Isolating membrane and preparation method thereof, secondary battery and electric device

By using a porous structure support layer and an elastic ion-conducting filler isolation film in a lithium secondary battery, the problem of lithium metal dendrite growth is solved and the cycle life and electrical performance of the battery are improved.

CN118801044APending Publication Date: 2024-10-18CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310391757.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Traditional lithium secondary batteries are prone to lithium metal dendrite growth during the charging process, resulting in reduced cycle life.

Method used

An isolation film is used, which includes a support layer and an elastic ion-conducting filler. The support layer has a porous structure and the surface is an electronic insulating material. The elastic ion-conducting filler is an electronic insulating material and can exert compressive stress on the front and side of the lithium metal deposition layer. , inhibiting the growth of lithium dendrites.

Benefits of technology

Effectively inhibits the growth of lithium dendrites during the charging process of secondary batteries, improves the cycle life of secondary batteries, and improves the migration and electrical performance of lithium ions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118801044A_ABST
    Figure CN118801044A_ABST
Patent Text Reader

Abstract

The invention provides an isolating membrane which comprises a supporting layer, the supporting layer is of a porous structure, the surface of the supporting layer is made of an electronic insulating material, holes of the supporting layer are internally provided with elastic conductive ion filler, and the elastic conductive ion filler is made of the electronic insulating material; the invention also relates to a preparation method of the corresponding isolating membrane, a secondary battery and an electric device. The isolating membrane provided by the invention can effectively inhibit the growth of lithium metal dendrites in the charging process of the secondary battery, so that the cycle life of the secondary battery can be effectively prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of secondary batteries, and in particular to an isolation membrane and a preparation method thereof, a secondary battery and an electrical device. Background Art

[0002] In recent years, as the application scope of secondary batteries becomes wider and wider, secondary batteries are widely used in energy storage power supply systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields.

[0003] As secondary batteries have made great progress, higher requirements have been placed on their cycle life. Traditional lithium secondary batteries are prone to lithium metal dendrite growth during the charging process, which reduces the cycle life of the battery.

[0004] Therefore, how to inhibit the growth of lithium metal dendrites during the charging process of the secondary battery and thus improve the cycle life of the secondary battery has become one of the key areas of focus for those skilled in the art. Summary of the invention

[0005] The present application is made in view of the above-mentioned problems, and one of its purposes is to provide a separator that can effectively inhibit the growth of lithium metal dendrites during the charging process of a secondary battery, thereby improving the cycle life of the secondary battery.

[0006] In order to achieve the above-mentioned purpose, the first aspect of the present application provides an isolation membrane, including a support layer, the support layer has a porous structure, and the surface of the support layer is an electronic insulating material; an elastic ion-conducting filler, the elastic ion-conducting filler is arranged in the pores of the support layer, and the elastic ion-conducting filler is an electronic insulating material.

[0007] The support layer surface and elastic ion-conducting filler of the isolation membrane of the present application are both made of electronic insulating materials, which can block electron conduction and play an isolating role between the positive and negative electrodes of the battery; the elastic ion-conducting filler has good ion conductivity and elasticity, and can apply compressive stress to the front of the lithium metal deposition layer to inhibit the growth of lithium dendrites on the front; the porous structure in the support layer is conducive to the migration of lithium ions, and can provide filling space for the elastic ion-conducting filler. During the lithium metal deposition process, the support layer can apply compressive stress to the side of the lithium metal deposition layer to inhibit the lateral lithium dendrite growth of the lithium metal deposition layer. Therefore, the isolation membrane of the present application can inhibit the growth of lithium dendrites on the front and side of the lithium metal deposition layer of the secondary battery during the charging process, thereby improving the cycle life of the secondary battery.

[0008] In any embodiment, the ionic conductivity of the elastic ion-conductive filler at 25° C. is 10 -4 S / cm~10 -3In this way, lithium ions can be better conducted in the separator, thus improving the electrical performance of the secondary battery.

[0009] In any embodiment, the elastic ion-conducting filler comprises an organic polymer; the organic polymer comprises one or more of polycarbonate, polysulfate, polysulfonate, polyphosphate, polycarboxylate, polysulfone, polyamide, polynitrile, polyether, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polyvinyl alcohol. In this way, the elastic ion-conducting filler can have suitable elasticity and good ion conductivity.

[0010] In any embodiment, the elastic ion-conductive filler further comprises one or more of an electrolyte salt and filler particles.

[0011] In any embodiment, the mass content of the organic polymer in the elastic ion-conductive filler is 70% to 95%, the mass content of the electrolyte salt is 1% to 10%, and the mass content of the filling particles is 1% to 10%.

[0012] In any embodiment, the filling particles include one or more of Al2O3, PVDF, garnet-type oxide solid electrolyte, lithium titanium aluminum phosphate solid electrolyte, perovskite solid electrolyte and sulfide solid electrolyte.

[0013] In any embodiment, the material of the support layer includes a porous aluminum layer with an aluminum oxide film on the surface. In this way, the support layer can have good structural strength, better apply compressive stress to the side of the lithium metal deposition layer during the charging process of the secondary battery, and better inhibit the lateral growth of lithium metal dendrites of the lithium metal deposition layer.

[0014] In any embodiment, the total pore area of ​​the support layer accounts for 80% to 95%. This is more conducive to the transmission of lithium ions and reduces the material performance requirements of the support layer.

[0015] In any embodiment, the total pore area of ​​the support layer accounts for 90% to 95%. In this way, the cycle performance of the secondary battery can be further improved.

[0016] In any embodiment, the average single pore area of ​​the porous structure in the support layer is 78.5 μm 2 ~1926.5μm 2 In this way, the problem of uneven lithium deposition caused by lithium ions being deposited on the surface of the negative electrode active material layer of the battery through the holes can be reduced, and the risk of local lithium dendrite growth and puncturing the isolation membrane can be reduced.

[0017] In any embodiment, the average single pore area of ​​the porous structure in the support layer is 78.5 μm2 ~314μm 2 . The cycle performance of the secondary battery can be further improved.

[0018] In any embodiment, the strength of the support layer is greater than the creep strength of metallic lithium, so that the growth of lithium dendrites lateral to the lithium metal deposition layer during the lithium metal deposition process can be well suppressed.

[0019] In any embodiment, the holes in the support layer are arranged in an array, which is more conducive to the uniform migration of lithium ions in the isolation membrane.

[0020] In any embodiment, the hole is a columnar hole, and the axis of the hole is parallel to the thickness direction of the isolation membrane. In this way, it is more conducive for the elastic ion-conducting filler to apply compressive stress to the front of the lithium metal deposition layer, and it is also more conducive for the support layer to apply compressive stress to the side of the lithium metal deposition layer; thereby better suppressing the growth of lithium dendrites on the front and side of the lithium metal deposition layer.

[0021] In any embodiment, the isolation film has a thickness of 8 μm to 20 μm.

[0022] In any embodiment, the thickness of the separator is 12 μm to 20 μm. In this way, the growth of lithium dendrites can be further suppressed, the expansion thickness of the battery cell can be reduced, and the cycle performance of the secondary battery can be further improved.

[0023] The second aspect of the present application provides a method for preparing the isolation film of the first aspect of the present application, comprising the following steps:

[0024] Providing a support layer, wherein the support layer has a porous structure, and the surface of the support layer is an electronic insulating material;

[0025] An elastic ion-conducting filler is formed in the holes of the support layer, and the elastic ion-conducting filler is an electronic insulating material.

[0026] The preparation method of the isolation film has a simple preparation process, and the isolation film prepared by the method can effectively inhibit the growth of lithium dendrites during the lithium metal deposition process, thereby improving the cycle life of the secondary battery.

[0027] In any embodiment, forming the elastic ion-conducting filler in the pores of the support layer comprises the following steps: coating the elastic ion-conducting filler in the pores of the support layer, so that the elastic ion-conducting filler can be quickly and directly filled in the pores to form an isolation membrane.

[0028] In any embodiment, forming the elastic ion-conducting filler in the pores of the support layer comprises the following steps: filling the pores of the support layer with a slurry containing a cross-linking agent, a polymer monomer and an initiator, and forming the elastic ion-conducting filler after cross-linking and curing. In this way, the elastic ion-conducting filler can be formed by in-situ cross-linking and curing in the pores, so that the elastic ion-conducting filler can be filled more uniformly.

[0029] The third aspect of the present application provides a secondary battery, which includes the isolation membrane of the first aspect of the present application, or includes the isolation membrane prepared by the preparation method of the second aspect of the present application. The secondary battery adopts the isolation membrane of the present application, can inhibit the growth of lithium dendrites, and has a good cycle life.

[0030] In any embodiment, the secondary battery includes a negative electrode plate, the negative electrode plate has a negative electrode active material, and the negative electrode active material includes one or more of lithium metal and graphite. In this way, the negative electrode active material is a negative electrode material with lithium metal precipitated on the negative electrode plate in a fully charged state.

[0031] A fourth aspect of the present application provides an electrical device, which includes the secondary battery of the third aspect of the present application.

[0032] The isolation membrane of the present application is provided with a support layer, the support layer has a porous structure, and an elastic ion-conducting filler is provided in the pores of the support layer, and the surface of the support layer and the elastic ion-conducting filler are both made of electronic insulating materials. The isolation membrane can inhibit the growth of lithium dendrites on the front and side of the lithium metal deposition layer of the secondary battery during charging, thereby improving the cycle life of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 is a schematic diagram of lithium metal deposition on the negative electrode sheet;

[0034] Figure 2 It is a schematic diagram of lithium dendrites growing on the side of lithium metal deposition layer;

[0035] Figure 3 It is a schematic diagram of the positions of the positive electrode sheet, the separator and the negative electrode sheet in a secondary battery according to one embodiment of the present application;

[0036] Figure 4 is a schematic diagram of a top view of the structure of a support layer in an isolation membrane according to an embodiment of the present application;

[0037] Figure 5 is a schematic diagram of a secondary battery according to an embodiment of the present application;

[0038] Figure 6 yes Figure 5 An exploded view of a secondary battery according to an embodiment of the present application is shown;

[0039] Figure 7 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.

[0040] Description of reference numerals:

[0041] 1. Lithium metal deposition layer; 2. Lithium dendrites; 3. Isolation membrane; 31. Support layer; 32. Elastic ion-conducting filler; 311. Holes; 5. Secondary battery; 51. Shell; 52. Electrode assembly; 53. Cover plate; 54. Positive electrode plate; 55. Negative electrode plate; 6. Electrical device. DETAILED DESCRIPTION

[0042] Hereinafter, the embodiments of the isolation membrane, secondary battery and electrical device of the present application are specifically disclosed in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0043] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0044] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0045] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0046] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0047] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0048] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0049] The weights described in the description of the embodiments of the present invention may be weight units known in the chemical industry, such as μg, mg, g, and kg.

[0050] During the charging process of traditional lithium secondary batteries, lithium metal dendrites will grow at the negative electrode. The growth of lithium metal dendrites will lead to lithium metal pulverization, dead lithium accumulation, rapid battery capacity decay and even short circuit failure, which will reduce the cycle life of the secondary battery. In the initial lithium deposition process of lithium secondary batteries, it is necessary to overcome the nucleation work to carry out the nucleation process. As the lithium deposition proceeds, the nucleus gradually grows. The electrode potential of lithium metal is extremely low and it is very easy to react with the electrolyte. The uneven thickness of the generated SEI film will cause differences in the lithium ion transmission speed, resulting in uneven lithium metal deposition. The uneven deposition of lithium metal will cause the SEI to rupture, and the lithium deposition rate at the rupture will increase, causing dendrite growth.

[0051] like Figure 1 and Figure 2As shown, the deposited lithium metal has good creep properties. Due to the compressive stress exerted by the isolation membrane on the deposited lithium metal, it is difficult to grow lithium dendrites 2 on the front of the lithium metal deposition layer 1. However, as the amount of deposition increases, the lithium metal is deposited to a certain thickness, and the side of the lithium metal deposition layer 1 is in a stress-free state, which makes it very easy for lithium dendrites 2 to grow. Therefore, seeking a solution that can effectively inhibit the growth of lithium dendrites 2 during the charging process of the secondary battery, especially inhibiting the growth of lithium dendrites 2 on the side of the lithium metal deposition layer 1, thereby improving the cycle life of the secondary battery is one of the research directions that technicians in this field focus on. In this regard, the present application provides a separation membrane, which can effectively inhibit the growth of lithium dendrites 2 during the charging process of the secondary battery and improve the cycle life of the secondary battery by setting a support layer and an elastic ion-conducting filler.

[0052] See also Figure 3 and Figure 4 In some embodiments, the first aspect of the present application provides an isolation membrane 3, which includes a support layer 31, the support layer 31 has a porous structure, and an elastic ion-conducting filler 32 is provided in the pores 311 of the support layer 31, and the surface of the support layer 31 and the elastic ion-conducting filler 32 are both electronic insulating materials.

[0053] The isolation membrane 3 of the present application is provided with a support layer 31 having a porous structure, and an elastic ion-conducting filler 32 is provided in the pores 311 of the support layer 31, and the surface of the support layer 31 and the elastic ion-conducting filler 32 are both made of electronic insulating materials. The support layer 31 and the elastic ion-conducting filler 32 of the isolation membrane 3 are both made of electronic insulating materials, which can block electron conduction and play an isolating role between the positive and negative electrodes of the battery; the elastic ion-conducting filler 32 has good ionic conductivity and elasticity, and can apply compressive stress to the front of the lithium metal deposition layer 1 to inhibit the growth of the front lithium dendrite 2; at the same time, as the lithium metal is deposited on the pole piece, the elastic ion-conducting filler 32 can be compressed; the porous structure in the support layer 31 is conducive to the migration of lithium ions, and can provide a filling space for the elastic ion-conducting filler 32. During the lithium metal deposition process, the support layer 31 can apply compressive stress to the side of the lithium metal deposition layer 1 to inhibit the growth of the lateral lithium dendrite 2. In this way, the isolation film 3 of the present application can inhibit the growth of lithium dendrites 2 on the front and side of the lithium metal deposition layer 1 during the charging process of the secondary battery, thereby improving the cycle life of the secondary battery.

[0054] It should be noted that the above-mentioned electronic insulating material does not mean that the material absolutely cannot conduct electrons, but means that the material has extremely low electronic conductivity. It can be understood that the surface of the support layer 31 is an electronic insulating material, which means that the outer surface of the support layer 31 and the inner surface of the hole are both electronic insulating materials, so that the entire surface of the support layer 31 has extremely low electronic conductivity.

[0055] In some embodiments, the ionic conductivity of the elastic ion-conductive filler 32 at 25° C. is 10 -4 S / cm~10 -3 In this way, lithium ions can be better conducted in the separator 3 .

[0056] In some embodiments, the elastic ion-conducting filler 32 includes an organic polymer; the organic polymer includes one or more of polycarbonate, polysulfate, polysulfonate, polyphosphate, polycarboxylate, polysulfone, polyamide, polynitrile, polyether, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polyvinyl alcohol. Using these organic polymers as the elastic ion-conducting filler 32 can make the elastic ion-conducting filler 32 have certain elasticity and good ion conductivity.

[0057] In some embodiments, the elastic ion-conductive filler 32 further includes electrolyte salt and filling particles. The electrolyte salt can further improve the ion conductivity of the elastic ion-conductive filler 32, and the filling particles can improve the compressive strength of the filler.

[0058] In some embodiments, the mass content of the organic polymer in the elastic ion-conductive filler 32 is 70% to 95%, the mass content of the electrolyte salt is 1% to 10%, and the mass content of the filling particles is 1% to 10%.

[0059] In some embodiments, the filling particles include one or more of Al2O3, PVDF, garnet-type oxide solid electrolyte (LLZO), lithium aluminum titanium phosphate solid electrolyte (LATP), perovskite-type solid electrolyte (LLTO) and sulfide solid electrolyte.

[0060] In some embodiments, the material of the support layer 31 includes a porous aluminum layer with an aluminum oxide film on the surface. Among them, using light metal aluminum as the material of the support layer 31 can make the density of the support layer 31 lower and reduce the overall weight of the isolation membrane; at the same time, the extremely thin aluminum oxide film formed on the aluminum surface can inhibit electronic conduction; and porous aluminum has a high specific strength. Using the above material as the support layer 31 can make the support layer 31 have good structural strength, can better apply compressive stress to the side of the lithium metal deposition layer 1 during the charging process of the secondary battery, and better inhibit the lateral lithium metal dendrite growth of the lithium metal deposition layer 1.

[0061] In some embodiments, the support layer 31 is a porous aluminum foil formed by laser drilling, and an aluminum oxide film can be formed on the surface of the porous aluminum foil by natural oxidation.

[0062] It can be understood that the porous aluminum layer having an aluminum oxide film on its surface has an aluminum oxide film not only on the upper surface, lower surface and side surface of the porous aluminum layer, but also on the inner surface of the pores of the porous aluminum layer, to ensure that the support layer 31 has good electronic insulation.

[0063] In some embodiments, the total pore area of ​​the support layer 31 accounts for 80% to 95%. The pore structure in the support layer 31 is conducive to the migration of lithium ions. During the charge and discharge process of the secondary battery, lithium ions can be deposited on the negative electrode side through the pore structure, and can be smoothly migrated from the negative electrode side to the positive electrode sheet to ensure the electrochemical performance of the battery. If the total pore area of ​​the support layer 31 accounts for too large a proportion, in order to inhibit the growth of lithium dendrites 2 on the side of the lithium metal deposition layer 1, the required strength of the support layer 31 is relatively high, which puts higher requirements on the material selection of the support layer 31; if the total pore area of ​​the support layer 31 accounts for too small a proportion, it will inhibit the transmission of lithium ions to a certain extent. By setting the total pore area of ​​the support layer 31 to 80% to 95%, it is more conducive to the transmission of lithium ions, and at the same time, the material performance requirements of the support layer 31 are reduced.

[0064] It can be understood that the total hole area ratio of the support layer 31 refers to the percentage of the sum of the areas of all holes 311 in the support layer 31 to the total area of ​​the support layer 31. The total hole area ratio of the support layer 31 can be 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%; or a range consisting of any two of the above values.

[0065] In some embodiments, the total pore area of ​​the support layer 31 accounts for 90% to 95%. In this way, the cycle performance of the secondary battery can be further improved.

[0066] In some embodiments, the average single pore area of ​​the porous structure in the support layer 31 is 78.5 μm 2 ~1926.5μm 2 In this way, the problem of uneven lithium deposition caused by lithium ions being deposited on the surface of the negative electrode active material layer of the battery through the holes 311 can be reduced, thereby reducing the risk of local lithium dendrites 2 growing and piercing the separator 3.

[0067] It is understood that the average area of ​​a single hole refers to the average area of ​​a single hole 311 in the support layer 31. The average area of ​​a single hole 311 in the support layer 31 can be 78.5 μm 2 , 100μm 2 , 200μm 2 、300μm 2 , 400μm 2 , 500μm 2、600μm 2 、700μm 2 、800μm 2 , 900μm 2 , 1000μm 2 、1100μm 2 , 1200μm 2 、1300μm 2 、1400μm 2 、1500μm 2 、1600μm 2 、1700μm 2 、1800μm 2 、1900μm 2 、1926.5μm 2 ; or a range consisting of any two of the above values.

[0068] In some embodiments, the average single pore area of ​​the porous structure in the support layer 31 is 78.5 μm 2 ~314μm 2 In this way, the cycle performance of the secondary battery can be further improved.

[0069] In some embodiments, the strength of the support layer 31 is greater than the creep strength of metallic lithium, so that the growth of lithium dendrites 2 on the side of the lithium metal deposition layer 1 during the lithium metal deposition process can be well suppressed.

[0070] In some embodiments, the holes 311 in the support layer 31 are arranged irregularly. For example, the holes 311 are randomly arranged in the support layer 31 .

[0071] In some embodiments, the holes 311 in the support layer 31 are arranged in an array, which is more conducive to the uniform migration of lithium ions in the isolation membrane 3.

[0072] In some embodiments, the multiple holes 311 in the support layer 31 are spaced apart from each other, that is, the multiple holes 311 in the support layer 31 are independent of each other.

[0073] In some embodiments, the plurality of holes 311 in the support layer 31 are interconnected, and the size of the interconnected portion is smaller than the diameter of the hole 311 or is equal to the diameter of the hole 311 .

[0074] In some embodiments, the hole 311 is a columnar hole, and the axis of the hole 311 is parallel to the thickness direction of the isolation film 3. In this way, the elastic ion-conducting filler 32 in the hole 311 can be squeezed and deformed along the stacking direction of the lithium metal deposition layer 1 during the lithium metal deposition process, which is more conducive to the elastic ion-conducting filler 32 applying compressive stress to the front of the lithium metal deposition layer 1, and is also more conducive to the support layer 31 applying compressive stress to the side of the lithium metal deposition layer 1; thereby better suppressing the growth of lithium dendrites 2 on the front and side of the lithium metal deposition layer 1.

[0075] In some embodiments, the thickness of the isolation film 3 is 8 μm to 20 μm. It is understood that the thickness of the isolation film 3 can be, but is not limited to, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm, or 20 μm.

[0076] In any embodiment, the thickness of the separator 3 is 12 μm to 20 μm. In this way, the growth of lithium dendrites can be further suppressed, the expansion thickness of the battery cell can be reduced, and the cycle performance of the secondary battery can be further improved.

[0077] The second aspect of the present application further provides a method for preparing the isolation film 3 of the first aspect of the present application, comprising the following steps:

[0078] Providing a support layer 31, wherein the support layer 31 has a porous structure, and the surface of the support layer 31 is an electronic insulating material;

[0079] An elastic ion-conducting filler 32 is formed in the hole 311 of the support layer 31 , and the elastic ion-conducting filler 32 is an electronic insulating material.

[0080] The present application forms an elastic ion-conducting filler 32 in the holes 311 of the support layer 31, so that the isolation membrane 3 in which the holes 311 of the support layer 31 are filled with the elastic ion-conducting filler 32 can be easily obtained; the support layer 31 in the isolation membrane 3 can inhibit the lateral growth of lithium dendrites 2 of the lithium metal deposition layer 1 during the lithium metal deposition process, and the elastic ion-conducting filler 32 can conduct lithium ions and has a certain elasticity, so as to inhibit the growth of lithium dendrites 2 on the front of the lithium metal deposition layer 1 during the lithium metal deposition process.

[0081] In some embodiments, forming the elastic ion-conducting filler 32 in the pores 311 of the support layer 31 comprises the following step: coating the elastic ion-conducting filler 32 in the pores 311 of the support layer 31. In this way, by directly coating the elastic ion-conducting filler 32 in the pores 311 of the support layer 31, the elastic ion-conducting filler 32 can be quickly filled in the pores 311.

[0082] In some embodiments, forming the elastic ion-conducting filler 32 in the pores 311 of the support layer 31 comprises the following steps: filling the pores 311 of the support layer 31 with a slurry containing a cross-linking agent, a polymer monomer, and an initiator, and cross-linking and curing the slurry to form the elastic ion-conducting filler 32. For example, the slurry may be filled in the pores 311 by dipping, and the elastic ion-conducting filler 32 may be formed after the slurry is cross-linked and cured in situ. In this way, the elastic ion-conducting filler 32 may be formed in the pores 311 of the support layer 31 by cross-linking and curing in situ, and the filling of the elastic ion-conducting filler 32 may be made more uniform.

[0083] In some embodiments, the cross-linking and curing of the slurry may be initiated by electron beam initiation, ultraviolet light initiation, thermal initiation, or the like.

[0084] In some embodiments, the initiator includes a peroxide compound initiator and an azo initiator, the peroxide compound initiator includes, for example, acyl peroxides (such as benzoyl peroxide, lauroyl peroxide) and persulfates (such as ammonium persulfate), etc.; the azo initiator includes, for example, azobisisobutyronitrile and azobisisoheptanenitrile, etc. The temperature of thermal initiation is 50°C to 85°C.

[0085] In some embodiments, the slurry may further include one or more of a plasticizer, a thickener, filler particles, and an electrolyte salt.

[0086] In some embodiments, the crosslinking agent is an acrylate crosslinking agent. Including methyl methacrylate, butyl methacrylate, methyl acrylate, ethyl acrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, butyl acrylate, isodecyl acrylate, isooctyl acrylate, lauryl acrylate, isobornyl acrylate, isobornyl methacrylate, ethoxyethoxyethyl acrylate, cyanoacrylate, caprolactone acrylate, 2-phenoxyethyl acrylate, tetrahydrofuran acrylate, ethoxylated tetrahydrofuran acrylate, cyclotrimethylolpropane acrylate, 2-carboxyethyl acrylate, cyclohexyl acrylate, ethylene glycol diacrylate, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, diethylene glycol diacrylate, diethylene glycol dimethacrylate, triethylene glycol diacrylate, triethylene glycol dimethacrylate, tetraethylene glycol diacrylate, tetraethylene glycol dimethacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,3-butanediol diacrylate, 1,3- Butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, dipropylene glycol diacrylate, dipropylene glycol dimethacrylate, tripropylene glycol diacrylate, tripropylene glycol dimethacrylate, neopentyl glycol diacrylate, neopentyl glycol dimethacrylate, 2 (propoxy) neopentyl glycol diacrylate, polyethylene glycol diacrylate, polyethylene glycol dimethacrylate, polypropylene glycol dimethacrylate, polycyclopentyl glycol diacrylate One or more of hexyl acrylate, methoxy polyethylene glycol acrylate, ethoxylated trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, methoxy polyethylene glycol methacrylate, pentaerythritol triacrylate, propoxylated glycerol triacrylate, tri(2-hydroxyethyl)isocyanuric acid triacrylate, di(trimethylolpropane) tetraacrylate, pentaerythritol tetraacrylate, 4(ethoxy)pentaerythritol tetraacrylate and dipentaerythritol hexaacrylate.

[0087] In some embodiments, the monomer is one or more of carbonate monomers, sulfate monomers, sulfonate monomers, phosphate monomers, carboxylate monomers, sulfone monomers, amide monomers, nitrile monomers, and ether monomers. For example, the monomer may be one or more of vinyl carbonate, vinyl sulfite, vinyl ethylene carbonate, 1,3-propenyl-sultone, methyl vinyl sulfone, ethyl vinyl sulfone, methyl methacrylate, vinyl acetate, and acrylamide.

[0088] In some embodiments, the carbonate monomer includes one or more of vinylene carbonate, vinylethylene carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate, and chloroethylene carbonate.

[0089] In some embodiments, the sulfate ester monomer includes one or more of vinyl vinyl sulfite, vinyl sulfite, 4-methyl vinyl sulfate, and 4-ethyl vinyl sulfate.

[0090] In some embodiments, the sulfonate monomer includes one or more of 1,3-propylene sultone, 1,3-propane sultone, 1,4-butane sultone, and methylenedisulfonate.

[0091] In some embodiments, the phosphate monomer includes one or more of dimethyl vinyl phosphate, diethyl vinyl phosphate, diethyl propenyl phosphate, diethyl butenyl phosphate, diethyl 1-buten-2-yl phosphonate, diethyl ethynyl phosphate, vinyl trifluoromethyl phosphate, vinyl-1-trifluoroethyl phosphate, diethyl fluorovinyl phosphate and 1-trifluoropropenylethyl phosphate.

[0092] In some embodiments, the carboxylate monomer includes vinyl acetate.

[0093] In some embodiments, the sulfone monomer includes one or more of methyl vinyl sulfone, ethyl vinyl sulfone, sulfolene, sulfolane, and ethylene sulfoxide.

[0094] In some embodiments, the amide monomer includes acrylamide.

[0095] In some embodiments, the nitrile monomer includes one or more of acrylonitrile, succinonitrile, glutaronitrile, and adiponitrile.

[0096] In some embodiments, the ether monomer includes one or more of 1,3-dioxolane, ethylene oxide, 1,2-propylene oxide, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, ethylene glycol dimethyl ether, ethylene glycol diglycidyl ether, and triethylene glycol divinyl ether.

[0097] In some embodiments, the plasticizer includes one or more selected from ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.

[0098] In some embodiments, the electrolyte salt includes one or more selected from lithium salts and sodium salts. Optionally, the electrolyte salt includes one or more selected from lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorophosphate, lithium difluorodioxalatophosphate, lithium tetrafluorooxalatophosphate, NaPF6, NaClO4, NaBCl4, NaSO3CF3, Na(CH3)C6H4SO3.

[0099] In some embodiments, the thickener is a polymer material that can be dissolved in the plasticizer, including one or more of polyvinyl formal, polyvinylidene fluoride and their copolymers. Its main function is to adjust the viscosity of the slurry and prevent the slurry from penetrating into the internal pores of the electrode.

[0100] The third aspect of the present application provides a secondary battery, which includes the isolation film 3 of the first aspect of the present application, or includes the isolation film 3 prepared by the preparation method of the second aspect of the present application. The secondary battery of the present application, by adopting the isolation film 3 of the present application, can effectively inhibit the growth of lithium dendrites 2 during the charging process of the secondary battery, thereby improving the cycle life of the secondary battery.

[0101] In some embodiments, the secondary battery includes a positive electrode sheet 54 , a separator 3 , a negative electrode sheet 55 , and an electrolyte, wherein the separator 3 is located between the positive electrode sheet 54 and the negative electrode sheet 55 , and the electrolyte is filled between the positive electrode sheet 54 and the negative electrode sheet 55 .

[0102] In some embodiments, the negative electrode active material in the negative electrode plate 55 is a negative electrode active material with lithium metal precipitated on the negative electrode surface in a fully charged state. For example, the negative electrode active material may be one or more of lithium metal and graphite. When the negative electrode active material is graphite, it may be artificial graphite, natural graphite, soft carbon, hard carbon, etc., and the graphite capacity on the negative electrode plate 55 is less than the capacity of the positive electrode plate 54.

[0103] In some embodiments, the positive electrode plate 54 has a positive electrode active material, and the positive electrode active material can be one or more of lithium iron phosphate (LFP), nickel cobalt manganese oxide lithium ternary positive electrode material (NCM), nickel cobalt aluminum oxide lithium ternary positive electrode material (NCA) and lithium cobalt oxide (LCO).

[0104] A fourth aspect of the present application provides an electrical device, which includes the secondary battery of the third aspect of the present application.

[0105] The secondary battery and the electric device of the present application will be described below with reference to the drawings as appropriate.

[0106] Unless otherwise specified, the components, material types or contents of the batteries mentioned are applicable to both lithium-ion secondary batteries and sodium-ion secondary batteries.

[0107] In one embodiment of the present application, a secondary battery is provided.

[0108] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.

[0109]

Positive electrode

[0110] The positive electrode plate includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0111] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.

[0112] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc. Polymer material substrate (such as substrates of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.)

[0113] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery known in the art.

[0114] As an example, the positive electrode active material of a lithium-ion secondary battery may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.

[0115] As an example, the positive electrode active material of the sodium ion secondary battery may include at least one of the following materials: at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.

[0116] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. The sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.

[0117] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si; n represents (YO4) n- valence state.

[0118] Polyanionic compounds can also be those with sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal can be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.

[0119] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedral unit (ZO y ) m+ and an optional halogen anion. Y can be at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, which may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.

[0120] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2 (P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).

[0121] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal may be at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.

[0122] The weight ratio of the positive electrode active material in the positive electrode film layer is 80 to 100 weight %, based on the total weight of the positive electrode film layer.

[0123] In some embodiments, the positive electrode film layer may also optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0 to 20 weight%, based on the total weight of the positive electrode film layer.

[0124] In some embodiments, the positive electrode film layer may further include a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0-20% by weight, based on the total weight of the positive electrode film layer.

[0125] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry, wherein the positive electrode slurry has a solid content of 40wt% to 80wt%, and the viscosity at room temperature is adjusted to 5000mPa·s to 25000mPa·s, the positive electrode slurry is coated on the surface of the positive electrode collector, and after drying, the positive electrode sheet is formed by cold rolling; the positive electrode powder coating unit surface density is 150mg / m 2 ~350 mg / m 2 The compaction density of the positive electrode is 3.0g / cm 3 ~3.6g / cm 3 , optional 3.3g / cm 3 ~3.5g / cm 3 .

[0126] The calculation formula of the compacted density is:

[0127] Compacted density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).

[0128] The mass M of the positive electrode active material per unit area of ​​the positive electrode film can be obtained by weighing using a standard balance.

[0129] The thickness T of the positive electrode film can be measured by using a micrometer, for example, a Mitutoyo 293-100 micrometer with an accuracy of 0.1 μm. It should be noted that the thickness of the positive electrode film described in the present invention refers to the thickness of the positive electrode film in the positive electrode sheet used for assembling the battery after cold pressing.

[0130]

Negative electrode

[0131] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0132] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.

[0133] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Among them, the metal material includes but is not limited to copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc., and the polymer material substrate includes but is not limited to polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE) and other substrates.

[0134] In some embodiments, the negative electrode active material may be a negative electrode active material for a battery known in the art.

[0135] As an example, the negative electrode active material of the lithium ion secondary battery may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate and lithium metal, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0136] As an example, the negative electrode active material of the sodium ion secondary battery is generally a hard carbon material, a two-dimensional metal carbide or a nitride. Preferably, the negative electrode active material of the sodium ion secondary battery is generally a hard carbon material.

[0137] The weight ratio of the negative electrode active material in the negative electrode film layer is 70 to 100 weight %, based on the total weight of the negative electrode film layer.

[0138] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS). The weight ratio of the binder in the negative electrode film layer is 0 to 30% by weight, based on the total weight of the negative electrode film layer.

[0139] In some embodiments, the negative electrode film layer may further include a conductive agent. The conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. The weight ratio of the conductive agent in the negative electrode film layer is 0 to 20 weight %, based on the total weight of the negative electrode film layer.

[0140] In some embodiments, the negative electrode film layer may further include other additives, such as a thickener (such as sodium carboxymethyl cellulose (CMC-Na)), etc. The weight ratio of the other additives in the negative electrode film layer is 0 to 15 weight %, based on the total weight of the negative electrode film layer.

[0141] In some embodiments, the negative electrode sheet can be prepared by the following method: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as deionized water) to form a negative electrode slurry, wherein the solid content of the negative electrode slurry is 30wt% to 70wt%, and the viscosity at room temperature is adjusted to 2000mPa·s to 10000mPa·s; the obtained negative electrode slurry is coated on the negative electrode collector, and after a drying process, cold pressing such as rolling, a negative electrode sheet is obtained. The negative electrode powder coating unit area density is 75mg / m 2 ~220 mg / m 2 , the compaction density of the negative electrode is 1.2g / m 3 ~2.0g / m 3 .

[0142] The mass M of the negative electrode active material per unit area of ​​the negative electrode film can be obtained by weighing using a standard balance.

[0143] The thickness T of the negative electrode film can be measured by using a micrometer, for example, a Mitutoyo 293-100 micrometer with an accuracy of 0.1 μm. It should be noted that the thickness of the negative electrode film described in the present invention refers to the thickness of the negative electrode film in the negative electrode sheet used for assembling the battery after cold pressing.

[0144]

Electrolytes

[0145] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.

[0146] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.

[0147] In some embodiments, the electrolyte salt of the lithium ion secondary battery can be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP) and lithium tetrafluorooxalatophosphate (LiTFOP).

[0148] The electrolyte salt of the sodium ion secondary battery can be selected from one or more of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.

[0149] The concentration of the electrolyte salt is generally 0.5 mol / L to 5 mol / L.

[0150] In some embodiments, the solvent can be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).

[0151] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.

[0152]

Isolation film

[0153] In some embodiments, the secondary battery further includes a separator, which is the separator described above.

[0154] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0155] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.

[0156] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0157] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 5 The secondary battery 5 is a square structure as an example.

[0158] In some embodiments, reference Figure 6 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0159] In some embodiments, the secondary batteries 5 can be assembled into a battery module. The number of secondary batteries 5 contained in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0160] In the battery module, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.

[0161] Optionally, the battery module may further include a housing having a housing space, and the plurality of secondary batteries 5 are housed in the housing space.

[0162] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.

[0163] The battery pack may include a battery box and a plurality of battery modules disposed in the battery box. The battery box includes an upper box body and a lower box body, and the upper box body can be covered on the lower box body to form a closed space for accommodating the battery modules. The plurality of battery modules can be arranged in the battery box in any manner.

[0164] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.

[0165] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.

[0166] Figure 7 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.

[0167] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be light and thin, and a secondary battery may be used as a power source.

[0168] The following are some examples.

[0169] In order to make the technical problems, technical solutions and beneficial effects solved by the present application clearer, the present application will be further described in detail below in conjunction with the embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its applications. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.

[0170] If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the field or the product instructions are used. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0171] Example 1

[0172] 1) Preparation of positive electrode

[0173] NCM811, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were mixed in a N-methylpyrrolidone solvent system at a weight ratio of 94:3:3, and then coated on aluminum foil, dried, and cold pressed to obtain a positive electrode sheet with a coating amount of 3.5 mAh / cm 2 , cut into corresponding size for later use.

[0174] 2) Preparation of negative electrode sheet

[0175] Graphite, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are fully stirred and mixed in an N-methylpyrrolidone solvent system in a weight ratio of 94:3:3, and then coated on a copper foil, dried and cold pressed to obtain a negative electrode sheet, which is then cut into corresponding sizes for use.

[0176] 3) Preparation of isolation membrane

[0177] A porous aluminum layer with an aluminum oxide film layer on the surface is used as a support layer material. Filling particles Al2O3, electrolyte salt lithium hexafluorophosphate, elastic polymer monomer, initiator and dispersing solvent are uniformly mixed to obtain a homogeneous slurry. The homogeneous slurry is coated on the surface of the porous aluminum support layer by a coating method. Due to the capillary phenomenon, the slurry is fully infiltrated into the pores of the support layer. The slurry is solidified under heating conditions to form an elastic ion-conducting filler in the pores of the support layer to obtain an isolation membrane.

[0178] The elastic polymer monomer is a mixture of butyl acrylate and polyethylene glycol diacrylate, the mass ratio of the two is 7.5:1, and the relative molecular mass of polyethylene glycol diacrylate is 600; the initiator is a thermal initiator azobisisobutyronitrile; the amount of the initiator is 3% of the mass of the elastic polymer monomer; the heating curing time is 3h, and the heating curing temperature is 55°C; the mass content of the filling particles in the elastic ion-conducting filler is 5%, the mass content of the electrolyte salt is 5%, and the mass content of the elastic polymer monomer is 90%; the 25°C ionic conductivity of the elastic ion-conducting filler is about 5*10 -4 S / cm; the total pore area of ​​the support layer accounts for 90%, and the average area of ​​a single pore is 314μm 2 ; The thickness of the isolation film is 12μm.

[0179] 4) Battery assembly

[0180] Use double-sided positive electrodes and single-sided negative electrodes with composite isolation membranes to assemble laminated battery cells, and assemble bare battery cells in the order of negative electrode, isolation membrane, positive electrode, isolation membrane, and negative electrode, so that the isolation membrane is between the positive and negative electrodes to play an isolating role, and place the bare battery cells in an outer package to obtain dry battery cells.

[0181] 5) Battery filling

[0182] The electrolyte solvent is EC:EMC:DMC=1:1:1, the lithium salt is LiFSI, the concentration is 1M / L, 0.3g of liquid is injected into each battery cell, and after injection, it is vacuum packaged and left to soak.

[0183] Example 2

[0184] This embodiment is basically the same as the embodiment 1, except that the mass content of the electrolyte salt in the elastic ion-conductive filler is different, and the 25°C ionic conductivity of the elastic ion-conductive filler is different. In this embodiment, the mass content of the electrolyte salt in the elastic ion-conductive filler is 1%, and the 25°C ionic conductivity of the elastic ion-conductive filler is about 10 -4 S / cm.

[0185] Example 3

[0186] This embodiment is basically the same as the embodiment 1, except that the mass content of the electrolyte salt in the elastic ion-conductive filler is different, and the 25°C ionic conductivity of the elastic ion-conductive filler is different. In this embodiment, the mass content of the electrolyte salt in the elastic ion-conductive filler is 10%, and the 25°C ionic conductivity of the elastic ion-conductive filler is about 10%. -3 S / cm.

[0187] Example 4

[0188] This embodiment is basically the same as the embodiment 1, and the only difference is that the type of filling particles in the elastic ion-conducting filler is different. In this embodiment, the filling particles in the elastic ion-conducting filler are lithium lanthanum zirconium oxide (LLZO) solid electrolyte.

[0189] Example 5

[0190] This embodiment is basically the same as the embodiment 1, and the only difference is that the type of filling particles in the elastic ion-conducting filler is different. In this embodiment, the filling particles in the elastic ion-conducting filler are PVDF.

[0191] Example 6

[0192] This embodiment is basically the same as the embodiment 1, except that the content of the filling particles in the elastic ion-conducting filler is different. In this embodiment, the mass content of the filling particles in the elastic ion-conducting filler is 1%.

[0193] Example 7

[0194] This embodiment is basically the same as the embodiment 1, except that the content of the filling particles in the elastic ion-conducting filler is different. In this embodiment, the mass content of the filling particles in the elastic ion-conducting filler is 10%.

[0195] Example 8

[0196] This embodiment is basically the same as the embodiment 1, except that the total hole area ratio of the support layer is different. In this embodiment, the total hole area ratio of the support layer is 80%.

[0197] Example 9

[0198] This embodiment is basically the same as the embodiment 1, except that the total hole area ratio of the support layer is different. In this embodiment, the total hole area ratio of the support layer is 95%.

[0199] Example 10

[0200] This embodiment is basically the same as embodiment 1, except that the average area of ​​a single hole in the support layer is different. In this embodiment, the average area of ​​a single hole in the support layer is 78.5 μm 2 .

[0201] Embodiment 11

[0202] This embodiment is basically the same as embodiment 1, except that the average area of ​​a single hole in the support layer is different. In this embodiment, the average area of ​​a single hole in the support layer is 1926.5 μm 2 .

[0203] Example 12

[0204] This embodiment is basically the same as the embodiment 1, and the only difference is that the thickness of the isolation film is different. In this embodiment, the thickness of the isolation film is 8 μm.

[0205] Embodiment 13

[0206] This embodiment is basically the same as the embodiment 1, and the only difference is that the thickness of the isolation film is different. In this embodiment, the thickness of the isolation film is 20 μm.

[0207] Comparative Example 1

[0208] This comparative example is basically the same as Example 1, except that the isolation film adopts a traditional PP isolation film.

[0209] Performance Testing

[0210] 1) Battery cell expansion thickness test

[0211] Before testing the battery cell, measure the test thickness L0. At an ambient temperature of 25°C, let it stand for 5 minutes, charge to 4.25V at 1 / 3C, then charge at constant voltage at 4.25V to a current ≤0.05mA, let it stand for 5 minutes, discharge to 2.8V at 1 / 3C, let it stand for 5 minutes, charge to 4.25V at 1 / 3C, then charge at constant voltage at 4.25V to a current ≤0.05mA, record the battery cell thickness L1, and calculate the expansion △L=L1-L0.

[0212] 2) Cycle performance test

[0213] At 25° C., the lithium ion batteries prepared in the examples and comparative examples were charged at a 3C rate and discharged at a 1C rate, and a 3%-97% SOC cycle test was performed until the capacity of the lithium ion battery was less than 80% of the initial capacity, and the number of cycles was recorded.

[0214] 3) Calculation of ionic conductivity

[0215] The coating is applied on the surface of a blank aluminum foil, cut into small discs with a diameter of 20 mm, and encapsulated in a button battery. The electrochemical AC impedance method of an electrochemical workstation is used for testing, and a Nyquist diagram is drawn. The obtained Nyquist diagram is analyzed using the equivalent circuit curve fitting method, and the horizontal coordinate of the intersection of the semicircle and the oblique line in the Nyquist diagram is used as the resistance R. The test voltage can be 10 mV, and the test frequency can be 0.1 Hz to 100 KHz.

[0216] According to the formula λ=d / RS, λ represents ionic conductivity, d represents thickness, R represents resistance, and S represents area, the ionic conductivity λ1 of the coating is calculated. The ionic conductivity of the electrolyte is directly tested using a conductivity meter to obtain λ2.

[0217] 4) Total hole area ratio and single hole average area test

[0218] The hole area can be evenly divided by a certain number of through holes. The hole area can be tested using conventional methods and equipment in the art, for example, a digital optical microscope (Keyence, VHX-7000) can be used to take a picture of a 1 cm2 area, and the image recognition system with its own software can be used to distinguish the difference between the hole and the foil, and the image recognition is used to calculate the area. The software can count the number of holes per unit area, thereby obtaining the average area of ​​a single hole, the total hole area, and the hole area percentage data.

[0219] The parameters and performances of the secondary batteries of the above embodiments and comparative examples are shown in Table 1.

[0220] Table 1

[0221]

[0222] From Table 1, we can see that:

[0223] The expanded thickness of the secondary battery cells in each embodiment of the present application is significantly smaller than that of conventional isolation membranes, and the number of cycles of the secondary battery is significantly higher than that of conventional isolation membranes, indicating that the isolation membrane of the present application can effectively inhibit the volume expansion of the cell and increase the cycle life of the secondary battery.

[0224] Comparing Example 1, Example 8 and Example 9, it can be seen that when the total pore area of ​​the support layer is 90% to 95%, the cycle performance of the secondary battery can be further improved. Comparing Example 1, Example 10 and Example 11, it can be seen that the average single pore area of ​​the support layer is 78.5 μm 2 ~314μm 2 By comparing Example 1, Example 12 and Example 13, it can be seen that when the thickness of the separator is 12 μm to 20 μm, the growth of lithium dendrites can be further inhibited, the expansion thickness of the battery cell can be reduced, and the cycle performance of the secondary battery can be further improved.

[0225] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. A separation film, characterized in that: include: A support layer, wherein the support layer has a porous structure, and a surface of the support layer is an electronic insulating material; and The elastic ion-conducting filler is arranged in the holes of the supporting layer, and the elastic ion-conducting filler is an electronic insulating material.

2. The isolation film according to claim 1, characterized in that: The ionic conductivity of the elastic ion-conductive filler at 25°C is 10 -4 S / cm~10 -3 S / cm.

3. The isolation film according to claim 1, characterized in that: The elastic ion-conductive filler includes an organic polymer; the organic polymer includes one or more of polycarbonate, polysulfate, polysulfonate, polyphosphate, polycarboxylate, polysulfone, polyamide, polynitrile, polyether, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer and polyvinyl alcohol.

4. The isolation film according to claim 1, characterized in that: The elastic ion-conductive filler further comprises one or more of an electrolyte salt and filler particles.

5. The isolation film according to claim 1, characterized in that: The elastic ion-conductive filler also includes electrolyte salt and filling particles. The mass content of the organic polymer in the elastic ion-conductive filler is 70% to 95%, the mass content of the electrolyte salt is 1% to 10%, and the mass content of the filling particles is 1% to 10%.

6. The isolation film according to claim 5, characterized in that: The filling particles include one or more of Al2O3, PVDF, garnet-type oxide solid electrolyte, lithium titanium aluminum phosphate solid electrolyte, perovskite solid electrolyte and sulfide solid electrolyte.

7. The isolation membrane according to any one of claims 1 to 6, characterized in that: The material of the support layer includes a porous aluminum layer with an aluminum oxide film on the surface.

8. The isolation membrane according to any one of claims 1 to 6, characterized in that: The total pore area of ​​the support layer accounts for 80% to 95%; Optionally, the total pore area of ​​the support layer accounts for 90% to 95%.

9. The isolation membrane according to any one of claims 1 to 6, characterized in that: The average single hole area of ​​the porous structure in the support layer is 78.5 μm 2 ~1926.5μm 2 ; Optionally, the average single pore area of ​​the porous structure in the support layer is 78.5 μm 2 ~314μm 2 .

10. The isolation membrane according to any one of claims 1 to 6, characterized in that: The strength of the support layer is greater than the creep strength of metallic lithium.

11. The isolation membrane according to any one of claims 1 to 6, characterized in that: The holes in the support layer are arranged in an array.

12. The isolation membrane according to any one of claims 1 to 6, characterized in that: The hole is a columnar hole, and the axis of the hole is parallel to the thickness direction of the isolation film.

13. The isolation membrane according to any one of claims 1 to 6, characterized in that: The thickness of the isolation film is 8 μm to 20 μm; Optionally, the isolation film has a thickness of 12 μm to 20 μm.

14. A method for preparing an isolation film, characterized in that: The steps include: Providing a support layer, wherein the support layer has a porous structure, and the surface of the support layer is an electronic insulating material; and An elastic ion-conducting filler is formed in the holes of the support layer, and the elastic ion-conducting filler is an electronic insulating material.

15. The method for preparing an isolation film according to claim 14, characterized in that: Forming an elastic ion-conducting filler in the pores of the support layer comprises the following steps: coating the elastic ion-conducting filler in the pores of the support layer.

16. The method for preparing an isolation film according to claim 14, characterized in that: The method of forming an elastic ion-conducting filler in the pores of the support layer comprises the following steps: filling the pores of the support layer with a slurry containing a cross-linking agent, a polymer monomer and an initiator, and forming the elastic ion-conducting filler after cross-linking and curing.

17. A secondary battery, characterized in that: An isolation film comprising the isolation film according to any one of claims 1 to 13, or an isolation film prepared by the preparation method according to any one of claims 14 to 16.

18. The secondary battery according to claim 17, characterized in that: The secondary battery includes a negative electrode sheet having a negative electrode active material, wherein the negative electrode active material includes one or more of lithium metal and graphite.

19. An electrical device, characterized in that: A secondary battery comprising the secondary battery according to claim 17 or 18.