Additive-modified aqueous zinc ion electrolyte and application thereof

By adding glutathione to the aqueous zinc ion electrolyte, the problems of dendrite growth and surface corrosion of zinc ion batteries at high current densities are solved, more uniform zinc deposition and higher cycle stability are achieved, and zinc ion batteries are improved. Overall performance of ion batteries.

CN118825440APending Publication Date: 2024-10-22ZHONGBEI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114281.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Aqueous zinc-ion batteries have problems with dendrite growth, surface corrosion and passivation layer formation under high current density and high zinc utilization, resulting in short cycle life and low zinc utilization.

Method used

Adding glutathione as an additive to the aqueous zinc ion electrolyte forms an SEI film through chemical adsorption and changes the solvation structure of zinc, optimizing zinc deposition behavior and reducing surface current density and side reactions.

Benefits of technology

It significantly extends the cycle life of zinc-ion batteries, improves the cycle stability of the battery and the utilization rate of zinc, especially showing excellent performance under high current density and high zinc utilization rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118825440A_ABST
    Figure CN118825440A_ABST
Patent Text Reader

Abstract

The invention discloses an additive-modified aqueous zinc ion electrolyte and application thereof. The invention belongs to the technical field of aqueous zinc ion batteries. The additive disclosed by the invention is glutathione which is rich in sulfydryl and carboxyl functional groups; as a bifunctional additive, the zinc oxide can be preferentially combined with zinc ions to reduce solvated water molecules; meanwhile, the metal zinc can be adsorbed on a Zn (111) crystal face in a chemical adsorption mode through deprotonation of sulfydryl and carboxyl, and a layer of solid electrolyte interface film is formed, so that the local current density of the surface is reduced, and the deposition behavior of the metal zinc is adjusted. Through the synergistic effects, the growth of zinc dendrites and the occurrence of side reactions can be effectively inhibited, so that the trace additive can prolong the cycle life of the aqueous zinc metal battery to 9000 hours or more. And the preparation method has the advantages of simple preparation process, environmental protection, low cost and the like, and has wide application prospects in the field of aqueous zinc ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aqueous zinc ion batteries, and in particular relates to an additive-modified aqueous zinc ion electrolyte and application thereof. Background Art

[0002] As over-reliance on fossil fuels has exacerbated energy depletion, environmental pollution and climate deterioration, the global energy landscape is shifting from traditional fossil energy to clean and efficient new energy. However, due to the intermittent and undispatched nature of renewable energy sources such as solar energy, tidal energy, and wind energy, directly applying these unstable energy sources will damage the existing power grid system. Therefore, the development of economically feasible energy storage technologies and devices is crucial for the stable conversion and utilization of renewable energy in the power grid.

[0003] In recent years, lithium-ion batteries have dominated the fields of electronic intelligence and large-scale energy storage devices due to their high energy density. However, their high manufacturing cost, high toxicity, flammable electrolytes and other problems have seriously hindered the wider application of lithium-ion batteries. Therefore, it is imperative to develop safe, reliable and low-cost energy storage technologies. Aqueous zinc-ion batteries (AZIBs) have attracted great interest as an alternative to alkali metal ion batteries due to their high safety, low cost and environmental friendliness. Zinc metal is the most promising aqueous anode material with a high theoretical capacity (5855 mAh cm -3 and 820 mAh g -1 ), low redox potential (-0.76 V vs standard hydrogen electrode) and good compatibility with aqueous electrolytes.

[0004] However, zinc ions tend to deposit at energetically favorable charge transfer sites on the zinc negative electrode, forming initial small protrusions. In order to reduce the surface energy, subsequent zinc ions also tend to concentrate on these small protrusions and deposit, causing them to gradually grow into preliminary dendrites. The resulting "tip effect" will further aggravate the uneven distribution of the electric field on the negative electrode surface, aggravate the growth of dendrites, lead to capacity decay, and even short circuit. At the same time, the electroplating / stripping cycle is always accompanied by hydrogen evolution reaction and surface corrosion. As hydrogen is precipitated, the local pH value will increase sharply because OH - The concentration increases rapidly, and the generated OH - Will be with Zn 2+ Reacts with H2O to form a passivation layer on the zinc surface. This reduces the reversibility of the electroplating / stripping process, increases internal resistance, and limits the utilization of zinc. Currently, researchers have carried out a lot of research on issues such as dendrites, corrosion, and passivation. For example, interface modification, structural design, and electrolyte engineering optimization have made great progress under low current density conditions based on these strategies, but there are few inventions that achieve high-performance zinc anodes at high current density and high zinc utilization. Summary of the invention

[0005] In view of the shortcomings of the prior art, the primary purpose of the present invention is to provide an additive-modified aqueous zinc ion electrolyte and its application. The electrolyte additive is low in cost, environmentally friendly, and simple to prepare. It can simultaneously improve the cycle life of aqueous zinc ion batteries under high current density and high area capacity and low current density and low area capacity.

[0006] Specifically, the invention scheme of the present disclosure is as follows: An additive-modified aqueous zinc ion electrolyte comprises an electrolyte and an additive; the electrolyte is a soluble zinc salt, and the additive is glutathione.

[0007] In the above technical solution, the soluble zinc salt is one or more of zinc sulfate, zinc trifluoromethanesulfonate, zinc perchlorate or zinc nitrate.

[0008] In the above technical solution, the soluble zinc salt is preferably zinc trifluoromethanesulfonate.

[0009] In the above technical solution, the concentration of the soluble zinc salt is 1-3 mol L -1 .

[0010] In the above technical solution, the concentration of the soluble zinc salt is preferably 2 mol L -1 .

[0011] In the above technical solution, the concentration of the additive is 0.5-4 g L -1 .

[0012] In the above technical solution, the concentration of the additive is preferably 2 g L -1 .

[0013] The invention discloses an application of an aqueous zinc ion electrolyte modified by an additive in a zinc ion battery. The zinc ion battery comprises a positive electrode, a diaphragm, a negative electrode and the aqueous zinc ion electrolyte modified by the additive.

[0014] In the above technical solution, the positive electrode material is vanadium pentoxide, manganese dioxide, sodium vanadate or lithium manganate.

[0015] In the above technical solution, the diaphragm is a glass fiber diaphragm.

[0016] In the above technical solution, the negative electrode material is zinc powder, zinc foil or zinc foam.

[0017] In the above technical solution, the additive-modified aqueous zinc ion battery electrolyte can significantly extend the cycle life of the battery at both low current density and high current density, and improve the cycle stability of the battery.

[0018] The advantages of the present invention are: By adding glutathione additives to the aqueous electrolyte of zinc-ion batteries, on the one hand, it can be preferentially adsorbed on the Zn (111) crystal surface by chemical adsorption under the synergistic effect of thiol and carboxyl groups to form a SEI film, which reduces the local current density on the surface, regulates the Zn deposition behavior, and separates water molecules from the zinc negative electrode to alleviate the occurrence of side reactions. On the other hand, it can change the Zn 2+ The solvation structure reduces the number of solvated water molecules, increases the zinc deposition overpotential, refines the grains, and makes the zinc deposition more uniform, thereby achieving excellent cycle stability at high current density and high zinc utilization. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The Zn||Zn symmetric battery in Example 1 of the present invention with different concentrations of additive electrolytes and the control group at 2 mA cm -2 , 2 mAh cm -2 Cyclic test performance diagram when .

[0020] Figure 2 In Example 2 of the present invention, 2 g L -1 The additive electrolyte and the comparative Zn||Zn symmetric battery at 1 mA cm -2 , 0.5 mAh cm -2 Cyclic test performance diagram when .

[0021] Figure 3 In Example 3 of the present invention, 2 g L -1 The additive electrolyte and the comparative Zn||Zn symmetric battery at 10 mA cm -2 , 20 mAh cm -2 Cyclic test performance diagram when (using zinc foil with a thickness of 50 um, DOD Zn is 74%).

[0022] Figure 4 In Example 4 of the present invention, 2 g L -1 SEM images of zinc deposits in the additive electrolyte and the Zn||Zn symmetric cell of the control group.

[0023] Figure 5 In Example 5 of the present invention, 2 g L -1 SEM cross-sectional images of zinc deposits in the additive electrolyte and the Zn||Zn symmetric cell of the control group.

[0024] Figure 6 In Example 6 of the present invention, 2 g L -1The full battery charge and discharge cycle performance diagram of the additive electrolyte and the comparison group.

[0025] Figure 7 In Example 7 of the present invention, 2 g L -1 Full battery rate performance diagram of the additive electrolyte and the comparison group. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be fully described below in conjunction with the accompanying drawings and examples. It should be understood that the following embodiments are only used to illustrate the present invention, rather than to limit the present invention. Other embodiments obtained by ordinary technicians in this field without making creative work are all within the scope of protection of the present invention.

[0027] Example 1 (1) Preparation of negative electrode sheets. The zinc foil was cut into discs with diameters of 12 mm and 16 mm, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0028] (2) Prepare 2 mol L -1 Then, different amounts of glutathione were added to make the concentrations of 0.5, 1, 2, and 4 g L -1 , and magnetically stirred for 6 h to make it evenly dissolved in the zinc trifluoromethanesulfonate solution.

[0029] (3) Zinc sheets were used as positive and negative electrodes, glass fibers were used as separators, and 130 μL of electrolyte containing different concentrations of glutathione was added to assemble 2032 button-type symmetrical batteries. -1 Symmetrical batteries were assembled under the same electrolyte conditions as a control group.

[0030] (4) The assembled button cell was cycled with a BlueDian electrochemical test system under constant current conditions of 2 mA cm -2 , 2 mAh cm -2 .

[0031] The cycling stability of Zn||Zn symmetric batteries with different concentrations of glutathione electrolytes under long-term cycling was observed. Figure 1 As shown in the figure, it can be seen that adding 2 g L -1 The glutathione electrolyte showed the best cycling stability after stable cycling for 3100 h. -1 The cycle life of symmetrical batteries with zinc trifluoromethanesulfonate electrolyte increases by 1000%.

[0032] Example 2 (1) Preparation of negative electrode sheets. The zinc foil was cut into 12 mm and 16 mm discs, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0033] (2) Prepare 2 mol L -1 of zinc trifluoromethanesulfonate solution, and then add 2 g L -1 Glutathione The mixture was magnetically stirred for 6 h to make it uniformly dissolved in the zinc trifluoromethanesulfonate solution.

[0034] (3) Use zinc sheets as positive and negative electrodes and glass fiber as separator. Add 130 μL of 2 g L -1 Glutathione electrolyte was used to assemble a 2032 button-type symmetrical battery. At the same time, 2 mol L -1 Symmetrical batteries were assembled under the same electrolyte conditions as a control group.

[0035] (4) The button cell was cycled with a Blue Electric electrochemical test system. The cycle test conditions were: 1 mA cm -2 , 0.5 mAh cm -2 .

[0036] Observe the addition of 2 g L -1 Symmetric Zn||Zn battery with glutathione electrolyte at 1 mA cm -2 , 0.5 mAh cm -2 The cyclic stability of Figure 2 As shown. Contains 2 g L -1 Symmetrical cell with glutathione electrolyte at 1 mA cm -2 , 0.5mAh cm -2 It can be cycled stably for more than 9000 h, while the control sample short-circuited after only 70 h, indicating that hydrogen evolution and dendrite formation led to battery failure.

[0037] Example 3 (1) Preparation of negative electrode sheets. The zinc foil was cut into 12 mm and 16 mm discs, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0038] (2) Prepare 2 mol L -1 of zinc trifluoromethanesulfonate solution, and then add 2 g L -1 The glutathione was evenly dissolved in the zinc trifluoromethanesulfonate solution by magnetic stirring for 6 hours.

[0039] (3) Use zinc sheets as positive and negative electrodes and glass fiber as separator. Add 130 μL of 2 g L -1 Glutathione electrolyte was used to assemble a 2032 button-type symmetrical battery. At the same time, 2 mol L -1 Symmetrical batteries were assembled under the same electrolyte conditions as a control group.

[0040] (4) The assembled button cell was cycled with a BlueDian electrochemical test system under constant current conditions of 10 mA cm -2 , 20 mAh cm -2 .

[0041] The results are as follows Figure 3 Even at high DOD Zn When the Zn||Zn symmetric battery with glutathione added was 74%, it could also maintain a stable cycle for up to 770 hours. In contrast, a short circuit occurred in the control group after only 16 hours, indicating that glutathione has great potential in practical applications.

[0042] Example 4 (1) Preparation of negative electrode sheets. The zinc foil was cut into 12 mm and 16 mm discs, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0043] (2) Prepare 2 mol L -1 of zinc trifluoromethanesulfonate solution, and then add 2 g L -1 The glutathione was uniformly dissolved in the zinc trifluoromethanesulfonate solution by magnetic stirring for 6 h.

[0044] (3) Zinc sheets were used as positive and negative electrodes and glass fiber was used as a separator. 200 μL of 2 g L -1 Glutathione electrolyte was used to assemble a 2032 button-type symmetrical battery. At the same time, 2 mol L -1 Symmetrical batteries were assembled under the same electrolyte conditions as a control group.

[0045] (4) The obtained button cell was tested by a blue electrochemical test system at a current density of 5 mA cm -2 , deposited 2 mAhcm -2 of metallic zinc.

[0046] The button cell after cycling was disassembled and the electrode sheet was tested by SEM. The results are as follows: Figure 4 As shown in ab. Figure 4 a is the use of 2 mol L -1SEM image of the electrode surface after zinc metal deposition in a symmetrical battery assembled with zinc trifluoromethanesulfonate electrolyte. Figure 4 In b, 2 g L -1 SEM image of the electrode surface after the deposition of metal zinc in a symmetric battery assembled with glutathione additive electrolyte. It can be seen that the zinc flakes are deposited more uniformly and densely after the addition of glutathione additive, avoiding the failure of the battery due to the formation of dendrites piercing the diaphragm.

[0047] Example 5 (1) Preparation of negative electrode sheets. The zinc foil was cut into 12 mm and 16 mm discs, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0048] (2) Prepare 2 mol L -1 of zinc trifluoromethanesulfonate solution, and then add 2 g L -1 The glutathione was uniformly dissolved in the zinc trifluoromethanesulfonate solution by magnetic stirring for 6 h.

[0049] (3) Use zinc sheets as positive and negative electrodes and glass fiber as separator. Add 200 μL of 2 g L -1 Glutathione electrolyte was used to assemble a 2032 button-type symmetrical battery. At the same time, 2 mol L -1 Symmetrical batteries were assembled under the same electrolyte conditions as a control group.

[0050] (4) The obtained button cell was tested by the Blue Electric electrochemical test system at 2 mA cm -2 Pre-deposited at a current density of 6 mAh cm -2 of metallic zinc.

[0051] The button cell after zinc deposition was disassembled, and the electrode sheet was tested by SEM to observe the deposition morphology of the cross section. The results are as follows: Figure 5 As shown in ab, Figure 5 a is the addition of 2 mol L -1 SEM image of the electrode cross section after deposition of a symmetrical battery assembled with zinc trifluoromethanesulfonate electrolyte. Figure 5 In b, 2 g L -1 SEM image of the electrode cross section after deposition of a symmetric battery assembled with glutathione additive. It can be seen from the figure that after adding glutathione additive, in the zinc trifluoromethanesulfonate electrolyte, the surface of the zinc negative electrode presents a rough surface composed of irregular clusters, while in the electrolyte containing 2 g L -1 In the glutathione additive electrolyte, the surface of the zinc negative electrode showed a dense morphology, confirming that the addition of glutathione additive can significantly inhibit the formation of dendrites.

[0052] Example 6 (1) Preparation of positive electrode sheets. The positive electrode was uniformly mixed according to the mass ratio of commercial V2O5 / conductive carbon black / PVDF = 7:2:1, coated on a stainless steel mesh, and the sample was placed in an oven at 80°C for 12 h before being cut into sheets with a diameter of 12 mm.

[0053] (2) Preparation of negative electrode sheet. The zinc foil was cut into discs with a diameter of 16 mm, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0054] (3) Prepare 2 mol L -1 of zinc trifluoromethanesulfonate solution, and then add 2 g L -1 The glutathione was uniformly dissolved in the zinc trifluoromethanesulfonate solution by magnetic stirring for 6 h.

[0055] (4) Use 12 mm V2O5 as the positive electrode, 16 mm zinc sheet as the negative electrode, and glass fiber as the separator. Add 130 uL of 2 g L -1 Glutathione electrolyte was used to assemble a 2032 button-type full battery. At the same time, 2 molL -1 The full battery was assembled under the same electrolyte conditions as the control group.

[0056] (5) The obtained button cell was tested by the Blue Electric electrochemical test system with a charge and discharge cut-off voltage range of 0.3-1.6 V and a current density of 5 A g -1 Perform a cycle test.

[0057] The electrochemical performance of the full battery under long-term cycling after adding glutathione as an additive to the electrolyte was observed to test the practical application prospects of glutathione. Figure 6 As shown in the figure, it can be seen that at 5 A g -1 Use 2 g L -1 The full battery assembled with glutathione zinc ion electrolyte still maintains 296 mAhg after 2000 charge and discharge cycles. -1 The discharge capacity of the control sample decreases rapidly with time, and decays to 82 mAh g after only 470 charge and discharge cycles. -1 This indicates that in the control sample, as the cycle progresses, the discharge capacity decreases rapidly due to gas accumulation and dendrites detaching from the roots and dissociating into the electrolyte.

[0058] Example 7 (1) Preparation of positive electrode sheets. The positive electrode was uniformly mixed according to the mass ratio of commercial V2O5 / conductive carbon black / PVDF = 7:2:1, coated on a stainless steel mesh, and the sample was placed in an oven at 80°C for 12 h before being cut into sheets with a diameter of 12 mm.

[0059] (2) Preparation of negative electrode sheet. The zinc foil was cut into discs with a diameter of 16 mm, and then the discs were ultrasonically cleaned with deionized water and anhydrous ethanol for 3 times, each time for 10 min, and then placed in an oven to dry for 1 h to obtain zinc electrode sheets.

[0060] (3) Prepare 2 mol L -1 of zinc trifluoromethanesulfonate solution, and then add 2 g L -1 The glutathione was added and magnetically stirred for 6 h to make it evenly dissolved in the zinc trifluoromethanesulfonate solution.

[0061] (4) Use 12 mm V2O5 as the positive electrode, 16 mm zinc sheet as the negative electrode, and glass fiber as the separator. Add 130 uL of 2 g L -1 Glutathione electrolyte was used to assemble a 2032 button-type full battery. At the same time, 2 molL -1 The full battery was assembled under the same electrolyte conditions as the control group.

[0062] (5) The button cell was subjected to rate charge and discharge test using the Blue Electric electrochemical test system. The cycle conditions were first 0.2 A g -1 After activation at a current density of 0.5 A g -1 , 1.0 A g -1 , 2.0 A g -1 , 3.0 A g -1 , 4.0 A g -1 , 5.0A g -1 After 10 cycles at each current density, the -1 The current density was 1.34 W / m and the cycle was continued for 50 cycles.

[0063] The results are as follows Figure 7 The indicated use contained 2 g L -1 The discharge specific capacity of aqueous zinc-ion batteries using glutathione zinc-ion electrolyte at different current densities is significantly higher than that of aqueous zinc-ion batteries using zinc-ion electrolyte without additives, and when the current density increases from 5.0 A g -1 Reduced to 0.5 A g -1 It still maintains a high discharge specific capacity and good cycle stability, indicating that the test electrolyte has excellent rate performance.

[0064] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An aqueous zinc ion electrolyte modified by an additive, characterized in that: The invention comprises an electrolyte and an additive, wherein the electrolyte is a soluble zinc salt and the additive is glutathione.

2. The aqueous zinc ion electrolyte modified by an additive according to claim 1, characterized in that: The soluble zinc salt is one or more of zinc sulfate, zinc trifluoromethanesulfonate, zinc perchlorate and zinc nitrate.

3. The aqueous zinc ion electrolyte modified by an additive according to claim 2, characterized in that: The soluble zinc salt is zinc trifluoromethanesulfonate.

4. The aqueous zinc ion electrolyte modified by an additive according to claim 1, characterized in that: The concentration of the soluble zinc salt is 1-3 mol L -1 .

5. The aqueous zinc ion electrolyte modified by an additive according to claim 4, characterized in that: The concentration of the electrolyte is 2 mol L -1 .

6. The aqueous zinc ion electrolyte modified by an additive according to claim 1, characterized in that: The concentration of the additive is 0.5-4 g L -1 .

7. The aqueous zinc ion electrolyte modified by an additive according to claim 6, characterized in that: The concentration of the additive was 2 g L -1 .

8. Application of an additive-modified aqueous zinc ion electrolyte in a zinc ion battery, characterized in that: The zinc ion battery comprises a positive electrode, a separator, a negative electrode and an aqueous zinc ion electrolyte modified by additives.

9. The use of an additive-modified aqueous zinc ion electrolyte in a zinc ion battery according to claim 8, characterized in that: The positive electrode material is vanadium pentoxide, manganese dioxide, sodium vanadate or lithium manganate, the diaphragm is a glass fiber diaphragm, and the negative electrode material is zinc powder, zinc foil or foamed zinc.

10. The use of an additive-modified aqueous zinc ion electrolyte in a zinc ion battery according to claim 8, characterized in that: The aqueous zinc ion battery electrolyte can prolong the cycle life of the battery at both low current density and high current density, and improve the cycle stability of the battery.