Nonaqueous electrolyte secondary battery
By using graphite particles and Si compounds with different internal porosity in the negative electrode mixture layer of a non-aqueous electrolyte secondary battery, and adding specific concentrations of fluoroethylene carbonate and sultone to the non-aqueous electrolyte, it is formed The composite coating solves the problem of reduced output power after charging and discharging, and improves the stability and life of the battery.
Patent Information
- Application Number
- CN202380024659.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-09
- Filing Date
- 2023-03-03
- Publication Date
- 2024-10-18
AI Technical Summary
The output power of existing non-aqueous electrolyte secondary batteries is easily reduced after repeated charging and discharging, and existing technology cannot effectively solve this problem.
The negative electrode mixture layer contains graphite particles A and graphite particles B with different internal porosity, as well as Si compounds, and uses fluoroethylene carbonate and sultone with unsaturated bonds in the non-aqueous electrolyte to form a composite The film is used to inhibit the decomposition reaction on the surface of the negative electrode and keep the battery resistance stable.
It effectively suppresses the reduction in output power caused by charge and discharge cycles, prolongs the service life of the battery and improves the stability of the battery.
Smart Images

Figure CN118805282A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a non-aqueous electrolyte secondary battery. Background Art
[0002] Non-aqueous electrolyte secondary batteries using a carbon material such as graphite as a negative electrode active material are widely used as high energy density secondary batteries.
[0003] For example, Patent Document 1 discloses a nonaqueous electrolyte secondary battery using two types of graphite particles having different internal porosities, wherein a large number of graphite particles having a small internal porosity are contained on the outer surface side of the negative electrode mixture layer, and a nonaqueous electrolyte containing a diisocyanate compound is used.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2021 / 111932 Summary of the invention
[0007] In recent years, non-aqueous electrolyte secondary batteries have been increasingly required to have high output power. The inventors of the present invention have conducted in-depth research and found that even if the negative electrode described in Patent Document 1 is used, the output power at low SOC (State of Charge) may be reduced due to repeated charge and discharge. The technology described in Patent Document 1 does not study the reduction in output power at low SOC caused by repeated charge and discharge, and there is still room for improvement.
[0008] An object of the present invention is to provide a non-aqueous electrolyte secondary battery in which a decrease in output due to charge and discharge cycles is suppressed.
[0009] A nonaqueous electrolyte secondary battery as one embodiment of the present invention is characterized in that it comprises a positive electrode, a negative electrode, and a nonaqueous electrolyte, the negative electrode comprising a negative electrode current collector and a negative electrode mixture layer provided on the negative electrode current collector, the negative electrode mixture layer comprising graphite particles A, graphite particles B, and a Si compound, the internal porosity of the graphite particles A being 5% or less, the internal porosity of the graphite particles B being 8% to 20%, the Si compound comprising an ion conductive layer and Si particles dispersed in the ion conductive layer, when the negative electrode mixture layer is divided into two equal parts in the thickness direction, the graphite particles A are contained more in a half region on the outer surface side than in a half region on the negative electrode current collector side, the nonaqueous electrolyte comprises at least fluoroethylene carbonate and sultone having an unsaturated bond, and in the nonaqueous electrolyte, when the concentration of sultone is X mass % and the concentration of fluoroethylene carbonate is Y mass %, 0.01≤X≤1.5, 0.5≤Y≤15, and 0.01≤X / Y≤0.5 are satisfied.
[0010] According to the nonaqueous electrolyte secondary battery of the present invention, it is possible to suppress a decrease in output power due to charge and discharge cycles. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment.
[0012] Figure 2 It is a cross-sectional view of a negative electrode as an example of an embodiment.
[0013] Figure 3 This is a cross-sectional view of graphite particles in the negative electrode mixture layer. DETAILED DESCRIPTION
[0014] The nonaqueous electrolyte secondary battery as one embodiment of the present invention is characterized in that it has a positive electrode, a negative electrode and a nonaqueous electrolyte, the negative electrode has a negative electrode collector and a negative electrode mixture layer arranged on the negative electrode collector, the negative electrode mixture layer comprises graphite particles A, graphite particles B and a Si compound, the internal porosity of the graphite particles A is less than 5%, the internal porosity of the graphite particles B is 8% to 20%, the Si compound comprises an ion conductive layer and Si particles dispersed in the ion conductive layer, and the negative electrode mixture layer is formed in a thickness direction. When divided into two equal parts, the graphite particles A are contained more in the half region on the outer surface side than in the half region on the negative electrode current collector side, the non-aqueous electrolyte contains at least fluoroethylene carbonate and sultone having an unsaturated bond (hereinafter, sometimes described as sultone), and in the non-aqueous electrolyte, when the concentration of sultone is set to X mass % and the concentration of fluoroethylene carbonate is set to Y mass %, 0.01≤X≤1.5, 0.5≤Y≤15 and 0.01≤X / Y≤0.5 are satisfied.
[0015] It is believed that the non-aqueous electrolyte containing fluoroethylene carbonate and sultone at a predetermined concentration is decomposed by fluoroethylene carbonate and sultone, thereby forming a composite film on the surface of the graphite particles and Si compound in the negative electrode, and the decomposition reaction of the non-aqueous electrolyte on the negative electrode surface during charge and discharge is suppressed. Generally speaking, the volume change of the Si compound with charge and discharge is large, and with this volume change, the film on the surface of the Si compound is destroyed, which easily causes the continuous decomposition reaction of the non-aqueous electrolyte. It is believed that if it is a composite film formed by the above-mentioned fluoroethylene carbonate and sultone, it is not easy to be destroyed even for the volume change of the Si compound, and it is not easy to cause the continuous decomposition reaction of the non-aqueous electrolyte. In addition, it is believed that by including more graphite particles A with an internal porosity of less than 5% in half of the area on the outer surface side of the negative electrode mixture layer compared with half of the area on the negative electrode collector side of the negative electrode mixture layer, the reactivity of the outer surface of the negative electrode mixture layer can also be suppressed, so the decomposition reaction of the non-aqueous electrolyte in the negative electrode is suppressed. It is presumed that by suppressing the decomposition reaction of the nonaqueous electrolyte in this way, a high-quality film on the surface of the negative electrode is maintained, and an increase in battery resistance after charge and discharge cycles is suppressed, thereby suppressing a decrease in output power.
[0016] Hereinafter, an example of an embodiment will be described in detail with reference to the accompanying drawings. It should be noted that the nonaqueous electrolyte secondary battery of the present invention is not limited to the embodiment described below. In addition, the drawings referred to in the description of the embodiment are schematic diagrams.
[0017] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment. Figure 1 The non-aqueous electrolyte secondary battery 10 shown has: a wound electrode body 14 in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13, a non-aqueous electrolyte, insulating plates 18 and 19 respectively arranged on the upper and lower sides of the electrode body 14, and a battery case 15 for accommodating the above components. The battery case 15 is composed of a case body 16 in a cylindrical shape with a bottom and a sealing body 17 that blocks the opening of the case body 16. It should be noted that other forms of electrode bodies such as a laminated electrode body in which a positive electrode and a negative electrode are alternately laminated with a separator can be used instead of the wound electrode body 14. In addition, as the battery case 15, a cylindrical, square, coin-shaped, button-shaped metal outer can, a bag outer body formed by laminating a resin sheet and a metal sheet, etc. can be exemplified.
[0018] The case body 16 is, for example, a metal outer can in a bottomed cylindrical shape. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure the airtightness of the battery interior. The case body 16 has, for example, an extension portion 22 in which a part of the side surface extends inwardly and supports the sealing body 17. The extension portion 22 is preferably formed in an annular shape along the circumference of the case body 16, and supports the sealing body 17 on its upper surface.
[0019] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions. If the internal pressure of the non-aqueous electrolyte secondary battery 10 rises due to heat caused by an internal short circuit, for example, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cover 27 side, and the current path between the lower valve body 24 and the upper valve body 26 is cut off. If the internal pressure rises further, the upper valve body 26 breaks, and the gas is discharged from the opening of the cover 27.
[0020] exist Figure 1 In the non-aqueous electrolyte secondary battery 10 shown, the positive electrode lead 20 attached to the positive electrode 11 extends to the sealing body 17 side through the through hole of the insulating plate 18, and the negative electrode lead 21 attached to the negative electrode 12 extends to the bottom side of the case body 16 through the outside of the insulating plate 19. The positive electrode lead 20 is connected to the bottom plate of the sealing body 17, that is, the lower surface of the filter 23, by welding or the like, and the top plate of the sealing body 17, that is, the cover 27 electrically connected to the filter 23 becomes the positive terminal. The negative electrode lead 21 is connected to the bottom inner surface of the case body 16 by welding or the like, and the case body 16 becomes the negative terminal.
[0021] Hereinafter, each component of the nonaqueous electrolyte secondary battery 10 will be described in detail.
[0022] [negative electrode]
[0023] Figure 2 1 is a cross-sectional view of a negative electrode as an example of an embodiment. The negative electrode 12 includes a negative electrode current collector 40 and a negative electrode mixture layer 42 provided on the negative electrode current collector 40 .
[0024] The negative electrode current collector 40 is made of, for example, a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having the metal disposed on the surface.
[0025] The negative electrode mixture layer 42 contains graphite particles and Si compounds as negative electrode active materials. In addition, the negative electrode mixture layer 42 preferably contains a binder, etc. The negative electrode 12 can be made, for example, as follows: prepare a negative electrode mixture slurry containing a negative electrode active material, a binder, etc., apply the negative electrode mixture slurry on the negative electrode collector 40 and dry it to form a negative electrode mixture layer 42, and roll the negative electrode mixture layer 42 to make it. It should be noted that the details of the method for making the negative electrode mixture layer 42 are described later.
[0026] Figure 3is a cross-sectional view of graphite particles in the negative electrode mixture layer. Figure 3 As shown, in the cross-sectional view of the graphite particle 30, the graphite particle 30 has closed voids 34 that are not connected from the inside of the particle to the particle surface (hereinafter referred to as internal voids 34) and voids 36 that are connected from the inside of the particle to the particle surface (hereinafter referred to as external voids 36).
[0027] The graphite particles 30 include graphite particles A having an internal porosity of 5% or less and graphite particles B having an internal porosity of 8% to 20%. From the perspective of suppressing the decomposition reaction of the non-aqueous electrolyte, the internal porosity of the graphite particles A may be 5% or less, preferably 1% to 5%, and more preferably 3% to 5%. From the perspective of suppressing the decomposition reaction of the non-aqueous electrolyte, the internal porosity of the graphite particles B may be 8% to 20%, preferably 10% to 18%, and more preferably 12% to 16%. Here, the internal porosity of the graphite particles is a two-dimensional value obtained by the ratio of the area of the internal voids 34 of the graphite particles to the cross-sectional area of the graphite particles. In addition, the internal porosity of the graphite particles is obtained by the following steps.
[0028] <Method for measuring internal void ratio>
[0029] (1) Exposing the cross section of the negative electrode mixture layer. For example, a method of exposing the cross section includes cutting a portion of the negative electrode and processing it using an ion milling device (eg, IM4000PLUS manufactured by Hitachi High-Tech Corporation) to expose the cross section of the negative electrode mixture layer.
[0030] (2) A backscattered electron image of the cross section of the exposed negative electrode mixture layer is taken using a scanning electron microscope. The backscattered electron image is taken at a magnification of 3,000 to 5,000 times.
[0031] (3) The cross-sectional image obtained as described above is read into a computer and binarized using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health, U.S.A.) to obtain a binary processed image in which the particle cross section in the cross-sectional image is converted to black and the voids in the particle cross section are converted to white.
[0032] (4) Graphite particles A and B with a particle size of 5 μm to 50 μm are selected from the binary processed image, and the area of the cross section of the graphite particles and the area of the internal voids present in the cross section of the graphite particles are calculated. Here, the area of the cross section of the graphite particles refers to the area of the region surrounded by the periphery of the graphite particles, that is, the area of the entire cross section of the graphite particles. In addition, for voids with a width of less than 3 μm in the cross section of the graphite particles, it is sometimes difficult to determine whether they are internal voids or external voids in image analysis, so voids with a width of less than 3 μm can be set as internal voids. Then, the internal void ratio of the graphite particles is calculated based on the calculated area of the cross section of the graphite particles and the area of the internal voids in the cross section of the graphite particles (area of the internal voids in the cross section of the graphite particles × 100 / area of the cross section of the graphite particles). The internal void ratio of graphite particles A and B is the average value of 10 graphite particles A and B respectively.
[0033] The graphite particles A and B are produced, for example, as follows.
[0034] <Graphite Particle A Having an Internal Porosity of 5% or Less>
[0035] For example, coke (precursor) as the main raw material is crushed into a specified size, and in a state where they are agglomerated with a binder, they are fired at a temperature above 2600°C, graphitized, and then sieved to obtain graphite particles A of the desired size. Here, the internal porosity can be adjusted to less than 5% according to the particle size of the precursor after crushing, the particle size of the precursor in an agglomerated state, etc. For example, the average particle size (volume-based median particle size D50) of the crushed precursor is preferably in the range of 12μm to 20μm. In addition, when the internal porosity is reduced within a range of less than 5%, it is preferred to increase the particle size of the crushed precursor.
[0036] <Graphite particles B having an internal porosity of 8% to 20%>
[0037] For example, coke (precursor) as the main raw material is crushed into a specified size, and after agglomerating them with a binder, they are further pressed into a block state and fired at a temperature of 2600°C or above to graphitize them. The block-shaped molded body after graphitization is crushed and sieved to obtain graphite particles B of the desired size. Here, the internal porosity can be adjusted to 8% to 20% by the amount of volatile components added to the block-shaped molded body. In the case where a part of the binder added to the coke (precursor) volatilizes during firing, the binder can be used as a volatile component. Asphalt can be exemplified as such a binder.
[0038] The graphite particles A and B are not particularly limited to natural graphite, artificial graphite, etc., but artificial graphite is preferred from the perspective of ease of adjusting the internal porosity. The interplanar spacing (d002 ) is preferably 0.3354 nm or more, more preferably 0.3357 nm or more, and preferably less than 0.340 nm, more preferably 0.338 nm or less. In addition, the crystallite size (Lc(002)) of the graphite particles A and B obtained by X-ray diffraction is preferably 5 nm or more, more preferably 10 nm or more, and preferably 300 nm or less, more preferably 200 nm or less. The interplanar spacing (d 002 When the crystallite size (Lc(002)) and the crystallite size (Lc(002)) satisfy the above ranges, the battery capacity of the non-aqueous electrolyte secondary battery tends to be larger than when the above ranges are not satisfied.
[0039] Will Figure 2 When the negative electrode mixture layer 42 shown is divided into two equal parts in the thickness direction, the graphite particles A are contained more in the region 42b of the half on the outer surface side than in the region 42a of the half on the negative electrode collector side. Thus, the decomposition reaction of the non-aqueous electrolyte in the negative electrode is suppressed, thereby suppressing the reduction in output power. It should be noted that dividing the negative electrode mixture layer 42 into two equal parts in the thickness direction means that when the stacking direction of the negative electrode collector 40 and the negative electrode mixture layer 42 is set to the thickness direction of the negative electrode mixture layer 42, it is divided into two halves at the middle M of the thickness of the negative electrode mixture layer 42. In addition, when the negative electrode mixture layer 42 is divided into two equal parts in the thickness direction, the negative electrode mixture layer 42 located near when observed from the negative electrode collector 40 is set to the region 42a of the half on the negative electrode collector side, and the negative electrode mixture layer 42 located far away when observed from the negative electrode collector 40 is set to the region 42b of the half on the outer surface side.
[0040] Compared with the half region 42a on the negative electrode collector side, the graphite particles A are contained more in the half region 42b on the outer surface side. From the perspective of suppressing the decomposition reaction of the non-aqueous electrolyte in the negative electrode, the ratio of the graphite particles A to the graphite particles B in the half region 42b on the outer surface side is preferably 20:80 to 100:0, and more preferably 50:50 to 100:0 in terms of mass ratio. In addition, the ratio of the graphite particles A to the graphite particles B in the half region 42a on the negative electrode collector side is preferably 10:90 to v:100 in terms of mass ratio, and more preferably 0:100.
[0041] The content of the graphite particles A in the negative electrode mixture layer 42 is, for example, 20% by mass to 80% by mass, or 25% by mass to 50% by mass, relative to the total mass of the graphite particles A and the graphite particles B.
[0042] The Si compound contained in the negative electrode mixture layer 42 includes an ion conductive layer and Si particles dispersed in the ion conductive layer. From the perspective of increasing the capacity, the content of Si particles in the Si compound is preferably 40 mass % to 70 mass %. The ion conductive phase is a silicate phase, an amorphous carbon phase, or the like.
[0043] SiO, which is an example of Si compound, has a particle structure in which fine Si particles are dispersed in a silicate phase. Suitable SiO has a sea-island structure in which fine Si particles are dispersed substantially uniformly in an amorphous silicon oxide matrix.
[0044] SiC, another example of Si compound, has a particle structure in which fine Si particles are dispersed in an amorphous carbon phase. Suitable SiC has a sea-island structure in which fine Si particles are dispersed substantially uniformly in a matrix of an amorphous carbon phase.
[0045] The ion conductive layer is preferably an amorphous carbon phase. That is, the Si compound is preferably SiC.
[0046] The content of the Si compound in the negative electrode mixture layer is, for example, 5% to 20% by mass relative to the total mass of the negative electrode active material. This can increase the battery capacity and suppress the reduction in charge and discharge cycle characteristics. It should be noted that the content of the Si compound in the half region 42a on the negative electrode collector side and the content of the Si compound in the half region 42b on the outer surface side may be different, but are preferably substantially the same.
[0047] An example of a method for preparing the negative electrode mixture layer 42 is described. For example, a negative electrode active material containing graphite particles B (containing graphite particles A as needed), a binder, and a solvent such as water are mixed to prepare a negative electrode mixture slurry for the negative electrode collector side. In addition, a negative electrode active material containing a larger amount of graphite particles A (containing graphite particles B as needed) than the negative electrode mixture slurry for the negative electrode collector side, a binder, and a solvent such as water are mixed to prepare a negative electrode mixture slurry for the outer surface side. Then, after the negative electrode mixture slurry for the negative electrode collector side is applied to both sides of the negative electrode collector and dried, the negative electrode mixture slurry for the outer surface side is applied to both sides of the coating formed by the negative electrode mixture slurry for the negative electrode collector side and dried, thereby forming the negative electrode mixture layer 42. In the above method, after the negative electrode mixture slurry for the negative electrode collector side is applied and dried, the negative electrode mixture slurry for the outer surface side is applied, but it can also be a method in which the negative electrode mixture slurry for the negative electrode collector side is applied and before drying before the negative electrode mixture slurry for the outer surface side is applied, and the negative electrode mixture slurry for the negative electrode collector side and the negative electrode mixture slurry for the outer surface side can also be applied at the same time.
[0048] Examples of the binder include fluorine resins, polyimide resins, acrylic resins, polyolefin resins, polyacrylonitrile (PAN), styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or its salts, polyacrylic acid (PAA) or its salts (PAA-Na, PAA-K, etc., and partially neutralized salts), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more.
[0049] [positive electrode]
[0050] The positive electrode 11 is composed of, for example, a positive electrode current collector such as a metal foil and a positive electrode mixture layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable within the potential range of the positive electrode, or a film having the metal disposed on the surface. The positive electrode mixture layer may include, for example, a positive electrode active material, a binder, a conductive agent, and the like.
[0051] The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive agent, etc., on a positive electrode current collector, drying the mixture to form a positive electrode mixture layer, and then rolling the positive electrode mixture layer.
[0052] As the positive electrode active material, a lithium transition metal composite oxide containing transition metal elements such as Ni can be exemplified. The lithium transition metal composite oxide preferably contains Ni and at least one element selected from Mn, Co and Al. The content of Ni in the lithium transition metal composite oxide is, for example, 80 mol% to 95 mol% relative to the total molar number of metal elements other than Li. The lithium transition metal composite oxide can be, for example, represented by the general formula Li a Ni x M1 y M1 z O 2-b (wherein, 0.8≤a≤1.2, 0.8≤x≤0.95, 0.05≤y≤0.2, 0≤z≤0.15, 0≤b<0.05, x+y+z=1, M1 is at least one element selected from Mn, Co and Al, and M2 is at least one element selected from Fe, Ti, Si, Nb, Zr, Mo and Zn).
[0053] Examples of the conductive agent include carbon black (CB), acetylene black (AB), Ketjen black, carbon nanotubes (CNT), graphene, graphite and other carbon particles, etc. These may be used alone or in combination of two or more.
[0054] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyimide-based resins, acrylic resins, polyolefin-based resins, and polyacrylonitrile (PAN), etc. These may be used alone or in combination of two or more.
[0055] [Non-aqueous electrolyte]
[0056] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous electrolyte comprises at least fluoroethylene carbonate (FEC) and sultone with an unsaturated bond as a non-aqueous solvent. In addition, in the non-aqueous electrolyte, when the concentration of sultone is set to X mass % and the concentration of FEC is set to Y mass %, 0.01≤X≤1.5, 0.5≤Y≤15 and 0.01≤X / Y≤0.5 are satisfied. Thus, the decomposition reaction of the non-aqueous electrolyte on the negative electrode surface during charge and discharge is suppressed. It is speculated that this is because FEC and sultone are decomposed to form a composite film on the negative electrode surface.
[0057] The sultone is not particularly limited as long as it has an unsaturated bond. Examples of the sultone include 1-propenyl-1,3-sultone and 1-butenyl-1,4-sultone. As the sultone, 1-propenyl-1,3-sultone is preferred.
[0058] The non-aqueous electrolyte can include a non-aqueous solvent other than FEC and sultone. As a non-aqueous solvent other than FEC and sultone, carbonates, lactones, ethers, ketones, esters, etc. can be used, and these solvents can be mixed and used more than two kinds. In the case of mixing more than two kinds of solvents, it is preferred to use a mixed solvent comprising cyclic carbonates and linear carbonates. For example, as cyclic carbonates, ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), etc. can be used, and as linear carbonates, dimethyl carbonate (DMC), ethyl methyl carbonate (EMC) and diethyl carbonate (DEC), etc. can be used. As esters, it is preferred to use carboxylic acid esters such as methyl acetate (MA) and methyl propionate (MP). In addition, the non-aqueous solvent can contain halogen substitutes other than FEC such as methyl fluoropropionate (FMP).
[0059] The non-aqueous electrolyte preferably contains lithium bis(fluorosulfonyl)imide (LiF SI) as an electrolyte salt. As a result, the effect of suppressing the reduction of output power becomes more significant. It is speculated that this is because a better quality film is formed on the surface of the negative electrode. When the concentration of LiF SI in the non-aqueous electrolyte is set to Z mass%, it is preferred to satisfy 0.01≤Z≤5 and 0.1≤X / Z≤1.
[0060] The electrolyte salt may include lithium sulfonyl imide other than LiF SI. As lithium sulfonyl imide other than LiF SI, for example, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(nonafluorobutanesulfonyl)imide, lithium bis(pentafluoroethanesulfonyl)imide (LIBETI) etc. may be cited. They may be used alone or in combination of two or more.
[0061] The electrolyte salt may include lithium salts other than lithium sulfonimide. Examples of lithium salts other than lithium sulfonimide include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, borate salts such as Li2B4O7, Li(B(C2O4)F2), etc. Among them, from the viewpoints of ionic conductivity, electrochemical stability, etc., LiPF6 is preferably used. The concentration of LiPF6 is preferably set to 0.8 mol to 1.8 mol per 1 L of the non-aqueous solvent.
[0062] The non-aqueous electrolyte may contain vinylene carbonate (VC), ethylene sulfite (ES), cyclohexylbenzene (CHB), o-terphenyl (OTP), propanesultone-based compounds, etc. Among them, from the viewpoint of high capacity, etc., it is preferable to contain VC. The addition amount of VC is not particularly limited. For example, it is 0.1% by mass to 5% by mass relative to the total mass of the non-aqueous electrolyte.
[0063] [Separator]
[0064] The separator 13 is, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous membranes, woven fabrics, non-woven fabrics, etc. As the material of the separator, olefin-based resins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin-based resin. In addition, it may be a multi-layer separator including a polyethylene layer and a polypropylene layer, or a separator in which a material such as an aromatic polyamide-based resin or ceramic is coated on the surface of the separator.
[0065] Examples
[0066] Hereinafter, the present invention will be further described by way of examples, but the present invention is not limited to these examples.
[0067] [Example 1]
[0068] [Fabrication of positive electrode]
[0069] As the positive electrode active material, lithium nickel cobalt aluminate containing aluminum (LiNi 0.91 Co 0.04 Al 0.05O2). 100 parts by mass of the above positive electrode active material, 1 part by mass of acetylene black and 0.9 parts by mass of polyvinylidene fluoride were mixed in a solvent of N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode mixture slurry. The slurry was applied to both sides of an aluminum foil having a thickness of 15 μm, and after the coating was dried, the coating was rolled using a calendering roller, thereby producing a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode collector.
[0070] [Preparation of Graphite Particles A]
[0071] The coke was crushed to an average particle size (median particle size D50) of 12 μm. Pitch was added as a binder to the crushed coke to agglomerate the coke to an average particle size (median particle size D50) of 17 μm. The agglomerate was calcined at a temperature of 2800° C. to graphitize, and then sieved using a 250-mesh sieve to obtain graphite particles A having an average particle size (median particle size D50) of 23 μm.
[0072] [Preparation of Graphite Particles B]
[0073] The coke was crushed to an average particle size (median particle size D50) of 15 μm, and pitch was added as a binder to the crushed coke to make it agglomerated. 3 ~1.9g / cm 3 The block-shaped body was sintered at a temperature of 2800°C to graphitize. Next, the block-shaped body after graphitization was crushed and sieved using a 250-mesh sieve to obtain graphite particles B with an average particle size (median particle size D50) of 23 μm.
[0074] [Production of negative electrode]
[0075] Mixed graphite obtained by mixing 60 parts by mass of graphite particles A and 40 parts by mass of graphite particles B was mixed with SiC at a mass ratio of 92:8, and used as the negative electrode active material A contained in the half area on the outer surface side of the negative electrode mixture layer. They were mixed in a manner that the mass ratio of negative electrode active material A: carboxymethyl cellulose (CMC): styrene-butadiene copolymer rubber (SBR) was 100:1:1, and the negative electrode mixture slurry on the outer surface side was prepared. In addition, graphite particles B and SiC were mixed in a mass ratio of 92:8, and used as the negative electrode active material B contained in the half area on the negative electrode collector side of the negative electrode mixture layer. They were mixed in a manner that the mass ratio of negative electrode active material B: carboxymethyl cellulose (CMC): styrene-butadiene copolymer rubber (SBR) was 100:1:1, and the negative electrode mixture slurry on the negative electrode collector side was prepared. It should be noted that, as described above, the ratio of the Si compound to the total mass of the negative electrode active material is the same on the outer surface side and the collector side. In addition, the content of Si particles in SiC was 50 mass %.
[0076] The negative electrode mixture slurry on the negative electrode collector side is applied to both sides of a copper foil having a thickness of 8 μm. After the coating is dried, the negative electrode mixture slurry on the outer surface side is applied to the coating and dried, and the coating is rolled using a calendering roller, thereby producing a negative electrode having a negative electrode mixture layer formed on both sides of the negative electrode collector. That is, the mass ratio of graphite particles A: graphite particles B in half of the area on the outer surface side of the negative electrode mixture layer is 60:40, and the mass ratio of graphite particles A: graphite particles B in half of the area on the negative electrode collector side of the negative electrode mixture layer is 0:100. In addition, in the produced negative electrode, the internal porosity of graphite particles A and graphite particles B was measured, and the results were 3% and 15%, respectively.
[0077] [Preparation of non-aqueous electrolyte]
[0078] In a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) mixed so that the volume ratio is 20:5:75, LiPF6 is dissolved at a concentration of 1.35 mol / L. Furthermore, 3% by mass of vinylene carbonate (VC) is added to the total mass of the mixed solvent and LiPF6, and it is used as a basic non-aqueous electrolyte. Next, 0.5 parts by mass of 1-propenyl-1,3-sultone, 2 parts by mass of fluoroethylene carbonate (FEC), and 1 part by mass of lithium bis(fluorosulfonyl)imide (LiF SI) are added to 100 parts by mass of the basic non-aqueous electrolyte to prepare a non-aqueous electrolyte. Therefore, in the non-aqueous electrolyte, the concentration X of sultone is 0.5% by mass, the concentration Y of FEC is 1.9% by mass, and the concentration Z of LiFSI is 1.0% by mass.
[0079] [Manufacturing of Secondary Batteries]
[0080] (1) A positive electrode lead made of aluminum was attached to a positive electrode collector, and a negative electrode lead made of nickel-copper-nickel was attached to a negative electrode collector. The positive electrode and the negative electrode were then wound with a polyethylene separator interposed therebetween to prepare a wound electrode assembly.
[0081] (2) Insulating plates are disposed above and below the electrode body, respectively, the negative electrode lead is welded to the case body, the positive electrode lead is welded to the sealing body, and the electrode body is housed in the case body.
[0082] (3) After injecting a non-aqueous electrolyte into the case body by decompression, the open end of the case body is crimped to the sealing body via a gasket to prepare a secondary battery.
[0083] [Evaluation of DCIR increase rate]
[0084] Under a temperature environment of 25°C, a secondary battery that has been fully discharged to a state of 2.5V at a constant current of 0.2C is charged at a constant current of 0.3C until the battery voltage reaches 3.4V, and then charged at a constant voltage of 3.4V until the current value reaches 0.002C. The SOC of the secondary battery at this time is 10%. Then, after the secondary battery is left to stand for 2 hours in an open circuit state, it is discharged at a constant current of 0.5C for 10 seconds. Based on the open circuit voltage (OCV), the closed circuit voltage (CCV) 10 seconds after discharge, and the current value (I 10s ), calculate the DC resistance (DCIR) using the following formula and use this value as the initial DCIR.
[0085] DCIR=(OCV-CCV) / I 10s
[0086] Next, in a temperature environment of 25°C, the secondary battery was charged at a constant current of 0.3C until the battery voltage reached 4.2V, and then charged at a constant voltage of 4.2V until the current value reached 0.02C. Then, it was discharged at a constant current of 0.5C to 2.5V. This charge and discharge was regarded as one cycle, and 100 cycles were performed.
[0087] For the secondary battery after 100 cycles, the DCIR was calculated in the same manner as the initial DCIR, and this value was defined as the post-cycle DCIR. The DCIR increase rate was determined from the initial DCIR and the post-cycle DCIR using the following formula.
[0088] DCIR increase rate (%) = (DCIR after cycle - initial DCIR) / initial DCIR × 100
[0089] <Example 2>
[0090] In the preparation of the negative electrode, the mixing ratio of the mixed graphite and SiC of the negative electrode active material A and the mixing ratio of the graphite particles B and SiC of the negative electrode active material B were changed to a mass ratio of 90:10, and in the preparation of the non-aqueous electrolyte, the addition amount of FEC was changed to 5 parts by mass. Otherwise, the non-aqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the non-aqueous electrolyte, the concentration X of sultone was 0.5% by mass, the concentration Y of FEC was 4.7% by mass, and the concentration Z of LiF SI was 0.9% by mass.
[0091] <Example 3>
[0092] In the preparation of the negative electrode, the mixing ratio of the mixed graphite and SiC of the negative electrode active material A and the mixing ratio of the graphite particles B and SiC of the negative electrode active material B were changed to a mass ratio of 88:12, and in the preparation of the non-aqueous electrolyte, the addition amount of FEC was changed to 10 parts by mass. Otherwise, the non-aqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the non-aqueous electrolyte, the concentration X of sultone was 0.4% by mass, the concentration Y of FEC was 9.0% by mass, and the concentration Z of LiF SI was 0.9% by mass.
[0093] <Example 4>
[0094] In the preparation of the non-aqueous electrolyte, the addition amount of 1-propenyl-1,3-sultone was changed to 0.2 parts by mass, and the addition amount of FEC was changed to 5 parts by mass. Except for this, the non-aqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the non-aqueous electrolyte, the concentration X of sultone was 0.2% by mass, the concentration Y of FEC was 4.7% by mass, and the concentration Z of LiF SI was 0.9% by mass.
[0095] <Example 5>
[0096] In the preparation of the negative electrode, the mixing ratio of the mixed graphite and SiC of the negative electrode active material A and the mixing ratio of the graphite particles B and SiC of the negative electrode active material B were changed to a mass ratio of 95:5. In the preparation of the non-aqueous electrolyte, the addition amount of 1-propenyl-1,3-sultone was changed to 0.1 parts by mass, and the addition amount of FEC was changed to 5 parts by mass. Except for this, the non-aqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the non-aqueous electrolyte, the concentration X of sultone was 0.1% by mass, the concentration Y of FEC was 4.7% by mass, and the concentration Z of LiF SI was 0.9% by mass.
[0097] <Example 6>
[0098] In the preparation of the nonaqueous electrolyte, the addition amount of LiF SI was changed to 4 parts by mass, and the nonaqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the nonaqueous electrolyte, the concentration X of sultone was 0.5% by mass, the concentration Y of FEC was 1.9% by mass, and the concentration Z of LiF SI was 3.8% by mass.
[0099] <Comparative Example 1>
[0100] In the preparation of the negative electrode, the negative electrode mixture slurry on the outer surface side was applied to both sides of the copper foil, and after the coating was dried, the negative electrode mixture slurry on the negative electrode collector side was applied on the coating. Except for this, the operation was carried out in the same manner as in Example 1 to prepare a non-aqueous electrolyte secondary battery and evaluate it.
[0101] <Comparative Example 2>
[0102] In the preparation of the non-aqueous electrolyte, except that 1-propenyl-1,3-sultone was not added, a non-aqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the non-aqueous electrolyte, the concentration Y of FEC was 1.9% by mass, and the concentration Z of LiF SI was 1.0% by mass.
[0103] <Comparative Example 3>
[0104] In the preparation of the non-aqueous electrolyte, the addition amount of 1-propenyl-1,3-sultone was changed to 2.0 parts by mass, and a non-aqueous electrolyte secondary battery was prepared and evaluated in the same manner as in Example 1. It should be noted that in the non-aqueous electrolyte, the concentration X of sultone was 1.9% by mass, the concentration Y of FEC was 1.9% by mass, and the concentration Z of LiF SI was 1.0% by mass.
[0105] The evaluation results of the secondary batteries of the examples and comparative examples are shown in Table 1. All the evaluations were performed under the same conditions as those described in Example 1. In addition, Table 1 also shows the mass ratio of graphite particles A to graphite particles B in the half on the outer surface side and the half on the collector side of the negative electrode mixture layer, the content of SiC in the negative electrode mixture layer, the concentration X of 1-propenyl-1,3-sultone relative to the basic non-aqueous electrolyte, the concentration Y of FEC, the concentration Z of LiF SI, X / Y, and X / Z.
[0106] [Table 1]
[0107]
[0108] Even after repeated charge and discharge, the increase ratio of DCIR of the secondary battery of the embodiment is suppressed relative to the initial DCIR. On the other hand, after repeated charge and discharge, the increase ratio of DCIR of the secondary battery of the comparative example relative to the initial DCIR is not suppressed compared with the embodiment. It can be seen that by including two graphite particles with different internal porosities and a specified Si compound in the negative electrode mixture layer, and containing a large amount of graphite particles with a small internal porosity in the half area on the outer surface side of the negative electrode mixture layer, and containing a specified concentration of sultone and fluoroethylene carbonate in the non-aqueous electrolyte, the reduction in output power caused by the charge and discharge cycle can be suppressed.
[0109] Description of Reference Numerals
[0110] 10: non-aqueous electrolyte secondary battery, 11: positive electrode, 12: negative electrode, 13: separator, 14: electrode body, 15: battery case, 16: case body, 17: sealing body, 18, 19: insulating plates, 20: positive electrode lead, 21: negative electrode lead, 22: extension, 23: filter, 24: lower valve body, 25: insulating member, 26: upper valve body, 27: cover, 28: gasket, 30: graphite particles, 34: internal gap, 36: external gap, 40: negative electrode collector, 42: negative electrode mixture layer, 42a: half of the area on the negative electrode collector side, 42b: half of the area on the outer surface side.
Claims
1. A non-aqueous electrolyte secondary battery comprising a positive electrode, a negative electrode and a non-aqueous electrolyte, The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on the negative electrode current collector. The negative electrode mixture layer includes graphite particles A, graphite particles B and a Si compound as negative electrode active materials. The internal porosity of the graphite particles A is less than 5%, and the internal porosity of the graphite particles B is 8% to 20%. The Si compound comprises an ion conducting layer and Si particles dispersed in the ion conducting layer, When the negative electrode mixture layer is divided into two equal parts in the thickness direction, the graphite particles A are contained more in the half region on the outer surface side than in the half region on the negative electrode current collector side. The non-aqueous electrolyte contains at least fluoroethylene carbonate and sultone having an unsaturated bond, In the non-aqueous electrolyte, when the concentration of the sultone is X mass % and the concentration of the fluoroethylene carbonate is Y mass %, 0.01≤X≤1.5, 0.5≤Y≤15, and 0.01≤X / Y≤0.5 are satisfied.
2. The nonaqueous electrolyte secondary battery according to claim 1, wherein: The content of the graphite particles A in the negative electrode mixture layer is 20% by mass to 80% by mass based on the total mass of the graphite particles A and the graphite particles B.
3. The non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein: The content of the Si particles in the Si compound is 40 mass % to 70 mass %.
4. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein The ion conducting layer is an amorphous carbon phase.
5. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 4, wherein The content of the Si compound in the negative electrode mixture layer is 5% by mass to 20% by mass based on the total mass of the negative electrode active material.
6. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein The non-aqueous electrolyte contains lithium bis(fluorosulfonyl)imide.
7. The nonaqueous electrolyte secondary battery according to claim 6, wherein: When the concentration of lithium bis(fluorosulfonyl)imide in the non-aqueous electrolyte is Z mass %, 0.01≤Z≤5 and 0.1≤X / Z≤1 are satisfied.
8. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 7, wherein The sultone is 1-propenyl-1,3-sultone.
9. The nonaqueous electrolyte secondary battery according to any one of claims 1 to 8, wherein The positive electrode comprises a lithium transition metal composite oxide, The lithium transition metal composite oxide comprises Ni and at least one element selected from the group consisting of Mn, Co and Al. The content of Ni in the lithium transition metal composite oxide is 80 mol % to 95 mol % based on the total molar number of metal elements excluding Li.