanecarboxylate is 11%.
[0041] Example 5
[0042] The preparation of the electrolyte in this example is the same as in Example 1 except that the mass fraction of the electrolyte additive cyano(3-phenoxyphenyl)methyl 2,2-dimethyl-3-(3,3,3-trifluoro-1-propene-1-yl)cyclopropanecarboxylate is 2%.
[0043] Example 6
[0044] The preparation of the electrolyte in this embodiment is the same as that in Example 1, except that the sulfur-containing additive vinyl sulfate in Example 1 is replaced by the base solvent (DMC, EMC, FEC, and EC are configured as the base solvent in a mass ratio of 50:20:10:20).
[0045] Example 7
[0046] The preparation of the electrolyte of this embodiment is the same as that of Embodiment 1, except that the mass of the carbonate additive vinylene carbonate in Embodiment 1 is replaced by the base solvent (DMC, EMC, FEC, and EC are configured as the base solvent in a mass ratio of 50:20:10:20).
[0047] Example 8
[0048] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of vinyl sulfate is 2.5% and the mass fraction of vinylene carbonate is 1%.
[0049] Example 9
[0050] The preparation of the electrolyte in this embodiment is the same as that in Embodiment 1 except that the mass fraction of vinyl sulfate is 0.7% and the mass fraction of vinylene carbonate is 0.1%.
[0051] Comparative Example 1
[0052] The preparation of the electrolyte in this comparative example is the same as that in Example 1, except that the electrolyte additive cyano(3-phenoxyphenyl)methyl 2,2-dimethyl-3-(3,3,3-trifluoro-1-propene-1-yl)cyclopropanecarboxylate in Example 1 is replaced by the base solvent (DMC, EMC, FEC, and EC are configured as the base solvent in a mass ratio of 50:20:10:20).
[0053] Comparative Example 2
[0054] The electrolyte additives in this comparative example are acetonitrile, fluoroethylene carbonate and methyl acetate.
[0055] Preparation of electrolyte
[0056] S1. Dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), fluoroethylene carbonate (FEC), and ethylene carbonate (EC) are mixed in a mass ratio of 50:20:10:20, and the mixture is stirred to obtain a first mixture;
[0057] S2. LiPF6 6 Add the first mixture and stir until the mixture is evenly mixed to obtain a second mixture;
[0058] S3. Add electrolyte additives acetonitrile, fluoroethylene carbonate, methyl acetate, sulfur-containing additive vinyl sulfate (DTD) and carbonate additive vinylene carbonate (VC) to the second mixture and stir, stir and mix to obtain an electrolyte. In the electrolyte of this embodiment, LiPF 6 The concentration is 1 mol / L, the mass fraction of acetonitrile is 0.57%, the mass fraction of fluoroethylene carbonate is 4.40%, the mass fraction of methyl acetate is 1.03%, the mass fraction of vinyl sulfate is 1.5%, and the mass fraction of vinylene carbonate is 0.5%.
[0059] Preparation of lithium-ion batteries
[0060] (1) Preparation of positive electrode sheet
[0061] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O 2 , conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 94:3:3 and added into solvent N-methylpyrrolidone (NMP), mixed evenly to obtain a positive electrode slurry with a solid content of 45%. The positive electrode slurry is coated on both surfaces of the positive electrode current collector aluminum foil to form a positive electrode active coating. After vacuum drying, a positive electrode sheet is obtained.
[0062] (2) Preparation of negative electrode sheet
[0063] Silicon-carbon negative electrode material (SiC), conductive agent conductive carbon black (SP), single-walled carbon nanotubes (SWCNT) and binder polyacrylic acid (PAA) are mixed in a mass ratio of 80:9:1:10 and added to a solvent deionized water, mixed evenly, to prepare a negative electrode slurry with a solid content of 25%, and the negative electrode slurry is coated on both surfaces of the negative electrode current collector copper foil to form a negative electrode active coating, and after vacuum drying, a negative electrode sheet is prepared.
[0064] (3) Selection of electrolyte
[0065] The electrolytes obtained in the above-mentioned embodiments and comparative examples and the common electrolyte of the control group (EC:DMC:DEC mass ratio of 30:40:30, LiPF6 1 mol / L) were selected to prepare lithium-ion batteries.
[0066] (4) Selection of isolation membrane
[0067] The isolation film includes a polyethylene (PE) film and ceramic layers respectively arranged on two surfaces of the PE film, wherein the total thickness of the two ceramic layers is 3 μm, the thickness of the PE film is 9 μm, and the total thickness of the isolation film is 12 μm.
[0068] (5) Preparation of lithium-ion batteries
[0069] The positive electrode sheet, the isolation film, and the negative electrode sheet are stacked in order, and the isolation film is placed between the positive electrode sheet and the negative electrode sheet to play an isolating role, so as to prepare a bare battery cell; the bare battery cell is placed in an outer packaging shell, and after drying, an electrolyte is injected, and a lithium-ion battery is obtained through vacuum packaging, standing, forming, shaping and other processes.
[0070] Performance Testing
[0071] The rate performance of the battery was tested under lithium-ion battery test conditions. The test was conducted on the LAND battery test system of Wuhan Jinnuo Electronics Co., Ltd. at room temperature (25°C). The conventional charge and discharge voltage was limited to 2.5V to 4.2V, and a high voltage cycle of 2.5 to 4.4V was designed. The cycle performance and rate performance are shown in Table 1 below.
[0072] 1) 2.5~4.2V at room temperature, 1C / 1C cycle 900 weeks capacity retention rate
[0073] At 25°C, the lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.
[0074] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0075] 2) Room temperature 2.5 ~ 4.4V, 1C / 1C cycle 900 weeks capacity retention rate
[0076] At 25°C, the lithium-ion battery is charged to 4.4V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and allowed to stand for 10 minutes. Then, the lithium-ion battery is discharged to 2.5V at a constant current rate of 1C and allowed to stand for 10 minutes. This is considered one charge and discharge cycle. The lithium-ion battery is charged and discharged for 900 cycles according to the above method, and the capacity retention rate of the lithium-ion battery after 900 cycles of charge and discharge at 1C / 1C is calculated.
[0077] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.
[0078] 3) Room temperature 6C rate performance - constant current charging ratio
[0079] At 25°C, the lithium-ion battery was discharged at a constant current rate of 1C to 2.5V, and then stood for 10 minutes. Then, the lithium-ion battery was charged at a constant current and constant voltage rate of 6C to 4.2V, with a cut-off current of 0.05C, and stood for 10 minutes. The constant current charging capacity Q of the lithium-ion battery was recorded. 1 , constant current constant voltage charging total capacity Q 2 , calculate the 6C rate charging constant current charging ratio according to the following formula: 6C rate charging constant current charging ratio = constant current charging capacity Q 1 / Constant current and constant voltage charging total capacity Q 2 ×100%.
[0080] 4) 1C discharge capacity retention rate at low temperature (-20℃)
[0081] At 25°C, the lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C. After standing for 10 minutes, the discharge capacity at this time is measured as the discharge capacity at 25°C, recorded as q 1 Then, at 25℃, the lithium-ion battery is charged to 4.2V at a constant current and constant voltage rate of 1C, with a cut-off current of 0.05C, and left to stand for 10 minutes. After the lithium-ion battery is left at -20℃ for 2 hours, it is discharged to 2.5V at a constant current rate of 1C at -20℃. The discharge capacity at this time is measured as the discharge capacity at -20℃, recorded as q 2, calculate the 1C discharge capacity retention rate at low temperature (-20°C) according to the following formula: 1C discharge capacity retention rate at -20°C = discharge capacity q at -20°C 2 / Discharge capacity at 25℃q 1 ×100%.
[0082] 5) Battery thermal runaway ARC (adiabatic accelerated calorimeter) test
[0083] The lithium-ion battery is heated from room temperature to 45±2℃ in the chamber. After being left for 90 minutes, the temperature rise rate of the battery is detected. If the temperature rise exceeds 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR>0.02℃ / min), it is considered that a self-exothermic reaction occurs inside the lithium-ion battery, and the adiabatic environment is maintained until the lithium-ion battery has thermal runaway; if the temperature rise does not exceed 0.2℃ within 10 minutes (i.e., the self-heating temperature rise rate SHR≤0.02℃ / min), continue to the next step temperature rise test; each temperature step is 5℃, and the steps are repeated on each step. The ARC test temperature range is 45-300℃, the self-heating starting temperature is T1 (temperature rise rate SHR>0.02℃ / min), and the thermal runaway starting temperature is T2 (temperature rise rate SHR>1℃ / min).
[0084] Table 1
[0085]
[0086] From the analysis of Table 1, we can see that:
[0087] After the electrolytes of Examples 1 to 9 of the present invention are used to prepare lithium-ion batteries, they show good performance in terms of cycle capacity retention (including 2.5 to 4.2V cycles and high voltage cycles 2.5 to 4.4V), high rate performance-constant current charging ratio (fast charging), low temperature discharge capacity retention rate and battery thermal runaway ARC test (self-heating starting temperature T1 and thermal runaway starting temperature T2), while Comparative Examples 1 to 2 and the control group do not belong to the technical scheme of the present invention, so the performance in the above four aspects is significantly deteriorated. This fully demonstrates that the electrolyte prepared using the technical scheme of the present invention is applied to lithium batteries, which can improve the stability of the SEI film and the kinetic performance of lithium-ion batteries, effectively improve the cycle performance and rate performance of lithium-ion batteries, and improve the low temperature and high voltage performance of the electrolyte, while making the electrolyte have a flame retardant effect, thereby improving the safety performance of lithium-ion batteries.
[0088] The electrolyte additives of Examples 2 and 3 are other electrolyte additives that meet the general structural formula of the electrolyte additives of the technical solution of the present invention. From the test results in Table 1, the lithium-ion batteries prepared using the electrolytes of Examples 2 and 3 also show good technical effects in the cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test.
[0089] Compared with Example 1, the F atom in the electrolyte additive in the electrolyte of Example 3 is on the phenyl group of the phenyl ether structure, and the fluorine content is different. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Example 3 has a lower technical effect than Example 1 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test. The lithium ion battery prepared using the electrolyte of Example 3 also has a lower technical effect than Example 2 in terms of 2.5V~4.2V cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test, which indicates that the substitution site and fluorine content of the F atom or fluoroalkyl in the electrolyte additive of the present invention will affect the electrolyte, thereby affecting the performance of the lithium ion battery prepared using the electrolyte in the above four aspects.
[0090] Compared with Example 1, the electrolyte additive used in the electrolyte of Example 4 is more - the mass fraction of the electrolyte additive in the electrolyte is 11%, and the electrolyte additive used in the electrolyte of Example 5 is less - the mass fraction of the electrolyte additive in the electrolyte is 2%. The electrolyte additives used in the electrolytes of Example 4 and Example 5 are not within the further preferred range of the mass fraction of the electrolyte additive of 3% to 9%. The amount of electrolyte additive used in Example 4 is more, the conductivity of the electrolyte is reduced, and the technical effects of the lithium ion battery prepared using the electrolyte of Example 4 in terms of cycle capacity retention rate, low temperature discharge capacity retention rate and battery thermal runaway ARC test are reduced. The amount of electrolyte additive used in Example 5 is less, and the ability to improve the stability of the SEI film and the kinetic performance of the lithium ion battery is weakened. The technical effects of the lithium ion battery prepared using the electrolyte of Example 5 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are reduced.
[0091] Compared with Example 1, no sulfur-containing additive is added to the electrolyte of Example 6, no carbonate additive is added to the electrolyte of Example 7, and the mass fractions of the sulfur-containing additive and the carbonate additive in the electrolytes of Examples 8 and 9 are not within a further preferred range - the mass fraction of the sulfur-containing additive is 1% to 2%, and the mass fraction of the carbonate additive is 0.2% to 0.8%, that is, the mass fractions of the sulfur-containing additive and the carbonate additive in the electrolyte of Example 8 are both greater than the preferred range, and the mass fractions of the sulfur-containing additive and the carbonate additive in the electrolyte of Example 9 are both less than the preferred range. From the test results in Table 1, the lithium-ion battery prepared using the electrolyte of Example 6 has better technical effects than Example 8 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test. The mass fractions of the sulfur-containing additive and the carbonate additive in the electrolyte of Example 8 are not within the preferred range, and the technical effect is not as good as that of Example 6 (without the addition of the sulfur-containing additive vinyl sulfate). This shows that the combination of the sulfur-containing additive and the carbonate additive and their respective mass fractions within the preferred range can achieve unexpected synergistic technical effects.
[0092] Compared with Example 1, Comparative Example 1 does not use electrolyte additives. Therefore, from the test results in Table 1, compared with Example 1, the technical effects of the lithium ion battery prepared using the electrolyte of Comparative Example 1 in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test are significantly reduced.
[0093] The electrolyte additives used in Comparative Example 2 are acetonitrile, fluoroethylene carbonate and methyl acetate. The combination of acetonitrile, fluoroethylene carbonate and methyl acetate satisfies the electrolyte additive structural formula of Example 1 and has multiple functional groups such as cyano, fluorine atom and carboxylate. From the test results in Table 1, the lithium ion battery prepared using the electrolyte of Comparative Example 2 has significantly reduced technical effects in terms of cycle capacity retention rate, high rate performance-constant current charging ratio, low temperature discharge capacity retention rate and battery thermal runaway ARC test. This shows that even if the electrolyte additive used simultaneously meets the functional group characteristics of the general structural formula of the electrolyte additive in the technical scheme of the present invention, replacing it with the electrolyte additive in the technical scheme of the present invention cannot simultaneously achieve the above four technical effects.
[0094] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An electrolyte, characterized in that: The electrolyte includes an electrolyte additive, and the general structural formula of the electrolyte additive is shown in the following formula (I): Among them, at least one of R1 to R2 contains a F atom, R1 is a halogenated hydrocarbon group, and R2 contains a phenyl ether structure.
2. The electrolyte according to claim 1, characterized in that: The R1 is shown in the following formula (II), and R2 is shown in the following formula (III): Among them, R3~R 18 At least one of them is a F atom or a fluoroalkyl group, and * is a connecting end.
3. The electrolyte according to claim 1, characterized in that: In the electrolyte, the mass fraction of the electrolyte additive is 3% to 9%.
4. The electrolyte according to claim 1, characterized in that: The electrolyte also includes linear carbonates and cyclic carbonates.
5. The electrolyte according to claim 4, characterized in that: The linear carbonate includes at least one of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate and methyl propyl carbonate.
6. The electrolyte according to claim 4, characterized in that: The cyclic carbonate includes at least one of ethylene carbonate, fluoroethylene carbonate and propylene carbonate.
7. The electrolyte according to claim 1, characterized in that: The electrolyte further comprises a sulfur-containing additive and a carbonate additive; in the electrolyte, the mass fraction of the sulfur-containing additive is 1% to 2%, and the mass fraction of the carbonate additive is 0.2% to 0.8%.
8. The electrolyte according to claim 7, characterized in that: The sulfur-containing additive includes at least one of vinyl sulfate, propylene sulfite, 1,3-propane sultone, and propenyl-1,3-sultone.
9. The electrolyte according to claim 7, characterized in that: The carbonate additive includes at least one of vinylene carbonate and bis(2,2,2-trifluoroethyl) carbonate.
10. A lithium ion battery, characterized in that: Comprising the electrolyte as claimed in any one of claims 1 to 9.
Citation Information
Patent Citations
Electrolyte for ternary cathode material lithium ion battery and ternary cathode material lithium ion battery
CN106356562A
Battery electrolyte additive, battery electrolyte and lithium ion battery
CN110718715A
Non-aqueous electrolyte and lithium ion battery
CN112467202A
Non-aqueous electrolyte and lithium ion battery containing same
CN116190794A
Process for preparing gamma-cyhalothrin
US20060148892A1