Battery

By optimizing the specific surface area ratio of the cathode and anode materials in the lithium-ion battery, and adding the formula 1 compound and LiBF4 to the electrolyte, a stable interface film is formed, which solves the problem of lithium-ion battery cycle fast charging performance degradation at high voltages. , improving the battery’s cycle and fast charging performance.

CN118800969APending Publication Date: 2024-10-18GUANGZHOU TINCI MATERIALS TECH
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411069923.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

During high-rate charge and discharge cycles of lithium-ion batteries, the dissolution of metal ions in the cathode active material leads to a decrease in the stability of the solid electrolyte interface and a decrease in the deintercalation and deintercalation ability of lithium ions, resulting in rapid attenuation of battery capacity, especially the deterioration of fast charging performance under high voltage cycles. .

Method used

By using a specific specific surface area ratio of the positive active material layer and the negative active material layer in the battery, and adding a specific ratio of the formula 1 compound and LiBF4 to the electrolyte, stable SEI and CEI films are formed to inhibit the dissolution of metal ions and optimize the battery. cycle fast charging performance.

Benefits of technology

Minimize the negative impact of positive and negative active materials on battery fast charging performance under high voltage, improve the battery's cycle fast charging performance and safety, and ensure the rapid deintercalation and transmission of lithium ions on the interface film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800969A_ABST
    Figure CN118800969A_ABST
Patent Text Reader

Abstract

A positive pole piece comprises a positive active material layer, the positive active material layer comprises a positive active material, based on the total mass of the positive active material layer, the mass ratio of the positive active material is B, and the specific surface area of the positive active material is C m < 2 > / g; the negative pole piece comprises a negative active material, and the specific surface area of the negative active material is E; the electrolyte comprises a compound as shown in a formula 1 and LiBF4, based on the total mass of the electrolyte, the mass ratio of the compound as shown in the formula 1 is G, and the formula that (10 * B * G * E2) / C is larger than or equal to 0.20 and smaller than or equal to 3.88 is met, and # imgabs0 is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of batteries, and specifically relates to a battery. Background Art

[0002] Lithium-ion batteries are widely used in consumer electronics, electric vehicles, energy storage and other fields due to their high energy density and cycle performance. Currently, the discharge capacity of lithium-ion batteries is mainly increased by increasing the upper cut-off voltage or compaction density to meet consumers' high-capacity demand for lithium-ion batteries.

[0003] However, during the high-rate battery charge and discharge cycle process, metal ions in the positive electrode active material will dissolve, further catalyzing the oxidation decomposition of the electrolyte to produce gas, resulting in reduced stability of SEI (Solid Electrolyte Interface) and CEI (Cathode Electrolyte Interface), reduced deintercalation and intercalation ability of lithium ions between the positive and negative electrodes, causing the battery capacity to decay rapidly, thereby deteriorating the battery's fast-charging performance. This problem is particularly prominent under high voltage.

[0004] Based on this, how to improve the cycle fast charging performance of high-voltage lithium-ion batteries has become an urgent problem to be solved. Summary of the invention

[0005] The present application aims to solve at least one of the technical problems in the related art to a certain extent. To this end, one object of the present application is to provide a battery. The battery has excellent cycle fast charging performance.

[0006] In a first aspect, the present application provides a battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material, and based on the total mass of the positive electrode active material layer, the mass proportion of the positive electrode active material is B, and the specific surface area of ​​the positive electrode active material is C m 2 / g; the negative electrode sheet includes a negative electrode active material, and the specific surface area of ​​the negative electrode active material is E m 2 / g; an electrolyte, the electrolyte comprising the compound of Formula 1 and LiBF4, based on the total mass of the electrolyte, the mass proportion of the compound of Formula 1 is G, and satisfies the following formula: 0.20≤(10×B×G×E 2 ) / C≤3.88,

[0007]

[0008] The battery in the present application includes a positive electrode sheet, a negative electrode sheet and an electrolyte, and the electrolyte includes a compound shown in Formula 1 and LiBF4. During the fast charging process of the battery, although the compound shown in Formula 1 can preferentially form a stable SEI film on the surface of the negative electrode to improve the battery cycle performance, there is still a problem of gas production during the long cycle process, which affects the safety of the battery. LiBF4 can not only inhibit gas production, but also participate in the formation of a stable CEI, inhibit the dissolution of metal ions in the positive electrode active material, and improve the stability of the positive electrode side. Therefore, the combination of the two can improve the cycle performance of the battery during fast charging. However, the inventors found that during the actual cycle of the battery, the compound shown in Formula 1 and LiBF4 in the electrolyte have limited effects on the battery's cycle fast charging performance, especially the fast charging performance. The battery cycle fast charging performance is also related to the mass ratio B of the positive electrode active material in the positive electrode active material layer and the specific surface area C m of the positive electrode active material. 2 / g, the specific surface area Em of the negative electrode active material in the negative electrode sheet 2 / g, the mass proportion G of the compound of formula 1 in the electrolyte is closely related. The inventors found that when the battery has high voltage and high rate charge and discharge cycles, when the above parameters meet the following formula: 0.20≤(10×B×G×E 2 ) / C≤3.88, the positive electrode, negative electrode and electrolyte of the battery are best matched, which can minimize the negative impact of the positive electrode active materials and negative electrode active materials on the fast charging performance and cycle performance of the battery, so that the battery has excellent cycle fast charging performance at high voltage. This is because the comprehensive performance of the battery is jointly determined by the electrolyte, positive electrode, negative electrode, and diaphragm parameters. In this application, only when the amount of positive electrode active material satisfies the above formula can the adhesion between the positive electrode active material and the electrode sheet be ensured, thereby improving the cycle performance of the battery. On the other hand, only when the specific surface area of ​​the positive and negative electrodes satisfies the above formula can lithium ions be quickly deintercalated on the formed SEI and CEI interface films, showing excellent kinetic performance, thereby improving the fast charging performance of the battery. Therefore, when the above parameters meet the given formula, the battery has excellent cycle fast charging performance at high voltage.

[0009] In some embodiments, 95%≤B≤99%.

[0010] In some embodiments, 0.2≤C≤2.

[0011] In some embodiments, 0.2≤E≤3.5.

[0012] In some embodiments, 0.5%≤G≤3%.

[0013] In some embodiments, the mass ratio of the compound represented by Formula 1 to LiBF4 is (0.5-3): (0.1-1).

[0014] In some embodiments, based on the total mass of the electrolyte, the mass proportion of LiBF4 is 0.1%-1%.

[0015] In some embodiments, the electrolyte further includes a nitrile compound.

[0016] In some embodiments, the nitrile compound includes at least one of succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,2,3-tris(2-cyanoxy)propane, 1,3,6-hexanetrinitrile and tetracyanoethylene.

[0017] In some embodiments, based on the total mass of the electrolyte, the mass proportion of the nitrile compound is 0.2%-3%.

[0018] In some embodiments, the mass ratio of the compound represented by Formula 1, LiBF4 and the nitrile compound is (0.5-3):(0.1-1):(0.2-3).

[0019] In some embodiments, the positive electrode active material includes at least one of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium-manganese-rich material, lithium nickel-manganese oxide material, lithium iron manganese phosphate and lithium manganese oxide.

[0020] In some embodiments, the negative electrode active material includes at least one of graphite and silicon-carbon material.

[0021] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. DETAILED DESCRIPTION

[0022] The embodiments of the present application are described in detail below, which are intended to be used to explain the present application but should not be construed as limiting the present application.

[0023] During the high-rate battery charge and discharge cycle, metal ions in the positive electrode active material will dissolve, further catalyzing the oxidation decomposition of the electrolyte to produce gas, resulting in reduced stability of SEI and CEI, and reduced deintercalation and insertion ability of lithium ions between the positive and negative electrodes, causing the battery capacity to decay rapidly, thereby degrading the battery's fast-charging performance. This problem is particularly prominent under high voltage.

[0024] In a first aspect, the present application provides a battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, wherein the positive electrode sheet comprises a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material, and based on the total mass of the positive electrode active material layer, the mass proportion of the positive electrode active material is B, and the specific surface area of ​​the positive electrode active material is C m 2 / g; the negative electrode sheet includes a negative electrode active material, and the specific surface area of ​​the negative electrode active material is E m 2 / g; an electrolyte, the electrolyte comprising the compound of Formula 1 and LiBF4, based on the total mass of the electrolyte, the mass proportion of the compound of Formula 1 is G, and satisfies the following formula: 0.20≤(10×B×G×E 2 ) / C≤3.88,

[0025]

[0026] As an example, (10×B×G×E 2 ) / C can have a value of 0.20, 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 3.88, etc.

[0027] The battery in the present application includes a positive electrode sheet, a negative electrode sheet and an electrolyte, and the electrolyte includes a compound shown in Formula 1 and LiBF4. During the fast charging process of the battery, although the compound shown in Formula 1 can preferentially form a stable SEI film on the surface of the negative electrode to improve the battery cycle performance, there is still a problem of gas production during the long cycle process, which affects the safety of the battery. LiBF4 can not only inhibit gas production, but also participate in the formation of a stable CEI, inhibit the dissolution of metal ions in the positive electrode active material, and improve the stability of the positive electrode side. Therefore, the combination of the two can improve the cycle performance of the battery during fast charging. However, the inventors found that during the actual cycle of the battery, the compound shown in Formula 1 and LiBF4 in the electrolyte have limited effects on the battery's cycle fast charging performance, especially the fast charging performance. The battery cycle fast charging performance is also related to the mass ratio B of the positive electrode active material in the positive electrode active material layer and the specific surface area C m of the positive electrode active material. 2 / g, the specific surface area Em of the negative electrode active material in the negative electrode sheet 2 / g, the mass proportion G of the compound of formula 1 in the electrolyte is closely related. The inventors found that when the battery has high voltage and high rate charge and discharge cycles, when the above parameters meet the following formula: 0.20≤(10×B×G×E 2 ) / C≤3.88, the positive electrode, negative electrode and electrolyte of the battery are optimally matched, which can minimize the negative effects of the positive electrode active materials and the negative electrode active materials on the fast charging performance and cycle performance of the battery, making the battery have excellent cycle fast charging performance at high voltage.

[0028] It is understood that in this application, the unit of the specific surface area of ​​the positive electrode active material and the negative electrode active material is m 2 / g, but the present application does not limit the unit of the specific surface area of ​​the positive electrode active material and the negative electrode active material. For example, the unit of the specific surface area can also be m 2 / Kg,cm 2 / g, etc. When the unit of specific surface area is m 2 When the unit is other than g, the unit is converted to m 2 When the formula value obtained after adding 1:1% to 5:1 is between 0.20 and 3.88, it is also within the protection scope of the present application.

[0029] In some embodiments, 95%≤B≤99%, for example, B can be 95%, 96%, 96.5%, 97%, 98%, 98.5%, 99%, etc. The higher the amount of positive electrode active material, the higher the theoretical capacity can be provided. However, when the amount exceeds a certain range, the adhesion between the positive electrode active material and the binder is poor, which greatly reduces the conductivity and thus affects the cycle performance of the battery. The present application ensures the conductivity stability of the battery by controlling the positive electrode active material within the above range, and is conducive to controlling (10×B×G×E 2 ) / C is in the range of 0.20-3.88, thereby improving the fast charging performance of the battery under high voltage.

[0030] In some embodiments, 0.2≤C≤2, for example, C can be 0.2, 0.3, 0.6, 0.9, 1.3, 1.5, 2, etc. There are active sites on the surface of the positive electrode active material. The larger the specific surface area of ​​the positive electrode active material, the more active sites there are, and LiBF4 can combine with the active sites on the surface of the positive electrode active material to form CEI. When the specific surface area is too small, it is difficult for LiBF4 to form a complete CEI on the positive electrode surface. If the specific surface area is too large, a thicker CEI will be formed, which is not conducive to the release of lithium ions. The present application controls the specific surface area of ​​the positive electrode active material to be 0.2m 2 / g-2m 2 / g range, a low impedance and high stability CEI film can be formed, the kinetic performance is improved, and it is beneficial to control (10×B×G×E 2 ) / C is in the range of 0.20-3.88, thereby improving the fast charging performance of the battery under high voltage.

[0031] In some embodiments, 0.2≤E≤3.5, for example, E can be 0.2, 0.8, 1.2, 1.6, 2, 2.8, 3.5, etc. There are also active sites on the surface of the negative electrode material. However, when the specific surface area difference between the positive and negative electrode active materials is too large, it will also lead to the kinetic mismatch between the positive and negative electrodes of the battery. In this application, the specific surface area of ​​the negative electrode active material is controlled to be 0.2m 2 / g-3.5m 2 / g range, the specific surface area of ​​the positive electrode active material matches the specific surface area of ​​the negative electrode active material, which can improve the kinetic performance of the battery and is conducive to controlling (10×B×G×E 2 ) / C is in the range of 0.20-3.88, thereby improving the fast charging performance of the battery under high voltage.

[0032] In some embodiments, 0.5%≤G≤3%, for example, G is 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, etc. When G is within this range, the content of the compound of Formula 1 in the electrolyte is moderate, which can ensure the formation of effective CEI and SEI films with low impedance and high stability on the positive and negative electrode surfaces, and is conducive to controlling (10×B×G×E 2 ) / C is in the range of 0.20-3.88, thereby improving the fast charging performance of the battery under high voltage.

[0033] Since the cycle performance and fast charging performance of lithium-ion batteries are jointly determined by the positive electrode, the negative electrode and the electrolyte, the inventors found that when the compound shown in Formula 1 and LiBF4 are added to the electrolyte, the cycle performance and fast charging performance of the battery can be optimized by adjusting the values ​​of B, G, E and C: wherein, a higher mass proportion B of the positive electrode active material means that more positive electrode active materials participate in the reaction, which can provide more lithium ions, thereby increasing the capacity of the battery; a larger specific surface area C of the positive electrode active material means more lithium ion embedding / de-embedding sites, which can increase the charge and discharge rate of the battery; the specific surface area E of the negative electrode active material is similar to C, which affects the diffusion and reaction rate of lithium ions in the negative electrode, and experiments show that the specific surface area of ​​the negative electrode active material has a square-level effect on the battery performance; the mass proportion G of the compound shown in Formula 1 in the electrolyte affects the SEI film-forming quality of the electrolyte, thereby affecting the cycle performance.

[0034] That is, based on experience and experiments, it is found that within a certain range, each parameter is positively correlated with the effect of cycling and fast charging, and the product (10×B×G×E 2 ) divided by the specific surface area C of the positive electrode active material is for normalization so that the formula is applicable to positive electrode active materials with different specific surface areas. That is, if B, E and G increase, the battery performance may be improved, but at the same time a larger C is required to maintain the charge and discharge rate and cycle stability.

[0035] Formula (10×B×G×E 2 ) / C actually refers to the matching degree of the positive electrode, negative electrode and electrolyte in the battery. Experiments show that (10×B×G×E 2 When the value of ) / C is between 0.20-3.88, the positive electrode, negative electrode and electrolyte of the battery are optimally matched, which can minimize the negative impact of the positive electrode active materials and negative electrode active materials on the fast charging performance and cycle performance of the battery, making the battery have excellent cycle fast charging performance at high voltage. If the formula value is too large or too small, it will lead to unreasonable matching between the negative electrode and the positive electrode, thereby affecting the ion transport of lithium ions in the positive and negative electrodes, and further affecting the cycle performance and rate performance of the battery.

[0036] In some embodiments, based on the total mass of the electrolyte, the mass proportion of LiBF4 is 0.1%-1%, for example, it can be 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1%, etc. Therefore, controlling the mass proportion of LiBF4 within the above range is sufficient to inhibit gas production, and can also participate in the formation of a stable CEI, inhibiting the dissolution of metal ions in the positive electrode active material, and can improve the cycle fast charging performance of the battery at high voltage.

[0037] In some embodiments, the mass ratio of the compound shown in Formula 1 to LiBF4 is (0.5-3): (0.1-1). For example, it can be 2:0.5, 2:0.1, 2:1, 0.5:0.5, 3:0.5, etc. By controlling the mass ratio of the compound shown in Formula 1 to LiBF4 in the electrolyte within the above range, the synergistic effect of the two can be fully exerted, the dissolution of metal ions in the positive electrode active material can be suppressed, the stability of the positive electrode and the negative electrode can be improved, and the cycle performance of the battery during fast charging can be further improved.

[0038] In some embodiments, the electrolyte also includes nitrile compounds. When the battery charging cut-off voltage is above 4.5V, the metal ions in the positive electrode active material will still dissolve under high pressure, and catalyze the decomposition of the electrolyte to produce gas. On this basis, continuing to introduce nitriles into the electrolyte can further improve the fast charging performance under high voltage. This is mainly due to the strong complexation of cyanide and metal ions, which not only inhibits the dissolution of metal ions in the positive electrode active material, avoids excessive oxidative decomposition of the electrolyte during the cycle, but also improves the CEI film and improves the stability of the battery. Therefore, in the electrolyte, the compound shown in Formula 1, LiBF4 and nitrile compounds, the three are used in combination, which can further improve the fast charging performance of the battery under high voltage.

[0039] In some embodiments, the mass ratio of the compound represented by Formula 1, LiBF4 and the nitrile compound is (0.5-3): (0.1-1): (0.2-3). For example, it can be 1:0.5:2, 0.5:0.5:2, 3:0.5:2, 1:0.1:2, 1:1:2, 1:0.5:0.2, 1:0.5:3, etc. Therefore, by controlling the mass ratio of the compound represented by Formula 1, LiBF4 and the nitrile compound within the above range, the synergistic effect of the three can be fully exerted, and the cycle fast charging performance of the battery at a high voltage of more than 4.5V can be further improved.

[0040] In some embodiments, the nitrile compound includes at least one of succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,2,3-tris(2-cyanoxy)propane, 1,3,6-hexanetrinitrile and tetracyanoethylene. The above nitrile compounds are used as electrolyte additives to further improve the cycle fast charging performance of the battery at a high voltage of more than 4.5V.

[0041] In some embodiments, based on the total mass of the electrolyte, the mass proportion of the nitrile compound is 0.2%-3%. For example, it can be 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, etc. Thus, by controlling the content of the nitrile compound in the electrolyte within the above range, the effect of insufficient nitrile compound to inhibit the dissolution of metal ions can be reduced, and the impedance increase caused by excessive nitrile compound can be reduced, which can further improve the cycle fast charging performance of the battery at a high voltage of more than 4.5V.

[0042] In some embodiments, the positive electrode active material includes at least one of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium-rich manganese material, nickel-manganese oxide lithium material, lithium iron manganese phosphate and lithium manganese oxide. The above positive electrode active materials have high energy density and excellent cycle performance, thereby improving the cycle stability of the battery at high voltage.

[0043] In some embodiments, the battery is a lithium-ion battery, and the positive electrode active material includes lithium cobalt oxide, which has excellent cycle performance and high energy density, low probability of side reactions with the compound represented by formula 1, LiBF4 and nitrile compounds in the electrolyte of the present application, and strong high voltage resistance, thereby improving the battery's cycle fast charging performance at high voltage.

[0044] In some embodiments, the electrolyte further includes a non-aqueous organic solvent, and the non-aqueous organic solvent includes at least one of ethylene carbonate, propylene carbonate, γ-butyrolactone, phenyl acetate, 1,4-butane sultone, ethyl methyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl formate, ethyl acetate, methyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, ethylene glycol dimethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, methyl trifluoroethyl carbonate, (2,2,2)-trifluoroethyl carbonate, 2,2-difluoroethyl acetate, 2,2-difluoroethyl propionate and 2,2-difluoroethyl methyl carbonate. The mass proportion of the non-aqueous organic solvent in the electrolyte is 60%-80%. For example, it can be 60%, 65%, 70%, 75%, 80%, etc. When the solvent is within the above range, the battery can be guaranteed to have stable electrochemical properties.

[0045] In some embodiments of the present application, the electrolyte further includes a lithium salt, and the lithium salt includes at least one of LiPF6, LiAsF6, LiClO4, LiB(C2O4)2, LiBF2C2O4, LiN(SO2F)2, LiN(SO2CF3)2, LiPO2F2, LiPF2(C2O4)2 and LiPF4C2O4; the mass proportion of the lithium salt in the electrolyte is 10%-18%. For example, it can be 10%, 12%, 14%, 15%, 18%, etc. The electrolyte salt is controlled within the above range to ensure that the battery has stable electrochemical properties.

[0046] Typically, a battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte, and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0047] The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer arranged on at least one side surface of the positive electrode current collector, wherein the positive electrode active material layer comprises the positive electrode active material mentioned above.

[0048] In some embodiments of the present application, the positive electrode current collector may include a metal foil or a composite positive electrode current collector. For example, the metal foil may be aluminum foil. The composite positive electrode current collector may include a polymer material base and a metal layer formed on at least one side of the polymer material base. For example, the composite positive electrode current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT) and other substrates).

[0049] In some embodiments of the present application, the positive electrode active material layer may further optionally include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0050] In some embodiments of the present application, the positive electrode active material layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.

[0051] In some embodiments of the present application, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, and the binder are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.

[0052] The negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer disposed on at least one side surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material.

[0053] In some embodiments of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), etc.).

[0054] In some embodiments of the present application, the negative electrode active material may be a negative electrode active material for a battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: natural graphite, artificial graphite, soft carbon, hard carbon, mesophase carbon microspheres, nanocarbon, elemental silicon, silicon oxide, silicon carbon composite, silicon alloy, elemental tin, tin oxide, tin carbon composite, tin alloy, lithium titanate.

[0055] In some embodiments of the present application, the negative electrode active material includes at least one of graphite and silicon-carbon material. The above negative electrode active material can better match the positive electrode active material and the electrolyte, adapt to the high voltage and high rate scenarios of the battery, so that the battery has excellent cycle fast charging performance under high voltage.

[0056] In some embodiments of the present application, the negative electrode active material layer may further optionally include a binder. The binder may include at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).

[0057] In some embodiments of the present application, the negative electrode active material layer may further include a conductive agent, which may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0058] In some embodiments of the present application, the negative electrode active material layer may further optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0059] In some embodiments of the present application, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.

[0060] The present application has no particular limitation on the type of isolation membrane, and any known porous isolation membrane with good chemical stability and mechanical stability can be selected.

[0061] In some embodiments of the present application, the material of the isolation membrane may include at least one of glass fiber, non-woven fabric, polyolefin membrane, aromatic polyamide membrane, polytetrafluoroethylene membrane, and polyethersulfone membrane.

[0062] In some embodiments of the present application, the thickness of the isolation film may be 10 μm-12 μm, for example, 10 μm, 11 μm, 12 μm, etc.

[0063] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.

[0064] Example 1

[0065] 1. Preparation of positive electrode sheet

[0066] The positive electrode active material (lithium cobalt oxide), binder polyvinylidene fluoride PVDF, conductive carbon black, and conductive carbon nanotubes were mixed evenly in a weight ratio of 95:2.3:2:0.7, and N-methylpyrrolidone NMP was added and stirred under the action of a vacuum mixer until the mixed system became a positive electrode slurry with uniform fluidity; the positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and the coating amount was 35g / m 2 After drying at 85°C, cold pressing is performed, trimming, cutting, and slitting are performed. After slitting, drying is performed at 85°C under vacuum conditions for 4 hours, and the tabs are welded to obtain the positive electrode sheet. The specific surface area C of lithium cobalt oxide is 0.6m 2 / g.

[0067] 2. Preparation of negative electrode sheet

[0068] The negative electrode active material graphite, the conductive agent carbon black, the thickener sodium carboxymethyl cellulose (CMC-Na), and the binder styrene-butadiene rubber were mixed in a weight ratio of 95:1.5:1:2.5, and deionized water was added to obtain the negative electrode slurry under the action of a vacuum mixer; the negative electrode slurry was evenly coated on the negative electrode current collector copper foil, and the coating amount was 20g / m 2 After drying at 85°C, cold pressing is performed, trimming, cutting, and slitting are performed. After slitting, drying is performed at 85°C under vacuum conditions for 4 hours, and the tabs are welded to obtain the negative electrode sheet. The specific surface area E of the graphite is 1.6 m 2 / g.

[0069] 3. Preparation of electrolyte

[0070] In a glove box filled with argon (water <10ppm, oxygen <1ppm), the solvents ethylene carbonate, propylene carbonate, diethyl carbonate, and propyl propionate are mixed uniformly in a mass ratio of 1:1:1:2, and fully dried lithium hexafluorophosphate is quickly added to the mixed solvent. The molar concentration of lithium hexafluorophosphate in the electrolyte is 1 mol / L, and the compound shown in formula 1, LiBF4, and succinonitrile are added in sequence, and the electrolyte is obtained after being fully mixed. Among them, the mass proportion of the compound shown in formula 1 in the electrolyte is 2%, the mass proportion of LiBF4 in the electrolyte is 0.2%, and the mass proportion of succinonitrile in the electrolyte is 2%.

[0071] 4. Isolation film

[0072] A polyethylene isolation film with a thickness of 8 μm was selected.

[0073] 5. Lithium-ion battery preparation

[0074] The positive electrode sheet, negative electrode sheet and separator prepared according to the above process are wound into a lithium-ion battery with a thickness of 4.7 mm, a width of 55 mm and a length of 60 mm, and vacuum baked at 85°C for 10 hours, and the above-prepared electrolyte is injected. After standing for 24 hours, the battery is placed in an environment of 45°C, a pressure of 3 kg is applied, and after charging to 4.5V at 0.1C (195mA), it is stood for more than 24 hours under the same temperature and pressure conditions (to fully activate the battery) to obtain a battery.

[0075] Among them, (10×B×G×E 2 ) / C=0.81.

[0076] The preparation methods of the lithium-ion batteries of Examples 2-27 and Comparative Examples 1-8 are substantially the same as that of Example 1, but the electrolyte compositions, positive electrode active materials, and negative electrode active materials thereof are different, as shown in Table 1.

[0077] Among them, Comparative Example 1 contains two additives (the compound shown in Formula 1 and LiBF4), but the formula (10×B×G×E 2 ) / C value is too low; Comparative Example 2 contains three additives (compound shown in Formula 1, LiBF4 and nitrile compound), but the formula (10×B×G×E 2 ) / C value is too low; Comparative Example 3 contains two additives (the compound shown in Formula 1 and LiBF4), but the formula (10×B×G×E 2 ) / C value is too high; Comparative Example 4 contains three additives (compound shown in Formula 1, LiBF4 and nitrile compound), but the formula (10×B×G×E 2 ) / C value is too high; LiBF4 is not added to the electrolytes of Comparative Examples 5 and 7, and the compound represented by Formula 1 is not added to the electrolytes of Comparative Examples 6 and 8.

[0078] Table 1

[0079]

[0080]

[0081] The batteries prepared in Examples 1-27 and Comparative Examples 1-8 were subjected to a room temperature cycle fast charge test at 25°C, and the capacity retention rate and expansion rate of the batteries after 800 cycles were recorded. The performance test results are shown in Table 2.

[0082] At 25°C, place the lithium-ion battery aside for 5 minutes, charge it to 4.50V at a constant current rate of 2C, place it aside for another 5 minutes, then charge it at a constant current and constant voltage until the current is less than or equal to 0.05C, place it aside for 5 minutes, and then discharge it to 3.0V at a constant current rate of 1C. Perform the charge and discharge test for 800 cycles in this way, record the maximum discharge capacity of the first 5 cycles as Q, select the discharge capacity at 800 cycles as Q1, and the calculation method for the capacity retention rate after 800 cycles is as follows:

[0083] Capacity retention rate after 800 cycles (%) = Q1 / Q×100.

[0084] The thickness of the fresh battery is measured by a thickness tester, recorded as P1, and the thickness of the battery after 800 cycles is recorded as P2. The calculation formula for the expansion rate of the battery after 800 cycles is:

[0085] Cycle 800 cycles battery expansion rate (%) = P2 / P1×100

[0086] Table 2

[0087]

[0088] It can be seen from the data in Table 2 that the capacity retention rates of the batteries of Examples 1-27 are significantly higher than those of Comparative Examples 5-8, and the expansion rates are lower, indicating that the synergistic effect of LiBF4 and the compound represented by Formula 1 can ensure the fast-charging performance of the battery under high voltage. It can be seen from Examples 1, 9-27 and Examples 2-8 that nitrile compounds can further improve the fast-charging performance of the battery under high voltage. In addition, Comparative Examples 2 and 4 add a suitable ratio of the compound represented by Formula 1 and LiBF4, and Comparative Examples 1 and 3 add a suitable ratio of the compound represented by Formula 1, LiBF4 and a nitrile compound, but the formula (10×B×G×E 2 ) / C calculated value is not between 0.2 and 3.88, and the capacity retention rate of the battery is also much lower than that of Examples 1-27, indicating that the present application adds the compound shown in Formula 1 and LiBF4 in the electrolyte and the formula value satisfies between 0.2 and 3.88, or adds the compound shown in Formula 1, LiBF4 and a nitrile compound in the electrolyte and the formula value satisfies between 0.2 and 3.88, which can achieve excellent cycle fast charging performance under high voltage.

[0089] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0090] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A battery, characterized in that: include: A positive electrode sheet, the positive electrode sheet comprising a positive electrode active material layer, the positive electrode active material layer comprising a positive electrode active material, based on the total mass of the positive electrode active material layer, the mass proportion of the positive electrode active material is B, and the specific surface area of ​​the positive electrode active material is Cm 2 / g; A negative electrode sheet, the negative electrode sheet comprising a negative electrode active material, the specific surface area of ​​the negative electrode active material is E m 2 / g; An electrolyte, the electrolyte comprising a compound represented by Formula 1 and LiBF4, wherein the mass proportion of the compound represented by Formula 1 is G based on the total mass of the electrolyte, Satisfy the following formula: 0.20≤(10×B×G×E 2 ) / C≤3.88, 2. The battery according to claim 1, characterized in that 95%≤B≤99%。 3. The battery according to claim 1, characterized in that 0.2≤C≤2。 4. The battery according to claim 1, characterized in that 0.2≤E≤3.5。 5. The battery according to claim 1, characterized in that 0.5%≤G≤3%。 6. The battery according to any one of claims 1 to 5, characterized in that The mass ratio of the compound represented by Formula 1 to the LiBF4 is (0.5-3):(0.1-1).

7. The battery according to any one of claims 1 to 5, characterized in that Based on the total mass of the electrolyte, the mass proportion of LiBF4 is 0.1%-1%.

8. The battery according to any one of claims 1 to 5, characterized in that The electrolyte also includes a nitrile compound.

9. The battery according to claim 8, characterized in that The mass ratio of the compound represented by Formula 1, the LiBF4 and the nitrile compound is (0.5-3): (0.1-1): (0.2-3); and / or, Based on the total mass of the electrolyte, the mass proportion of the nitrile compound is 0.2%-3%; and / or, The nitrile compound includes at least one of succinonitrile, adiponitrile, 1,2-bis(2-cyanoethoxy)ethane, 1,2,3-tris(2-cyanoxy)propane, 1,3,6-hexanetrinitrile and tetracyanoethylene.

10. The battery according to any one of claims 1 to 5, characterized in that The positive electrode active material comprises at least one of lithium cobalt oxide, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium-manganese-rich material, lithium nickel-manganese oxide material, lithium iron manganese phosphate and lithium manganese oxide; and / or, The negative electrode active material includes at least one of graphite and silicon-carbon material.

Citation Information

Cited By

  • Formation method of battery and battery

    CN119009211A

  • Battery

    DE212024000367U1

  • battery

    EP4730465A1

  • battery

    WO2026031369A1