Battery

By using sulfate compounds and lithium salts containing oxalate as electrolyte additives in the battery, the free movement of lithium salts is restricted, and the problems of gas production and SEI film rupture in high-energy-density batteries are solved, and the battery is improved High temperature performance and cycle stability.

CN118800970BActive Publication Date: 2024-11-22GUANGZHOU TINCI MATERIALS TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411283546.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-22
Estimated Expiration
2044-09-13

AI Technical Summary

Technical Problem

High-energy density lithium-ion batteries are prone to gas production and SEI film rupture problems under high temperature conditions, resulting in poor battery high-temperature performance.

Method used

The battery design adopts a battery including sulfate compounds and lithium salts containing oxalate as electrolyte additives. Through the clamp structure of sulfate compounds and the mutual repulsion of lithium salts, the free movement of lithium salts is restricted, and gas production reactions are reduced. Destruction of SEI membrane.

Benefits of technology

It effectively alleviates the gas production and SEI film rupture problems in high-energy density batteries, and improves the high-temperature performance and long-cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118800970B_ABST
    Figure CN118800970B_ABST
Patent Text Reader

Abstract

The present application discloses a battery, including: a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the porosity of the negative electrode plate is φ, in units of %; the thickness of the separator is t, in units of μm; the pore size of the separator is R, in units of μm; the ratio of the total mass of the electrolyte to the discharge capacity of the battery is N, in units of g / Ah; the electrolyte includes an electrolyte additive, and the electrolyte additive includes: a sulfate compound and a first lithium salt, wherein the first lithium salt includes a lithium salt containing oxalate, the sulfate compound has a structure shown in Formula I, and the mass fraction of the sulfate compound in the electrolyte is C, in units of %; the battery satisfies Formula A, #imgabs0#, Formula A. Thus, the battery can effectively alleviate the problems of gas production and SEI membrane rupture and recombination in high energy density batteries, and improve the high temperature performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular, to a battery. Background Art

[0002] With the development of the new energy industry, higher energy density of power batteries has become a hot spot in the industry's research and development. The use of high-energy-density negative electrode active materials and high-specific-energy positive electrode active materials can effectively improve the energy density of lithium-ion batteries. However, at present, high-energy-density batteries are prone to gas production and SEI membrane (Solid Electrolyte Interface) rupture under high temperature conditions, which makes the high-temperature performance of the battery poor. Therefore, it is urgent to develop batteries with better high-temperature performance. Summary of the invention

[0003] In a first aspect of the present application, the present application proposes a battery, comprising: a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the porosity of the negative electrode sheet is φ, in units of %; the thickness of the separator is t, in units of μm; the pore size of the separator is R, in units of μm; the ratio of the total mass of the electrolyte to the discharge capacity of the battery is N, in units of g / Ah; the electrolyte comprises an electrolyte additive, the electrolyte additive comprises: a sulfate compound and a first lithium salt additive, the first lithium salt additive comprises a lithium salt containing oxalate, the sulfate compound has a structure shown in Formula I, Formula I, R1, R8 are independently selected from hydrogen, C1-C5 hydrocarbon group,

[0004] R2, R3, R4, R5, R6, and R7 are each independently selected from a C1-C3 alkylene group, a C1-C3 alkoxy group, an oxygen atom, or , n is an integer of 0-4, the mass fraction of the sulfate ester compound in the electrolyte is C, in units of %; the battery satisfies formula A, , Formula A. Therefore, the battery can effectively alleviate the problems of gas production and SEI film rupture and recombination in high energy density batteries and improve the high temperature performance of the battery.

[0005] In some embodiments, φ is 60%-80%; and / or t is 12 μm-20 μm; and / or R is 0.03 μm-0.12 μm; and / or C is 0.1%-10%; and / or N is 2.0-5.0. Thus, the high temperature performance of the battery can be further improved.

[0006] In some embodiments, R1 and R8 are independently selected from hydrogen,

[0007] At least one of R2, R3, and R4 is selected from or , and at least one of R2, R3, and R4 is selected from an oxygen atom,

[0008] At least one of R5, R6 and R7 is selected from or , and at least one of R5, R6, and R7 is selected from an oxygen atom,

[0009] n is 2.

[0010] In some embodiments, the sulfate compound has one of the following structures:

[0011] , , , , .

[0012] In some embodiments, the first lithium salt additive includes at least one of lithium difluorooxalatoborate, lithium dioxalatoborate, lithium tetrafluorooxalatophosphate, lithium difluorodioxalatophosphate, and lithium trioxalatophosphate, thereby helping to improve the high temperature performance, conductivity, and cycle performance of the battery.

[0013] In some embodiments, the molar ratio of the first lithium salt additive to the sulfate compound is 1:(1-5). Thus, the inhibitory effect of the sulfate compound on the first lithium salt additive can be further enhanced, so that the hindered first lithium salt additive is not easy to move freely.

[0014] In some embodiments, the mass fraction of the first lithium salt additive in the electrolyte is 0.1%-5%, and / or the mass fraction of the sulfate compound in the electrolyte is 1%-10%. Thus, the stability of the battery under high temperature and long cycle can be improved.

[0015] In some embodiments, the electrolyte additive further includes an electrolyte lithium salt, and the electrolyte lithium salt includes at least one of LiBF4, LiPF6, LiAsF6, and LiN(SO2F)2. Thus, the electrolyte lithium salt can further inhibit the corrosion of the SEI film and the CEI film by hydrofluoric acid.

[0016] In some embodiments, the mass ratio of the electrolyte lithium salt to the first lithium salt additive is 1: (0.4-2).

[0017] In some embodiments, the mass fraction of the electrolyte lithium salt in the electrolyte is 0.1%-1%. Thus, the stability of the battery under high temperature and long cycle can be further improved.

[0018] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes at least one of lithium iron phosphate and a ternary material. Among them, the ternary material satisfies the chemical formula LiNi x Co y M1 z1 M2 z2 O2, where M1 and M2 are each independently selected from one of Al, Mn, and Fe, and M1 and M2 are different, 0 < x ≤ 1, 0 < y < 1, 0 < z1 < 1, 0 ≤ z2 < 1, and x + y + z1 + z2 = 1.

[0019] In some embodiments, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material, and the mass fraction of silicon in the negative electrode active material is greater than 8%. Detailed implementation manners

[0020] The following embodiments are exemplary and are only used to explain the present application and should not be construed as a limitation to the present application.

[0021] Unless otherwise defined, all technical and scientific terms used in the present application have the same meaning as commonly understood by those skilled in the technical field to which the present application belongs; the terms used in the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application; unless otherwise specified, the numerical values of the various parameters mentioned in the present application can be measured by various commonly used measurement methods in the art (for example, they can be tested according to the methods given in the embodiments of the present application).

[0022] The terms "include" and "have" and any variations thereof in the description and claims of the present application are open-ended expressions, that is, they include the content specified in the present application, but do not exclude other aspects.

[0023] In a first aspect of the present application, the present application provides a battery, including: a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. The porosity of the negative electrode sheet is φ, in units of %; the thickness of the separator is t, in units of μm; the pore size of the separator is R, in units of μm; the ratio of the total mass of the electrolyte to the discharge capacity of the battery is N, in units of g / Ah; the electrolyte includes an electrolyte additive, and the electrolyte additive includes: a sulfate compound and a first lithium salt additive. The first lithium salt additive includes a lithium salt containing an oxalate group, and the sulfate compound has the structure shown in Formula I, Formula I, where R1 and R8 are each independently selected from hydrogen and a C1-C5 hydrocarbon group,

[0024] R2, R3, R4, R5, R6, and R7 are each independently selected from a C1-C3 alkylene group, a C1-C3 alkoxy group, an oxygen atom, or , n is an integer of 0-4, the mass fraction of the sulfate ester compound in the electrolyte is C, in units of %; the battery satisfies formula A, , Formula A. Therefore, the battery can effectively alleviate the problems of gas production and SEI film rupture and recombination in high energy density batteries and improve the high temperature performance of the battery.

[0025] In the present application, the sulfate ester compound has a pincer structure, and the pincer structure is surrounded by multiple double-bonded oxygens (such as carbonyl groups, sulfur-oxygen double bonds, etc.) and single-bonded oxygen atoms. The lithium salt containing oxalate has a structure similar to an "X" type, and the molecular structure also has multiple carbonyl groups. When these two polar molecules are mixed, based on the spatial stereoscopic structure of the two polar molecules, the lithium salt molecules containing oxalate can be inserted into the structural gaps of the carbonyl and sulfur-oxygen double bonds in the sulfate ester compound, so as to limit the free movement of the lithium salt containing oxalate to a certain extent; on the other hand, when mixed, the two polar molecules will repel each other due to the large number of carbonyl groups and / or sulfur-oxygen double bonds in their structures. This mutually repulsive orientation force causes the lithium salt molecules containing oxalate and the molecules of the sulfate ester compound to rotate relative to each other to balance the force between them. A repulsive effect, that is, the planar configuration of the two substances tends to an intersecting state from a quasi-parallel state, which is conducive to the large cluster structure of the carbonyl and sulfur-oxygen double bonds in the sulfate ester compounds tending to insert into the structural gap of the oxalate-containing lithium salt molecules, thereby producing a steric hindrance to the oxalate-containing lithium salt. The repulsive effect between the two polar molecules is conducive to the clamp-shaped structure of the sulfate ester to restrict the free movement of the oxalate-containing lithium salt molecules; under the dual effects of mutual repulsion between molecular forces and spatial restrictions, the hindered oxalate-containing lithium salt is more difficult to produce free movement.

[0026] When the electrolyte additive is used in a battery, the free movement of the hindered oxalate-containing lithium salt is reduced, thereby reducing the direct contact between the oxalate and the electrode, making it difficult for the oxalate to produce gas. At the same time, it also reduces the damage to the SEI film caused by the expansion of the battery due to gas production, thereby improving the stability under high temperature and long cycles.

[0027] Furthermore, φ×C×N in Formula A can indicate the total influence of favorable factors as a whole. Specifically, when the porosity φ of the negative electrode plate is large, the transmission rate of lithium ions can be improved, thereby improving the fast charge cycle performance; the greater the mass fraction C of sulfate ester compounds in the electrolyte within a specific range, the better the improvement effect on performance; the ratio N of the total mass of the electrolyte to the discharge capacity of the battery reflects the strong discharge capacity of sulfate ester compounds; t×R in Formula A can indicate the total influence of unfavorable factors as a whole. Specifically, when the thickness t of the isolation membrane is too thick, or the pore size R of the isolation membrane is too large, the internal impedance of the battery will be large, and large molecular impurities will pass through the isolation membrane and cause side reactions at the pole piece, which will deteriorate the battery performance. Therefore, when When the internal impedance of the battery is too high, the adverse side reactions will be aggravated. When it is too large, the battery output voltage is unstable and toxic gas may be generated.

[0028] Furthermore, when the sulfate ester compound is used in combination with the first lithium salt additive, the aforementioned battery is suitable for a battery system using a medium-nickel positive electrode and a silicon-based negative electrode, and can exert its advantageous effects in this battery system.

[0029] It should be noted that in the electrolyte additive of the present application: the mutual repulsion between polar molecules produces orientation force and spatial restriction effect, which does not completely prevent the oxalate-containing lithium salt from exerting its advantages, but effectively slows down the movement of the oxalate-containing lithium salt, making it difficult for its gas production reaction to occur, thereby reducing the damage to the SEI membrane, and promoting the performance stability of the battery under high temperature and long cycle.

[0030] The term C1-C5 hydrocarbon group refers to a saturated straight-chain or branched hydrocarbon radical containing 1 to 5 carbon atoms, such as CH3-, C2H5-, etc.

[0031] The term C1-C3 alkylene refers to a straight chain saturated hydrocarbon group containing 1 to 3 carbon atoms, such as methylene, ethylene, and the like.

[0032] The term C1-C3 alkoxy refers to a group -OR, wherein R is a C1-C3 alkyl group, such as ethoxy, n-propoxy, and the like.

[0033] As an example, n is an integer from 0 to 4, such as 0, 1, 2, 3, 4, etc.

[0034] Sulfate ester compounds have a pincer structure, and the pincer structure is surrounded by multiple double-bonded oxygen atoms (such as carbonyl, sulfur-oxygen double bonds, etc.) and single-bonded oxygen atoms.

[0035] When the first lithium salt additive is used in the electrolyte of the battery, it helps to improve the high temperature performance, conductivity and cycle performance of the battery. This is because the oxalate in the first lithium salt additive has a larger electronegativity with respect to the fluorine element, and can also form a covalent bond with the carbon element, thereby increasing the boiling point of the electrolyte; at the same time, it can also cause the compounds in the electrolyte to form small solvent clusters to promote the fluidity and conductivity of the electrolyte.

[0036] In some embodiments, φ is 60%-80%; and / or t is 12 μm-20 μm; and / or R is 0.03 μm-0.12 μm; and / or C is 0.1%-10%; and / or N is 2.0-5.0. Thus, the high temperature performance of the battery can be further improved.

[0037] When the porosity φ of the negative electrode sheet is within the aforementioned range, more space for expansion can be provided, thereby effectively alleviating the volume expansion of the negative electrode active material, for example, silicon-based material, and effectively maintaining the integrity of the negative electrode SEI film.

[0038] When the thickness t of the isolation film is within the aforementioned range, it can not only hinder the movement of the lithium salt containing oxalate, but also have less adverse effect on the lithium ion transmission rate.

[0039] When the ratio N of the total mass of the electrolyte to the discharge capacity of the battery is within the aforementioned range, the discharge capacity of the battery is better.

[0040] When the pore size R of the isolation membrane is within the aforementioned range, the migration ability of lithium ions in the electrolyte is better.

[0041] In some embodiments, R1 and R8 are independently selected from hydrogen,

[0042] At least one of R2, R3, and R4 is selected from or , and at least one of R2, R3, and R4 is selected from an oxygen atom,

[0043] At least one of R5, R6 and R7 is selected from or , and at least one of R5, R6, and R7 is selected from an oxygen atom,

[0044] n is 2.

[0045] In some embodiments, the sulfate compound has one of the following structures:

[0046] , , , , .

[0047] In some embodiments, the first lithium salt additive includes at least one of lithium difluorooxalatoborate, lithium dioxalatoborate, lithium tetrafluorooxalatophosphate, lithium difluorodioxalatophosphate, and lithium trioxalatophosphate, thereby helping to improve the high temperature performance, conductivity, and cycle performance of the battery.

[0048] As an example, the first lithium salt additive is lithium difluorooxalate borate, which is beneficial for improving electrical conductivity, optimizing high and low temperature performance and thermal stability.

[0049] In some embodiments, the molar ratio of the first lithium salt additive to the sulfate compound is 1:(1-5). Thus, the inhibitory effect of the sulfate compound on the first lithium salt additive can be further enhanced, so that the hindered first lithium salt additive is not easy to move freely.

[0050] In some embodiments, the molar ratio of the first lithium salt additive to the sulfate ester compound is 1:(1-5), for example, 1:1, 1:1.6, 1:2, 1:3, 1:3.4, 1:4, 1:5, etc.

[0051] In some embodiments, the molar ratio of the first lithium salt additive to the sulfate compound is 1:(2-4). Thus, the sulfate compound is in a slightly excessive state relative to the first lithium salt additive, which can further enhance the inhibitory effect of the sulfate compound on the first lithium salt additive, thereby making it difficult for the hindered first lithium salt additive to move freely.

[0052] In some embodiments, the mass fraction of the first lithium salt additive in the electrolyte is 0.1%-5%.

[0053] As an example, the mass fraction of the first lithium salt additive in the electrolyte is 0.1%, 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, etc. Thus, the stability of the battery under high temperature and long cycle is further improved.

[0054] In some embodiments, the mass fraction C of the sulfate ester compound in the electrolyte is 1%-10%.

[0055] As an example, the mass fraction of the sulfate compound in the electrolyte is 1%, 1.07%, 1.4%, 1.7%, 2%, 3%, 3.4%, 4%, 5%, 6%, 6.9%, 7%, 8%, 8.7%, 9%, 10%, etc. Thus, the stability of the battery under high temperature and long cycle is further improved.

[0056] There is fluorine in the electrolyte. As the battery reaction proceeds, fluorine will produce hydrogen fluoride, which will corrode the SEI membrane and CEI membrane, causing problems such as attenuation of the battery's high-temperature storage capacity and gas production and swelling.

[0057] In some embodiments, the electrolyte additive also includes an electrolyte lithium salt, and the electrolyte lithium salt includes at least one of LiBF4, LiPF6, LiAsF6, and LiN(SO2F)2. As a result, the electrolyte lithium salt can further inhibit the corrosion of hydrofluoric acid on the SEI membrane and the CEI membrane. As a result, the first lithium salt additive, the sulfate compound and the electrolyte lithium salt interact with each other, not only making it difficult for the hindered oxalate-containing lithium salt to move freely. The first lithium salt additive can also inhibit the hydrolysis of the oxalate-containing lithium salt, and at the same time, for the fluorine-containing lithium salt therein, it can weaken the generation of fluoride ions and reduce the generation of hydrofluoric acid, thereby reducing the corrosion of hydrofluoric acid on the SEI membrane and the CEI membrane, increasing the high-temperature storage capacity of the battery, and helping to reduce the gas bulging of the battery.

[0058] Furthermore, the electrolyte lithium salt is LiBF4. LiBF4 has strong stability at high temperatures, which is beneficial for further inhibiting the generation of hydrogen fluoride and improving the high temperature performance of the battery.

[0059] In some embodiments, the mass ratio of the electrolyte lithium salt to the first lithium salt additive is 1: (0.4-2).

[0060] In some embodiments, the mass ratio of the electrolyte lithium salt to the first lithium salt additive is 1:(0.4-2), for example, 1:0.4, 1:0.5, 1:1, 1:1.5, 1:75, 1:1, etc.

[0061] In some embodiments, the mass fraction of the electrolyte lithium salt in the electrolyte is 0.1%-1%. Thus, the stability of the battery under high temperature and long cycle can be further improved.

[0062] As an example, the mass fraction of the electrolyte lithium salt in the electrolyte is 0.1%, 0.15%, 0.3%, 0.5%, 0.8%, 1%, etc. Thus, the stability of the battery under high temperature and long cycle is further improved.

[0063] In the present application, the electrolyte may also optionally include a second additive, and the second additive may be selected according to the specific application of the electrolyte in different batteries.

[0064] In some embodiments, the second additive includes at least one of dithiothreitol (DTD), dithiothreitol carbonate, fluoroethylene carbonate (FEC), dithiothreitol carbonate, dithiothreitol sulfate, 1,3-propane sultone, 1,3-propylene sultone, dithiothreitol, tris(trimethylsilyl) borate, and tris(trimethylsilyl) phosphate. Thus, the electrolyte is particularly suitable for use in silicon negative electrode batteries to further improve the cycle performance and high temperature storage performance of the battery.

[0065] In some embodiments, the mass fraction of the second additive in the electrolyte is 0.5%-20%, for example 0.5%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, 15%, 20%, etc.

[0066] In the present application, the electrolyte may be a non-aqueous electrolyte, and the solvent of the non-aqueous electrolyte is an organic solvent.

[0067] In some embodiments, the organic solvent includes at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, dimethyl carbonate, diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, γ-butyrolactone, γ-valerolactone, δ-valerolactone, and ε-caprolactone.

[0068] In some embodiments, the mass fraction of the organic solvent in the electrolyte is 10%-80%.

[0069] In some embodiments, the organic solvent includes EC, PC, EMC and DEC. EC has a high dielectric constant, which can ensure that the lithium salt is fully dissolved and ionized, which is beneficial to improve the conductivity of the electrolyte and ensure the cycle life; EMC and DEC are linear carbonates, which have the advantages of low viscosity and low melting point compared with cyclic carbonates (EC). Therefore, PC, EMC, DEC and EC are mixed as electrolyte solvents to improve battery performance.

[0070] In some embodiments, the mass ratio of the organic solvent to the sulfate compound in the electrolyte is (8-170):1, such as 8:1, 15:1, 30:1, 40:1, 75:1, 95:1, 120:1, 140:1, 170:1, etc. Thus, the stability of the battery under high temperature and long cycle is further improved.

[0071] In the present application, the electrolyte may further include a third lithium salt, and the third lithium salt may further include at least one of lithium perchlorate, lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, and lithium hexafluoroarsenate.

[0072] In some embodiments, the mass fraction of the third lithium salt in the electrolyte is 10%-20%, for example, 10%, 13%, 15%, 18%, 20%, etc.

[0073] Generally, in addition to the electrolyte, the battery further includes a positive electrode plate, a negative electrode plate, and a separator. During the charging and discharging process of the battery, active ions are embedded and extracted back and forth between the positive electrode plate and the negative electrode plate. The electrolyte plays a role in conducting ions between the positive electrode plate and the negative electrode plate. The separator is disposed between the positive electrode plate and the negative electrode plate, mainly to prevent short circuit between the positive electrode and the negative electrode, and at the same time allows ions to pass through.

[0074] In some embodiments, the positive electrode plate includes a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes at least one of lithium iron phosphate and a ternary material. Among them, the ternary material satisfies the chemical formula LiNi x Co y M1 z1 M2 z2 O2, where M1 and M2 are each independently selected from one of Al, Mn, and Fe, and M1 and M2 are different, 0 < x ≤ 1, 0 < y < 1, 0 < z1 < 1, 0 ≤ z2 < 1, and x + y + z1 + z2 = 1.

[0075] In some embodiments, when the ternary material is a cobalt-containing positive electrode active material, under the dual action of the steric hindrance and the intermolecular force repulsion between the sulfate compound and the first lithium salt additive, the oxalate structure near the electrode is significantly reduced, so that the probability of the dissolved Co element forming cobalt oxalate precipitate with oxalate is greatly reduced, thereby reducing the damage of the precipitate to the electrode and reducing the impedance of the battery; the sulfate compound can also react with the dissolved Co element to form a complex reaction, reducing the occurrence of side reactions of the dissolved Co element in the battery system, and further improving the stability of the battery under high-temperature long-term cycling; partial decomposition of the sulfate compound also occurs at the negative electrode of the battery to form a solid electrolyte interface film, and this solid electrolyte interface film can play a role in restricting the extraction of Co elements. Therefore, the electrolyte containing the electrolyte additive of the first aspect or the electrolyte of the second aspect is particularly suitable for use with a cobalt-containing positive electrode active material in the battery system.

[0076] As an example, the positive electrode active material includes LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622), LiNi 0.6 Co 0.1 Mn 0.3 O2 (NCM613), LiNi 0.5 Co 0.2 Mn 0.3 O2 (NCM523), etc.

[0077] In some embodiments, the positive electrode active material includes lithium iron phosphate. As a result, the sulfate ester compound can also react with the dissolved metal elements (such as Fe element) to reduce the occurrence of side reactions of the dissolved metal elements in the battery system, thereby improving the stability of the battery under high temperature and long cycle; the battery negative electrode will also partially decompose the sulfate ester compound and form a solid electrolyte interface film, which can limit the release of metal elements.

[0078] In some embodiments, the positive electrode active material layer may further include a binder, and specific examples of the binder include, but are not limited to, one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, and styrene-butadiene rubber (SBR).

[0079] In some embodiments, the positive electrode active material layer may further include a conductive agent, and specific examples of the conductive agent include, but are not limited to, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and the like.

[0080] In some embodiments, the positive electrode current collector may be a metal foil, such as an aluminum foil.

[0081] In some embodiments, the negative electrode plate includes a negative current collector and a negative active material layer located on at least one side of the negative current collector, the negative active material layer includes a negative active material, and the mass fraction of silicon in the negative active material is greater than 8%. The energy density of the battery can be effectively improved by increasing the specific capacity of the negative active material. The current specific capacity of graphite materials has reached its theoretical capacity upper limit (372mAh / g), while the highest theoretical specific capacity of silicon-based negative active materials can reach 4200mAh / g, and silicon-based negative active materials have great application prospects. The volume of silicon-based negative active materials changes greatly during the charge and discharge process of the battery. During repeated charge and discharge cycles, due to the excessive change in its own volume expansion and contraction, the SEI film on the surface of the silicon-based negative electrode will repeatedly break and form, and the electrolyte will be continuously consumed, resulting in poor battery cycle performance. In this application, by optimizing the composition of the electrolyte additive, the corrosion and gas production problems of SEI can be effectively improved.

[0082] In some embodiments, the negative electrode active material layer may further include a binder, and specific examples of the binder include, but are not limited to, one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), polyacrylamide (PAM), and polyvinylidene fluoride (PVDF).

[0083] In some embodiments, the negative electrode active material layer may further include a conductive agent, and specific examples of the conductive agent include, but are not limited to, superconducting carbon, acetylene black, carbon black, graphene, and the like.

[0084] In some embodiments, the negative active material layer may further include a thickener, such as sodium carboxymethyl cellulose (CMC-Na).

[0085] The present application has no particular restriction on the type of isolation membrane, and various porous structure isolation membranes with good stability can be selected, such as polyethylene isolation membranes, polypropylene isolation membranes, PE ceramic coated isolation membranes, etc.

[0086] The scheme of the present application is described below through specific embodiments. It should be noted that the following embodiments are only used to illustrate the present application and should not be regarded as limiting the scope of the present application.

[0087] In the following embodiments:

[0088] Compound 1 is: ,CAS:2520352-94-5;

[0089] Compound 2 is: ,CAS:201419-80-9.

[0090] Compound 3 is: .

[0091] Compound 4 is: .

[0092] Compound 5 is: .

[0093] The following examples are used to illustrate the application of the electrolyte additive of the present application and the electrolyte containing the same in a lithium-ion battery with an NCM613 positive electrode.

[0094] Example 1a

[0095] Positive electrode preparation:

[0096] The positive electrode active material NCM613, the binder polyvinylidene fluoride (PVDF), the conductive agent SP, and the conductive agent CNT are mixed in a weight ratio of 95:3:0.5:1.5, and N-methylpyrrolidone (NMP) is added to form a slurry, and the solid content is controlled to 55%. Stir under the action of a vacuum mixer until the mixed system becomes a positive electrode slurry with uniform fluidity; the positive electrode slurry is evenly coated on an aluminum foil with a thickness of 16μm; the aluminum foil coated with the positive electrode slurry is dried in an oven at 120°C for 8h. Finally, after roller pressing, the compaction density of the positive electrode sheet is controlled to be 3.5g / cm 3 , cut to obtain the positive electrode sheet.

[0097] Negative electrode sheet preparation:

[0098] Graphite / Zichen Silicon Carbon 550-M5-230415 negative electrode active material, conductive agent SP, binder SBR (JSR-104A), thickener CMC (crt30000PA) were mixed in a weight ratio of 95:1.5:2:1.5, and water was added to form a slurry. The solid content of the slurry was controlled to 45%, and the negative electrode slurry was obtained by stirring under the action of a vacuum mixer; the negative electrode slurry was evenly coated on a copper foil with a thickness of 9μm; the copper foil coated with the negative electrode slurry was dried at 85°C for 5h. Finally, after roller pressing, the compaction density of the negative electrode sheet was controlled to be 1.6g / cm 3 , cut to obtain the negative electrode sheet, the porosity φ of the negative electrode sheet is 70%.

[0099] Preparation of electrolyte:

[0100] In a glove box filled with argon (water <10ppm, oxygen <1ppm), the solvents EC:PC:DEC:EMC were mixed evenly in a mass percentage of 3:3:4:10 to obtain an organic solvent. The following electrolyte additives (compound 1 and the first lithium salt additive (lithium difluorooxalatoborate)), electrolyte lithium salt (LiBF4), and the second additive (FEC and DTD) were added to the organic solvent and stirred evenly to obtain a non-aqueous electrolyte. The mass of the electrolyte was 9g.

[0101] Preparation of isolation membrane:

[0102] A double-layer PP ceramic coated isolation membrane is selected, the thickness t of the isolation membrane is 16 μm, and the pore size R of the isolation membrane is 0.08 μm.

[0103] Preparation of lithium-ion batteries:

[0104] The prepared positive electrode sheet, separator, and negative electrode sheet are wound to obtain a bare cell without liquid injection; the bare cell is placed in an outer package, and the prepared electrolyte is injected into the dried bare cell. After vacuum packaging, standing, forming, shaping, and sorting, a lithium-ion battery is obtained. The battery discharge capacity is obtained by first fully charging the battery, then discharging it at half the battery capacity at 0.5C, and recording the discharge time multiplied by the discharge current, which is the discharge capacity.

[0105] The differences between Examples 2a-19a, Comparative Examples 1a-3a and Example 1a are shown in Table 1-1.

[0106] Table 1-1

[0107]

[0108] The differences between Examples 20a-27a and Example 1a are shown in Tables 1-2.

[0109] Table 1-2

[0110]

[0111] The above-mentioned embodiments and comparative examples were tested as follows, and the test results are shown in Table 2.

[0112] (1) High temperature storage performance test: The lithium-ion battery was placed in a 60°C constant temperature box for 6 hours, and charged to an upper limit voltage of 4.4V at a constant current and voltage of 1C, with a cut-off current of 0.05C. After the battery was fully charged, it was left to stand for 5 minutes, and then discharged at a constant current of 1C to a cut-off voltage of 2.75V. The gas production of the fully charged (100% SOC) battery was measured before storage (drainage method); after 60 days of storage, the capacity remaining rate and the drainage method were used to test the gas production, where

[0113] Remaining capacity (%) = remaining capacity after discharge / initial capacity × 100%.

[0114] Drainage gas production (m3) = (initial weight - weight after drainage) / water density.

[0115] (2) High temperature cycle performance test:

[0116] At 45°C, the lithium-ion battery is first charged at a constant current of 1C to a voltage of 4.5V, at which time the thickness of the lithium-ion battery is recorded as H0, and then discharged at a constant current of 1C to 2.75V, and the initial capacity before storage is recorded as C0; the lithium-ion battery is first charged at a constant current of 0.3C to a voltage of 4.5V, and the initial capacity is recorded as Q0, and the capacity at 800 cycles is recorded as Q1. The 1C, 500-cycle capacity retention rate is calculated by formula (1):

[0117] Storage at 45℃ for 500 hours Capacity retention rate (%) = Q1 / Q0×100%

[0118] (3) Normal temperature cycle performance test:

[0119] The prepared lithium-ion battery was placed in a 25°C environment, charged with a 1C constant current to a voltage of 4.5V, and then discharged with a 1C constant current to 2.75V. The initial capacity was recorded as Q0, and the capacity at 800 cycles was recorded as Q1. The 1C, 500-cycle capacity retention rate was calculated by formula (1):

[0120] 500 cycles capacity retention rate (%) = Q1 / Q0×100%

[0121] The relevant test results of the above embodiments and comparative examples are shown in Table 2.

[0122] Table 2

[0123]

[0124] According to Table 2 above, the gas production of the lithium ion batteries of Examples 1a-27a is lower than that of the lithium ion batteries of Comparative Examples 1a-3a, and the cycle performance and high temperature performance of the lithium ion batteries of Examples 1a-27a are also better than those of the lithium ion batteries of Comparative Examples 1a-3a, indicating that when the electrolyte additive or electrolyte of the present application is used in a battery, the hindered free movement of the lithium salt containing oxalate is reduced, thereby reducing the contact between the oxalate and the battery electrodes, making the gas production reaction of the oxalate less likely to occur, and also reducing the damage to the SEI caused by the gas bulging of the battery, thereby improving the stability of the battery under high temperature and long cycle.

[0125] Compared with Example 16a, the gas production of the lithium ion battery of Example 16a is slightly increased, and the cycle performance and high temperature performance are slightly reduced, indicating that the electrolyte lithium salt helps to improve the high temperature and long cycle performance of the battery and reduce gas production. Compared with Comparative Example 1a, the high temperature performance and cycle performance of the lithium ion battery of Example 1a are better than those of Comparative Example 1a. This is because when the electrolyte additive or the electrolyte does not contain the first lithium salt additive (such as lithium difluorooxalate borate), the first lithium salt additive used to improve the high temperature performance and cycle performance of the battery will decrease. Compared with Example 2a, the gas production of the lithium ion battery of Example 1a is lower than that of the lithium ion battery of Comparative Example 2a, and the cycle performance and high temperature performance of the lithium ion battery of Example 1a are also better than those of the lithium ion battery of Comparative Example 2a. This is because when the electrolyte additive or the electrolyte does not contain sulfate compounds, the restriction between the sulfate compounds and the first lithium salt additive will be weakened, thereby aggravating the gas production reaction of the first lithium salt additive, affecting the high temperature and long cycle performance of the battery. Compared with Example 3a, the gas production of the lithium ion battery of Example 1a is lower than that of the lithium ion battery of Comparative Example 3a, and the cycle performance and high temperature performance of the lithium ion battery of Example 1a are also better than those of the lithium ion battery of Comparative Example 3a, indicating that the presence of these two components in the electrolyte additive or the electrolyte can improve the high temperature and normal temperature cycle performance of the battery.

[0126] The following examples are used to illustrate the application of the electrolyte additive of the present application and the electrolyte containing the same in a lithium-ion battery with a LiFePO4 positive electrode.

[0127] Example 1b

[0128] Example 1b is the same as Example 1a, except that the positive electrode sheet is prepared as follows:

[0129] The lithium iron phosphate positive electrode active material, the conductive agent carbon black SP, the binder polyvinylidene fluoride, and the dispersant polyacrylate are dispersed at a mass ratio of 97.2:0.8:1.8:0.2, and the positive electrode slurry is obtained by high-speed stirring. The positive electrode slurry is used to prepare the positive electrode sheet. The single-sided surface density of the positive electrode sheet is 230g / m 2 , compacted density is 2.50g / cm 3 .

[0130] See Table 3 for the differences between Examples 2b-11b, Comparative Examples 1b-3b and Example 1b.

[0131] Table 3

[0132]

[0133] The above-mentioned high-temperature storage performance test, high-temperature cycle performance test, and normal-temperature cycle performance test were performed on the above-mentioned embodiments and comparative examples. The test results are shown in Table 4.

[0134] Table 4

[0135]

[0136] According to Table 4 above, the gas production of the lithium ion batteries of Examples 1b-11b is lower than that of the lithium ion batteries of Comparative Examples 1b-3b, and the cycle performance and high temperature performance of the lithium ion batteries of Examples 1b-11b are also better than those of the lithium ion batteries of Comparative Examples 1b-3b, indicating that the electrolyte additive or electrolyte of the present application, when used in batteries, can improve the stability of the battery under high temperature and long cycle and reduce gas production.

[0137] Compared with Example 8b, Examples 1b-7b show that the gas production of the lithium-ion battery of Example 8b is slightly increased, and the cycle performance and high-temperature performance are slightly reduced, indicating that the electrolyte lithium salt helps to improve the high-temperature long-cycle performance of the battery and reduce gas production.

[0138] Compared with comparative example 1b, the high temperature performance and cycle performance of the lithium ion battery of embodiment 1b are better than those of comparative example 1b. This is because when the electrolyte additive or the electrolyte does not contain the first lithium salt additive (such as lithium difluorooxalatoborate), the first lithium salt additive used to improve the high temperature performance and cycle performance of the battery will decrease.

[0139] Compared with Example 2b, the gas production of the lithium ion battery of Example 1b is lower than that of the lithium ion battery of Comparative Example 2b, and the cycle performance and high temperature performance of the lithium ion battery of Example 1b are also better than those of the lithium ion battery of Comparative Example 2b. This is because when the electrolyte additive or the electrolyte does not contain sulfate ester compounds, the restrictive effect between the sulfate ester compounds and the first lithium salt additive is weakened, thereby intensifying the gas production reaction of the first lithium salt additive, affecting the high temperature and long cycle performance of the battery.

[0140] Comparing Example 1b with Comparative Example 3b, the gas production of the lithium ion battery of Example 1b is lower than that of the lithium ion battery of Comparative Example 3b, and the cycle performance and high temperature performance of the lithium ion battery of Example 1b are also better than those of the lithium ion battery of Comparative Example 3b, indicating that the electrolyte additive or the presence of these two components in the electrolyte can improve the high-temperature and normal-temperature cycle performance of the battery.

[0141] Unless otherwise specified, all scientific and technological terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. All patents and publications related to this application are incorporated herein by reference in their entirety. The term "comprising" or "including" is an open expression, i.e., including the content specified in this application, but does not exclude the content of other aspects.

[0142] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present application. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0143] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change and modify the above embodiments within the scope of the present application.

Claims

1. A battery, characterized in that: include: Positive electrode sheet, negative electrode sheet, separator and electrolyte; The porosity of the negative electrode sheet is φ, with the unit of %; The thickness of the isolation membrane is t, in μm, and the pore size of the isolation membrane is R, in μm; The ratio of the total mass of the electrolyte to the discharge capacity of the battery is N, in g / Ah; The electrolyte includes an electrolyte additive, and the electrolyte additive includes: a sulfate compound and a first lithium salt additive, the first lithium salt additive includes a lithium salt containing oxalate, and the sulfate compound has a structure shown in Formula I, Formula I, R1 and R8 are independently selected from hydrogen, R2 is selected from or , and at least one of R3 and R4 is selected from an oxygen atom, R6 is selected from or , and at least one of R5 and R7 is selected from an oxygen atom, At least one of R2 and R6 is selected , n is 2, The mass fraction of the sulfate compound in the electrolyte is C, in units of %; The battery satisfies formula A, , formula A, Among them, φ is 60%-80%, t is 12μm-20μm, R is 0.03μm-0.12μm, C is 0.1%-10%, and N is 2.0-5.

0.

2. The battery according to claim 1, characterized in that The sulfate compound has one of the following structures: 、 、 、 。 3. The battery according to claim 1, characterized in that The first lithium salt additive includes at least one of lithium difluorooxalatoborate, lithium dioxalatoborate, lithium tetrafluorooxalatophosphate, lithium difluorodioxalatophosphate, and lithium trioxalatophosphate.

4. The battery according to any one of claims 1 to 3, characterized in that: The molar ratio of the first lithium salt additive to the sulfate ester compound is 1:(1-5).

5. The battery according to claim 4, characterized in that The mass fraction of the first lithium salt additive in the electrolyte is 0.1%-5%, and / or the mass fraction of the sulfate ester compound in the electrolyte is 1%-10%.

6. The battery according to any one of claims 1 to 3, characterized in that: The electrolyte additive also includes an electrolyte lithium salt, and the electrolyte lithium salt includes at least one of LiBF4, LiPF6, LiAsF6, and LiN(SO2F)2.

7. The battery according to claim 6, characterized in that The mass ratio of the electrolyte lithium salt to the first lithium salt additive is 1: (0.4-2).

8. The battery according to claim 7, characterized in that The mass fraction of the electrolyte lithium salt in the electrolyte is 0.1%-1%.

9. The battery according to any one of claims 1 to 3, characterized in that: The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes at least one of lithium iron phosphate and ternary material. Among them, the ternary material satisfies the chemical formula LiNi x Co y M1 z1 M2 z2 O2, where M1 and M2 are each independently selected from one of Al, Mn, and Fe, and M1 and M2 are different, 0 < x ≤ 1, 0 < y < 1, 0 < z1 < 1, 0 ≤ z2 < 1, and x + y + z1 + z2 = 1.

10. The battery according to any one of claims 1 to 3, characterized in that: The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer located on at least one side of the negative electrode current collector. The negative electrode active material layer includes a negative electrode active material. The mass fraction of silicon in the negative electrode active material is greater than 8%.

Citation Information

Cited By

  • Battery

    DE212024000355U1