Au-M bimetallic catalyst for preparing r-butyrolactone by oxidizing 1, 4-butanediol
By loading Au nanoparticles on the carrier and depositing metal M using atomic layer deposition technology, an Au-M bimetallic catalyst was prepared, which solved the problems of low activity and poor stability of the Au catalytic system and achieved low oxygen partial pressure and temperature. The efficient BDO oxidation significantly improves the selectivity and conversion rate of γ-butyrolactone.
Patent Information
- Application Number
- CN202410783449.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-22
AI Technical Summary
The existing Au catalytic system has problems of low activity and poor stability when oxidizing BDO to prepare γ-butyrolactone, and requires higher pressure and long reaction time, and it is difficult to recover and separate the homogeneous catalyst.
Au nanoparticles are loaded on the carrier, and metal M is deposited with different cycle numbers through atomic layer deposition technology to prepare an Au-M bimetallic catalyst and regulate the interaction between Au and metal M to improve catalytic activity and selectivity.
It efficiently catalyzes BDO oxidation at lower oxygen partial pressure and temperature, significantly improves the selectivity and conversion rate of γ-butyrolactone, and improves the stability of the catalyst.
Smart Images

Figure HDA0004897895280000011 
Figure HDA0004897895280000012 
Figure HDA0004897895280000013
Abstract
Description
Technical Field
[0001] The invention relates to a catalyst, in particular to a bimetallic catalyst, specifically an Au-M bimetallic catalyst for efficiently catalyzing the oxidation of 1,4-butanediol to prepare r-butyrolactone and a preparation method thereof. Background Art
[0002] γ-Butyrolactone (GBL) is an important organic synthesis intermediate and is widely used in fine chemicals such as medicine and fragrances, as well as polymer synthesis. The preparation of GBL by dehydrogenation of 1,4-butanediol (BDO) is an important way to obtain GBL industrially. Traditional catalytic oxidation requires the participation of stoichiometric oxidants, such as potassium permanganate and potassium dichromate, which produce a large amount of toxic byproducts. Using oxygen as an oxidant to achieve aerobic oxidation of BDO is a green, environmentally friendly and sustainable approach.
[0003] Homogeneous catalysts, such as Ir, Ru, and Cu complexes, are widely used in the aerobic oxidation of BDO. However, these homogeneous catalytic processes often require the addition of some expensive or toxic organic additives, and homogeneous catalysts are also difficult to recover and separate. Therefore, the use of heterogeneous catalysts such as supported Cu and Au for the oxidation reaction of BDO is more in line with practical industrial applications. Compared with the Cu-catalyzed gas-phase oxidation system, the Au-catalyzed liquid-phase oxidation system often requires a lower reaction temperature to achieve the aerobic oxidation of BDO, and has attracted widespread attention from researchers. At present, for the Au catalytic system, researchers mainly study the effect of the interaction between different carriers and Au on the catalytic oxidation performance of BDO by changing the carrier (TiO2, Al2O3, CeO2, hydrotalcite, hydroxyapatite, etc.). This single Au catalytic system often needs to react in oxygen at a higher pressure (>1MPa), has a long reaction time, and generally has the problems of low activity and poor stability. Therefore, it is very necessary to develop an Au catalyst with high catalytic activity and stability for the oxidation of BDO to prepare GBL. Summary of the invention
[0004] The purpose of the present invention is to provide an Au-M bimetallic catalyst, which can efficiently catalyze the conversion of BDO to generate GBL.
[0005] The present invention loads a certain amount of Au nanoparticles on a carrier, and uses atomic layer deposition (ALD) technology to deposit different cycles of metal M on the Au surface to prepare an Au-M bimetallic catalyst. Under a hydrogen atmosphere, high-temperature treatment of the Au-M bimetallic catalyst can regulate the interaction between Au and metal M, thereby regulating the activity and selectivity of the catalyst in the BDO oxidation reaction.
[0006] The present invention provides a method for preparing an Au-M bimetallic catalyst capable of efficiently catalyzing the oxidation of 1,4-butanediol to prepare r-butyrolactone, comprising the following steps:
[0007] (1) Loading of Au nanoparticles on the material surface
[0008] Preparation of Au / carrier samples by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 1-10mmol / L HAuCl4 aqueous solution, and take 10-200mL into a beaker; then prepare a 1-20g / L PVA aqueous solution, according to m Au :m PVA The ratio is 1:1-10, and the PVA solution is added to the HAuCl4 solution at a stirring speed of 200-1000rpm; then 5-20mmol / L NaBH4 solution is prepared according to n Au :n NaBH4 The ratio of NaBH4 to HAuCl4 and PVA is 1:1-10, and the stirring speed is 200-1000rpm. After stirring for 1-12h, 0.5-5.0g of carrier is added, and concentrated H2SO4 is slowly added dropwise to the system under vigorous stirring. The pH value of the mixed solution is adjusted to 1-5, and stirring is continued for 1-6h. After the reaction is completed, ultrapure water is used for centrifugal washing until neutral, and then placed in a 60-200°C forced air oven for 12-24h to obtain an Au / carrier sample.
[0009] The Au / carrier sample was prepared by the impregnation method: a certain amount of HAuCl4·3H2O was weighed and dissolved in ultrapure water to prepare a 1-10 mmol / L HAuCl4 aqueous solution, and 10-200 mL was measured and placed in a beaker; then 0.5-5.0 g of the carrier was added to the beaker, and stirred at 30-100°C for 12h-24h, the resulting paste sample was placed in an oven at 50-200°C for drying, and then the paste sample was calcined in a muffle furnace at 200-500°C for 1-3h to obtain the Au / carrier sample.
[0010] Au / carrier samples were prepared by sedimentation precipitation method (with NaOH as precipitant): first, 1.0 g of carrier was weighed into 10 mL-200 mL of water, stirred for 1 h-5 h to make the carrier evenly dispersed, then 10-200 mL of 1-10 mmol / L HAuCl4 solution was measured, dripped into the dispersed carrier drop by drop, and vigorously stirred for 12-24 h; then 0.1-2 mol / L NaOH solution was prepared, added to the aqueous solution of HAuCl4 and carrier, the pH was controlled at 9-13, the stirring speed was 200-1000 rpm, and stirred for 12-24 h. After the reaction was completed, it was allowed to stand for 0.5-5 h, filtered, and washed with deionized water until Cl in the system was -All of them are removed (check with 0.01-0.1 mol / L AgNO3 solution until no white precipitate is generated, which means it is clean); finally, the sample is dried at 50-200°C for 12-24h to obtain an Au / carrier sample.
[0011] The Au / carrier samples were prepared by sedimentation precipitation method (with urea as precipitant): first, 1.0 g of carrier was weighed into 10 mL-200 mL of water, stirred for 1 h-5 h to make the carrier evenly dispersed, then 10-200 mL of 1-10 mmol / L HAuCl4 solution was measured and dripped into the dispersed carrier drop by drop, and stirred vigorously for 12-24 h; then, the ... precipitation precipitation method (with urea as precipitant): first, 1.0 g of carrier was weighed into 10 mL-200 mL of water, stirred for 1 h-5 h to make the carrier evenly dispersed, then 10-200 mL of 1-10 mmol / L HAuCl4 solution was dripped into the dispersed carrier drop by drop, and stirred vigorously for 12-24 h; then, the Au / carrier samples were prepared by precipitation precipitation method: first, 1.0 g of carrier was weighed into 10 mL-200 mL of water, stirred for 1 h-5 h to make the carrier evenly dispersed, then 10-200 mL of 1-10 mmol / L HAuCl4 solution was dripped into the dispersed carrier drop by drop, and stirred vigorously for 12-24 h; then, the Au / carrier samples were prepared by precipitation precipitation method: first, 1.0 g of carrier was weighed into 10 mL-200 mL of water, stirred for 1 h-5 h to make the carrier even Au :n 尿素 Weigh a certain amount of urea at a ratio of 1:50-200, add it to the aqueous solution of HAuCl4 and carrier, and stir at 50-120℃ for 1-6h. After the reaction is completed, let it stand for 0.5-5h, filter, and wash with deionized water until the Cl in the system is - All of them are removed (check with 0.01-0.1 mol / L AgNO3 solution until no white precipitate is generated, which means it is clean); finally, the sample is dried at 50-200°C for 12-24h to obtain an Au / carrier sample.
[0012] (2) Preparation of Au-M bimetallic catalyst
[0013] Weigh 5-50 mg of Au / carrier sample and place it on a quartz plate, add 1-10 mL of diluent to evenly disperse the sample on the quartz plate, control the thickness to be 0.01-2 mm, wait for the diluent to evaporate to dryness, place the quartz plate in an atomic layer deposition (ALD) device, and set the atomic layer deposition parameters as follows: nitrogen flow rate of 50 sccm, deposition temperature of 120-350 ° C, metal M precursor temperature of 25-100 ° C, formalin temperature of 20-300 ° C, and the thickness of the sample to be uniformly dispersed on the quartz plate. The temperature is 25-60°C, and the precursor of metal M is first introduced into the deposition chamber by steam pulse, with a pulse time of 0.01-2s, a breath holding time of 0.1-20s, and a pumping time of 20-300s; then formalin pulse is introduced into the deposition chamber, with a pulse time of 0.01-2s, a breath holding time of 0.1-20s, and a pumping time of 20-300s to complete a deposition cycle of metal M; repeat 2-50 cycles to obtain an Au-M bimetallic catalyst.
[0014] Alternatively, the atomic layer deposition parameters are set as follows: a nitrogen flow rate of 50 sccm, an ozone flow rate of 50 sccm, a deposition temperature of 120-350°C, a temperature of the metal M precursor of 25-100°C, and the metal M precursor is introduced into the deposition chamber in the form of a steam pulse, with a pulse time of 0.01-2s, a breath-holding time of 0.1-20s, and a pumping time of 20-300s; then an ozone pulse is introduced into the deposition chamber, with a pulse time of 0.1-0.5s, a breath-holding time of 2-10s, and a pumping time of 60-120s, thereby completing a deposition cycle of the metal M; repeat 2-50 cycles to obtain an Au-M bimetallic catalyst.
[0015] The carrier in step (1) includes one of oxides such as titanium oxide (TiO2), cerium oxide nanorods (CeO2), hydroxyapatite (HAP), and hydrotalcite (HT).
[0016] The diluent in step (2) includes water, methanol or ethanol.
[0017] The precursor of the metal M in the step (2) is hexafluoroacetylacetonate palladium, biscyclopentadienyl cobalt, bis(hexafluoroacetylacetonate)copper(II), trimethylmethylcyclopentadienyl platinum, bis(ethylcyclopentadienyl)ruthenium(II), hexacarbonyl molybdenum, bis(cyclopentadienyl)nickel, bis(cyclopentadienyl)iron, etc.
[0018] Compared with the prior art, the present invention has the following beneficial effects: the present invention loads a certain amount of Au nanoparticles on a carrier, and uses atomic layer deposition (ALD) to deposit metal M with different cycles on the Au surface to prepare an Au-M bimetallic catalyst, which can catalyze the aerobic oxidation of BDO at a relatively low oxygen partial pressure and temperature to synthesize GBL with high selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is the transmission electron microscope image of 30Cu-Au / TiO2
[0020] Figure 2 This is the transmission electron microscope image of 10Pd-Au / CeO2
[0021] Figure 3 This is the transmission electron microscope image of 10Pd-Au / CeO2
[0022] Figure 4 This is the transmission electron microscope image of 10Co-Au / TiO2
[0023] Figure 5 This is the transmission electron microscope image of 30Pd-Au / TiO2
[0024] Figure 6 This is the transmission electron microscope image of 10Pt-Au / TiO2
[0025] Figure 7 This is the transmission electron microscope image of 20Ru-Au / TiO2
[0026] Figure 8 This is the transmission electron microscope image of 50Ni-Au / TiO2
[0027] Fig. 9 This is the transmission electron microscope image of 50Mo-Au / TiO2
[0028] Fig.10 This is the transmission electron microscope image of 30Cu-Au / TiO2
[0029] Fig.11 This is the transmission electron microscopy image of 30Pd-Au / HAP
[0030] Fig.12 This is the transmission electron microscopy image of 30Mo-Au / HAP
[0031] Fig.13 This is the transmission electron microscope image of 20Fe-Au / TiO2
[0032] Fig.14 This is the transmission electron microscopy image of 40Ru-Au / HT
[0033] Fig.15 This is the transmission electron microscope image of 20Co-Au / CeO2
[0034] Fig.16 This is the transmission electron microscopy image of 10Pt-Au / HAP DETAILED DESCRIPTION
[0035] Example 1
[0036] Preparation of Au / TiO2 by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 1mmol / L HAuCl4 aqueous solution, and take 200mL into a beaker; then prepare a 10g / L PVA aqueous solution and add it according to m Au :m PVA PVA was added to the HAuCl4 solution at a ratio of 1:1, and the stirring speed was 600 rpm for 2 h; then 5 mmol / L NaBH4 solution was prepared according to n Au :n NaBH4In a ratio of 1:2, NaBH4 was added to the mixed solution of HAuCl4 and PVA at a stirring speed of 600 rpm. After stirring for 2 hours, 1.0 g of TiO2 carrier was added, and concentrated H2SO4 solution was slowly added dropwise under vigorous stirring. The pH value of the above mixed solution was adjusted to 1, and stirring was continued for 3 hours. After the reaction was completed, ultrapure water was used for centrifugal washing until neutral, and then it was placed in a 60°C forced air oven for 12 hours to obtain Au / TiO2.
[0037] Weigh 20 mg of Au / TiO2 and place it on a quartz plate. Add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.05 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in the atomic layer deposition (ALD) equipment. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 250°C, and the precursor bis(hexafluoroacetylacetonate)copper(II) temperature is 80°C. First, introduce bis(hexafluoroacetylacetonate)copper(II) vapor into the deposition chamber with a pulse time of 0.4s, a breath holding time of 2s, and a vacuum time of 20s; then introduce an ozone pulse into the deposition chamber with a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 60s. This completes a Cu deposition cycle. Repeat 30 cycles to obtain a 30Cu-Au / TiO2 bimetallic catalyst. The morphology of the sample is as shown in the figure. Figure 1 shown.
[0038] 30Cu-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 20 mg, toluene was 20 mL, 1,4-butanediol was 200 mg, oxygen was 0.3 MPa, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 90%, and the selectivity of γ-butyrolactone was 93%.
[0039] Example 2
[0040] Au / CeO2 was prepared by sedimentation precipitation method (with NaOH as precipitant): First, weigh 1.0g of CeO2 powder in 60mL of water and stir for 2h to disperse the carrier evenly. Then, measure 10mL of 10mmol / L HAuCl4 solution and drip it into the dispersed carrier drop by drop, stirring vigorously for 12h. Then, prepare 0.1mol / L NaOH solution and add it to the aqueous solution of HAuCl4 and CeO2 carrier, control the pH to 9, stir at 800rpm, stir for 14h, let stand for 3h after the reaction, filter, and wash with deionized water until Cl in the system is completely removed. - All of them were removed (checked with 0.1 mol / L AgNO3 solution until no white precipitate was generated, which means it was clean). Finally, the sample was dried at 80°C for 12h to obtain Au / CeO2.
[0041] Weigh 20 mg of Au / CeO2 and place it on a quartz wafer. Add 1 mL of anhydrous methanol to evenly disperse the sample on the quartz wafer, control the thickness to 0.15 mm, and after the anhydrous methanol evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, deposition temperature of 150 ° C, precursor hexafluoroacetylacetonate palladium temperature of 60 ° C, first introduce hexafluoroacetylacetonate palladium vapor into the deposition chamber, the pulse time is 0.5 s, the breath holding time is 4 s, and the exhaust time is 30 s; then introduce formalin pulses into the deposition chamber, the pulse time is 0.7 s, the breath holding time is 2 s, and the exhaust time is 150 s. This completes a Pd deposition cycle. Repeat 10 cycles to obtain a 10Pd-Au / CeO2 bimetallic catalyst. The morphology of the sample is as shown in the figure. Figure 2 shown.
[0042] 10Pd-Au / CeO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 10Pd-Au / CeO2 20mg, toluene was 20mL, 1,4-butanediol was 200mg, 0.3MPa oxygen was used, the reaction time was 4h, the conversion rate of 1,4-butanediol was 93%, and the selectivity of γ-butyrolactone was 99%.
[0043] Example 3
[0044] Au / CeO2 was prepared by sedimentation precipitation method (with urea as precipitant): 1.0g of CeO2 powder was weighed into 10mL of water and stirred for 2h to make the carrier evenly dispersed. Then 10mL of 10mmol / L HAuCl4 solution was added dropwise into the dispersed carrier and stirred vigorously for 12h; then the mixture was stirred at 400℃ for 24h. Au :n 尿素 Weigh a certain amount of urea in a ratio of 1:50, add it to the aqueous solution of HAuCl4 and carrier CeO2, and stir it at 80℃ for 6h. After the reaction is completed, let it stand for 3h, filter it, and wash it with deionized water until the Cl in the system is - All of them were removed (checked with 0.01 mol / L AgNO3 solution until no white precipitate was generated, which means it was clean). Finally, the sample was dried at 80°C for 12h to obtain Au / CeO2.
[0045] Weigh 20 mg of Au / CeO2 and place it on a quartz wafer. Add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz wafer, control the thickness to 0.05 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, deposition temperature of 150°C, and precursor hexafluoroacetylacetonate palladium temperature of 60°C. First, introduce hexafluoroacetylacetonate palladium vapor into the deposition chamber with a pulse time of 0.5 s, a breath holding time of 4 s, and a vacuum time of 30 s; then introduce formalin pulses into the deposition chamber with a pulse time of 0.7 s, a breath holding time of 2 s, and a vacuum time of 150 s. This completes a Pd deposition cycle. Repeat 10 cycles to obtain a 10Pd-Au / CeO2 bimetallic catalyst. The morphology of the sample is as shown below. Figure 3 shown.
[0046] 10Pd-Au / CeO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 10Pd-Au / CeO2 10 mg, toluene was 20 mL, 1,4-butanediol was 200 mg, 0.3 MPa of oxygen was used, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 92%, and the selectivity of γ-butyrolactone was 97%.
[0047] Example 4
[0048] Au / TiO2 was prepared by the impregnation method: a certain amount of HAuCl4·3H2O was weighed and dissolved in ultrapure water to prepare a 6mmol / L HAuCl4 aqueous solution, and 50mL was measured and placed in a beaker; then 2.0g of carrier TiO2 was added to the beaker and stirred at 40°C for 12h, and then the obtained paste sample was placed in an oven at 80°C for drying, and then the sample was calcined in a muffle furnace at 350°C for 2h to obtain the sample Au / TiO2.
[0049] Weigh 20 mg of Au / TiO2 and place it on a quartz wafer. Add 1 mL of water to evenly disperse the sample on the quartz wafer, control the thickness to 0.05 mm, and after the water evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, ozone flow rate of 50 sccm, deposition temperature of 300°C, and precursor biscyclopentadienyl cobalt temperature of 80°C. First, introduce biscyclopentadienyl cobalt vapor into the deposition chamber with a pulse time of 0.3s, a breath holding time of 6s, and a vacuum time of 70s; then introduce an ozone pulse into the deposition chamber with a flow rate of 50 sccm, a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 120s. This completes a Co deposition cycle. Repeat 10 cycles to obtain a 10Co-Au / TiO2 bimetallic catalyst. The morphology of the sample is as shown in the figure. Figure 4 shown.
[0050] 10Co-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 10Co-Au / TiO2 20 mg, toluene was 20 mL, 1,4-butanediol was 200 mg, 0.3 MPa oxygen was used, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 99%, and the selectivity of γ-butyrolactone was 96%.
[0051] Example 5
[0052] Preparation of Au / TiO2 by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 2mmol / L HAuCl4 aqueous solution, and take 100mL into a beaker; then prepare a 5g / L PVA solution and add it according to m Au :m PVA The ratio of PVA solution to HAuCl4 solution was 1:1.2, and the stirring speed was 300 rpm; then 10 mmol / L NaBH4 solution was prepared according to n Au :n NaBH4 In a ratio of 1:2, NaBH4 was added to the mixed solution of HAuCl4 and PVA at a stirring speed of 700 rpm. After stirring for 10 hours, 2.0 g of carrier TiO2 was added, and concentrated H2SO4 solution was slowly added dropwise under vigorous stirring. The pH value of the mixed solution was adjusted to 2, and stirring was continued for 3 hours. After the reaction was completed, ultrapure water was used for centrifugal washing until neutral, and then it was placed in a 60°C forced air oven for 12 hours to obtain Au / TiO2.
[0053] Then, weigh 20 mg of Au / TiO2 and place it on a quartz wafer, add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz wafer, control the thickness to 0.05 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, deposition temperature of 150°C, and precursor hexafluoroacetylacetonate palladium temperature of 60°C. First, introduce hexafluoroacetylacetonate palladium vapor into the deposition chamber with a pulse time of 0.5 s, a breath holding time of 4 s, and a vacuum time of 30 s; then introduce formalin pulses into the deposition chamber with a pulse time of 0.7 s, a breath holding time of 2 s, and a vacuum time of 150 s. This completes a Pd deposition cycle. Repeat 30 cycles to obtain 30Pd-Au / TiO2 bimetallic catalysts. The morphology of the sample is as shown in the figure. Figure 5 shown.
[0054] 30Pd-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 100°C, the catalyst was 20 mg, the solvent was tributyl phosphate 20 mL, 1,4-butanediol 200 mg, 0.3 MPa oxygen, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 92%, and the selectivity of γ-butyrolactone was 97%.
[0055] Example 6
[0056] Au / TiO2 was prepared by sedimentation precipitation method (with urea as precipitant): 1.0 g of carrier TiO2 powder was weighed into 200 mL of water, stirred for 2 h to make the carrier evenly dispersed, then 10 mL of 10 mmol / L HAuCl4 solution was measured and dripped into the dispersed carrier drop by drop, and stirred vigorously for 12 h. Au :n 尿素 Weigh a certain amount of urea at a ratio of 1:100, add it to the aqueous solution of HAuCl4 and the carrier, and stir at 80℃ for 6h. After the reaction is completed, let it stand for 4h, filter it, and wash it with deionized water until the Cl in the system is - All of them were removed (checked with 0.01 mol / L AgNO3 solution until no white precipitate was generated, which means it was clean). Finally, the sample was dried at 80°C for 12h to obtain Au / TiO2.
[0057] Weigh 20 mg of Au / TiO2 and place it on a quartz plate, add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.05 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in the atomic layer deposition (ALD) equipment. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 350°C, and the precursor trimethylmethylcyclopentadienyl platinum temperature is 75°C. First, introduce trimethylmethylcyclopentadienyl platinum vapor into the deposition chamber with a pulse time of 0.8s, a breath holding time of 2s, and a vacuum time of 90s; then introduce ozone into the deposition chamber with a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 160s. This completes a Pt deposition cycle. Repeat 10 cycles to obtain a 10Pt-Au / TiO2 bimetallic catalyst. The morphology of the sample is as shown in the figure. Figure 6 shown.
[0058] 10Pt-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 100°C, the catalyst was 10Pt-Au / TiO2 20 mg, the solvent was tributyl phosphate 20 mL, 1,4-butanediol 200 mg, 0.3 MPa oxygen, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 99%, and the selectivity of γ-butyrolactone was 97%.
[0059] Example 7
[0060] Preparation of Au / TiO2 by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 5mmol / L HAuCl4 aqueous solution, and take 15mL into a beaker; then prepare a 2g / L PVA aqueous solution, according to m Au :m PVA PVA was added to the HAuCl4 solution at a ratio of 1:10, and the stirring speed was 1000 rpm; then 15 mmol / L NaBH4 solution was prepared according to n Au :n NaBH4 In a ratio of 1:6, NaBH4 was added to the mixed solution of HAuCl4 and PVA at a stirring speed of 800 rpm. After stirring for 12 hours, 1.0 g of carrier TiO2 was added, and concentrated H2SO4 solution was slowly added dropwise under vigorous stirring. The pH value of the above mixed solution was adjusted to 5, and stirring was continued for 3 hours. After the reaction was completed, ultrapure water was used for centrifugal washing until neutral, and then it was placed in a forced air oven at 80°C for 12 hours to obtain Au / TiO2.
[0061] Weigh 20 mg of Au / TiO2 and place it on a quartz plate. Add 1 mL of anhydrous methanol to evenly disperse the sample on the quartz plate, control the thickness to 0.05 mm, and after the anhydrous methanol evaporates to dryness, place the quartz plate in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 350°C, precursor bis(ethylcyclopentadienyl)ruthenium(II) temperature is 80°C, first introduce bis(ethylcyclopentadienyl)ruthenium(II) vapor into the deposition chamber, the pulse time is 0.3s, the breath holding time is 2s, and the exhaust time is 60s; then introduce ozone pulses into the deposition chamber, the pulse time is 0.3s, the breath holding time is 2s, and the exhaust time is 110s, thus completing a Ru deposition cycle. Repeat 20 cycles to obtain a 20Ru-Au / TiO2 bimetallic catalyst. The morphology of the sample is as shown in Figure 7 shown.
[0062] 20Ru-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 20 mg 20Ru-Au / TiO2, the solvent was 20 mL toluene, 200 mg 1,4-butanediol was added, 0.3 MPa oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 90%, and the selectivity of γ-butyrolactone was 94%.
[0063] Example 8
[0064] Au / TiO2 was prepared by the impregnation method: a certain amount of HAuCl4·3H2O was weighed and dissolved in ultrapure water to prepare a 3.5mmol / L HAuCl4 aqueous solution, and 200mL was measured and placed in a beaker; then 3.0g of carrier TiO2 was added to the beaker and stirred at 40°C for 12h, and then the obtained paste sample was placed in an oven at 80°C for drying, and then the paste sample was calcined in a muffle furnace at 450°C for 3h to obtain the sample Au / TiO2.
[0065] Weigh 20 mg of Au / TiO2 and place it on a quartz plate. Add 1 mL of water to evenly disperse the sample on the quartz plate, control the thickness to 0.05 mm, and after the water evaporates to dryness, place the quartz plate in the atomic layer deposition (ALD) equipment. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 200°C, precursor di(cyclopentadiene)nickel temperature is 85°C, di(cyclopentadiene)nickel vapor is first introduced into the deposition chamber with a pulse time of 0.2s, a breath holding time of 2s, and a vacuum time of 50s; then ozone is introduced into the deposition chamber with a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 120s. This completes a Ni deposition cycle. Repeat 50 cycles to obtain 50Ni-Au / TiO2 bimetallic catalysts. The morphology of the sample is as shown below. Figure 8 shown.
[0066] 50Ni-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 20mg 50Ni-Au / TiO2, the solvent was 20mL tributyl phosphate, and 1,4-butanediol was 200mg. 0.3MPa oxygen was introduced, the reaction time was 4h, the conversion rate of 1,4-butanediol was 92%, and the selectivity of γ-butyrolactone was 97%.
[0067] Example 9
[0068] Au / TiO2 was prepared by sedimentation precipitation method (with urea as precipitant): first, 1.0g of carrier TiO2 powder was weighed into 100mL of water and stirred for 2h to make the carrier evenly dispersed. Then, 100mL of 3.2mmol / L HAuCl4 solution was measured and dripped into the dispersed carrier drop by drop, and stirred vigorously for 12h; then, the mixture was stirred at 400℃ for 24h. Au :n 尿素 Weigh a certain amount of urea in a ratio of 1:200, add it to the aqueous solution of HAuCl4 and the carrier, and stir it at 80℃ for 6h. After the reaction is completed, let it stand for 3h, filter it, and wash it with deionized water until the Cl in the system is -All of them were removed (checked with 0.012 mol / L AgNO3 solution until no white precipitate was generated, which means it was clean). Finally, the sample was dried at 80°C for 12 hours to obtain a powder sample of Au / TiO2.
[0069] Weigh 20 mg of sample Au / TiO2 and place it on a quartz wafer. Add 1 mL of anhydrous methanol to evenly disperse the sample on the quartz wafer, control the thickness to 0.08 mm, and after the anhydrous methanol evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 150°C, precursor molybdenum hexacarbonyl temperature is 85°C, molybdenum hexacarbonyl vapor is first introduced into the deposition chamber with a pulse time of 0.4s, a breath holding time of 9s, and a vacuum time of 20s; then ozone is introduced into the deposition chamber with a pulse time of 0.5s, a breath holding time of 8s, and a vacuum time of 140s. This completes a Mo deposition cycle. Repeat 50 cycles to obtain a 50Mo-Au / TiO2 bimetallic catalyst. The morphology of the sample is as shown below. Fig. 9 shown.
[0070] 50Mo-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 100°C, the catalyst was 50Mo-Au / TiO2 20 mg, the solvent was tributyl phosphate 20 mL, 1,4-butanediol 200 mg, 0.3 MPa of oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 95%, and the selectivity of γ-butyrolactone was 91%.
[0071] Example 10
[0072] Preparation of Au / TiO2 by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 4.0mmol / L HAuCl4 aqueous solution, and take 50mL into a beaker; then prepare a 5g / L PVA aqueous solution and adjust the concentration according to m Au :m PVA The ratio was 1:9, and the PVA solution was added to the HAuCl4 solution with a stirring speed of 1000 rpm; then a 20 mmol / L NaBH4 solution was prepared according to n Au :n NaBH4 In a ratio of 1:10, NaBH4 was added to the mixed solution of HAuCl4 and PVA, and after stirring for 2 hours, 1.0g of carrier TiO2 was added, and concentrated H2SO4 solution was slowly added dropwise under vigorous stirring, and the pH of the mixed solution was adjusted to 2. Stirring was continued for 3 hours. After the reaction was completed, ultrapure water was used for centrifugal washing until neutral, and then placed in a 60°C forced air oven for 12 hours to obtain the Au / TiO2 sample.
[0073] Weigh 20 mg Au / TiO2 and place it on a quartz plate, add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.25 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in the atomic layer deposition (ALD) equipment. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 250 ° C, precursor bis(hexafluoroacetylacetonate)copper(II) temperature is 80 ° C, first introduce bis(hexafluoroacetylacetonate)copper(II) vapor into the deposition chamber, the pulse time is 0.4 s, the breath holding time is 2 s, and the exhaust time is 20 s; then introduce ozone pulses into the deposition chamber, the pulse time is 0.3 s, the breath holding time is 2 s, and the exhaust time is 60 s, thus completing a Cu deposition cycle. Repeat 30 cycles to obtain 30Cu-Au / TiO2 bimetallic catalysts. The morphology of the sample is as shown in Fig.10 shown.
[0074] 30Cu-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 30Cu-Au / TiO2 20 mg, the solvent was tributyl phosphate 20 mL, 1,4-butanediol 200 mg, 0.3 MPa of oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 95%, and the selectivity of γ-butyrolactone was 97%.
[0075] Embodiment 11
[0076] Au / HAP was prepared by sedimentation precipitation method (with urea as precipitant): first, 1.0 g of carrier HAP was weighed into 50 mL of water and stirred for 2 h to make the carrier evenly dispersed. Then, 10 mL of 4.7 mmol / L HAuCl4 solution was added dropwise to the dispersed carrier and stirred vigorously for 12 h. Au :n 尿素 A certain amount of urea was weighed in a ratio of 1:120, added to the aqueous solution of HAuCl4 and the carrier, and stirred at 80℃ for 6h. After the reaction was completed, it was allowed to stand for 3h, filtered, and washed with deionized water until the Cl in the system was - All of them were removed (checked using 0.01 mol / L AgNO3 solution until no white precipitate was generated, which means it was washed clean); finally, the sample was dried at 80°C for 12h to obtain Au / HAP.
[0077] Weigh 20 mg of sample Au / HAP and place it on a quartz wafer. Add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz wafer, control the thickness to 0.75 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, deposition temperature of 150°C, and precursor hexafluoroacetylacetonate palladium temperature of 60°C. First, introduce hexafluoroacetylacetonate palladium vapor into the deposition chamber with a pulse time of 0.5s, a breath holding time of 4s, and a vacuum time of 30s; then introduce formalin pulses into the deposition chamber with a pulse time of 0.7s, a breath holding time of 2s, and a vacuum time of 150s. This completes a Pd deposition cycle. Repeat 30 cycles to obtain a 30Pd-Au / HAP bimetallic catalyst. The morphology of the sample is as shown in the figure. Fig.11 shown.
[0078] 30Pd-Au / HAP was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 120°C, the catalyst was 30Pd-Au / HAP 20 mg, the solvent was tributyl phosphate 20 mL, 1,4-butanediol 200 mg was added, 0.3 MPa of oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 90%, and the selectivity of γ-butyrolactone was 97%.
[0079] Example 12
[0080] Au / HAP was prepared by sedimentation precipitation method (with urea as precipitant): first, 1.0 g HAP powder was weighed into 200 mL water and stirred for 2 h to make the carrier evenly dispersed. Then, 50 mL of 5.0 mmol / L HAuCl4 solution was measured and added dropwise to the dispersed carrier and stirred vigorously for 12 h. Au :n 尿素 Weigh a certain amount of urea at a ratio of 1:200, add it to the aqueous solution of HAuCl4 and the carrier, and stir it at 80℃ for 6h. After the reaction is completed, let it stand for 3h, filter it, and wash it with deionized water until the Cl in the system is - All of them were removed (checked with 0.05 mol / L AgNO3 solution until no white precipitate was generated, which means it was washed clean); finally, the sample was dried at 110°C for 16 hours to obtain Au / HAP.
[0081] Weigh 20 mg of sample Au / HAP and place it on a quartz plate, add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.75 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in the atomic layer deposition (ALD) equipment. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 150°C, precursor molybdenum hexacarbonyl temperature is 85°C, molybdenum hexacarbonyl vapor is first introduced into the deposition chamber with a pulse time of 0.4s, a breath holding time of 9s, and a pumping time of 20s; then ozone is introduced into the deposition chamber with a pulse time of 0.5s, a breath holding time of 8s, and a pumping time of 140s, thus completing a Mo deposition cycle. Repeat 30 cycles to obtain a 30Mo-Au / HAP bimetallic catalyst. The morphology of the sample is as shown in Fig.12 shown.
[0082] 30Mo-Au / HAP was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 20 mg 30Mo-Au / HAP, the solvent was 20 mL tributyl phosphate, and the 1,4-butanediol was 200 mg. 0.3 MPa of oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 91%, and the selectivity of γ-butyrolactone was 99%.
[0083] Example 13
[0084] Preparation of Au / TiO2 by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 5.2mmol / L HAuCl4 aqueous solution, and take 100mL into a beaker; then prepare a 10g / L PVA aqueous solution, and Au :m PVA The ratio of 1:2 was set, and the PVA solution was added to the HAuCl4 solution with a stirring speed of 1000 rpm. Then a 20 mmol / L NaBH4 solution was prepared according to n Au :n NaBH4 In a ratio of 1:8, NaBH4 was added to the mixed solution of HAuCl4 and PVA at a stirring speed of 600 rpm. After stirring for 2 hours, 3.0 g of carrier TiO2 was added, and concentrated H2SO4 solution was slowly added dropwise under vigorous stirring. The pH value of the above mixed solution was adjusted to 2, and stirring was continued for 3 hours. After the reaction was completed, ultrapure water was used for centrifugal washing until neutral, and then it was placed in a 60°C forced air oven for 12 hours to obtain Au / TiO2.
[0085] Weigh 20 mg of Au / TiO2 and place it on a quartz plate. Add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.05 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in the atomic layer deposition (ALD) equipment. The set deposition parameters are: nitrogen flow rate is 50 sccm, ozone flow rate is 50 sccm, deposition temperature is 250°C, and the precursor di(cyclopentadienyl)iron deposition temperature is 80°C. First, introduce di(cyclopentadienyl)iron vapor into the deposition chamber with a pulse time of 2s, a breath holding time of 2s, and a vacuum time of 20s; then introduce an ozone pulse into the deposition chamber with a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 200s. This completes a Fe deposition cycle. Repeat 20 cycles to obtain a 20Fe-Au / TiO2 bimetallic catalyst. The morphology of the sample is as shown in the figure. Fig.13 shown.
[0086] 20Fe-Au / TiO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 120°C, 20 mg of catalyst 20Fe-Au / TiO2 was added, 20 mL of solvent tributyl phosphate, 200 mg of 1,4-butanediol, 0.3 MPa of oxygen was introduced, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 85%, and the selectivity of γ-butyrolactone was 99%.
[0087] Embodiment 14
[0088] Au / HT was prepared by sedimentation precipitation method (with urea as precipitant): 1.0 g of carrier HT powder was weighed into 80 mL of water and stirred for 2 h to make the carrier evenly dispersed. Then 50 mL of 5 mmol / L HAuCl4 solution was measured and dripped into the dispersed carrier drop by drop, and stirred vigorously for 12 h; then the precipitate was added according to n Au :n 尿素 Weigh a certain amount of urea at a ratio of 1:200, add it to the aqueous solution of HAuCl4 and the carrier, and stir it at 80℃ for 6h. After the reaction is completed, let it stand for 3h, filter it, and wash it with deionized water until the Cl in the system is - All of them were removed (checked with 0.05 mol / L AgNO3 solution until no white precipitate was generated, which means it was clean). Finally, the sample was dried at 90°C for 12 hours to obtain Au / HT.
[0089] Weigh 20 mg of sample Au / HT and place it on a quartz plate, add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.15 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, ozone flow rate of 50 sccm, deposition temperature of 350°C, precursor bis(ethylcyclopentadienyl)ruthenium(II) temperature of 80°C, first introduce bis(ethylcyclopentadienyl)ruthenium(II) vapor into the deposition chamber, the pulse time is 0.3 s, the breath holding time is 2 s, and the exhaust time is 60 s; then introduce ozone pulses into the deposition chamber, the pulse time is 0.3 s, the breath holding time is 2 s, and the exhaust time is 110 s, thus completing a Ru deposition cycle. Repeat 40 cycles to obtain 40Ru-Au / HT bimetallic catalysts. The morphology of the sample is as shown in Fig.14 shown.
[0090] 40Ru-Au / HT was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 80°C, the catalyst was 20 mg, the solvent was tributyl phosphate was 20 mL, 1,4-butanediol was added with 200 mg, 0.3 MPa of oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 89%, and the selectivity of γ-butyrolactone was 97%.
[0091] Embodiment 15
[0092] Preparation of Au / CeO2 by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 5mmol / L HAuCl4 aqueous solution, and take 100mL into a beaker; then prepare a 5g / L PVA aqueous solution and add 100mL of HAuCl4 to the beaker. Au :m PVA The ratio was 1:5, and the PVA solution was added to the HAuCl4 solution at a stirring speed of 800 rpm; then a 12 mmol / L NaBH4 solution was prepared according to n Au :n NaBH4 In a ratio of 1:8, NaBH4 was added to the mixed solution of HAuCl4 and PVA at a stirring speed of 800 rpm. After stirring for 2 hours, 4.0 g CeO2 was added, and concentrated H2SO4 solution was slowly added dropwise under vigorous stirring. The pH value of the above mixed solution was adjusted to 3, and stirring was continued for 3 hours. After the reaction was completed, ultrapure water was used for centrifugal washing until neutral, and then it was placed in a 60°C forced air oven for 12 hours to obtain Au / CeO2.
[0093] Weigh 20 mg of Au / CeO2 and place it on a quartz wafer. Add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz wafer, control the thickness to 0.05 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz wafer in an atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, ozone flow rate of 50 sccm, deposition temperature of 300°C, and precursor biscyclopentadienyl cobalt temperature of 80°C. First, introduce biscyclopentadienyl cobalt vapor into the deposition chamber with a pulse time of 0.3s, a breath holding time of 6s, and a vacuum time of 70s; then introduce an ozone pulse into the deposition chamber, and then introduce an ozone pulse into the deposition chamber with a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 200s to complete a Co deposition cycle. Repeat 20 cycles to obtain a 20Co-Au / CeO2 bimetallic catalyst. The morphology of the sample is as shown in the figure. Fig.15 shown.
[0094] 20Co-Au / CeO2 was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 100°C, the catalyst was 20 mg, the solvent was tributyl phosphate 20 mL, 1,4-butanediol 200 mg was added, 0.3 MPa of oxygen was charged, the reaction time was 4 h, the conversion rate of 1,4-butanediol was 95%, and the selectivity of γ-butyrolactone was 97%.
[0095] Example 16
[0096] Au / HAP was prepared by sedimentation precipitation method (with urea as precipitant): first, 1.0 g of carrier HAP powder was weighed into 70 mL of water and stirred for 2 h to make the carrier evenly dispersed. Then, 10 mL of 7.2 mmol / L HAuCl4 solution was measured and dripped into the dispersed carrier drop by drop, and stirred vigorously for 12 h. Au :n 尿素 Weigh a certain amount of urea at a ratio of 1:100, add it to the aqueous solution of HAuCl4 and carrier, and stir at 80℃ for 6h. After the reaction is completed, let it stand for 5h, filter it, and wash it with deionized water until the Cl in the system is - All of them were removed (checked with 0.1 mol / L AgNO3 solution until no white precipitate was generated, which means it was washed clean). Finally, the sample was dried at 80°C for 12h to obtain Au / HAP.
[0097] Weigh 20 mg of Au / HAP and place it on a quartz plate, add 1 mL of anhydrous ethanol to evenly disperse the sample on the quartz plate, control the thickness to 0.35 mm, and after the anhydrous ethanol evaporates to dryness, place the quartz plate in a low-temperature vacuum atomic layer deposition (ALD) device. The set deposition parameters are: nitrogen flow rate of 50 sccm, deposition temperature of 350°C, and precursor trimethylmethylcyclopentadienyl platinum temperature of 75°C. First, introduce trimethylmethylcyclopentadienyl platinum vapor into the deposition chamber with a pulse time of 0.8s, a breath holding time of 2s, and a vacuum time of 90s; then introduce ozone into the deposition chamber with a flow rate of 50 sccm, a pulse time of 0.3s, a breath holding time of 2s, and a vacuum time of 160s. This completes a Pt deposition cycle. Repeat 10 cycles to obtain a 10Pt-Au / HAP bimetallic catalyst. The morphology of the sample is as shown in Fig.16 shown.
[0098] 10Pt-Au / HAP was applied to the aerobic oxidation reaction of 1,4-butanediol. The reaction temperature was 100°C, the catalyst was 20 mg 10Pt-Au / HAP, the solvent was 20 mL tributyl phosphate, and 1,4-butanediol was 200 mg. 0.3 MPa of oxygen was introduced. The reaction time was 4 h. The conversion rate of 1,4-butanediol was 95%, and the selectivity of γ-butyrolactone was 93%.
Claims
1. A method for preparing an Au-M bimetallic catalyst for catalyzing the oxidation of 1,4-butanediol to prepare r-butyrolactone, characterized in that: The steps include: (1) Loading of Au nanoparticles on the material surface Preparation of Au / carrier samples by sol-solidification method: Weigh a certain amount of HAuCl4·3H2O and dissolve it in ultrapure water to prepare a 1-10mmol / L HAuCl4 aqueous solution, and take 10-200mL into a beaker; then prepare a 1-20g / L PVA aqueous solution, according to m Au :m PVA The ratio is 1:1-10, and the PVA solution is added to the HAuCl4 solution at a stirring speed of 200-1000rpm; then 5-20mmol / L NaBH4 solution is prepared according to n Au :n NaBH4 The ratio of NaBH4 to HAuCl4 and PVA is 1:1-10, the stirring speed is 200-1000rpm, after stirring for 1-12h, 0.5-5.0g of carrier is added, concentrated H2SO4 is slowly added dropwise to the system under vigorous stirring, the pH value of the mixed solution is adjusted to 1-5, and stirring is continued for 1-6h. After the reaction is completed, ultrapure water is used for centrifugal washing until neutral, and then placed in a 60-200°C forced air oven for 12-24h to obtain an Au / carrier sample; (2) Preparation of Au-M bimetallic catalyst Weigh 5-50 mg of Au / carrier sample and place it on a quartz plate, add 1-10 mL of diluent to evenly disperse the sample on the quartz plate, control the thickness to be 0.01-2 mm, wait for the diluent to evaporate to dryness, place the quartz plate in an atomic layer deposition (ALD) device, and set the atomic layer deposition parameters as follows: nitrogen flow rate of 50 sccm, deposition temperature of 120-350 ° C, metal M precursor temperature of 25-100 ° C, formalin temperature of 20-300 ° C, and the thickness of the sample to be uniformly dispersed on the quartz plate. The temperature is 25-60°C, the precursor of metal M is first introduced into the deposition chamber by steam pulse, the pulse time is 0.01-2s, the breath holding time is 0.1-20s, and the air pumping time is 20-300s; then formalin pulse is introduced into the deposition chamber, the pulse time is 0.01-2s, the breath holding time is 0.1-20s, and the air pumping time is 20-300s, to complete a deposition cycle of metal M; repeat 2-50 cycles to obtain Au-M bimetallic catalyst; Alternatively, the atomic layer deposition parameters are set as follows: a nitrogen flow rate of 50 sccm, an ozone flow rate of 50 sccm, a deposition temperature of 120-350°C, a temperature of the metal M precursor of 25-100°C, and the metal M precursor is introduced into the deposition chamber in the form of a steam pulse, with a pulse time of 0.01-2s, a breath-holding time of 0.1-20s, and a pumping time of 20-300s; then an ozone pulse is introduced into the deposition chamber, with a pulse time of 0.1-0.5s, a breath-holding time of 2-10s, and a pumping time of 60-120s, thereby completing a deposition cycle of the metal M; repeat 2-50 cycles to obtain an Au-M bimetallic catalyst.
2. The preparation method according to claim 1, characterized in that The Au / carrier sample prepared by the sol-solidification method is replaced by the Au / carrier sample prepared by the impregnation method, that is: a certain amount of HAuCl4·3H2O is weighed and dissolved in ultrapure water to prepare a 1-10mmol / L HAuCl4 aqueous solution, and 10-200mL is measured and placed in a beaker; then 0.5-5.0g of the carrier is added to the beaker, and stirred at 30-100°C for 12h-24h, the resulting paste sample is placed in an oven at 50-200°C for drying, and then the paste sample is calcined in a muffle furnace at 200-500°C for 1-3h to obtain the Au / carrier sample.
3. The preparation method according to claim 1, characterized in that: The Au / carrier sample prepared by the sol-solidification method was replaced by a deposition precipitation method using NaOH as a precipitant, that is, first weigh 1.0 g of the carrier in 10 mL-200 mL of water, stir for 1 h-5 h to evenly disperse the carrier, then measure 10-200 mL of 1-10 mmol / L HAuCl4 solution, dropwise add it to the dispersed carrier, and stir vigorously for 12-24 h; then prepare 0.1-2 mol / L NaOH solution, add it to the aqueous solution of HAuCl4 and the carrier, control the pH to 9-13, stir at 200-1000 rpm, stir for 12-24 h, stand for 0.5-5 h after the reaction, filter, and wash with deionized water until Cl in the system is - All are removed; finally, the sample is dried at 50-200°C for 12-24h to obtain an Au / carrier sample.
4. The preparation method according to claim 3, characterized in that: The above-mentioned NaOH as the precipitant is replaced by urea as the precipitant, that is, first weigh 1.0g of the carrier into 10mL-200mL of water, stir for 1h-5h to make the carrier evenly dispersed, then measure 10-200mL of 1-10mmol / L HAuCl4 solution, dropwise add it into the dispersed carrier, and stir vigorously for 12-24h; then according to n Au :n 尿素 Weigh a certain amount of urea at a ratio of 1:50-200, add it to the aqueous solution of HAuCl4 and carrier, and stir at 50-120℃ for 1-6h. After the reaction is completed, let it stand for 0.5-5h, filter, and wash with deionized water until the Cl in the system is - All are removed; finally, the sample is dried at 50-200°C for 12-24h to obtain an Au / carrier sample.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The carrier described in step (1) is one of titanium oxide (TiO2), cerium oxide nanorods (CeO2), hydroxyapatite (HAP) and hydrotalcite (HT) oxide.
6. The preparation method according to any one of claims 1 to 4, characterized in that: The diluent in step (2) is one of water, methanol or ethanol.
7. The preparation method according to any one of claims 1 to 4, characterized in that: The precursor of the metal M in the step (2) is hexafluoroacetylacetonate palladium, biscyclopentadienyl cobalt, bis(hexafluoroacetylacetonate)copper(II), trimethylmethylcyclopentadienyl platinum, bis(ethylcyclopentadienyl)ruthenium(II), hexacarbonyl molybdenum, bis(cyclopentadienyl)nickel or bis(cyclopentadienyl)iron.
8. A catalyst prepared by the preparation method as described in any one of claims 1 to 4.
9. Use of the catalyst as claimed in claim 8 in catalyzing the oxidation of 1,4-butanediol to prepare r-butyrolactone.
Citation Information
Patent Citations
Method for catalytic preparation of gamma-butyrolactone by using supported nano-gold catalyst
CN101139332A
Preparation method and application of supported nanogold catalyst
CN114733520A
Method for preparing 1, 4-butanediol through catalytic hydrogenation of gamma-butyrolactone
CN115448814A