By adding specific elements and heat treatment technology to copper materials, the problem of insufficient performance of pure copper contact wires in high-strength and extreme environments has been solved, and copper alloy contact wires with excellent comprehensive properties have been prepared, which improves their performance in high-speed operation and extreme environments. Adaptability and service life in the environment.

CN118808577APending Publication Date: 2024-10-22CHINA COPPER (KUNMING) COPPER INDUSTRY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411017934.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-22

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention is applied to the technical field of copper alloy contact lines, and discloses a method for preparing a copper alloy contact line based on copper material genetic engineering, the copper alloy component conforms to the form of CuX * CuY, X is selected from at least one of Si, Mn and Zn, and Y is selected from at least one of Ni, Cr and P. According to the method for preparing the copper alloy contact line based on the copper material genetic engineering, Si and Ni are added into a copper material, compounds Ni2Si and Ni3Si are formed through Si and Ni, when Ni2Si and Ni3Si are separated out of a solid solution, the strength and hardness of the alloy can be improved, so that the effect of strengthening the copper alloy is achieved, the effect of refining grains is achieved through the mode that Mn and Ni are added into the copper material to form MnNi, and therefore the copper alloy contact line is obtained. The mechanical property and the corrosion resistance of the prepared copper alloy can be further improved by means of the precipitation hardening effect of MnNi, the solid solution strengthening effect is achieved by adding Zn and dissolving a large amount of Zn in Cu and Ni, the strength and hardness are improved, and the corrosion resistance is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloy contact wires, and in particular to a method for preparing a copper alloy contact wire based on copper material genetic engineering. Background Art

[0002] In today's rapidly developing transportation field, especially in railway and rail transit systems, contact wires play a vital role. As a key component of power transmission, the performance of contact wires directly affects the safety, efficiency and stability of train operation. For a long time, pure copper contact wires have been widely used due to their excellent conductivity. However, with the continuous development of railway transportation, the requirements for contact wires are becoming increasingly stringent. Pure copper contact wires gradually expose a series of limitations when facing high-intensity mechanical stress, complex and changeable environmental conditions, and the continuously growing demand for power transmission. Although pure copper materials have good conductivity, they are relatively weak in strength and cannot withstand the huge tension and impact generated by high-speed operation and heavy loads, which easily leads to deformation, wear and even breakage of the contact wire. , seriously affecting the continuity and reliability of power supply. At the same time, the wear resistance of pure copper contact wire is poor. Under long-term friction, its surface is easily damaged, which in turn affects the efficiency and quality of power transmission. In addition, in high temperature environment, the performance of pure copper contact wire will also be affected to a certain extent, and softening may occur, reducing its carrying capacity and service life. In some areas with harsh climate, high humidity or chemical pollution, pure copper contact wire has insufficient corrosion resistance and is easily corroded, further shortening its service life and increasing maintenance costs. In order to overcome these defects of pure copper contact wire, scientific researchers are committed to the development of copper alloy contact wire. By adding appropriate amounts of alloying elements such as tin, magnesium, chromium, zinc, etc. to copper, the mechanical properties, physical properties and chemical properties of the contact wire can be significantly improved.However, the existing copper alloy contact wire technology is not perfect. On the one hand, some copper alloy contact wires inevitably sacrifice a certain degree of conductivity in the process of pursuing high strength and wear resistance, resulting in increased energy loss in the process of power transmission. On the other hand, the formulations and manufacturing processes of some copper alloys are still imperfect, resulting in high production costs, which limits their large-scale application. Furthermore, the fatigue resistance of existing copper alloy contact wires still needs to be improved. Under the influence of frequent train operations and changing environmental factors, fatigue cracks are prone to occur, which in turn affects the service life and safety of the contact wire. At the same time, for some special application scenarios, such as high-cold areas, high-altitude areas or environments with strong electromagnetic interference, the existing copper alloy contact wires are still insufficient in adapting to these extreme conditions. With the continuous acceleration and intelligent development of railways and rail transit, as well as higher requirements for energy conservation and environmental protection, unprecedented challenges have been posed to the comprehensive performance of contact wires. Not only do they need to have higher strength, better wear resistance, excellent conductivity and corrosion resistance, but they also need to be Breakthroughs have been made in fatigue resistance, ability to adapt to extreme environments, and cost control. Material genetic engineering is an interdisciplinary subject that combines biology and engineering. It aims to use genetic engineering technology to change the properties and functions of materials, and to improve the performance and application of materials by realizing the self-assembly, self-repair, self-sensing and self-adaptation of materials. The theoretical basis of material genetic engineering is material genomics. Through the analysis and interpretation of the material genome, we can understand the relationship between the genome structure and potential functions of the material. Then, genetic engineering technology is used to edit and design the material genes to achieve the desired material properties and functions. Material genetic engineering is widely used in the research and development of various materials. For example, in the field of metal materials, the sequence of metal genes can be changed to adjust the crystal structure and lattice parameters of the metal, thereby changing the mechanical properties and electrical properties of the metal. Therefore, a method for preparing copper alloy contact wire based on copper material genetic engineering is proposed. Therefore, a method for preparing copper alloy contact wire based on copper material genetic engineering is proposed. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a copper alloy contact wire based on copper material genetic engineering, so as to solve the problem of insufficient corrosion resistance and strength of pure copper contact wire under special environment proposed in the above background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions: a method for preparing a copper alloy contact wire based on copper material genetic engineering, wherein the copper alloy composition conforms to the form CuX*CuY, wherein X is selected from at least one of Si, Mn and Zn, and Y is selected from at least one of Ni, Cr and P; The preparation method comprises the following steps: S1. The single Cu block and the Y alloy raw material of the designed component are loaded into the upper continuous casting furnace according to the ratio; S2. The single substance Cu powder and the X alloy raw material powder of the designed composition are placed in an atmosphere furnace and heated and melted in a nitrogen-containing medium under protective conditions; S3. The rod-shaped embryo obtained in S1 and the block embryo after cooling and forming in S2 are placed in a vacuum furnace for secondary melting and sintering and densification and cast into round rod-shaped embryos; S4. The rod-shaped blank obtained in S4 is continuously hot-extruded, and finally a contact line is obtained by stretching; S5. Heat treat the processed contact wire to improve its mechanical properties and electrical conductivity.

[0005] Preferably, in the copper alloy, the total content of X element is greater than 0.7% and not higher than 15%, the total content of Y element is greater than 0.3%, wherein the content of Si is in the range of 0.4-3.5%, the content of Mn is in the range of 0.3-0.5%, the content of Zn is in the range of 7-13%, the content of Ni is in the range of 2.2-3.5%, the content of Cr is in the range of 0.02-1.8%, and the content of P is in the range of 0.3-0.7%.

[0006] Preferably, the copper alloy consists of the following components: Si-0.4%, Mn-0.3%, Zn-7%, Ni-2.2%, Cr-0.02% and the balance Cu.

[0007] Preferably, the copper alloy consists of the following components: Si-1.7%, Mn-0.4%, Zn-10%, Ni-2.8%, P-0.5% and the balance Cu.

[0008] Preferably, the copper alloy consists of the following components: Mn-0.5%, Zn-13%, Cr-1.8%, P-0.7% and the balance Cu.

[0009] Preferably, the heating temperature of the vacuum furnace in S3 is controlled at 1200-1800°C, and the vacuum degree of the vacuum furnace in S3 is not less than 2.0×10 -3 Pa, and the pressure rise rate of the vacuum furnace in S3 is ≤0.5Pa / h.

[0010] Preferably, the hot extrusion temperature in S4 is controlled at 650° C.-700° C., and an inert gas is introduced during the hot extrusion process for protection.

[0011] Preferably, the stretching speed of the rod-shaped blank in S4 is controlled at 600-900 mm / min, and the pressure in the mold cavity is between 900-1000 MPa.

[0012] Preferably, the heat treatment process in S5 includes annealing and tempering, wherein the annealing temperature of the contact line is controlled at 410-430°C.

[0013] Preferably, the tempering temperature in S5 is controlled at 390-410° C., and the tempering time is controlled at 1.5-2 h, and natural air cooling is performed after the tempering is completed.

[0014] Compared with the prior art, the invention has the following beneficial effects: the method for preparing the copper alloy contact wire based on copper material genetic engineering: By adding Si and Ni to copper materials, Si and Ni form compounds Ni2Si and Ni3Si. When Ni2Si and Ni3Si precipitate from the solid solution, the strength and hardness of the alloy can be increased, thereby strengthening the copper alloy. Furthermore, by adding Mn and Ni to the copper material to form MnNi, the grain refinement can be achieved, and the mechanical and corrosion resistance of the copper alloy can be further improved by the precipitation hardening effect of MnNi. Furthermore, by adding a large amount of Zn to dissolve in Cu and Ni, the effect of solid solution strengthening is achieved, the strength and hardness are improved, and the corrosion resistance is increased. At the same time, P is added to improve the strength, hardness, elastic limit, elastic modulus and fatigue strength of the alloy, and Cr is added to enhance the mechanical strength and heat resistance of the copper alloy. DETAILED DESCRIPTION

[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0016] The present invention provides a technical solution: a method for preparing a copper alloy contact wire based on copper material genetic engineering, wherein the copper alloy composition conforms to the form CuX*CuY, wherein X is selected from at least one of Si, Mn and Zn, and Y is selected from at least one of Ni, Cr and P; The preparation method comprises the following steps: S1. The single Cu block and the Y alloy raw material of the designed component are loaded into the upper continuous casting furnace according to the ratio; S2. The single substance Cu powder and the X alloy raw material powder of the designed composition are placed in an atmosphere furnace and heated and melted in a nitrogen-containing medium under protective conditions; S3. The rod-shaped embryo obtained in S1 and the block embryo after cooling and forming in S2 are placed in a vacuum furnace for secondary melting and sintering and densification and cast into round rod-shaped embryos; S4. The rod-shaped blank obtained in S4 is continuously hot-extruded, and finally a contact line is obtained by stretching; S5. Heat treat the processed contact wire to improve its mechanical properties and electrical conductivity.

[0017] In the copper alloy, the total content of X elements is greater than 0.7% and not higher than 15%, the total content of Y elements is greater than 0.3%, of which the content of Si is in the range of 0.4-3.5%, the content of Mn is in the range of 0.3-0.5%, the content of Zn is in the range of 7-13%, the content of Ni is in the range of 2.2-3.5%, the content of Cr is in the range of 0.02-1.8%, and the content of P is in the range of 0.3-0.7%.

[0018] The heating temperature of the vacuum furnace in S3 is controlled at 1200-1800℃, and the vacuum degree of the vacuum furnace in S3 is not less than 2.0××10 -3 Pa, and the pressure rise rate of the vacuum furnace in S3 is ≤0.5Pa / h.

[0019] In S4, the hot extrusion temperature is controlled at 650°C-700°C, and inert gas is introduced during the hot extrusion process for protection.

[0020] In S4, the stretching speed of the rod-shaped blank is controlled at 600-900 mm / min, and the pressure in the mold cavity is between 900-1000 MPa.

[0021] The heat treatment process in S5 includes annealing and tempering, wherein the annealing temperature of the contact line is controlled at 410-430°C.

[0022] In S5, the tempering temperature is controlled at 390-410°C, and the tempering time is controlled at 1.5-2h, and natural air cooling is performed after the tempering is completed.

[0023] Example 1

[0024] The copper alloy consists of the following components: Si-0.4%, Mn-0.3%, Zn-7%, Ni-2.2%, Cr-0.02% and the balance of Cu. The single-element Cu block, 2.2% Ni and 0.02% Cr are charged into an upward continuous casting furnace according to a proportion, and the single-element Cu powder and 0.4% Si, 0.3% Mn and 7% Zn powder are placed in an atmosphere furnace and protectively heated and melted in a nitrogen-containing medium; The rod-shaped embryos prepared in S1 and the block embryos formed after cooling in S2 are placed in a vacuum furnace for secondary melting, sintered and densified, and cast into round rod-shaped embryos; The rod-shaped blank prepared in S4 is continuously hot-extruded, and finally a contact wire is prepared by stretching; Heat treatment is performed on the processed contact wire to improve its mechanical properties and electrical conductivity.

[0025] Example 2

[0026] The copper alloy consists of the following components: Si-1.7%, Mn-0.4%, Zn-10%, Ni-2.8%, P-0.5% and the balance of Cu. The single-element Cu block, 2.8% Ni and 0.5% P are charged into an upward continuous casting furnace according to a proportion, and the single-element Cu powder and 1.7% Si, 0.4% Mn and 10% Zn powder are placed in an atmosphere furnace and protectively heated and melted in a nitrogen-containing medium; The rod-shaped embryos prepared in S1 and the block embryos formed after cooling in S2 are placed in a vacuum furnace for secondary melting, sintered and densified, and cast into round rod-shaped embryos; The rod-shaped blank prepared in S4 is continuously hot-extruded, and finally a contact wire is prepared by stretching; Heat treatment is performed on the processed contact wire to improve its mechanical properties and electrical conductivity.

[0027] Example 3

[0028] The copper alloy consists of the following components: Mn-0.5%, Zn-13%, Cr-1.8%, P-0.7% and the balance of Cu. The single-element Cu block, 1.8% Cr and 0.7% P are charged into an upward continuous casting furnace according to a proportion, and the single-element Cu powder, 0.5% Mn and 13% Zn powder are placed in an atmosphere furnace and protectively heated and melted in a nitrogen-containing medium; The rod-shaped embryos prepared in S1 and the block embryos formed after cooling in S2 are placed in a vacuum furnace for secondary melting, sintered and densified, and cast into round rod-shaped embryos; The rod-shaped blank prepared in S4 is continuously hot-extruded, and finally a contact wire is prepared by stretching; Heat treatment is performed on the processed contact wire to improve its mechanical properties and electrical conductivity.

[0029] The test data structures of the alloys obtained in the above embodiments are shown in the following table:

[0030] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a copper alloy contact wire based on copper material genetic engineering, characterized in that: The copper alloy composition conforms to the form CuX*CuY, wherein X is selected from at least one of Si, Mn and Zn, and Y is selected from at least one of Ni, Cr and P; The preparation method comprises the following steps: S1. The single Cu block and the Y alloy raw material of the designed component are loaded into the upper continuous casting furnace according to the ratio; S2. The single substance Cu powder and the X alloy raw material powder of the designed composition are placed in an atmosphere furnace and heated and melted in a nitrogen-containing medium under protective conditions; S3. The rod-shaped embryo obtained in S1 and the block embryo after cooling and forming in S2 are placed in a vacuum furnace for secondary melting and sintering and densification and cast into round rod-shaped embryos; S4. The rod-shaped blank obtained in S4 is continuously hot-extruded, and finally a contact line is obtained by stretching; S5. Heat treat the processed contact wire to improve its mechanical properties and electrical conductivity.

2. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: In the copper alloy, the total content of X element is greater than 0.7% and not higher than 15%, the total content of Y element is greater than 0.3%, wherein the content of Si is in the range of 0.4-3.5%, the content of Mn is in the range of 0.3-0.5%, the content of Zn is in the range of 7-13%, the content of Ni is in the range of 2.2-3.5%, the content of Cr is in the range of 0.02-1.8%, and the content of P is in the range of 0.3-0.7%.

3. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: The copper alloy consists of the following components: Si-0.4%, Mn-0.3%, Zn-7%, Ni-2.2%, Cr-0.02% and the balance of Cu.

4. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: The copper alloy consists of the following components: Si-1.7%, Mn-0.4%, Zn-10%, Ni-2.8%, P-0.5% and the balance of Cu.

5. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: The copper alloy consists of the following components: Mn-0.5%, Zn-13%, Cr-1.8%, P-0.7% and the balance of Cu.

6. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: The heating temperature of the vacuum furnace in S3 is controlled at 1200-1800°C, and the vacuum degree of the vacuum furnace in S3 is not less than 2.0×2.0×10 -3 Pa, and the pressure rise rate of the vacuum furnace in S3 is ≤0.5Pa / h.

7. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: The hot extrusion temperature in S4 is controlled at 650° C.-700° C., and an inert gas is introduced during the hot extrusion process for protection.

8. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: In the S4, the stretching speed of the rod-shaped blank is controlled at 600-900 mm / min, and the pressure in the mold cavity is between 900-1000 MPa.

9. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 1, characterized in that: The heat treatment process in S5 includes annealing and tempering, wherein the annealing temperature of the contact wire is controlled at 410-430°C.

10. The method for preparing a copper alloy contact wire based on copper material genetic engineering according to claim 9, characterized in that: In S5, the tempering temperature is controlled at 390-410° C., and the tempering time is controlled at 1.5-2 h. After the tempering is completed, natural air cooling is performed.