Pd-coated MOF gel mixed matrix membrane for improving hydrogen transmission and separation efficiency as well as preparation method and application of Pd-coated MOF gel mixed matrix membrane

By growing Pd in ​​situ on MOF gel to prepare Pd@MOF gel MMMs, the "trade-off" problem between the permeability and selectivity of pure polymer membranes is solved, achieving efficient hydrogen separation suitable for large-scale production.

CN118807499APending Publication Date: 2024-10-22HUNAN UNIV

Patent Information

Application Number
CN202410955428.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Existing pure polymer membranes exhibit a trade-off between permeability and selectivity in gas separation, and Pd tends to agglomerate when used as a filler, affecting the membrane's separation performance.

Method used

Pd@MOF gel composites were prepared by in-situ growth method, in which Pd was uniformly distributed on MOF gel to form Pd@MOF gel composites. Polymers such as polyimide or self-polymerizing microporous polymers were combined to form Pd@MOF gel MMMs. The introduction of Pd@MOF gel into the polymer can improve hydrogen permeability and selectivity.

Benefits of technology

It significantly improves the permeability and selectivity of hydrogen, avoids Pd agglomeration, enhances hydrogen separation efficiency, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118807499A_ABST
    Figure CN118807499A_ABST
Patent Text Reader

Abstract

The invention provides a Pd-coated MOF gel (Pd-coated MOF gel) mixed matrix membrane for improving hydrogen transmission and separation efficiency as well as a preparation method and application thereof, and belongs to the field of gas membrane separation. According to the film, Pd is uniformly distributed on ZIF-67 gel to form Pd-coated ZIF-67 gel, so that the problems that a traditional Pd nano-particle (Pd NPs) filler is easy to agglomerate and poor in dispersity are solved. The Pd-coated ZIF-67 gel has a three-dimensional interconnected gel network structure, a high-speed hydrogen mass transfer channel is provided, meanwhile, the aperture of the ZIF-67 gel is reduced by Pd NPs, and the hydrogen permeability is improved. Pd NPs are uniformly distributed on an MOF gel network, so that the agglomeration phenomenon in the polymer is effectively reduced, and good dispersity and mass transfer performance are kept. By introducing Pd (at) ZIF-67 gel into polyimide (P84) and an auto-polymerization microporous polymer (PIM-1), the membrane provided by the invention is remarkably improved in hydrogen permeation and H2 / CH4 selectivity, breaks through the Trade-off limitation of a pure polymer membrane, provides an efficient hydrogen separation and purification scheme, and is suitable for the fields of petrochemical industry, semiconductor manufacturing and the like needing high-purity hydrogen.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of gas membrane separation, and specifically relates to a Pd@MOF gel mixed matrix membrane and a preparation method thereof and application in H2 separation. Background Art

[0002] Pure hydrogen is widely needed in many industrial applications, such as fuel cells, petrochemical industry and semiconductor manufacturing. High-purity hydrogen is critical for these applications because impurities may cause equipment damage, reduced efficiency, and even cause safety issues. For example, in fuel cells, impurities may cause electrode poisoning and damage, which significantly reduces battery performance and service life; in the semiconductor manufacturing process, high-purity hydrogen can prevent device contamination and ensure product quality; in the petrochemical industry, high-purity hydrogen is used in hydrogenation reactions to avoid catalyst deactivation. Therefore, in order to ensure product quality, long life of equipment and safety at work, hydrogen purification is essential.

[0003] Although membrane separation technology is widely recognized as an efficient method for hydrogen purification, pure polymer membranes still face major challenges in the field of gas separation, namely the "trade-off" relationship between permeability and selectivity. This means that increasing the permeability of the membrane usually leads to a decrease in selectivity, and vice versa. To address this problem, researchers have developed mixed matrix membranes (MMMs) to improve gas separation efficiency by combining polymers with functional fillers. However, MMMs also face some practical application challenges, such as poor dispersion of fillers in the membrane and easy agglomeration, which leads to the formation of irregular gaps in the membrane, thereby affecting its separation effect.

[0004] Palladium (Pd) is widely used in the field of hydrogen purification due to its high selectivity and permeability to hydrogen. However, the use of pure Pd membranes has the problems of high cost and harsh preparation conditions. In addition, when Pd is used as a filler in MMMs, it is easy to agglomerate and form irregular voids, which affects the separation effect of the membrane. Metal organic framework gel (MOF gel) is a new type of high-performance material with the characteristics of high aspect ratio, easy dispersion, large specific surface area and the formation of a 3D interconnected network in the membrane. Through the in situ growth method, Pd can be evenly distributed on MOF gel to form a Pd@MOF gel composite material to overcome the shortcomings of Pd alone as a filler. Pd@MOF gel combines the advantages of MOF gel and Pd. First, Pd nanoparticles (NP) are easily evenly distributed on MOF gel, avoiding agglomeration and maintaining efficient gas separation performance. Second, the introduction of Pd reduces the number of mesopores and macropores in MOF gel, which helps to enhance the selectivity of H2 / CH4. In addition, Pd is evenly distributed in the 3D interconnected network of MOF gel, reducing the mass transfer resistance of hydrogen in the gel network and enhancing the diffusion coefficient of hydrogen in MMMs. By introducing Pd@MOF gel into polymers such as polyimide (P84) and self-polymerized microporous polymer (PIM-1), not only can the permeability of hydrogen be improved, but also the selectivity of H2 / CH4 can be significantly improved, breaking through the "trade-off" limitation of pure polymer membranes, thereby achieving efficient hydrogen separation and purification. The development of Pd@ZIF-67gel MMMs is expected to make significant progress in the field of hydrogen separation and meet the needs of industrial applications. Summary of the invention

[0005] The purpose of the present invention is to provide a Pd@MOF gel MMMs membrane, which has efficient hydrogen transmission and separation performance, and the preparation method is simple and suitable for large-scale production.

[0007] To achieve the above object, the specific technical solutions of the present invention are as follows:

[0008] Step (1): Weigh 0.224 g of palladium acetate (Pd(OAc)2) and 0.555 g of 30K polyvinyl pyrrolidone (PVP), dissolve them in 25 mL of ethanol. Heat and stir in a 70°C water bath for 2 hours to obtain a uniform black PVP Pd mixed solution;

[0009] Step (2): preparing a 0.13-0.53 mol / L metal ion solution using methanol as a solvent, and preparing an organic ligand solution according to a ratio of metal ion: imidazole: triethylamine of 1:8:8;

[0010] Step (3): Mix and stir the above organic ligand solution, immediately add 25 mL of PVP Pd mixed solution, stir vigorously for 2 minutes, and then stand for 24 hours. Wash the unreacted ligand three times with methanol to obtain Pd@MOF gel;

[0011] Step (4): dissolving an appropriate amount of polymer in an organic solvent to obtain a polymer solution;

[0012] Step (5): Use the same organic solvent as the polymer to replace the Pd@MOF gel three times, so that the Pd@MOF gel is evenly distributed in the same organic solvent as the polymer. Add a certain amount of polymer solution dropwise to the Pd@MOF gel, ultrasonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it at room temperature for 1 to 4 days, and finally place the film in a vacuum oven at 80 to 120°C and dry it for 12 to 24 hours to obtain Pd@MOF gelMMMs.

[0013] In step (2) of the present invention, the metal ion solution may be Zn 2+ or Co 2+ .

[0014] In step (4) of the present invention, the polymer may be selected from polyimide, self-polymerizing microporous polymer, polybenzimidazole and the like.

[0015] In step (5) of the present invention, the content of the Pd@MOF gel is 1 to 40 wt % of the mass of the Pd@MOF gel MMMs.

[0016] In step (5) of the present invention, the total mass concentration of the polymer and the Pd@MOF gel in the mixed solution for film casting is 1.5 to 3.0 wt%.

[0017] Preferably, the solvent of the film casting mixed solution is selected from chloroform and N,N-dimethylformamide.

[0018] In step (5) of the invention, the stirring time is 12 to 24 hours.

[0019] In step (5) of the present invention, the treatment temperature of the vacuum treatment is 80 to 150° C., and the treatment time is 12 to 24 hours.

[0020] According to one aspect of the present invention, there is provided an application of the above-mentioned Pd@MOF gel MMMs in gas separation.

[0021] Optionally, the Pd@MOF gel MMMs are used in the separation of gas mixtures containing H2.

[0022] Preferably, the gas comprises at least one of N2, CH4 and CO2.

[0023] In the present application, the gas mixture contacts one side of the Pd@MOF gel MMMs, thereby causing H2 to permeate the Pd@MOFgel MMMs to achieve a gas separation effect.

[0024] Compared with the prior art, the present invention has the following beneficial technical effects:

[0025] The Pd@MOF gel MMMs of the present invention are prepared by an in-situ growth method, and the Pd NPs are evenly distributed to avoid agglomeration, which significantly improves the hydrogen permeability and selectivity. The Pd@MOF gel has a high specific surface area and a 3D interconnected network structure, and the Pd evenly distributed on the gel network reduces the mass transfer resistance and improves the separation efficiency.

[0026] The film-making method provided by the invention is easy to operate, has strong applicability, is suitable for large-scale production, is environmentally friendly and energy-saving, and has broad industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the transmission electron microscopy image of Pd@ZIF-67gel in Examples 1-8.

[0028] Figure 2 Element distribution diagram of Pd@ZIF-67gel in Examples 1-8.

[0029] Figure 3 This is a high-resolution transmission electron microscopy image of Pd@ZIF-67gel in Examples 1-8.

[0030] Figure 4 This is the XRD pattern of Pd@ZIF-67gel in Examples 1-8.

[0031] Figure 5 This is the nitrogen adsorption diagram of Pd@ZIF-67gel in Examples 1-8.

[0032] Figure 6 This is the mesopore distribution diagram of Pd@ZIF-67gel in Examples 1-8.

[0033] Figure 7 This is the micropore distribution diagram of Pd@ZIF-67gel in Examples 1-8.

[0034] Figure 8 Hydrogen and methane adsorption diagrams of Pd@ZIF-67gel in Examples 1-8.

[0035] Fig. 9 The cross-sectional electron micrographs and Pd element distribution diagrams of the films prepared in Examples 1-4 are shown.

[0036] Fig.10 Fourier infrared images of the films prepared in Examples 1-4 and Comparative Example 1.

[0037] Fig.11 Fourier infrared images of the films prepared in Examples 5-8 and Comparative Example 2.

[0038] Fig.12 The gas separation performance of the membranes prepared in Comparative Examples 1, 3-6.

[0039] Fig.13 The gas separation performance of the membranes prepared in Examples 1-4.

[0040] Fig.14 Gas separation properties of the membranes prepared in Examples 5-8 and Comparative Examples 2, 7-9 DETAILED DESCRIPTION

[0041] The technical solution of the present invention is further described below through several specific embodiments, but the present application is not limited thereto. Without departing from the content and scope of the present invention, any changes and implementations should be included in the technical scope of the present invention.

[0042] Example 1:

[0043] Step (1): Weigh 0.224 g of palladium acetate (Pd(OAc)2) and 0.555 g of 30K polyvinyl pyrrolidone (PVP), dissolve them in 25 mL of ethanol. Heat and stir in a 70°C water bath for 2 hours to obtain a uniform black PVP Pd mixed solution;

[0044] Step (2): Prepare a 0.53 mol / L metal ion solution using methanol as solvent. 2+ : The ratio of imidazole to triethylamine is 1:8:8 to prepare an organic ligand solution;

[0045] Step (3): Mix and stir the above organic ligand solution, immediately add 25 mL of PVP Pd mixed solution, stir vigorously for 2 minutes, and then let stand for 24 hours. Wash the unreacted ligand three times with methanol to obtain Pd@MOF gel;

[0046] Step (4): dissolving 0.2 g of a self-microporous polymer (PIM-1) in chloroform to obtain a PIM-1 solution;

[0047] Step (5): Use chloroform to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in chloroform. Add the polymer solution dropwise to 0.02g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate at room temperature for 2 days, and finally place the film in a vacuum oven at 80°C for 24h to obtain 9.0wt% Pd@ZIF-67gel / PIM-1MMM.

[0048] Example 2:

[0049] Steps (1) to (4) are the same as in Example 1;

[0050] Step (5): Use chloroform to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in chloroform. Add the polymer solution dropwise to 0.04g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate at room temperature for 2 days, and finally place the film in a vacuum oven at 80°C for 24h to obtain 17.0wt% Pd@ZIF-67gel / PIM-1MMM.

[0051] Example 3:

[0052] Steps (1) to (4) are the same as in Example 1;

[0053] Step (5): Use chloroform to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in chloroform. Add the polymer solution dropwise to 0.06g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it at room temperature for 2 days, and finally place the film in a vacuum oven at 80°C to dry for 24h to obtain 23.0wt% Pd@ZIF-67gel / PIM-1MMM.

[0054] Example 4:

[0055] Steps (1) to (4) are the same as in Example 1;

[0056] Step (5): Use chloroform to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in chloroform. Add the polymer solution dropwise to 0.08g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it at room temperature for 2 days, and finally place the film in a vacuum oven at 80°C to dry for 24h to obtain 28.0wt% Pd@ZIF-67gel / PIM-1MMM.

[0057] Example 5:

[0058] Steps (1) to (3) are the same as in Example 1;

[0059] Step (4): dissolving 0.15 g of polyimide (P84) in N,N-dimethylformamide to obtain a P84 solution;

[0060] Step (5): Use N,N-dimethylformamide to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in N,N-dimethylformamide. Add the polymer solution dropwise to 0.02g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it under vacuum at 60℃ for 24h, and finally place the film in a vacuum oven at 150℃ for 18h to obtain 9wt% Pd@ZIF-67gel / P84 MMM.

[0061] Example 6:

[0062] Steps (1) to (4) are the same as in Example 5;

[0063] Step (5): Use N,N-dimethylformamide to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in N,N-dimethylformamide. Add the polymer solution dropwise to 0.04g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it under vacuum at 60℃ for 24h, and finally place the film in a vacuum oven at 150℃ for 18h to obtain 17wt% Pd@ZIF-67gel / P84 MMM.

[0064] Example 7:

[0065] Steps (1) to (4) are the same as in Example 5;

[0066] Step (5): Use N,N-dimethylformamide to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in N,N-dimethylformamide. Add the polymer solution dropwise to 0.06g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it under vacuum at 60℃ for 24h, and finally place the film in a vacuum oven at 150℃ for 18h to obtain 23wt% Pd@ZIF-67gel / P84 MMM.

[0067] Example 8:

[0068] Steps (1) to (4) are the same as in Example 5;

[0069] Step (5): Use N,N-dimethylformamide to replace Pd@ZIF-67gel three times to make Pd@ZIF-67gel evenly distributed in N,N-dimethylformamide. Add the polymer solution dropwise to 0.08g Pd@ZIF-67gel, sonicate and stir until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it under vacuum at 60℃ for 24h, and finally place the film in a vacuum oven at 150℃ for 18h to obtain 28wt% Pd@ZIF-67gel / P84 MMM.

[0070] Comparative Example 1:

[0071] Dissolve 0.2 g of PIM-1 in chloroform, stir at room temperature for 24 hours to form a casting solution, pour it into a smooth and flat round glass Petri dish, slowly evaporate at room temperature for 2 days, then soak the membrane in methanol for 1 day, and finally place the membrane in a vacuum oven at 80°C and dry it for 24 hours to obtain pure PIM-1MMM.

[0072] Comparative Example 2:

[0073] Dissolve 0.15 g of P84 in N,N-dimethylformamide, stir at room temperature for 24 hours to form a casting solution, pour it into a smooth and flat round glass Petri dish, slowly evaporate it under vacuum at 60°C for 24 hours, and finally place the film in a vacuum oven at 150°C to dry for 18 hours to obtain pure P84MMM.

[0074] Comparative Example 3:

[0075] Step (1) is the same as in Example 1;

[0076] Step (2): drying the Pd NP suspension in step (1) at 80° C. and redispersing it in chloroform;

[0077] Step (3): dissolving 0.2 g of PIM-1 in chloroform to obtain a PIM-1 solution;

[0078] Step (4): PIM-1 solution was added dropwise to a chloroform solution containing 0.002 g Pd NP, and the mixture was ultrasonically stirred for 24 h until the two were evenly mixed to form a casting mixed solution, which was then poured into a smooth and flat round glass culture dish and slowly evaporated at room temperature for 2 days. The membrane was then soaked in methanol for 1 day, and finally dried in a vacuum oven at 80 ° C for 24 h to obtain 1 wt% PdNP / PIM-1MMM.

[0079] Comparative Example 4:

[0080] Steps (1) to (3) are the same as those in Comparative Example 3;

[0081] Step (4): Add the PIM-1 solution dropwise to the chloroform solution containing 0.004 g of Pd NP, ultrasonicate and stir for 24 hours until the two are evenly mixed to form a casting mixed solution, pour it into a smooth and flat round glass culture dish, slowly evaporate it at room temperature for 2 days, then soak the membrane in methanol for 1 day, and finally place the membrane in a vacuum oven at 80°C and dry it for 24 hours to obtain 2wt% PdNP / PIM-1MMM.

[0082] Comparative Example 5:

[0083] Steps (1) to (3) are the same as those in Comparative Example 3; Step (4): PIM-1 solution was added dropwise to a chloroform solution containing 0.008 g Pd NP, and the mixture was ultrasonically stirred for 24 h until the two were evenly mixed to form a casting mixed solution. The solution was poured into a smooth and flat round glass culture dish, and slowly evaporated at room temperature for 2 days. The membrane was then soaked in methanol for 1 day. Finally, the membrane was dried in a vacuum oven at 80 ° C for 24 h to obtain 4 wt% PdNP / PIM-1MMM.

[0084] Comparative Example 6:

[0085] Steps (1) to (3) are the same as those in Comparative Example 3;

[0086] Step (4): PIM-1 solution was added dropwise to a chloroform solution containing 0.02 g Pd NP, and the two were ultrasonically stirred for 24 h until they were evenly mixed to form a casting mixed solution, which was then poured into a smooth and flat round glass culture dish and slowly evaporated at room temperature for 2 days. The membrane was then soaked in methanol for 1 day, and finally the membrane was placed in a vacuum oven at 80°C and dried for 24 h to obtain 9 wt% Pd NP / PIM-1MMM.

[0087] Comparative Example 7:

[0088] Steps (1)-(2) are the same as those in Comparative Example 3;

[0089] Step (3): dissolving 0.2 g of P84 in N,N-dimethylformamide to obtain a P84 solution;

[0090] Step (4): P84 solution was added dropwise to N,N-dimethylformamide solution containing 0.02 g Pd NP, and the mixture was ultrasonically stirred for 24 h until the two were evenly mixed to form a casting mixed solution. The solution was poured into a smooth and flat round glass culture dish, and slowly evaporated under vacuum at 60°C for 24 h. Finally, the film was placed in a vacuum oven at 150°C and dried for 18 h to obtain 9 wt% Pd NP / P84 MMM.

[0091] Comparative Example 8:

[0092] Steps (1) to (3) are the same as those in Comparative Example 7; Step (4): P84 solution was added dropwise to N,N-dimethylformamide solution containing 0.04 g Pd NP, and the mixture was ultrasonically stirred for 24 h until the two were evenly mixed to form a casting mixed solution, which was then poured into a smooth and flat round glass culture dish and slowly evaporated under vacuum at 60 ° C for 24 h. Finally, the film was placed in a vacuum oven at 150 ° C for 18 h to obtain 17 wt% Pd NP / P84 MMM.

[0093] Comparative Example 9:

[0094] Steps (1) to (3) are the same as those in Comparative Example 7;

[0095] Step (4): P84 solution was added dropwise to N,N-dimethylformamide solution containing 0.04 g Pd NP, and the mixture was ultrasonically stirred for 24 h until the two were evenly mixed to form a casting mixed solution, which was then poured into a smooth and flat round glass culture dish and slowly evaporated under vacuum at 60 ° C for 24 h. Finally, the film was placed in a vacuum oven at 150 ° C for 18 h to obtain 23 wt% Pd NP / P84 MMM.

[0096] The H2 permeability and selectivity of the MMMs in Examples 1-8 and Comparative Examples 1-9 at 0.1 MPa and 35°C when the gas mixture is H2 / CH4 are shown in Table 1. Table 1

[0097] It can be seen from Table 1 that in the PIM-1 matrix membrane, as the Pd@ZIF-67gel loading increased from 9wt% to 28wt%, the hydrogen permeability of Pd@ZIF-67gel / PIM-1MMM increased from 1498Barrer to 3620Barrer, and the H2 / CH4 selectivity increased significantly from 6.6 to 24.8. In contrast, as the Pd NP filler loading increased from 1wt% to 9wt%, the hydrogen permeability of Pd NP / PIM-1MMM decreased from 4673Barrer to 2180Barrer, and the H2 / CH4 selectivity increased from 6.3 to 10.9. It can be seen that the hydrogen permeability of 28wt% Pd@ZIF-67gel / PIM-1MMM is 14% higher than that of pure PIM-1 membrane, while the hydrogen permeability of 9wt% Pd NP / PIM-1MMM is 31% lower than that of pure PIM-1. In addition, the H2 / CH4 selectivity of 28wt% Pd@ZIF-67gel / PIM-1MMM was improved by 417% compared with that of pure PIM-1 membrane, while the H2 / CH4 selectivity of 9wt% Pd NP / PIM-1MMM was improved by 127% compared with that of pure PIM-1 membrane.

[0098] In the P84 matrix membrane, as the Pd@ZIF-67gel loading increased from 9wt% to 28wt%, the hydrogen permeability of Pd@ZIF-67gel / P84 MMM increased from 7.3Barrer to 8.7Barrer, and the H2 / CH4 selectivity increased significantly from 216.2 to 500.3. In contrast, as the Pd NP filler loading increased from 1wt% to 9wt%, the hydrogen permeability of Pd NP / P84 MMM decreased from 5.21Barrer to 3.3Barrer, and the H2 / CH4 selectivity increased from 253.6 to 256.8. It can be seen that the hydrogen permeability of 28wt% Pd@ZIF-67gel / P84 MMM is 14% higher than that of pure P84 membrane, while the hydrogen permeability of 9wt% Pd NP / P84 MMM is 56% lower than that of pure P84. In addition, the H2 / CH4 selectivity of 28wt%Pd@ZIF-67gel / P84MMM was improved by 147% compared with that of pure P84 membrane, while the H2 / CH4 selectivity of 9wt%Pd NP / P84 MMM was improved by 27% compared with that of pure P84 membrane.

[0099] In summary, the introduction of Pd@ZIF-67gel as a filler significantly improved the hydrogen permeability and selectivity of the PIM-1 and P84 matrix membranes. This significant performance improvement is attributed to the unique structure and properties of the Pd@ZIF-67 composite material. Compared with PdNP, Pd@ZIF-67gel not only has a specific adsorption for hydrogen, but also provides a high-speed hydrogen mass transfer channel through its three-dimensional interconnected gel network structure. At the same time, the combination of Pd and ZIF-67gel effectively reduces the pore size of ZIF-67gel, which can more effectively screen hydrogen molecules and inhibit the passage of methane. In addition, this gel structure effectively reduces the agglomeration of Pd NPs in the polymer, thereby maintaining good dispersibility and mass transfer performance, and greatly improving the membrane's permeability selectivity for hydrogen. This optimization strategy provides new ideas and methods for the development of high-performance hydrogen separation membranes, and has important academic research and industrial application value.

[0100] The above are only several embodiments of the present invention and are not intended to limit the present invention in any form. Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, using the above disclosed technical content to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A Pd@MOF gel mixed matrix membrane (Pd@MOF gel MMMs) for improving hydrogen transmission and separation efficiency and a preparation method and application thereof, characterized in that: The Pd@MOF gel MMMs comprises a polymer matrix and a Pd@MOF gel; The Pd@MOF gel is composed of MOF gel and Pd nanoparticles embedded on the surface and evenly distributed; The MOF gel is selected from zinc MOF gel and cobalt MOF gel.

2. The Pd@MOF gel MMMs according to claim 1, characterized in that: The zinc MOF gel is selected from ZIF-8gel; Preferably, the cobalt-based MOF gel is ZIF-67gel.

3. The Pd@MOF gel MMMs according to claim 1, characterized in that: The content of the Pd@MOF gel is 1wt% to 40wt% of the mass of the Pd@MOF gel MMMs.

4. The Pd@MOF gel MMMs according to claim 1, characterized in that: The polymer matrix is ​​selected from at least one of polyimide, polybenzimidazole and self-polymerized microporous polymer.

5. A method for preparing the Pd@MOF gel MMMs according to any one of claims 1 to 4, characterized in that: The Pd@MOF gel MMMs are obtained by forming a mixed film solution containing a polymer and MOF gel into a film and subjecting the film to vacuum treatment.

6. The preparation method according to claim 5, characterized in that: After mixing the solution a containing the polymer with the solution b containing Pd@MOFgel, the casting film mixed solution is obtained; The stirring time is 12 to 24 hours.

7. The preparation method according to claim 5, characterized in that: In the film casting mixed solution, the total mass concentration of the polymer and the Pd@MOF gel is 1.5-3wt%; Preferably, the solvent of the film casting mixed solution is selected from at least one of chloroform and N,N-dimethylformamide.

8. The preparation method according to claim 5, characterized in that: The treatment temperature of the vacuum treatment is 80-150° C., and the treatment time is 24-48 hours.

9. Use of the Pd@MOF gel MMMs according to any one of claims 1 to 4 or the Pd@MOF gel MMMs prepared by the preparation method according to any one of claims 5 to 8 in gas separation.

10. The use according to claim 9, characterized in that: Application of the Pd@MOF gel MMMs in separation of gas mixtures containing H2; Preferably, the gas comprises at least one of N2, CH4 and CO2.

Citation Information

Patent Citations

  • Metal organic framework gel mixed matrix membrane as well as preparation method and application thereof

    CN117443208A

Cited By

  • Method for separating CH4 / N2 through high-vacuum calcination of multi-MOF mixed matrix membrane

    CN119633624A

  • Preparation method of natural gas efficient hydrogen / helium extraction fluorinated MOFs mixed matrix membrane

    CN120094410B

  • Preparation method of hydrogen and nitrogen separation membrane material based on size screening and affinity recognition

    CN122399585A