Method of manufacturing patterned film and electroluminescent device and display device including patterned film
By using polythiol compound additives and radiation treatment in semiconductor nanoparticle films, the problems of optical property loss and insufficient resolution in the patterning process of existing technologies are solved, achieving efficient and stable patterning effects suitable for electronic devices and display devices.
Patent Information
- Application Number
- CN202410468063.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-06-14
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-22
AI Technical Summary
Existing techniques for patterning semiconductor nanoparticle films often result in the loss of optical properties and insufficient pattern resolution, especially when using photolithography processes, where polymer swelling and capillary forces can affect the uniformity and accuracy of the pattern.
By combining additives containing polythiol compounds with semiconductor nanoparticles and altering their solubility through radiation treatment, a patterned film is formed. Photocatalysis is then used to promote the reaction between organic ligands and additives, forming stable thiol-carbon crosslinks, thus avoiding the use of polymers.
It enables the formation of high-resolution patterned films without compromising the optical properties of semiconductor nanoparticles, thereby improving the precision of the pattern and optical efficiency, while maintaining or enhancing quantum efficiency and optical stability.
Smart Images

Figure CN118829329A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the priority of Application Nos. 10-2023-0051499 and 10-2023-0076415 filed on April 19, 2023 and June 14, 2023, respectively, in the Korean Intellectual Property Office, and all rights arising therefrom, the contents of both of which are incorporated herein by reference in their entirety. Technical Field
[0003] The present disclosure relates to a method of patterning a semiconductor nanocrystal film, and an electroluminescent device and a display apparatus including the patterned semiconductor nanocrystal film. Background Art
[0004] Semiconductor nanoparticles (e.g., semiconductor nanocrystal particles) can emit light. For example, quantum dots comprising semiconductor nanocrystals can exhibit quantum confinement effects, showing, for example, luminescent properties. For example, when electrons in an excited state are moved (e.g., transitioned) from a conduction band to a valence band by light excitation or by applying a voltage, light emission of semiconductor nanoparticles can be generated. By controlling the size, composition, or combination thereof of semiconductor nanoparticles, semiconductor nanoparticles can be configured to emit light in a desired wavelength region.
[0005] Semiconductor nanoparticles may find application in electronic or electro-optical devices (eg, display devices or sensors), and for such applications, it is desirable to develop techniques for patterning semiconductor nanoparticle-based films. Summary of the invention
[0006] Provided are methods of making a patterned film including semiconductor nanoparticles and patterned films made therefrom.
[0007] An electronic device (eg, an electroluminescent device) comprises the patterned film including the semiconductor nanoparticles.
[0008] A display device, such as a quantum dot light emitting diode ("QD-LED") display, includes the patterned film.
[0009] A method of manufacturing a patterned film (e.g., a patterned semiconductor nanocrystal film) having a first region configured to emit a first light includes:
[0010] forming a first film comprising semiconductor nanoparticles and an additive, wherein the additive comprises a polythiol compound comprising at least two thiol groups and the semiconductor nanoparticles are configured to emit a first light, the semiconductor nanoparticles comprise an organic ligand (e.g., on a surface thereof), and the organic ligand comprises a first functional group and a carbon-carbon unsaturated bond bonded to a surface of the semiconductor nanoparticle;
[0011] exposing a portion of the first film corresponding to the first region to radiation to induce a change in the solubility of the semiconductor nanoparticles in the exposed area relative to the first solvent to form a radiation-treated film;
[0012] The radiation treated film is contacted with a first solvent to remove at least a portion of the unexposed area of the radiation treated film to obtain a patterned film having a first region.
[0013] In the method, the semiconductor nanoparticles may be configured to act as (or be usable as) a photocatalyst for a reaction between the organic ligand and the polythiol compound.
[0014] The polythiol compound may include a dithiol compound, a trithiol compound, a tetrathiol compound, or a combination thereof.
[0015] The polythiol compound may have a molecular weight of about 10 g / mol to about 5,000,000 g / mol, about 50 g / mol to about 300,000 g / mol, about 500 g / mol to about 100,000 g / mol, or about 1000 g / mol to about 50,000 g / mol.
[0016] The polythiol compound may include -O-, -CO-, -COO-, -NR-, -CONR- (R in -NR- and -CONR- is independently hydrogen or a C1 to C10 hydrocarbon group), a substituted or unsubstituted C1 to C20 alkylene group, a substituted or unsubstituted C2 to C20 alkenylene group, a substituted or unsubstituted C2 to C20 alkynylene group, or a combination thereof (e.g., a moiety formed by connecting at least two of the foregoing groups).
[0017] The polythiol compound may include a central portion and at least one (e.g., at least two) HS-R-* (wherein R is a substituted or unsubstituted C1 to C30 aliphatic hydrocarbon group or a substituted or unsubstituted C1 (or C2) to C30 aliphatic hydrocarbon group in which at least one methylene group is replaced by a sulfonyl group, a carbonyl group, an ether, a sulfide, a sulfoxide, an ester, an amide, or a combination thereof), and the central portion may include a carbon atom, a substituted or unsubstituted C1 to C30 aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 alicyclic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a substituted or unsubstituted C3 to C30 heteroarylene group, a substituted or unsubstituted C3 to C30 heterocyclic group, or a combination thereof.
[0018] The polythiol compound may include a dimercaptoacetate compound, a trimercaptoacetate compound, a tetramercaptoacetate compound, a dimercaptopropionate compound, a trimercaptopropionate compound, a tetramercaptopropionate compound, an isocyanate compound including two or more mercaptoalkylcarbonyloxyalkyl groups, an isocyanurate compound including two or more mercaptoalkylcarbonyloxyalkyl groups, or a combination thereof.
[0019] The semiconductor nanoparticles may include Group II-VI compounds, Group III-V compounds, Group IV-VI compounds, Group IV elements or their compounds, Group II-III-VI compounds, Group I-III-VI compounds, Group I-II-IV-VI compounds, metal halide perovskite compounds, transition metal chalcogenide perovskite compounds, or combinations thereof.
[0020] The first light may have a red spectrum, a green spectrum, or a blue spectrum.
[0021] The half width of the first light may be greater than or equal to about 1 nanometer (nm) and less than or equal to about 70 nm.
[0022] The first functional group may include a carboxyl group, a thiol group, an amine group, a phosphine group, a phosphine oxide group, an ester group, a hydroxyl group, or a combination thereof.
[0023] The carbon-carbon unsaturated bond may include a carbon-carbon double bond.
[0024] The organic ligand may include a C1 to C50 aliphatic group.
[0025] In the first film or the patterned film, the amount of the semiconductor nanoparticles may be greater than or equal to about 60 weight % to less than or equal to about 99.99 weight %, or greater than or equal to about 70 weight % to less than or equal to about 95 weight %, based on the total weight of the first film or the patterned film.
[0026] The amount of the additive in the first film may be greater than or equal to about 0.01 wt % to less than or equal to about 40 wt %, or greater than or equal to about 5 wt % to less than or equal to about 30 wt %, based on the total weight of the first film.
[0027] The first film may further include or may not substantially include a polymerizable monomer. The amount of the polymerizable monomer in the first film may be less than or equal to about 5 wt %, less than or equal to about 3 wt %, or less than or equal to about 1 wt %, based on the total weight of the first film.
[0028] The polymerizable monomer may be a (meth)acrylic monomer including two or more carbon-carbon double bonds, a (meth)acrylic oligomer including a carbon-carbon double bond, a vinyl monomer, or a combination thereof.
[0029] The first film may or may not include an organic compound containing two or more azide groups; an organic polymer having an acid value of greater than or equal to about 50 mg KOH / gram of organic polymer and soluble in an alkaline aqueous solution; an organic compound containing an oxetane group and an aromatic hydrocarbon group; or a combination thereof.
[0030] The radiation may have an energy greater than a band gap energy of the semiconductor nanoparticles.
[0031] The radiation may be light having a peak emission wavelength of greater than or equal to about 150 nanometers (nm), greater than or equal to about 200 nm, greater than or equal to about 250 nm, greater than or equal to about 300 nm, greater than or equal to about 400 nm, greater than or equal to about 480 nm, greater than or equal to about 510 nm, or greater than or equal to about 580 nm, to less than or equal to about 600 nm, less than or equal to about 560 nm, less than or equal to about 500 nm, less than or equal to about 450 nm, or less than or equal to about 390 nm.
[0032] The radiation dose to the first film may be greater than or equal to about 0.1 mJ / cm 2 ), greater than or equal to about 10 mJ / cm 2 , to less than or equal to about 5000 mJ / cm 2 , less than or equal to about 1000mJ / cm 2 , less than or equal to about 500mJ / cm 2 , less than or equal to about 400mJ / cm 2 , or less than or equal to about 50 mJ / cm 2 .
[0033] The first solvent may include an organic solvent capable of dispersing (or configured to disperse) the semiconductor nanoparticles, particularly the semiconductor nanoparticles in the unexposed regions of the radiation-treated film. The organic solvent may be a polar solvent.
[0034] The organic solvent may include or may be a non-polar solvent.The change in solubility of the semiconductor nanoparticles in the exposed area of the radiation treated film to the first solvent may allow the semiconductor nanoparticles to have resistance (solubility or dispersibility) to the first solvent.
[0035] The patterned film may have a relative luminous efficiency of greater than or equal to about 70%, greater than or equal to about 75%, greater than or equal to about 80%, greater than or equal to about 90%, greater than or equal to about 100%, greater than or equal to about 103%, greater than or equal to about 106%, greater than or equal to about 108%, greater than or equal to about 110%, or greater than or equal to about 115% and less than or equal to about 200%, less than or equal to about 150%, less than or equal to about 130%, less than or equal to about 120%, less than or equal to about 110%, less than or equal to about 105%, wherein the relative luminous efficiency is defined as follows:
[0036] Relative luminous efficiency (%) = [A / B] x 100
[0037] A: Quantum efficiency of the patterned film
[0038] B: Quantum efficiency of a film comprising the semiconductor nanoparticles without the additive.
[0039] The luminous efficiency of the patterned film may be greater than or equal to the luminous efficiency of the semiconductor nanoparticles dispersed in a solution.
[0040] In an embodiment, an electroluminescent device includes: a first electrode and a second electrode (eg, facing each other); and a light-emitting layer disposed between the first electrode and the second electrode.
[0041] The light-emitting layer includes a patterned film, the patterned film includes a first region configured to emit a first light, the first region includes semiconductor nanoparticles and a portion containing carbon-sulfur bonds, and the semiconductor nanoparticles are configured to emit the first light and exhibit dissolution resistance to a (predetermined) first solvent.
[0042] The electroluminescent device may further include a hole transport layer disposed between the light-emitting layer and the first electrode.
[0043] The hole transport layer may include a hole transport material and may not include the semiconductor nanoparticles.
[0044] The light-emitting layer can be prepared by the method described herein.
[0045] The electroluminescent device may include a first pixel and a second pixel, and the first region may be disposed to correspond to the first pixel.
[0046] The first solvent may include a non-polar solvent.
[0047] The first solvent may include toluene, octane, hexane, chlorobenzene, dichlorobenzene, chloroform, xylene, or a combination thereof.
[0048] The first solvent may include dimethylformamide, γ-butyrolactone, N-methylpyrrolidone, dimethyl sulfoxide, ethylene dichloride, trichloroethylene, chloroform, chlorobenzene, dichlorobenzene, styrene, xylene, toluene, cyclohexene, or a combination thereof.
[0049] In the light emitting layer, two or more semiconductor nanoparticles may be connected through a portion containing a carbon-sulfur bond.
[0050] In the light-emitting layer, the carbon content may be greater than or equal to about 1 wt % to less than or equal to about 50 wt %, greater than or equal to about 10 wt % to less than or equal to about 30 wt %, or greater than or equal to about 15 wt % to less than or equal to about 25 wt %, based on the total weight of the light-emitting layer.
[0051] The light emitting layer may not include a chemical species formed by a reaction between an azide group and an alkyl group.
[0052] The light emitting layer may not include an organic polymer having an acid value of 50 mg KOH / gram of the organic polymer or more and being soluble in a basic aqueous solution.
[0053] The electroluminescent device may further include an electron transport layer between the light emitting layer and the second electrode, and the electron transport layer may include zinc oxide nanoparticles.
[0054] The semiconductor nanoparticles in the light-emitting layer may include Group II-VI compounds, Group III-V compounds, Group IV-VI compounds, Group IV elements or their compounds, Group II-III-VI compounds, Group I-III-VI compounds, Group I-II-IV-VI compounds, metal halide perovskite compounds, transition metal chalcogenide perovskite compounds, or combinations thereof.
[0055] The first light may have a red spectrum, a green spectrum, or a blue spectrum.
[0056] In an embodiment, a display device includes a first pixel and a second pixel, wherein the display device includes the electroluminescent device, and the first region is arranged to correspond to the first pixel of the electroluminescent device.
[0057] The display device may include a portable terminal device, a monitor, a laptop computer, a television, an electronic display, a camera, or an electronic component (eg, an electronic component of an electric vehicle).
[0058] According to the embodiment, a patterned film including semiconductor nanoparticles having improved optical properties (e.g., luminous efficiency) can be obtained. The patterned film based on semiconductor nanoparticles can exhibit improved organic solvent resistance, and it can be advantageously used in a variety of devices (e.g., display devices, sensors, etc.) involving complex patterns of semiconductor nanoparticles. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The above and other advantages and features of the present disclosure will become more apparent by further describing exemplary embodiments of the present disclosure in detail with reference to the accompanying drawings, in which:
[0060] Figure 1A is a flow chart of a patterning method according to an embodiment;
[0061] Figure 1B is a diagram schematically illustrating a method of patterning a semiconductor nanocrystal film according to an embodiment;
[0062] Figure 1C is a diagram schematically illustrating a patterned film having more than one light emitting region;
[0063] Figure 2A is a diagram schematically illustrating ligand cross-linking via a photocatalytic reaction in a patterning method of an embodiment;
[0064] Figure 2B is a diagram schematically illustrating passivation of the surface of a semiconductor nanocrystal by an additive in a patterning method of an embodiment;
[0065] Figure 2C is a diagram illustrating an energy scheme for photocatalysis of semiconductor nanoparticles in a patterning method of an embodiment;
[0066] Figure 2D is a diagram illustrating a reaction scheme between an additive and a ligand in a patterning method of an embodiment;
[0067] Figure 3A is a schematic cross-sectional view of one embodiment of an electroluminescent device;
[0068] Figure 3B is a schematic cross-sectional view of another embodiment of an electroluminescent device;
[0069] Figure 3Cis a schematic cross-sectional view of yet another embodiment of an electroluminescent device;
[0070] Figure 4A and Figure 4B is a top view of a patterned film based on perovskite semiconductor nanocrystals prepared in Example 1;
[0071] Figure 5 is a top view of a patterned film based on cadmium selenide semiconductor nanocrystals prepared in Example 2;
[0072] Figure 6 is the PLQY (percentage, %) versus UV dose (joules / square centimeter, J / cm 2 ) showing the results of Evaluation Example 4 (photostability test);
[0073] Figure 7 is the reciprocal of the intensity (in arbitrary units, au) versus the Raman shift (in centimeters, cm -1 ) shows the results of Raman spectroscopy analysis in Evaluation Example 1;
[0074] Figure 8 is a graph of intensity (arbitrary units, au) versus binding energy (electron volts, eV), illustrating the results of X-ray photoelectron spectroscopy (XPS) analysis in Evaluation Example 1;
[0075] Fig. 9 is a graph of photoluminescence (PL) intensity (arbitrary units, au) versus time (nanoseconds, ns), showing the results of the time-resolved photoluminescence (TRPL) analysis in Evaluation Example 1; and
[0076] Fig.10 This is a diagram showing a top view image of a pattern formed in Example 4. DETAILED DESCRIPTION
[0077] Hereinafter, exemplary embodiments of the present disclosure will be described in detail so that those skilled in the art will understand the present disclosure. However, the present disclosure may be embodied in many different forms and is not to be construed as being limited to the exemplary embodiments set forth herein.
[0078] In the accompanying drawings, the thickness of layers, films, panels, regions, etc., is exaggerated for clarity. The same reference numerals denote the same elements throughout the specification. It will be understood that when an element (e.g., a layer, film, region, or substrate) is referred to as being "on" another element, it may be directly on the other element, or there may be intervening elements. Conversely, when an element is referred to as being "directly on" another element, there are no intervening elements.
[0079] It will be further understood that the terms “comprising” or “including” when used in this specification indicate the presence of the described features, regions, wholes, steps, operations, elements and / or components (components), but do not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components (components) and / or collections thereof.
[0080] As used herein, the term "cross-sectional view" means a view observed when a given object is cut (e.g., substantially perpendicular to the bottom surface). As used herein, the term "top view" means a view obtained when a given object is observed from above (e.g., directly above).
[0081] The terms used herein are only used for the purpose of describing specific embodiments, and are not intended to be restrictive. As used herein, the singular forms "one (kind) (indefinite articles, a, an)" and "said (the)" are intended to include plural forms, including "at least one (kind)", unless the content clearly states otherwise. Therefore, in the claims, mentioning an element and then mentioning "said (the)" element includes one (kind) element and multiple (kind) elements. In addition, for example, the word "nanoparticle" can refer to a single nanoparticle or multiple nanoparticles. "At least one (kind)" is not interpreted as limiting "one (kind) (indefinite articles, a, an)". "Or" means "and / or". As used herein, the term "and / or" includes any and all combinations of one or more of the relevant listed items.
[0082] It will be understood that although the terms "first", "second", "third", etc. can be used herein to describe various elements (elements), components (components), regions, layers and / or parts, these elements (elements), components (components), regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish an element (element), component (component), region, layer or part from another element (element), component (component), region, layer or part. Therefore, the "first element (element)", "component (component)", "region", "layer" or "part" discussed below can be referred to as the second element (element), component (component), region, layer or part, without departing from the teaching of this article.
[0083] As used herein, "about" is inclusive of the stated value and means within an acceptable range of deviation for a particular value determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" may mean within one or more standard deviations of the stated value, or within ±10%, 5%, 3%, or 1%.
[0084] Relative terms such as "downward," "lower," or "bottom" and "upward," "upper," or "top" may be used herein to describe the relationship of one element to another element as illustrated in the figures. It will be understood that the relative terms are intended to encompass different orientations of the device in addition to the orientation depicted in the figures. For example, if the device in one of the figures is turned over, then elements described as being on the "lower" side of the other elements would be positioned on the "upper" side of the other elements. Thus, the exemplary term "lower" may encompass both "lower" and "upper" orientations, depending on the specific orientation of the figure.
[0085] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It will be further understood that terms (such as those defined in commonly used dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the present disclosure and the relevant art, and will not be interpreted in an idealized or overly formal sense unless explicitly defined as such in this article.
[0086] Exemplary embodiments are described herein with reference to cross-sectional views (which are schematic diagrams of idealized embodiments). Thus, variations in the shapes of the diagrams due to, for example, manufacturing techniques and / or tolerances are expected. Therefore, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as illustrated herein, but rather include deviations in shape, for example, caused by manufacturing. For example, a region illustrated or described as flat may typically have rough and / or nonlinear features. In addition, the illustrated sharp angles may be rounded. Therefore, the regions illustrated in the figures are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions and are not intended to limit the scope of the claims of the present invention.
[0087] As used herein, the values of work functions, conduction bands, or lowest unoccupied molecular orbitals ("LUMO") (or valence bands or highest occupied molecular orbitals ("HOMO")) energy levels are expressed as absolute values from the vacuum energy level. In addition, when a work function or energy level is referred to as "deep," "high," or "large," the work function or energy level has a large absolute value of "0 electron volts (eV)" based on the vacuum energy level, and when a work function or energy level is referred to as "shallow," "low," or "small," the work function or energy level has a small absolute value of "0 eV" based on the vacuum energy level. In one aspect, the work function herein refers to the minimum energy to move an electron from, for example, a solid metal (e.g., a metal surface) to a vacuum (e.g., just outside the solid surface).
[0088] As used herein, when no definition is otherwise provided, "substituted" means that the hydrogen of a compound, group or part is replaced by a C1 to C30 alkyl group, a C2 to C30 alkenyl group, a C2 to C30 alkynyl group, a C2 to C30 epoxy group, a C2 to C30 alkyl ester group, a C3 to C30 alkenyl ester group (e.g., an acrylate group, a methacrylate group), a C6 to C30 aryl group, a C7 to C30 alkylaryl group, group, a C1 to C30 alkoxy group, a C1 to C30 heteroalkyl group, a C3 to C40 heteroaryl group, a C3 to C30 heteroarylalkyl group, a C3 to C30 heteroalkylaryl group, a C3 to C30 cycloalkyl group, a C3 to C15 cycloalkenyl group, a C6 to C30 cycloalkynyl group, a C2 to C30 heterocycloalkyl group, a halogen (—F, —Cl, —Br or —I), a hydroxyl group (—OH), a nitro group (—NO 2 ), thiocyanate group (-SCN), cyano group (-CN), amino group (-NRR', wherein R and R' are independently hydrogen or a C1 to C6 alkyl group), azide group (-N 3 ), amidino group (-C(=NH)NH 2 ), hydrazino group (-NHNH 2 ), hydrazono group (=N(NH 2 )), aldehyde group (-C(=O)H), carbamoyl group (-C(O)NH 2 ), a thiol group (-SH), an ester group (-C(=O)OR, wherein R is a C1 to C6 alkyl group or a C6 to C12 aryl group), a carboxyl group (-COOH) or a salt thereof (-C(=O)OM, wherein M is an organic or inorganic cation), a sulfonic acid group (-SO 3 H) or its salt (-SO 3 M, where M is an organic or inorganic cation), a phosphate group (-PO 3 H 2 ) or its salt (-PO 3 MH or -PO 3 M 2 , wherein M is an organic or inorganic cation), or a combination thereof.
[0089] As used herein, when no definition is provided separately, "hydrocarbon" or "hydrocarbon group" refers to a compound or group (e.g., an alkyl, alkenyl, alkynyl, or aryl group) comprising carbon and hydrogen. A hydrocarbon group may be a monovalent group formed by removing one or more hydrogen atoms from an alkane, alkene, alkyne, or aromatic hydrocarbon or a group having a valence greater than one. In a hydrocarbon or hydrocarbon group, a methylene group, such as at least one methylene group, may be substituted by an oxygen moiety, a carbonyl moiety, an ester moiety, -NH-, or a combination thereof. Unless otherwise specified to the contrary, a hydrocarbon or hydrocarbon group (alkyl, alkenyl, alkynyl, or aryl) may have 1 to 60, 2 to 32, 3 to 24, or 4 to 12 carbon atoms.
[0090] As used herein, when no definition is otherwise provided, "alkyl" refers to a linear or branched saturated monovalent hydrocarbon group (methyl, ethyl, hexyl, etc.). In embodiments, the alkyl group may have 1 to 50 carbon atoms, or 2 to 18 carbon atoms, or 3 to 12 carbon atoms.
[0091] As used herein, when no definition is otherwise provided, "alkylene" refers to a linear or branched saturated polyvalent (e.g., divalent) hydrocarbon group (methylene, ethylene, hexylene, etc.). The alkylene group can have 1 to 50 carbon atoms, or 2 to 18 carbon atoms, or 3 to 12 carbon atoms.
[0092] As used herein, when not otherwise defined, "alkenyl" refers to a linear or branched monovalent hydrocarbon group having a carbon-carbon double bond. In embodiments, the alkenyl group may have 2 to 50 carbon atoms, or 3 to 18 carbon atoms, or 4 to 12 carbon atoms.
[0093] As used herein, when not otherwise defined, "alkenylene" refers to a linear or branched polyvalent (e.g., divalent) hydrocarbon group having a carbon-carbon double bond. The alkenylene group may have 2 to 50 carbon atoms, or 3 to 18 carbon atoms, or 4 to 12 carbon atoms.
[0094] As used herein, when not otherwise defined, "alkynyl" refers to a linear or branched monovalent hydrocarbon group having a carbon-carbon triple bond. In embodiments, an alkynyl group may have 2 to 50 carbon atoms, or 2 to 18 carbon atoms, or 2 to 12 carbon atoms.
[0095] As used herein, when no definition is provided otherwise, "alkynylene" refers to a linear or branched polyvalent (e.g., divalent) hydrocarbon group having a carbon-carbon triple bond. An alkynylene group can have 2 to 50 carbon atoms, or 2 to 18 carbon atoms, or 2 to 12 carbon atoms.
[0096] As used herein, when no definition is provided separately, "aryl" and "arylene" refer to monovalent and polyvalent (e.g., divalent) groups having a carbocyclic aromatic system, respectively. When an aryl or arylene group includes multiple rings, the multiple rings may be fused to each other. Examples of aryl include phenyl groups and naphthyl groups. Examples of arylene include phenylene groups, biphenylene groups, and naphthylene groups. In embodiments, an aryl or arylene group may have 6 to 50 carbon atoms, or 6 to 18 carbon atoms, or 6 to 12 carbon atoms.
[0097] As used herein, when no definition is otherwise provided, "hetero" means including 1 to 3 heteroatoms, for example, N, O, P, Si, B, Se, Ge, Te, S or combinations thereof.
[0098] As used herein, when no definition is provided separately, "heteroaryl" and "heteroarylidene" refer to monovalent and polyvalent (e.g., divalent) cyclic aromatic systems having heteroatoms such as N, O, P, Si, B, Se, Ge, Te, S or combinations thereof as ring atoms. When a heteroaryl or heteroarylidene group includes multiple rings, the multiple rings may be fused to each other. In an embodiment, a heteroaryl or heteroarylidene group may have 3 to 50 carbon atoms, or 6 to 18 carbon atoms, or 6 to 12 carbon atoms. Examples of heteroaryl groups include pyridyl groups, pyrimidyl groups, pyrazinyl groups, pyridazinyl groups, triazinyl groups, quinolyl groups, and isoquinolyl groups.
[0099] As used herein, when a definition is not otherwise provided, "alkoxy" refers to an alkyl group linked to oxygen (eg, alkyl-O-), such as a methoxy group, an ethoxy group, or a sec-butoxy group.
[0100] As used herein, when no definition is otherwise provided, "amine" is an amine composed of NR 3 A compound represented by wherein each R is independently hydrogen, a C1-C12 alkyl group, a C7-C20 alkylaryl group, a C7-C20 arylalkyl group or a C6-C18 aryl group.
[0101] As used herein, the term "peak emission wavelength" is the wavelength at which a given emission spectrum of light reaches its maximum.
[0102] As used herein, the expression "does not include cadmium (or other hazardous heavy metals)" means that the concentration of cadmium (or other heavy metals considered hazardous) may be less than or equal to about 100 parts per million by weight ("ppmw"), less than or equal to about 50 ppmw, less than or equal to about 10 ppmw, less than or equal to about 1 ppmw, less than or equal to about 0.1 ppmw, less than or equal to about 0.01 ppmw, or zero. In embodiments, cadmium (or other toxic heavy metals) may be substantially absent, or, if present, the amount of cadmium (or other heavy metals) may be less than or equal to the detection limit of a given analytical tool (e.g., an inductively coupled plasma atomic emission spectrometry instrument) or as an impurity level thereof.
[0103] Unless stated to the contrary, the numerical ranges recited herein are inclusive (including the endpoints).
[0104] Unless otherwise mentioned, the numerical ranges recited herein include any real number within and including the endpoints of the ranges described. In this specification, numerical endpoints or upper or lower values (e.g., listed as "greater than or equal to a value," "at least a value," or "less than or equal to a value," or listed as "from" or "to") can be used to form numerical ranges for a given feature. In other words, the upper and lower endpoints stated for various numerical values can be independently combined to provide a range.
[0105] As used herein, the term "group" may refer to a group of the periodic table of elements.
[0106] As used herein, “Group I” refers to Group IA and Group IB, and examples may include Li, Na, K, Rb, and Cs, but are not limited thereto.
[0107] As used herein, “Group II” refers to Group IIA and Group IIB, and examples of Group II metals may be Cd, Zn, Hg, and Mg, but are not limited thereto.
[0108] As used herein, “Group III” refers to Group IIIA and Group IIIB, and examples of Group IIIA metals may be Al, In, Ga, and Tl, and examples of Group IIIB may be scandium, yttrium, etc., but are not limited thereto.
[0109] As used herein, “Group IV” refers to Group IVA and Group IVB, and examples of Group IVA metals may be Si, Ge, and Sn, and examples of Group IVB metals may be titanium, zirconium, hafnium, etc., but are not limited thereto.
[0110] As used herein, "Group V" includes Group VA and includes nitrogen, phosphorus, arsenic, antimony, and bismuth, but is not limited thereto.
[0111] As used herein, "Group VI" includes Group VIA and includes sulfur, selenium, and tellurium, but is not limited thereto.
[0112] As used herein, "metal" includes semi-metals such as Si.
[0113] As used herein, nanoparticle is a structure having (e.g., at least one) a region or characteristic size of nanometer scale size. In embodiments, the size (or average size) of the nanostructure is less than or equal to about 500 nanometers (nm), less than or equal to about 300 nm, less than or equal to about 250 nm, less than or equal to about 150 nm, less than or equal to about 100 nm, less than or equal to about 50 nm, or less than or equal to about 30 nm, and may be greater than about 0.1 nm or greater than or equal to about 1 nm.
[0114] The nanoparticles may have any suitable shape.
[0115] Nanoparticles (e.g., semiconductor nanoparticles or metal oxide nanoparticles) may include nanowires, nanorods, nanotubes, branched nanostructures, nanotetrapods, nanotripods, nanobipods, nanodots, multi-pod shapes (e.g., at least two legs), etc., and are not limited thereto. The nanoparticles may be, for example, substantially crystalline or crystalline, substantially single crystalline or single crystalline, polycrystalline, (e.g., at least partially) amorphous, or a combination thereof.
[0116] Semiconductor nanoparticles such as quantum dots can be a type of nanostructure and can show quantum confinement or exciton confinement. As used herein, the term "quantum dot" or "semiconductor nanostructure" is not limited in its shape unless otherwise defined. Semiconductor nanoparticles or quantum dots can have a size less than the Bohr excitation diameter of a bulk (bulk) crystalline material with the same composition, and can show a quantum confinement effect.
[0117] Quantum dot or semiconductor nanoparticles include semiconductor nanocrystals that act as emission centers, and can be configured to emit light of desired wavelengths depending on the size and / or composition of the semiconductor nanocrystals. The emission center may or may not include a dopant. The presence of a dopant may not substantially affect the peak emission wavelength of the semiconductor nanocrystal, and the variation of the emission wavelength according to the presence of the dopant may be less than or equal to about 10nm, less than or equal to about 7nm, less than or equal to about 5nm, less than or equal to about 3nm, less than or equal to about 1nm, less than or equal to about 0.5nm, or about 0nm.
[0118] As used herein, the term quantum efficiency can be used interchangeably with the term quantum yield. Quantum efficiency can be relative quantum yield or absolute quantum yield, which can be easily measured by any suitable (e.g., commercially available) equipment. Quantum efficiency (or quantum yield) can be measured in solution state or solid state (with complex). As used herein, "quantum yield (or quantum efficiency)" can be the ratio of photons emitted (e.g., by nanostructures or nanostructure groups) relative to absorbed photons. Quantum efficiency can be measured by any suitable method. For example, there can be two methods for measuring fluorescence quantum yield or efficiency: absolute method and relative method.
[0119] The absolute method directly obtains the quantum yield by detecting all sample fluorescence using an integrating sphere. In the relative method, the fluorescence intensity of a standard sample (e.g., a standard dye) can be compared with the fluorescence intensity of an unknown sample to calculate the quantum yield of the unknown sample. Coumarin 153, coumarin 545, rhodamine 101 inner salt, anthracene, and rhodamine 6G can be used as standard dyes, depending on their photoluminescence ("PL") wavelength, but are not limited thereto.
[0120] The band gap energy of semiconductor nanoparticles can vary depending on the size and / or composition of the nanocrystal. For example, as the size of the semiconductor nanoparticles increases, the band gap energy of the semiconductor nanoparticles can become smaller, for example narrower, and the semiconductor nanoparticles can emit light with an increased emission wavelength, for example. Semiconductor nanocrystals can be used as luminescent materials in a variety of fields (for example, in display devices, energy devices, or bioluminescent devices).
[0121] The application of semiconductor nanoparticles in electronic devices or optoelectronic devices can relate to the process of providing high-resolution patterned film. It can be considered that inkjet printing, photolithography, etc. are used to provide patterned semiconductor nanoparticle film. For example, a photoresist based on organic polymer or organic monomer can be applied on substrate to obtain a film, then the film obtained is selectively exposed to radiation (for example, using a photomask), then the unexposed part is removed by contacting with a developer to obtain a desired pattern (for example, a photopolymer mask pattern, which can be used as a photopolymer mask to form a pattern of semiconductor nanoparticles). However, in such photolithography process, polymer can swell in the presence of a solvent, and along with pattern size reduction, pattern resolution can be impaired, because the capillary force of the dispersion solvent can have an increasingly dominant effect on the pattern shape to the effect of the pre-pattern (pre-pattern) wall of the photopolymer. Therefore, it is desirable to develop a method for manufacturing patterned semiconductor nanoparticle film without using a conventional photoresist based on polymer or monomer of substantial amount (significant amount).
[0122] The photolithography process can often cause significant surface damage to the deposited emissive nanomaterials, and thus can degrade their optical properties such as luminous efficiency or photoluminescence quantum yield. In some cases, luminescent materials (e.g., colloidal perovskite nanocrystal particles) may have unstable surface ligands and weak lattice energy characteristics based on ionic bonds, so during the patterning process, the loss of luminescent properties PLQY may occur. Therefore, it is desirable to develop a patterning method without causing substantial damage (significant damage) to the optical properties of the nanomaterials.
[0123] Method as disclosed herein can meet the technical requirements described above. In particular, the method can be capable of realizing photocatalytic patterning for luminescent nanomaterials (such as semiconductor nanoparticles). In the method, dual-role click chemistry reagents (such as additives) can be used as both cross-linking agents and defect passivators. Without wishing to be bound by theory, during radiation exposure as described herein, the excitons produced by the luminescent nanomaterial can photocatalytically help the formation of thiyl radicals (thiyl radicals), and thus the reaction between the reactive part (such as carbon-carbon double bond) of the additive and the organic ligand as described herein can occur, such as with relatively low radiation doses. Accordingly, the pattern of luminescent nanomaterials (such as the patterned film of luminescent materials) can be obtained, and the pattern obtained can show enhanced properties.
[0124] Methods as described herein can provide patterns (e.g., patterned films) of a variety of luminescent nanomaterials (e.g., semiconductor nanocrystal particles) while reducing or preventing the loss of optical properties of the nanomaterials. The manufactured patterns (e.g., RGB patterns) can be used as light-emitting elements, such as in electronic devices (e.g., photodiodes), displays, or self-luminous electronic devices (e.g., QD-LEDs) that can emit light with or without a light source.
[0125] Thus, the patterning method (or method of manufacturing a patterned film) can provide a film comprising a first region configured to emit a first light. The film may further include a second region configured to emit a second light different from the first light. The film may further include a third region configured to emit a third light different from the first light and the second light. The first light, the second light, and the third light may each independently have a red spectrum, a green spectrum, or a blue spectrum. As used herein, the description of the first light may apply to the second light and the third light, respectively.
[0126] The first light may have a predetermined peak emission wavelength. The half width (of the emission peak) of the first light may be greater than or equal to about 1 nm, greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 15 nm to less than or equal to about 70 nm, less than or equal to about 65 nm, less than or equal to about 60 nm, less than or equal to about 55 nm, less than or equal to about 50 nm, less than or equal to about 45 nm, less than or equal to about 40 nm, less than or equal to about 35 nm, or less than or equal to about 30 nm.
[0127] Embodiments of the patterning method include:
[0128] A first film is formed containing an additive and semiconductor nanoparticles, wherein the additive includes a polythiol compound containing two or more thiol groups, and wherein the semiconductor nanoparticles are configured to emit the first light, and the semiconductor nanoparticles include an organic ligand on a surface thereof, and wherein the organic ligand includes a carbon-carbon unsaturated bond and a first functional group (e.g., Figure 1A S2 in );
[0129] exposing a portion of the first film corresponding to the first region to radiation to change the solubility of the semiconductor nanoparticles in the first region (or in the exposed area) relative to a first solvent (e.g., Figure 1A S3 in );
[0130] The radiation-treated film is contacted with the first solvent (eg, removing the unexposed portion excluding the first region or at least a portion thereof) (eg, Figure 1A S4 in (5) to obtain a patterned film including the first region.
[0131] In the method, the formation of the film may include preparing a coating composition or coating liquid including the semiconductor nanoparticles and the additive S1, and applying the coating composition on a base (substrate) to form a film S2. (See Figure 1A and 1B ).
[0132] The patterning method (or the method for preparing the patterned film) may not involve the use of a photoresist including a polymer or a monomer. The coating composition may not include an electrically insulating (hereinafter referred to as insulating) polymer or its monomer. The insulating properties of the polymer may be a technical limitation in the manufacture of an electroluminescent device, and the density (e.g., number density) of the luminescent material (i.e., semiconductor nanoparticles) may be reduced, for example, in a light-emitting layer. In addition, the low refractive index properties of the polymer may have an adverse effect on the light conversion film or on display applications, for example, by reducing light extraction efficiency or widening the emission angle. In an embodiment, the method may provide a patterned film without using such a polymer, maintaining the optical properties of the nanomaterial (i.e., semiconductor nanoparticles) at a desired level. In the patterning method of the embodiment, the chemical changes in the portion (e.g., the first region) exposed to radiation may result in changes in the solubility properties (e.g., solubility) of the film to the solvent, and a pattern of desired semiconductor nanoparticles may be formed based on the solubility of the changes. Compared with conventional methods involving the use of photoresists, such methods may include fewer process steps and may increase the amount of luminescent materials (semiconductor nanoparticles) in the formed pattern. However, the inventors have found that direct exposure of radiation to a film containing semiconductor nanoparticles can have an adverse effect on the optical properties (e.g., luminous efficiency) of the semiconductor nanoparticles. Without wishing to be bound by any theory, it is believed that radiation can not only affect the properties (e.g., surface properties) of the semiconductor nanoparticles, but also that the photochemical reaction products due to the irradiation can lead to a reduction in the properties of the semiconductor nanoparticles. In the method of the embodiment, radiation can be irradiated to the film as described herein to provide a high-quality (e.g., with a resolution of less than about 10 microns) pattern while maintaining or improving the optical properties of the semiconductor nanoparticles.
[0133] The substrate is not particularly limited and can be appropriately selected considering the final application of the pattern. The substrate may include an insulating material, a conductive (e.g., electrically conductive) material, or a combination thereof. The substrate may include an organic material, an inorganic material, or a combination thereof. In an embodiment, the film pattern manufactured may be included in an electroluminescent device, and the substrate may include an electrode and a charge transport layer, if desired, but is not limited thereto.
[0134] In the method, the semiconductor nanoparticle may include a first semiconductor nanocrystal. The semiconductor nanoparticle may have a core-shell structure. In an embodiment, the semiconductor nanoparticle (or core-shell structure) may include a first semiconductor nanocrystal (or a core including it) and a shell of a second semiconductor nanocrystal disposed on the first semiconductor nanocrystal (or the core) and including a composition different from that of the first semiconductor nanocrystal.
[0135] The semiconductor nanoparticles may have a core-shell structure, and at the interface between the core and the shell, there may or may not be an alloyed intermediate layer. The alloyed intermediate layer may include a homogeneous alloy or may have a concentration gradient. A gradient alloy may have a concentration gradient, wherein the concentration of the element of the shell varies radially (e.g., decreases or increases in the direction toward the core).
[0136] Optionally, the shell may have a composition that varies in the radial direction. The shell may be a multilayer shell comprising two or more layers. In a multilayer shell, two adjacent layers may have compositions that differ from each other. In a multilayer shell, a layer, such as at least one layer, may independently comprise semiconductor nanocrystals having a single composition. In a multilayer shell, a layer, such as at least one layer, may independently have alloyed semiconductor nanocrystals. In a multilayer shell, a layer, such as at least one layer, may have a concentration gradient that varies in the radial direction with respect to the composition of the semiconductor nanocrystals.
[0137] As an example, in a semiconductor nanoparticle with a core-shell structure, the shell material may have a band gap energy greater than (e.g., higher than) the band gap energy of the core. The material of the shell may have a band gap energy less than (e.g., lower than) the band gap energy of the core. In the case of a multilayer shell, the band gap energy of the outermost layer material of the shell may be greater than the band gap energy of the core and the inner layer material of the shell (the layer closer to the core). In the case of a multilayer shell, the semiconductor nanocrystals of each layer may be selected to have an appropriate band gap, thereby effectively showing (e.g., exhibiting) a quantum confinement effect.
[0138] The semiconductor nanoparticles, the first semiconductor nanocrystals and / or the second semiconductor nanocrystals may independently include II-VI compounds, III-V compounds, IV-VI compounds, IV elements (simple substances) or compounds, I-III-VI compounds, II-III-VI compounds, I-II-IV-VI compounds, metal halide perovskite compounds, transition metal chalcogenide perovskite compounds, or combinations thereof. The semiconductor nanoparticles may or may not include harmful heavy metals such as cadmium, lead, mercury, or combinations thereof.
[0139] The II-VI group compound may be: a binary element compound such as ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, MgSe, MgS or a combination thereof; a ternary element compound such as ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, HgZnS, HgZnSe, HgZnTe, MgZnSe, MgZnS or a combination thereof; a quaternary element compound such as HgZnTeS, HgZnSeS, HgZnSeTe, HgZnSTe or a combination thereof; or a combination thereof. The II-VI group compound may further include a group III metal.
[0140] The III-V compound may be a binary element compound such as GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb or a combination thereof; a ternary element compound such as GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb or a combination thereof; a quaternary element compound such as GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs, InAlPSb or a combination thereof; or a combination thereof. The III-V compound may further include a Group II metal (e.g., InZnP).
[0141] The IV-VI group compound may be: a binary element compound such as SnS, SnSe, SnTe, PbS, PbSe, PbTe or a combination thereof; a ternary element compound such as SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe or a combination thereof; a quaternary element compound such as SnPbSSe, SnPbSeTe, SnPbSTe or a combination thereof; or a combination thereof.
[0142] An example of the I-III-VI group compound may be CuInSe 2 、CuInS 2 , CuInGaSe and CuInGaS, but not limited thereto.
[0143] Examples of the Group I-II-IV-VI compound may be CuZnSnSe and CuZnSnS, but are not limited thereto.
[0144] The Group IV element or compound may include: a single element (single substance) such as Si, Ge or a combination thereof; a binary element compound such as SiC, SiGe or a combination thereof; or a combination thereof.
[0145] The metal halide perovskite compound may be represented by Chemical Formula 1:
[0146] Chemical formula 1
[0147] ABX 3
[0148] In Chemical Formula 1, A is an alkali metal, NR4 + 、[CH(NH 2 ) 2 ] + , an organic guanidinium (guanidinium) or a combination thereof, B is a transition metal, a Group IVA metal, an alkaline earth metal, a rare earth metal or a combination thereof. X is at least one halogen selected from F, Cl, Br and I, and R is the same or different and is hydrogen or a C1-C10 alkyl group, such as a methyl group.
[0149] The alkali metal may include Rb, Cs, Fr or a combination thereof. The Group IVA metal may include Ge, Si, Sn, Pb or a combination thereof.
[0150] The metal halide perovskite compound may be CsPbCl 3 、CsPbBr 3 , CsPbI 3 、CsPb(Cl,I) 3 、CsPb(Br,I) 3 、CsPb(Br,Cl) 3 or a combination thereof.
[0151] As used herein, "(Cl, I), (Br, I) or (Br, I)" means that the compound includes two halogens (i.e., Cl and I, Br and I, or Br and Cl), and in the case where the compound includes two halogens (X1, X2), the molar ratio between the two is not particularly limited.
[0152] The transition metal chalcogenide may include a compound represented by Chemical Formula 2:
[0153] Chemical formula 2
[0154] M1M2Cha 3
[0155] In Chemical Formula 2, M1 is Ca, Sr, Ba or a combination thereof,
[0156] M2 is Ti, Zr, Hf or a combination thereof, and
[0157] Cha is S, Se, Te or a combination thereof.
[0158] The transition metal chalcogenide may include: BaZrS 3 , SrZrS 3 、CaZrS 3 、SrTiS 3 、BaTiS 3 or BaZr 1- x Ti x S 3(where x is greater than 0 and less than or equal to about 0.5); BaZrSe 3 、SrZrSe 3 、CaZrSe 3 、SrTiSe 3 、BaTiSe 3 or BaZr 1-x Ti x Se 3 (where x is greater than 0 and less than or equal to about 0.5); BaZrTe 3 、SrZrTe 3 、CaZrTe 3 、SrTiTe 3 、BaTiTe 3 or BaZr 1-x Ti x Te 3 (wherein x is greater than 0 and less than or equal to approximately 0.5); or a combination thereof.
[0159] The semiconductor nanoparticles including the metal halide compound or the transition metal chalcogenide may include a perovskite crystal structure confirmed by, for example, an X-ray diffraction spectrum.
[0160] In an embodiment, the semiconductor nanoparticle or the first semiconductor nanocrystal may include a metal (including indium, zinc, or a combination thereof) and a non-metal (including phosphorus, selenium, tellurium, sulfur, or a combination thereof). In an embodiment, the semiconductor nanoparticle or the second semiconductor nanocrystal may include a metal (including indium, zinc, or a combination thereof) and a non-metal (including phosphorus, selenium, tellurium, sulfur, or a combination thereof).
[0161] In an embodiment, the semiconductor nanoparticle or the first semiconductor nanocrystal may include InP, InZnP, ZnSe, ZnSeS, ZnSeTe, a metal halide perovskite compound, a transition metal chalcogenide perovskite compound, or a combination thereof; the second semiconductor nanocrystal may include ZnSe, ZnSeS, ZnS, ZnTeSe, or a combination thereof. In an embodiment, the semiconductor nanoparticle or the shell may include zinc, sulfur, and optionally selenium in the outermost layer.
[0162] In embodiments, the semiconductor nanoparticles can adjust the absorption / emission wavelength by adjusting, for example, their composition and / or size. The semiconductor nanoparticles can be configured to emit light of a desired color (first light).
[0163] In an embodiment, the (predetermined) peak emission wavelength of the semiconductor nanoparticle or the first light (or the second light or the third light) may have a wavelength range of ultraviolet to infrared wavelengths or greater. In an embodiment, the (predetermined) peak emission wavelength may be greater than or equal to about 300 nm, greater than or equal to about 500 nm, greater than or equal to about 510 nm, greater than or equal to about 520 nm, greater than or equal to about 530 nm, greater than or equal to about 540 nm, greater than or equal to about 550 nm, greater than or equal to about 560 nm, greater than or equal to about 570 nm, greater than or equal to about 580 nm, greater than or equal to about 590 nm, greater than or equal to about 600 nm, or greater than or equal to about 610 nm. The peak emission wavelength may be less than or equal to about 900 nm, less than or equal to about 800 nm, less than or equal to about 650 nm, less than or equal to about 640 nm, less than or equal to about 630 nm, less than or equal to about 620 nm, less than or equal to about 610 nm, less than or equal to about 600 nm, less than or equal to about 590 nm, less than or equal to about 580 nm, less than or equal to about 570 nm, less than or equal to about 560 nm, less than or equal to about 550 nm, or less than or equal to about 540 nm. The peak emission wavelength may be from about 500 nm to about 650 nm.
[0164] The semiconductor nanoparticles can emit green light (e.g., when a voltage is applied or irradiated with light). The peak emission wavelength of the green light can be in the following range: greater than or equal to about 500 nm (e.g., greater than or equal to about 510 nm, greater than or equal to about 515 nm, greater than or equal to about 520 nm, or greater than or equal to about 525 nm) and less than or equal to about 560 nm, such as less than or equal to about 540 nm, or less than or equal to about 530 nm.
[0165] The semiconductor nanoparticles may emit red light (e.g., when voltage is applied or irradiated with light), and the peak emission wavelength of the red light may be in the following range: greater than or equal to about 600 nm, for example, greater than or equal to about 610 nm and less than or equal to about 650 nm, or less than or equal to about 640 nm.
[0166] The semiconductor nanoparticles may emit blue light (e.g., when voltage is applied or irradiated with light), and their peak emission wavelength may be greater than or equal to about 440 nm (e.g., greater than or equal to about 450 nm, greater than or equal to about 455 nm, greater than or equal to about 460 nm, or greater than or equal to about 465 nm) and less than or equal to about 480 nm (e.g., less than or equal to about 475 nm, less than or equal to about 470 nm, or less than or equal to about 465 nm).
[0167] In an embodiment, the semiconductor nanoparticles may exhibit a luminescence spectrum (e.g., a photoluminescence or electroluminescence spectrum) having a relatively narrow half-width. In an embodiment, in the photoluminescence or electroluminescence spectrum, the semiconductor nanoparticles may exhibit the following half-width: less than or equal to about 45 nm, less than or equal to about 44 nm, less than or equal to about 43 nm, less than or equal to about 42 nm, less than or equal to about 41 nm, less than or equal to about 40 nm, less than or equal to about 39 nm, less than or equal to about 38 nm, less than or equal to about 37 nm, less than or equal to about 36 nm, less than or equal to about 35 nm, less than or equal to about 30 nm, less than or equal to about 25 nm, or less than or equal to about 20 nm. The half-width may be greater than or equal to about 1 nm, greater than or equal to about 5 nm, greater than or equal to about 10 nm, or greater than or equal to about 15 nm.
[0168] The semiconductor nanoparticles may exhibit (or may be configured to exhibit) a quantum efficiency (or quantum yield) of greater than or equal to about 10%, for example, greater than or equal to about 30%, greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 90%, or about 100%.
[0169] The semiconductor nanoparticles may have a size (or average size, hereinafter, "size") greater than or equal to about 1 nm and less than or equal to about 100 nm. The size may be a diameter or an equivalent diameter converted from an electron microscope image by assuming a spherical shape when it is not spherical. The size can be calculated from the results of inductively coupled plasma atomic emission spectrometry ("ICP-AES") analysis and optical analysis (e.g., UV-Vis absorption spectroscopy analysis). In an embodiment, the quantum dots may have the following size: about 1 nm to about 50 nm, for example, about 2 nm (or about 3 nm) to about 35 nm. In an embodiment, the size (or average size) of the quantum dots may be greater than or equal to about 3 nm, greater than or equal to about 4 nm, greater than or equal to about 5 nm, greater than or equal to about 6 nm, greater than or equal to about 7 nm, greater than or equal to about 8 nm, greater than or equal to about 9 nm, greater than or equal to about 10 nm, greater than or equal to about 11 nm, or greater than or equal to about 12 nm. In an embodiment, the size of the quantum dots may be less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 30 nm, less than or equal to about 25 nm, less than or equal to about 20 nm, less than or equal to about 19 nm, less than or equal to about 18 nm, less than or equal to about 17 nm, less than or equal to about 16 nm, less than or equal to about 15 nm, less than or equal to about 14 nm, less than or equal to about 13 nm, or less than or equal to about 12 nm.
[0170] The shape of the semiconductor nanoparticles is not particularly limited. For example, the shape of the quantum dots may include, but is not limited to, spheres, polyhedrons, pyramids, multi-foot shapes, hexahedrons, cubes, cuboids, nanotubes, nanorods, nanowires, nanosheets, or a combination thereof.
[0171] The semiconductor nanoparticles can be synthesized by any method, which is not particularly limited. In an embodiment, semiconductor nanocrystals having a size of several nanometers can be synthesized by a wet chemical process. In a wet chemical process, semiconductor nanocrystal particles or nanoparticles can be grown by reacting precursor materials in an organic solvent, and the growth of the nanocrystals can be controlled by coordinating an organic solvent or a ligand compound on the surface of the nanoparticles. The wet chemical process may include hot injection, ligand-assisted reprecipitation, or a combination thereof.
[0172] The method for collecting the manufactured semiconductor nanoparticles is not particularly limited. In embodiments, a non-solvent can be added to the reaction product after the reaction is completed, and the semiconductor nanoparticles coordinated with organic matter (e.g., ligand compound) can be separated. The non-solvent can be a polar solvent that is miscible with the solvent used in the core formation and / or shell formation reaction and cannot disperse the prepared nanocrystals. The non-solvent can be selected depending on the solvent used in the reaction, and can include, for example, acetone, ethanol, butanol, isopropanol, ethylene glycol, water, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), diethyl ether, formaldehyde, acetaldehyde, a solvent with a solubility parameter similar to the aforementioned non-solvent, or a combination thereof. The collection or separation of the semiconductor nanocrystal particles or quantum dots can include centrifugation, sedimentation, chromatography, or distillation. If necessary, the separated nanocrystals or quantum dots can be added to a washing solvent and washed. The type of the washing solvent is not particularly limited, and can be selected from those with a solubility parameter similar to the solubility parameter of the ligand and can, for example, include hexane, heptane, octane, chloroform, toluene, etc.
[0173] In an embodiment, the semiconductor nanoparticle may include an organic ligand on its surface. The organic ligand may be coordinated or bonded to the surface of the semiconductor nanoparticle. The organic ligand may be a ligand provided on the surface of the semiconductor nanoparticle during the synthesis of the semiconductor nanoparticle.
[0174] The organic ligand may include a first functional group and a carbon-carbon unsaturated bond, wherein the organic ligand may be bonded to the surface of the semiconductor nanoparticle via the first functional group. As used in the present disclosure, "bonding" means that the organic ligand may be non-covalently or covalently bonded to the surface of the semiconductor nanoparticle. The bonding may be based on van der Waals forces, hydrogen bonding, ionic interactions, dipole-dipole interactions and / or coordination bonds. The first functional group may include a carboxyl group, a thiol group, an amine group, a phosphine group, a phosphine oxide group, an ester group (e.g., a carboxylate group), a hydroxyl group or a combination thereof. The carbon-carbon unsaturated bond may include or may be a carbon-carbon double bond. When the semiconductor nanoparticle (which includes the organic ligand) and the additive are exposed to radiation, the organic ligand may react with the additive described herein, and therefore, the radiation may cause a change in the solubility of the semiconductor nanoparticle in the first solvent.
[0175] The organic ligand may include RCOOH, RNH 2 , R 2 NH, R 3 N, RSH, RH 2 PO, R 2 HPO, R 3 PO, RH 2 P.R 2 HP, R 3 P, ROH, RCOOR', RPO(OH) 2 , R 2 POOH or a combination thereof, wherein each R and R' independently may be a substituted or unsubstituted C1 or more, C6 or more, or C10 or more and C40 or less, C35 or less, or C25 or less aliphatic hydrocarbon group, or a substituted or unsubstituted C6 to C40 aromatic hydrocarbon group, or a combination thereof, provided that R, R' or both may include a carbon-carbon unsaturated bond, such as a carbon-carbon double bond. The aliphatic hydrocarbon may have a carbon number in the following range: C5-C40, C8-C30, C10-C25, C12-C20, C14-C18 or a combination thereof.
[0176] For example, the aliphatic hydrocarbon group can be a straight or branched hydrocarbon group containing one or more carbon-carbon unsaturated bonds in the carbon chain or at the end of the carbon chain. The organic ligand can be used alone or as a mixture of at least two compounds. R or R' can each independently include vinyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, tridecenyl, pentadecenyl, hexadecenyl, heptadecenyl, octadecenyl or nonadecenyl. The organic ligand may include a carboxylic acid compound having a C3-C30, C6-C25, C8-C22, C10-C20 or C15-C18 alkenyl or alkenylene group, such as acrylic acid, butenoic acid, pentenoic acid, hexenoic acid, heptenoic acid, octenoic acid, nonenoic acid, decenoic acid, undecenoic acid, dodecenoic acid, tridecenoic acid, tetradecenoic acid, pentadecenoic acid, hexadecenoic acid, heptadecenoic acid, octadecenoic acid (e.g., oleic acid); a thiol compound having a C3-C30, C6-C25, C8-C22, C10-C20 or C15-18 alkenyl or alkenylene group; a thiol compound having a C3-C30 , C6-C25, C8-C22, C10-C20 or C15-C18 alkenyl or alkenylene groups, such as oleylamine; a phosphine compound having a C3-C30, C6-C25, C8-C22, C10-C20 or C15-C18 alkenyl or alkenylene group; an alcohol compound having a C3-C30, C6-C25, C8-C22, C10-C20 or C15-C18 alkenyl or alkenylene group; an ester compound having a C3-C30, C6-C25, C8-C22, C10-C20 or C15-C18 alkenyl or alkenylene group; or a combination thereof.
[0177] The semiconductor nanoparticles may be dispersed in a first solvent to be described later, by, for example, including the organic ligand on the surface thereof.
[0178] Semiconductor nanoparticles (e.g., metal halide perovskite nanocrystals) have attracted attention as next generation luminescent materials. Semiconductor nanoparticles can show improved quantum yields, narrow light emission peaks, color tunability, and solution processability. However, there is still room for development for the microscale patterning technology of semiconductor nanoparticles for applications in actual displays and optoelectronic devices. The photolithography process of the prior art has many disadvantages (e.g., problems of uneven pattern formation due to swelling or capillary forces of photoresists) in the patterning of inorganic nanocrystals. In addition, when it is desired to provide a pattern of semiconductor nanoparticles by applying photolithography technology, it may be accompanied by the deterioration of the physical properties of the semiconductor nanoparticles. Unexpectedly, the inventors have found that by irradiating radiation to a film containing additives as described herein and semiconductor nanoparticles as described herein, a film pattern of improved quality can be formed without the substantial reduction of its luminescent properties.
[0179] Therefore, in the patterning method, the film further includes an additive having a thiol group. The additive may include a polythiol compound containing two or more thiol groups. In an embodiment, the additive may include or may not include a monothiol compound having a thiol group. The polythiol compound may include a dithiol compound, a trithiol compound, a tetrathiol compound or a combination thereof. In an embodiment, the photocatalytic reaction between the additive and the organic ligand may be promoted by the semiconductor nanoparticles, and therefore the reaction may occur at a relatively low radiation dose.
[0180] The additive or the polythiol compound may have a molecular weight of greater than or equal to about 10 g / mol, greater than or equal to about 50 g / mol, greater than or equal to about 100 g / mol, greater than or equal to about 150 g / mol, greater than or equal to about 200 g / mol, greater than or equal to about 250 g / mol, greater than or equal to about 300 g / mol, greater than or equal to about 350 g / mol, greater than or equal to about 400 g / mol, greater than or equal to about 450 g / mol, greater than or equal to about 500 g / mol, or greater than or equal to about 550 g / mol. The additive or the polythiol compound may have a molecular weight of less than or equal to about 5,000,000 g / mol, less than or equal to about 1,000,000 g / mol, less than or equal to about 500,000 g / mol, less than or equal to about 100,000 g / mol, less than or equal to about 50,000 g / mol, less than or equal to about 10,000 g / mol, less than or equal to about 5,000 g / mol, less than or equal to about 4,500 g / mol, less than or equal to about 4,000 g / mol, less than or equal to about 3,500 g / mol, less than or equal to about 5 ...5,000 g / mol, less than or equal to about 16,000 g / mol, less than or equal to about 17,000 g / mol, less than or equal to about 18,000 g / mol, less than or equal to about 19,000 g / mol, less than or equal to about 20,000 g / mol, less than or equal to about 21,000 g / mol, less than or equal to about 24,000 g / mol, less than or equal to about 26,000 g / mol, less than or equal to about 28,000 g / mol, less than or equal to about 29,000 g / mol, less than or equal to about 30,000 g / mol, less than or equal to g / mol, less than or equal to about 3,000 g / mol, less than or equal to about 2,500 g / mol, less than or equal to about 2,000 g / mol, less than or equal to about 1,750 g / mol, less than or equal to about 1,500 g / mol, less than or equal to about 1,250 g / mol, less than or equal to about 1,000 g / mol, less than or equal to about 750 g / mol, less than or equal to about 700 g / mol, less than or equal to about 500 g / mol, less than or equal to about 400 g / mol, less than or equal to about 300 g / mol, or less than or equal to about 250 g / mol.
[0181] The polythiol compound may further include -O-, -CO-, -COO-, -NR-, -CONR- (wherein R in -NR- and -CONR- is independently hydrogen or a C1 to C10 hydrocarbon group), a substituted or unsubstituted C1-C40 or C5-C20 alkylene group, a substituted or unsubstituted C2-C40 or C5-C20 alkenylene group, a substituted or unsubstituted C2-C40 or C5-C20 alkynylene group, or a combination thereof (e.g., any combination of the foregoing).
[0182] As used herein, the term "combination thereof" may mean a moiety formed by bonding at least two or more of the listed moieties. Thus, for example, the polythiol compound may include a moiety formed by connecting the alkylene moiety and the alkenylene moiety directly or via -O-, -CO-, -CO-, -NR-, -CONR- (wherein R is hydrogen or a C1 to C10 hydrocarbon group). In addition, for example, the polythiol compound may include a substituted or unsubstituted alkylene moiety (or alkenylene moiety or alkynylene moiety) in which at least one methylene group is replaced by -O-, -CO-, -COO-, -NR-, -CONR- (wherein R is hydrogen or a C1 to C10 hydrocarbon group).
[0183] The polythiol compound may include a central portion and at least one (e.g., two or more) HS-R-* (wherein R is a substituted or unsubstituted C1 to C30 aliphatic hydrocarbon group bonded to the central portion; a substituted or unsubstituted C2 to C30 aliphatic hydrocarbon group in which at least one methylene group is replaced by a sulfonyl group, a carbonyl group, an ether, a thioether, a sulfoxide, an ester, an amide, or a combination thereof; or a combination thereof). The central portion may include carbon atoms, a substituted or unsubstituted C1 to C30 aliphatic hydrocarbon group, a substituted or unsubstituted C3 to C30 alicyclic hydrocarbon group, a substituted or unsubstituted C6 to C30 aromatic hydrocarbon group, a substituted or unsubstituted C3 to C30 heteroarylene group, a substituted or unsubstituted C3 to C30 heterocyclic group, or a combination thereof.
[0184] The polythiol compound may include a dimercaptoacetate compound, a trimercaptoacetate compound, a tetramercaptoacetate compound, a dimercaptopropionate compound, a trimercaptopropionate compound, a tetramercaptopropionate compound, an isocyanate compound including two or more mercaptoalkylcarbonyloxyalkyl groups, an isocyanurate compound including two or more mercaptoalkylcarbonyloxyalkyl groups, or a combination thereof.
[0185] The thiol compound can be represented by Chemical Formula 3:
[0186] Chemical formula 3:
[0187]
[0188] In the chemical formula 3, R 1 is hydrogen, a substituted or unsubstituted C1 to C30 straight or branched alkyl group, a substituted or unsubstituted C6 to C30 aryl group, a substituted or unsubstituted C7 to C30 arylalkyl group, a substituted or unsubstituted C3 to C30 heteroaryl group, a substituted or unsubstituted C3 to C30 cycloalkyl group, a substituted or unsubstituted C3 to C30 heterocycloalkyl group, a substituted or unsubstituted C1 to C10 alkoxy group, a hydroxyl group, -NH 2, a substituted or unsubstituted C1 to C30 amine group (-NRR', wherein R and R' are independently hydrogen or a C1 to C30 linear or branched alkyl group, and are not hydrogen at the same time), an isocyanate group, a halogen, -ROR' (wherein R is a substituted or unsubstituted C1 to C20 alkylene group and R' is hydrogen or a C1 to C20 linear or branched alkyl group), an acyl halide group (-RC(=O)X, wherein R is a substituted or unsubstituted C1 to C20 alkylene group and X is a halogen), -C(=O)OR' (wherein R' is hydrogen or a C1 to C20 linear or branched alkyl group), -CN, -C(=O)NRR' or -C(=O)ONRR' (wherein R and R' are independently hydrogen or a C1 to C20 linear or branched alkyl group), or a combination thereof,
[0189] L 1 is a carbon atom, a substituted or unsubstituted C1 to C30 alkylene group, a substituted or unsubstituted C2 to C30 alkenylene group, a substituted or unsubstituted C3 to C30 cycloalkylene group, a substituted or unsubstituted C6 to C30 arylene group, a substituted or unsubstituted C3 to C30 heteroarylene group (e.g., quinoline, quinolone, triazine, triazinetrione moiety, etc.), a C3 to C30 heterocycloalkylene group, or at least one methylene group (—CH 2 -) is replaced by a sulfonyl group (-SO 2 -), a carbonyl group ((-C(=O)), an ether group (-O-), a thioether (-S-), a sulfoxide group (-SO-), an ester group (-C(=O)O-), an amide group (-C(=O)NR-, wherein R is hydrogen or a C1 to C10 alkyl group), or a substituted or unsubstituted C2 to C30 alkylene group or a substituted or unsubstituted C3 to C30 alkenylene group substituted with a combination thereof,
[0190] Y 1 is a single bond, a substituted or unsubstituted C1 to C30 alkylene group, a substituted or unsubstituted C2 to C30 alkenylene group, or at least one methylene group (—CH 2 -) is sulfonyl group (-S(=O) 2 -), a carbonyl group (-C(=O)-), an ether group (-O-), a thioether group (-S-), a sulfoxide group (-S(=O)-), an ester group (-C(=O)O-), an amide group (-C(=O)NR-, wherein R is hydrogen or a C1 to C10 straight chain or branched alkyl group), an imine group (-NR-, wherein R is hydrogen or a C1 to C10 straight chain or branched alkyl group), or a substituted C2 to C30 alkylene group or a substituted or unsubstituted C3 to C30 alkenylene group substituted by a combination thereof,
[0191] m is an integer of 1 or more, for example, 1 to 10,
[0192] k1 is an integer of 0 or 1 or greater, for example, 1 to 10,
[0193] k2 is 1 or more, for example, an integer from 1 to 10, and
[0194] The sum of m and k2 may be an integer greater than or equal to about 2, greater than or equal to about 3 (eg, 2, 3, 4, 5, or 6).
[0195] In an embodiment, in Chemical Formula 3, Y 1 is not a single bond, and m does not exceed Y 1 The valence of the compound, and the sum of k1 and k2 does not exceed L 1 valence.
[0196] The polythiol compound can be represented by chemical formula 3-1:
[0197] Chemical formula 3-1
[0198]
[0199] Among them, in chemical formula 3-1,
[0200] L 1 'With L in chemical formula 3 1 are the same, and may be, for example, carbon, a substituted or unsubstituted C1 to C30 aliphatic hydrocarbon group (e.g., an alkylene, alkenylene, alkynylene group); a substituted or unsubstituted C6 to C30 arylene group; a substituted or unsubstituted C3 to C30 heteroarylene group; a substituted or unsubstituted C3 to C30 cycloalkylene group; or a substituted or unsubstituted C3 to C30 heterocycloalkylene group; and,
[0201] Y a To Y d are independently a single bond, a substituted or unsubstituted C1 to C30 alkylene group, a substituted or unsubstituted C2 to C30 alkenylene group, or at least one methylene group (—CH 2 -) is sulfonyl group (-S(=O) 2 -), a carbonyl group (-C(=O)-), an ether group (-O-), a thioether group (-S-), a sulfoxide group (-S(=O)-), an ester group (-C(=O)O-), an amide group (-C(=O)NR-) (wherein R is hydrogen or a C1 to C10 straight or branched alkyl group), an imine group (-NR-) (wherein R is hydrogen or a C1 to C10 straight or branched alkyl group), or a substituted or unsubstituted C2 to C30 alkylene group or a substituted or unsubstituted C3 to C30 alkenylene group substituted with a combination thereof, and
[0202] R a To R dR of Formula 3 is independently 1 or SH, provided that R a To R d At least one or at least two of are SH.
[0203] The central part, for example, L of Chemical Formula 3 or Chemical Formula 3-1 1 or L 1 ', may include carbon atoms, substituted or unsubstituted C1 to C30 aliphatic hydrocarbon groups, triazine moieties, triazinetrione moieties, quinoline moieties, quinolone moieties, naphthalene moieties, or combinations thereof.
[0204] The thiol compound of Chemical Formula 3 may be a polythiol compound, and may include nonane dithiol, diol dimercaptopropionate (e.g., ethylene glycol dimercaptopropionate), trimethylolpropane tris(3-mercaptopropionate) having a structure of Chemical Formula 3-2, pentaerythritol tetrakis(3-mercaptopropionate) having a structure of Chemical Formula 3-3, pentaerythritol tetrakis(2-mercaptoacetate) having a structure of Chemical Formula 3-4, tris[2-(3-mercaptopropionyloxy)alkyl]isocyanurate having a structure of Chemical Formula 3-5, a compound having a structure of Chemical Formula 3-6, a compound having a structure of Chemical Formula 3-7, a compound having a structure of Chemical Formula 3-8, or a combination thereof:
[0205] Chemical formula 3-2
[0206]
[0207] Chemical formula 3-3
[0208]
[0209] Chemical formula 3-4
[0210]
[0211] Chemical formula 3-5
[0212]
[0213] Wherein, in Chemical Formula 3-5, R is a substituted or unsubstituted C1 to C10 alkylene group;
[0214] Chemical formula 3-6
[0215]
[0216] Wherein, n is an integer from 1 to 20,
[0217] Chemical formula 3-7
[0218]
[0219] Wherein, n is an integer from 1 to 20,
[0220] Chemical formula 3-8
[0221]
[0222] Here, n is an integer from 1 to 20.
[0223] Without wishing to be bound by any theory, it is believed that, in embodiments, radiation irradiated to a film containing an additive and semiconductor nanocrystals can result in the occurrence of a photochemical reaction to change the solubility (or dispersibility) of the irradiated portion of the film and can help eliminate some surface defects of the semiconductor nanoparticles. Unexpectedly, the inventors have found that in the methods disclosed herein, the photocatalytic activity of the semiconductor nanoparticles can promote or activate crosslinking between the ligands via the additive, rather than polymerization. The semiconductor nanocrystal particles can be (or can be used as) a photocatalyst for generating thiol radicals from thiol groups, and the carbon-carbon double bonds present in the ligands can participate in the thiol-ene reaction initiated by the semiconductor nanoparticles.
[0224] Without wishing to be bound by any theory, in direct photocatalytic patterning according to the methods disclosed herein, the reaction can be considered from an energy perspective as follows: in the method of the embodiment, the semiconductor nanocrystal particles can be exposed to photons greater than their band gap energy, excitons can be formed, and in the case where the redox level of the additive is above the energy level of the valence band maximum of the semiconductor nanocrystal particles, the holes excited from the excitons can jump to the thiol groups of the additive, thereby providing reactive thiol radicals. (See Figure 2C )
[0225] The additive or thiol compound may have a redox potential ranging from about 0.1 eV to about 10 eV, or from about 0.2 eV to about 5 eV, from about 0.3 eV to about 3 eV, from about 0.35 eV to about 2 eV, from about 0.4 eV to about 1 eV, from about 0.5 eV to about 0.7 eV, or combinations thereof.
[0226] Without wishing to be bound by any theory, when the film is irradiated with radiation in the method of the embodiments, for example, as described herein, the carbon-carbon unsaturated bonds included in the organic ligands of the semiconductor nanoparticles may react with the thiol moieties of the additive (hereinafter, thiol-ene reaction) (see Figure 2A ). The mechanism of the thiol-ene reaction can be shown as Figure 2D In. Figure 2D As shown in , the formed thiol radical can react with the ligand.
[0227] Reference Figure 2A , the thiol group can undergo a reaction with a carbon-carbon double bond to form a sulfur-carbon bond in the presence of energy (e.g., radiation such as light), and such a reaction may require a catalyst or a free radical product. Unexpectedly, the inventors have found that the semiconductor nanoparticles present in the film can be used as a photocatalyst. Without wishing to be bound by a particular theory, it is believed that the semiconductor nanocrystal particles (e.g., based on compounds) described herein can form excitons when exposed to radiation, and the excitons so formed can be used as catalysts for the thiol-ene reaction in the film (e.g., between the carbon-carbon unsaturated bonds in the ligands of the semiconductor nanoparticles and the additive). The inventors have found that the thiol-ene reaction in the film can be carried out with relatively high reaction efficiency (even in the presence of moisture and oxygen in the film), and therefore the chemical change can provide a significant difference in film properties (e.g., solubility) between the part exposed to the radiation and the part not exposed to the radiation, thereby forming a pattern with relatively high resolution (e.g., 10 microns or less or 5 microns or less line width), such as via a developing process.
[0228] From a practical point of view, the patterning process may not degrade the optical properties of the semiconductor nanoparticles and may provide relatively high-resolution patterns. The direct optical patterning of the embodiment may be based on ligand chemistry, and thus desorption of ligands may often occur during the patterning process, which may have an adverse effect on the passivation of the semiconductor nanoparticles, and this may result in a reduction in the quantum efficiency (or photoluminescence quantum yield) of the resulting pattern. Surprisingly, the inventors have discovered that the thiol portion of the additive may act as a defect passivator under the radiation exposure conditions of the method of the embodiment. Thus, protons may be separated from the thiol group of the additive to form RS - The thiolate forms passivate the surface of the semiconductor nanoparticle.Alternatively, the method may involve the use of relatively high stability semiconductor nanocrystal particles that include relatively strongly bound ligands.
[0229] This can be achieved by introducing zinc halides (ZnX 2, X is F, Cl, Br, I or a combination thereof) to prepare semiconductor nanoparticles (e.g., nanoparticles based on perovskite semiconductor nanocrystals) with relatively high stability. Without wishing to be bound by theory, zinc ions may preferentially bind to functional groups (e.g., oleate groups) bonded to the surface of the semiconductor nanoparticles. The final semiconductor nanocrystal particles synthesized in the presence of zinc halides may include alkylammonium halides (e.g., alkylammonium bromides) with high binding affinity as primary ligands. Without wishing to be bound by any theory, it is believed that the strong binding of ammonium-based ligands may increase the photoluminescence quantum yield of semiconductor nanocrystal particles. In addition, the inventors have found that in the case where the surface of the semiconductor nanoparticles is functionalized by alkylammonium groups, an additive containing a thiol group may be added to the nanoparticle dispersion solution to prevent or inhibit the reduction of dispersion stability, and the luminous efficiency of the semiconductor nanoparticles may not be substantially reduced, for example, even after the patterning process. The semiconductor nanoparticles of the embodiment may be ZnX 2 Processed perovskite-based semiconductor nanocrystal particles that can be used as photocatalysts and patterning components.
[0230] Without wishing to be bound by any theory, in semiconductor nanocrystal particles synthesized in the presence of zinc halide, ligands such as oleylamine and the like may be ligands with strong binding energy, and it is believed that the additive may be more effectively used as a passivating agent and thus further increase the optical properties of the semiconductor nanoparticles or films comprising the same. In embodiments, the thioether moiety formed by a thiol-ene reaction initiated by radiation (e.g., UV light) may be more effective for passivation.
[0231] The effective surface passivation by the dual action of the additives in the method of the embodiments can also increase the photostability of the patterned film. Surprisingly, the inventors have found that when using relatively high power UV light (e.g., about 40 mW cm -2 ) irradiation, the retention rate of the luminous efficiency of the patterned film according to the method of the embodiment can be relatively higher than that of the film manufactured without the additive. The relatively high stability of the patterned film obtained by the method of the embodiment can indicate that the method of the embodiment can be a non-destructive and effective patterning method and can be used to manufacture a variety of optoelectronic devices.
[0232] The additive may not cause substantial degradation of the optical properties of the semiconductor nanoparticles. For example, the addition of the additive may not cause a substantial shift in the peak emission wavelength of the luminescence spectrum of the semiconductor nanoparticles or the first absorption wavelength of the UV-Vis absorption spectrum. The patterning method may not cause substantial changes in the crystal structure or average size of the semiconductor nanoparticles (e.g., semiconductor nanocrystal particles). The photoluminescence quantum yield (e.g., absolute quantum yield) of the semiconductor nanocrystal particle film may be maintained during the patterning process, and the addition of the additive described herein may result in an increase in quantum yield (e.g., an increase of about 5% or greater, about 7% or greater, or about 9% or greater) compared to an unadded film prepared without the addition of the additive.
[0233] In the patterning method, due to the possible passivation of the defects of the semiconductor nanoparticles by the additive, the ink composition described herein may show increased dispersibility compared to the semiconductor nanocrystal dispersion without the additive. Therefore, in the patterning method according to the embodiment, when placed under dark conditions for an extended period of time (e.g., about 10 days), the ink composition may show precipitation of only a limited amount of semiconductor nanoparticles, or may not show any substantial precipitation of semiconductor nanoparticles, as observed by the naked eye. On the contrary, in the case of the original (pristine) solution including the semiconductor nanoparticles without the additive, precipitation of a significant amount of semiconductor nanoparticles can be observed. The relatively high colloidal stability of the ink composition may be further advantageous for the patterning method of the embodiment.
[0234] In the method disclosed herein, the introduction of the additive and the irradiation of the radiation may not cause substantial damage to the structure of the semiconductor nanocrystalline particles, and may contribute to enhancing the optical properties of the semiconductor nanoparticles or the patterned film including them. As measured by time-resolved photoluminescence (TRPL) analysis, after adding the additive, the average life span of the semiconductor nanoparticles may increase (e.g., from 3.5ns to 6.32ns), and the non-emitting recombination ratio may be reduced. As measured by TRPL analysis, the average life span of the semiconductor nanoparticles in the patterned film may be greater than or equal to about 3.5ns, greater than or equal to about 3.53ns, greater than or equal to about 6ns, or greater than or equal to about 6.3ns. The average life span of the semiconductor nanoparticles in the patterned film may be less than or equal to about 7ns.
[0235] Without wishing to be bound by any theory, the retention of the photophysical and structural properties of the semiconductor nanoparticles may indicate a dual role of the additive in the methods described herein (ie, a cross-linking agent and an effective defect passivator).
[0236] The additive can provide a total number of reactive functional groups suitable for providing a pattern with the composition, and can exhibit a desired compatibility with the semiconductor nanoparticles. As the number of reactive functional units increases, crosslinking efficiency can also increase. The additive can exhibit compatibility with a non-polar solvent for the semiconductor nanoparticles.
[0237] The additive may be dissolved in a non-polar solvent (e.g., toluene), and the prepared solution (e.g., about 0.025 M to about 2.5 M) may not exhibit obvious absorption characteristics for the radiation to be exposed (e.g., for UV light having a wavelength of about 365 nm to about 405 nm, such as the I-line or the H-line), and this may indicate that the thiol group of the additive may not be converted into a thiol radical in response to the radiation exposure itself, and the semiconductor nanocrystals described herein may be used as suitable photocatalysts.
[0238] In the patterning method, the carbon-carbon unsaturated bonds of the ligands of the adjacent semiconductor particles in the film can participate in the thiol-ene reaction with the thiol part of the additive, thereby changing the solubility of the semiconductor particles for the solvent (e.g., the first solvent described herein). Through the change in solubility, the film that is soluble relative to the first solvent before exposure can have dissolution resistance relative to the first solvent after exposure to the radiation. Through the change in solubility described herein, the semiconductor nanoparticles present in the region exposed to the radiation (e.g., present in the first region) may not be removed and retained during the development process described herein, and therefore, a patterned film of the desired semiconductor nanoparticles can be obtained. As used herein, the expression "soluble relative to a given solvent" may refer to the following situation: when the semiconductor nanoparticle film is in contact with a given solvent, the semiconductor nanoparticles included in the film can be dispersed in a given solvent (e.g., the first solvent) to form a colloidal dispersion state. As used herein, a colloidal dispersion state refers to a situation in which the size (or average size) of a discontinuous phase (e.g., a particle phase) in a continuous phase (e.g., a solid phase such as a polymer phase, or a liquid phase such as a solvent phase) may be within the following nanoscale: less than or equal to about 1 micrometer (μm), for example, less than or equal to about 900 nm, less than or equal to about 800 nm, less than or equal to about 700 nm, less than or equal to about 600 nm, less than or equal to about 500 nm, less than or equal to about 400 nm, less than or equal to about 300 nm, less than or equal to about 200 nm, less than or equal to about 150 nm, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 40 nm, or less than or equal to about 30 nm. The semiconductor nanoparticles or films comprising the same may have a dissolution resistance relative to a given solvent (e.g., a first solvent), and when in contact with a given solvent (e.g., a first solvent), the semiconductor nanoparticles (e.g., included in the film) may not or do not form a colloidal dispersion in the given solvent. For example, the semiconductor nanoparticles or films comprising the same may have a dissolution resistance relative to a given solvent, and when in contact with a given solvent (e.g., a first solvent), at least about 50%, about 60%, about 70%, about 80%, about 90%, about 95%, about 99% or more (e.g., substantially all) of the semiconductor nanoparticles included in the radiation-treated region of the film are not removed from the film into the solvent.
[0239] In the patterning method, the deterioration of the luminescent properties of the semiconductor nanoparticles can be effectively prevented. The semiconductor nanoparticles included in the patterned film can exhibit a luminescent efficiency comparable to or higher than the original luminescent efficiency measured for the same semiconductor nanoparticles in a dispersed solvent. Without wishing to be bound by any theory, in the patterned film, the additive can further bond to the surface of the semiconductor nanoparticles, and this can cause a change in the optical properties of the semiconductor nanoparticles (e.g., an increase in quantum efficiency). Without wishing to be bound by any theory, the additive (or its thiol group) present in the film can have an S-part (e.g., formed via deprotonation or by free radical formation after the radiation exposure). The S-part can further passivate surface defects, such as metal cations (e.g., zinc cations, lead cations, cesium cations, etc.) present on the surface of adjacent semiconductor nanoparticles (see Figure 2B ).
[0240] In the patterning method, the luminous efficiency (e.g., quantum efficiency) of the patterned film may be substantially the same as the quantum efficiency of the semiconductor nanoparticles before being included in the film (hereinafter referred to as the initial quantum efficiency), or may be at least about 3%, at least about 5%, or at least about 10% greater than the initial quantum efficiency. In an embodiment, the relative luminous efficiency of the patterned film relative to the initial luminous efficiency (about 100%) may be greater than or equal to about 70%, greater than or equal to about 75%, greater than or equal to about 80%, greater than or equal to about 85%, greater than or equal to about 90%, greater than or equal to about 100%, greater than or equal to about 101%, greater than or equal to about 103%, greater than or equal to about 105%, greater than or equal to about 107%, greater than or equal to about 110%, greater than or equal to about 115%, greater than or equal to about 120%, greater than or equal to about 130%, or greater than or equal to about 150%.
[0241] The patterned film may have a relative luminous efficiency greater than or equal to about 100%:
[0242] Relative luminous efficiency (%) = A / B x 100
[0243] A: Quantum efficiency of the patterned film
[0244] B: Quantum efficiency of the film made of the semiconductor nanoparticles without the above additives
[0245] The relative luminous efficiency may be greater than or equal to about 70%, greater than or equal to about 75%, greater than or equal to about 80%, greater than or equal to about 85%, greater than or equal to about 90%, greater than or equal to about 100%, greater than or equal to about 101%, greater than or equal to about 103%, greater than or equal to about 105%, greater than or equal to about 107%, greater than or equal to about 110%, greater than or equal to about 115%, greater than or equal to about 120%, greater than or equal to about 125%, greater than or equal to about 130%, or greater than or equal to about 150% and less than or equal to about 200%, less than or equal to about 180%, less than or equal to about 170%, less than or equal to about 160%, less than or equal to about 150%, less than or equal to about 140%, less than or equal to about 130%, less than or equal to about 125%, less than or equal to about 110%, less than or equal to about 106%, or less than or equal to about 104%.
[0246] The formation of a film (eg, a first film) including the additive and the semiconductor nanoparticles may include obtaining a composition (eg, ink, also referred to as a coating composition or ink composition) including the additive and the semiconductor nanoparticles (refer to Figure 1A S1). In an embodiment, the formation of the film may include washing the semiconductor nanoparticles, which may be performed before preparing the ink. Surprisingly, the inventors have found that a more improved pattern quality can be obtained by a washing process. The washing may be performed once or multiple times, such as twice or three times. In an embodiment, the semiconductor nanoparticles may include perovskite nanocrystal particles, and the semiconductor nanoparticles prepared therefrom may be washed with an acetate-based washing solvent (e.g., methyl acetate). Without wishing to be bound by any theory, unreacted ligands or solvents may be removed during the washing process, and this may lead to an improvement in pattern quality. The washing solvent may include a non-solvent as described herein. The surface state of the semiconductor nanoparticles may have an influence on pattern formation, and ligand exchange may be performed before preparing the composition after the properties of the surface of the semiconductor nanoparticles may be first checked and if necessary.
[0247] The composition may include a first solvent. The additive and the semiconductor nanoparticles may be dispersed or dissolved in the first solvent. The first solvent may be a solvent in which the semiconductor nanoparticles may form a colloidal dispersion and in which the additive may be dissolved. The first solvent may be a developing solvent in a developing process described herein. A change in the solubility of the semiconductor nanoparticles included in the area exposed to radiation relative to the first solvent may be caused by a thiol-ene crosslinking reaction assisted by the photocatalytic activity of the semiconductor nanoparticles.
[0248] The first solvent may be a polar solvent. The first solvent may be a non-polar solvent. Examples of the first solvent may include C3 to C30 amide solvents such as dimethylformamide, cyclic ester solvents such as γ-butyrolactone, linear ester solvents such as ethyl acetate, cyclic amide (e.g. lactam) solvents such as N-methylpyrrolidone, C2 to C30 sulfoxide-based solvents such as dimethyl sulfoxide, C1 to C30 halogenated hydrocarbon solvents such as dichloroethylene, trichloroethylene and chloroform, C3 to C30 alkane solvents such as octane, hexane and heptane, substituted or unsubstituted C6 to C30 aromatic hydrocarbon solvents such as chlorobenzene, dichlorobenzene, styrene, toluene, etc., alicyclic hydrocarbon solvents such as cyclohexene and cyclohexane, or a combination thereof.
[0249] The first solvent may include toluene, octane, hexane, chlorobenzene, dichlorobenzene, chloroform, xylene or a combination thereof. The first solvent may include dimethylformamide, γ-butyrolactone, N-methylpyrrolidone, dimethyl sulfoxide, dichloroethylene, trichloroethylene, chloroform, chlorobenzene, dichlorobenzene, styrene, xylene, toluene, cyclohexene or a combination thereof.
[0250] The method for preparing the ink composition is not particularly limited. In an embodiment, a semiconductor nanoparticle solution (or dispersion) including semiconductor nanoparticles in a first solvent can be prepared, and an additive can be added to the solution to prepare the composition. The concentration of the solution of the semiconductor nanoparticles can be appropriately selected. The concentration of the semiconductor nanoparticles in the semiconductor nanoparticle solution can be greater than or equal to about 0.01 mg / mL, greater than or equal to about 0.1 mg / mL, greater than or equal to about 0.5 mg / mL, greater than or equal to about 1 mg / mL, greater than or equal to about 1.5 mg / mL, greater than or equal to about 3 mg / mL, greater than or equal to about 4.5 mg / mL, greater than or equal to about 5 mg / mL, greater than or equal to about 7.5 mg / mL, greater than or equal to about 9 mg / mL, greater than or equal to about 10 mg / mL, greater than or equal to about 12 mg / mL, greater than or equal to about 14 mg / mL, greater than or equal to about 16 mg / mL, or greater than or equal to about 18 mg / mL. The concentration of the semiconductor nanoparticles in the semiconductor nanoparticle solution may be appropriately selected in consideration of the dispersibility of the semiconductor nanoparticles in the first solvent, and may be less than or equal to about 100 mg / mL, less than or equal to about 80 mg / mL, less than or equal to about 60 mg / mL, less than or equal to about 40 mg / mL, or less than or equal to about 35 mg / mL, but is not limited thereto. The amount of the additive may be, based on 0.1 mg of semiconductor nanoparticles, greater than or equal to about 0.01 μL, greater than or equal to about 0.05 μL and less than or equal to about 20 μL, less than or equal to about 10 μL, or less than or equal to about 5 μL, but is not limited thereto.
[0251] The amount of the additive in the ink composition may be appropriately selected in consideration of the amount of the semiconductor nanoparticles, the wavelength and dose of the radiation, the type of semiconductor nanoparticles to be used, and the line width of the pattern to be formed. In an embodiment, the amount of the additive in the ink composition may be, based on the total weight of the semiconductor nanoparticles, greater than or equal to about 0.001% by weight, greater than or equal to about 0.005% by weight, greater than or equal to about 0.01% by weight, greater than or equal to about 0.05% by weight, greater than or equal to about 0.1% by weight, greater than or equal to about 0.5% by weight, greater than or equal to about 1% by weight, greater than or equal to about 3% by weight, greater than or equal to about 5% by weight, greater than or equal to about 7% by weight, greater than or equal to about 9% by weight, or greater than or equal to about 10% by weight. In an embodiment, the amount of the additive in the ink composition may be less than or equal to about 50 wt %, less than or equal to about 45 wt %, less than or equal to about 40 wt %, less than or equal to about 35 wt %, less than or equal to about 30 wt %, less than or equal to about 25 wt %, less than or equal to about 20 wt %, less than or equal to about 15 wt %, less than or equal to about 12 wt %, or less than or equal to about 8 wt %, based on the total weight of the semiconductor nanoparticles. The concentration of each component in the ink composition (e.g., the semiconductor nanoparticles and the thiol compound) may be adjusted to obtain sufficient solubility changes caused by radiation for the development process.
[0252] In the ink composition or the film obtained therefrom (or the first region), the amount of the semiconductor nanoparticles (or the amount of the inorganic component) may be, based on the total weight of the composition or the total solid content of the composition or the total weight of the film, greater than or equal to about 5% by weight, greater than or equal to about 10% by weight, greater than or equal to about 15% by weight, greater than or equal to about 20% by weight, greater than or equal to about 25% by weight, greater than or equal to about 30% by weight, greater than or equal to about 35% by weight, greater than or equal to about 40% by weight, greater than or equal to about 45% by weight, greater than or equal to about 50% by weight, greater than or equal to about 55% by weight, greater than or equal to about 60% by weight, greater than or equal to about 65% by weight, greater than or equal to about 70% by weight, greater than or equal to about 75% by weight, greater than or equal to about 80% by weight, greater than or equal to about 85% by weight, greater than or equal to about 90% by weight, greater than or equal to about 95% by weight, greater than or equal to about 98% by weight, greater than or equal to about 99% by weight, or greater than or equal to about 99.5% by weight. The amount of the semiconductor nanoparticles in the composition may affect the distance between adjacent semiconductor nanoparticles in the film, and the amount of the semiconductor nanoparticles in the composition may be adjusted within a range sufficient for forming a patterned film.
[0253] In the ink composition or the film (or the first region) obtained therefrom, the amount of the semiconductor nanoparticles (or the amount of the inorganic component) may be, based on the total solid content of the composition or the total weight of the film, less than 100 wt%, less than or equal to about 99.99 wt%, less than or equal to about 97 wt%, less than or equal to about 95 wt%, less than or equal to about 93 wt%, less than or equal to about 91 wt%, less than or equal to about 88 wt%, less than or equal to about 85 wt%, less than or equal to about 83 wt%, less than or equal to about 81 wt%, less than or equal to about 78 wt%, less than or equal to about 74 wt%, less than or equal to about 71 wt%, less than or equal to about 68 wt%, or less than or equal to about 65 wt%. The balance of the film may be an organic component (e.g., an organic ligand or an organic component derived from an additive).
[0254] The ink composition or the film may further include or may not substantially include a polymerizable monomer. The amount of the polymerizable monomer in the film may be less than or equal to about 5% by weight, less than or equal to about 3% by weight, less than or equal to about 1% by weight, less than or equal to about 0.5% by weight, less than or equal to about 0.1% by weight, or less than or equal to about 0.05% by weight, based on the total weight of the film. The polymerizable monomer may be a (meth) acrylic monomer having one or more carbon-carbon double bonds (e.g., two, three, or four or more carbon-carbon double bonds), a (meth) acrylic oligomer containing two, three, or four or more carbon-carbon double bonds, a vinyl monomer containing two, three, or four or more carbon-carbon double bonds, or a compound selected from a combination thereof. The polymerizable monomer may be or include a di(meth) acrylate compound.
[0255] The ink composition or the film may not include: an organic compound containing two or more azide groups (hereinafter referred to as an azide compound); an organic binder polymer having an acid value of greater than or equal to about 50 mg KOH / gram of polymer and soluble in an alkaline aqueous solution; a hole transport organic compound including an oxetane group or a vinyl group and an aromatic hydrocarbon group; or a combination thereof.
[0256] The azide compound may include bisperfluorophenyl azide, 3,4-diazide-1-(phenylmethyl)pyrrolidine, 1,2-diazidebenzene, 1,4-diazidebenzene, 1,5-diazidehexane, 1,1′-methylenebis(4-azidobenzene), 4,4′-diazidediphenylethane, 2,6-bis(4-azidobenzylidene)cyclohexanone, or a combination thereof. The organic binder polymer may have an acid value of greater than or equal to about 80 mg KOH / gram polymer to less than or equal to about 200 mg KOH / gram polymer. The hole transport organic compound may include N4,N4'-bis(4-(6-((3-ethyloxetan-3-yl)methoxy)hexyl)phenyl)-N4,N4'-diphenylbiphenyl-4,4'-diamine (OTPD), N4,N4'-bis(4-(6-((3-ethyloxetan-3-yl)methoxy)hexyl)phenyl)-N4,N4'-bis(4-methoxyphenyl)biphenyl-4,4'-diamine (QUPD), N,N'-(4,4'-(cyclohexane-1,1-diyl)bis(4,1-phenylene))bis(N-(4-(6-(2-ethyloxetan-2-yloxy)hexyl)phenyl)-N4,N4'-bis(4-methoxyphenyl)biphenyl-4,4'-diamine (QUPD), N-(4-(vinylphenyl)methoxy)phenyl)-N-(4-(vinylphenyl)-1-nitrophenyl)-3,4,5-trifluoroaniline) (X-F6-TAPC), N4,N4'-di(naphthalene-1-yl)-N4,N4'-bis(4-vinylphenyl)biphenyl-4,4'-diamine (VNPB), 9,9-bis[4-[(4-vinylphenyl)methoxy]phenyl]-N2,N7-di-1-naphthyl-N2,N7-diphenyl-9H-fluorene-2,7-diamine (VB-FNPD), 3,5-di-9H-carbazol-9-yl-N,N-bis[4-[[6-[(3-ethyl-3-oxetanyl)methoxy]hexyl]oxy]phenyl]-aniline (Oxe-DCDPA), or a combination thereof.
[0257] The composition or ink thus prepared can be applied to a substrate (e.g., on an electrode or charge auxiliary layer) to form a film. The application method is not particularly limited and can be appropriately selected. The application may include spin coating, inkjet printing, spraying, dip coating, nozzle printing, roll-to-roll printing or a combination thereof. In an embodiment, the application may include spin coating. In an embodiment, the spin coating may be carried out at the following rotational speeds: greater than or equal to about 100 revolutions per minute (rpm), greater than or equal to about 300rpm, greater than or equal to about 500rpm, greater than or equal to about 700rpm, or greater than or equal to about 900rpm and less than or equal to about 5000rpm, less than or equal to about 4000rpm, less than or equal to about 3500rpm, less than or equal to about 3000rpm, less than or equal to about 2500rpm, less than or equal to about 2000rpm, less than or equal to about 1500rpm, less than or equal to about 1000rpm, or less than or equal to about 800rpm.
[0258] In the film thus obtained, a portion corresponding to the first region may be exposed to radiation, and the solubility of the semiconductor nanoparticles in the first region relative to the first solvent may vary as described herein. Exposure to radiation may be selectively performed using a photomask. The energy of the radiation may be appropriately selected. The radiation may be light. The peak emission wavelength of the light may be greater than or equal to about 150 nm, greater than or equal to about 200 nm, greater than or equal to about 250 nm, greater than or equal to about 300 nm, or greater than or equal to about 350 nm. The peak emission wavelength of the light may be less than or equal to about 450 nm, less than or equal to about 400 nm, less than or equal to about 390 nm, less than or equal to about 380 nm, less than or equal to about 370 nm, less than or equal to about 365 nm, or less than or equal to about 360 nm. The radiation energy may be determined taking into account the absorption characteristics of the semiconductor nanoparticles. The dose (e.g., light intensity dose) of the radiation for the film may be greater than or equal to about 0.1 mJ / cm 2 , greater than or equal to about 0.5 mJ / cm 2 , greater than or equal to about 1 mJ / cm 2 , greater than or equal to about 5 mJ / cm 2 , greater than or equal to about 10 mJ / cm 2 , greater than or equal to about 15 mJ / cm 2 , greater than or equal to about 20 mJ / cm 2 , greater than or equal to about 25 mJ / cm 2 , greater than or equal to about 30 mJ / cm 2 , greater than or equal to about 35 mJ / cm 2 , greater than or equal to about 40 mJ / cm 2 , greater than or equal to about 45 mJ / cm 2 , greater than or equal to about 50 mJ / cm 2 , greater than or equal to about 100 mJ / cm 2 , greater than or equal to about 500 mJ / cm 2 , greater than or equal to about 600 mJ / cm 2 , or greater than or equal to about 650 mJ / cm 2 The radiation dose to the film may be less than or equal to about 5000 mJ / cm 2 , less than or equal to about 4000mJ / cm 2 , less than or equal to about 3500mJ / cm 2 , less than or equal to about 3000mJ / cm 2 , less than or equal to about 2500mJ / cm 2 , less than or equal to about 2000mJ / cm 2, less than or equal to about 1500mJ / cm 2 , less than or equal to about 1000mJ / cm 2 , less than or equal to about 900mJ / cm 2 , less than or equal to about 500mJ / cm 2 , less than or equal to about 200mJ / cm 2 , less than or equal to about 100 mJ / cm 2 , less than or equal to about 48mJ / cm 2 , less than or equal to about 40mJ / cm 2 , less than or equal to about 35 mJ / cm 2 , less than or equal to about 30 mJ / cm 2 , or less than or equal to about 25 mJ / cm 2 The method of the embodiment can obtain a patterned film with improved quality even at a relatively low dose of light.
[0259] In the method, it is believed that the patterning mechanism may include a thiol-ene reaction, and the resolution of the desired pattern can be changed by adjusting the amount of radiation exposure. An I-line UV light source can be used, and by using a relatively low dose (e.g., less than or equal to about 400 mJ / cm 2 , or less than or equal to about 200 mJ / cm 2 ), a pattern of 1 μm or less, such as 500 nm or 450 nm or 300 nm or 200 nm or less, can be obtained. In an embodiment, an I-line UV light source can be used, and by using a relatively high dose (e.g., 500 mJ / cm 2 or greater, or 600mJ / cm 2 or larger), a pattern of 1 μm or larger or 1.5 μm or larger can also be obtained. In an embodiment, the semiconductor nanoparticles may include perovskite nanocrystals (particles), and UV light of about 275 nm may be used as the radiation, and in this case, the desired resolution can be achieved, for example, even at a relatively low dose (e.g., 100 mJ / cm 2 or less, or 60mJ / cm 2 or smaller).
[0260] The exposure time to radiation is not particularly limited and can be appropriately selected. The exposure time can be 1 second or longer, 3 seconds or longer, 5 seconds or longer and 60 minutes or shorter, 30 minutes or shorter, 20 minutes or shorter, 10 minutes or shorter, 5 minutes or shorter, 50 seconds or shorter, 30 seconds or shorter, or 10 seconds or shorter.
[0261] The film including the exposed first area can be contacted with a developing solvent (e.g., a first solvent), whereby at least a portion of the film (e.g., an unexposed portion) can be removed to obtain a patterned film including the first area. The first solvent used to prepare the composition and the solvent used for development can be the same or different. The first solvent can include an organic solvent capable of dispersing the semiconductor nanoparticles. The organic solvent can be a polar solvent. The organic solvent can be a non-polar solvent. The change in the solubility of the exposed film relative to the first solvent can allow the semiconductor nanoparticles to have dissolution resistance to the first solvent. The details of the first solvent are the same as described herein.
[0262] To form a high-resolution pattern, the additive concentration, radiation exposure dose, and peak emission wavelength of the radiation may be controlled. The thickness of the pattern is not particularly limited and may be appropriately adjusted in consideration of the final use of the patterned film. In embodiments, the thickness of the pattern may be greater than or equal to about 1 nm, greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 15 nm, or greater than or equal to about 20 nm and / or less than or equal to about 100 μm, less than or equal to about 50 μm, less than or equal to about 30 μm, less than or equal to about 20 μm, less than or equal to about 10 μm, less than or equal to about 5 μm, less than or equal to about 1 μm, less than or equal to about 900 nm, less than or equal to about 500 nm, less than or equal to about 300 nm, less than or equal to about 200 nm, less than or equal to about 150 nm, less than or equal to about 100 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 30 nm, less than or equal to about 10 nm, or less than or equal to about 5 nm, or a combination thereof.
[0263] Method as described herein can provide for making semiconductor nanoparticles (or films comprising them) that can form colloidal dispersions relatively accurately patterned without the substantial damage of their optical or structural properties. In the method, the dual action of click chemistry reagents (i.e. compounds with two or more, three or four or more thiol groups) and the semiconductor nanoparticles used as photocatalysts can provide patterns of desired quality under relatively low radiation amounts. Unexpectedly, the inventors have found that, according to the method of the embodiment, the photocatalytic activity of the semiconductor nanocrystal particles can significantly increase the yield of thiol-ene reaction. This increase can make it possible to realize the crosslinking between the semiconductor nanocrystal particles, causing the solubility to change to the degree that can form patterns, without the need for additional photoinitiators. The semiconductor nanocrystal particles in the obtained pattern can show increased luminous efficiency.
[0264] The underlying patterning mechanisms for the photochemical transformation of surface ligands and additives by radiation include, for example, the formation of thiol-ene reactions and the initiation of thiol-ene reactions, as described herein.
[0265] The pattern obtained according to the method as described herein can show improved quality (having a high resolution feature size of less than or equal to about 1 μm and / or increased luminous efficiency). According to the method, a clean and relatively uniform pattern can be obtained. Advantageously, a pattern with relatively high resolution can be obtained with relatively high uniformity. The pattern thus prepared can have a relatively low surface roughness, for example, less than or equal to about 500nm, less than or equal to about 400nm, less than or equal to about 300nm, less than or equal to about 250nm, or less than or equal to about 200nm and greater than or equal to about 1nm, greater than or equal to about 10nm, greater than or equal to about 50nm, or greater than or equal to about 100nm.
[0266] The obtained patterned film (or the first region of the patterned film) may have a line width of less than or equal to about 100 μm, less than or equal to about 80 μm, less than or equal to about 50 μm, less than or equal to about 25 μm, less than or equal to about 15 μm, less than or equal to about 10 μm, less than or equal to about 8 μm, less than or equal to about 5 μm, less than or equal to about 3 μm, less than or equal to about 2 μm, or less than or equal to about 1 μm. As determined by electron microscopy analysis, the obtained patterned film may have a line edge roughness (LER) of less than or equal to about 500 nm, less than or equal to about 450 nm, less than or equal to about 400 nm, less than or equal to about 350 nm, less than or equal to about 300 nm, less than or equal to about 250 nm, less than or equal to about 220 nm, less than or equal to about 200 nm, less than or equal to about 190 nm, or a combination thereof. Methods for measuring line edge roughness are known in the art and may be based on electron microscopy analysis results (eg, scanning electron microscopy analysis).Measurement of line edge roughness may be easily and reproducibly performed using commercially available image analysis equipment.
[0267] The patterned film obtained can show increased stability. Surprisingly, the inventors have found that the film of patterned semiconductor nanocrystal particles can show or maintain similar qualities (e.g., luminous efficiency) as just after manufacturing, for example, even if it is placed under ambient conditions for a predetermined period of time (e.g., 10 days or more, 50 days or more, 100 days or 150 days or more).
[0268] In the XPS analysis of the obtained patterned film, the S2p spectrum may show a changing peak depending on the change of the additive (e.g., thiol moiety). 1 / 2and S2p 3 / 2 The peak intensity may be exhibited at reduced binding energies (e.g., 164 eV or less (e.g., 163 eV or greater, or 163.75 eV or less) and 163 eV or less (e.g., 162 eV or greater, or 162.82 eV or less)), respectively. Without wishing to be bound by any theory, it may represent a cross-linked portion between the additive and the ligand. In the method according to the embodiment, continuous orthogonal patterning of red, green, and blue patterns may be achieved. The method of the embodiment may provide a pattern of semiconductor nanocrystal particles (e.g., a patterned film) that exhibits increased photoluminescence quantum efficiency (PLQY) and photostability in such continuous patterning without additional post-processing. Therefore, the patterned film obtained according to the method of the embodiment may include a first region 1 configured to emit a first light. The patterned film may further include a second region 2 configured to emit a second light, a third region 3 configured to emit a third light, or a combination thereof (see Figure 1C ). The peak emission wavelength of the first light, the peak emission wavelength of the second light, and the peak emission wavelength of the third light may be different from each other. The second region may be formed by repeating the above-mentioned patterning process on a substrate having a patterned film including the first region. The third region may be formed by repeating the patterning method described herein on a substrate having a patterned film including the first region and the second region. A partition wall may or may not be independently provided between the first region and the second region, between the second region and the third region, and between the third region and the first region, respectively.
[0269] Patterning methods as described herein can be extended to the patterning of metal oxide nanoparticles, carbon dots, graphene quantum dots, high carrier mobility semiconductor polymers and even organic small molecules and semiconductor nanocrystal particles. The patterning method can contribute to the non-destructive high-resolution patterning associated with manufacturing a variety of electronic devices or optoelectronic devices or their integrated circuits.
[0270] The patterned film obtained according to the method described herein can be used as a light-emitting layer in a variety of electronic devices (such as electroluminescent devices or display devices), or as a color conversion layer or color conversion panel in a photoluminescent device or panel. The display panel or electronic device may include a light source (or a light-emitting panel) and a patterned film, and the light source may be configured to provide a predetermined wavelength of light (such as blue light) to the patterned film. The type of light source is not particularly limited, and may include LED, OLED or a combination thereof. The pattern obtained according to the method of the embodiment can be used for next-generation devices such as augmented reality helmets, stretchable displays, hyperspectral image sensors and smart medical devices.
[0271] In an embodiment, the electroluminescent device includes: a first electrode 1 and a second electrode 5, for example, spaced apart from each other (for example, each having a surface opposite to each other, that is, each having a surface facing each other); a light-emitting layer 3 disposed between the first electrode 1 and the second electrode 5; optionally, a hole transport layer 2 disposed between the light-emitting layer 3 and the first electrode 1; optionally, an electron transport layer 4 disposed between the light-emitting layer 3 and the second electrode 5. The light-emitting layer includes a pattern of a film, which includes a first region configured to emit a first light, and the first region includes semiconductor nanoparticles and a portion containing a carbon-sulfur bond, and the semiconductor nanoparticles are configured to emit the first light and exhibit resistance to dissolution to a predetermined first solvent. The hole transport layer may include a hole transport material and may not include the semiconductor nanoparticles. The hole auxiliary layer may include a hole transport layer (e.g., an organic compound), a hole injection layer, or a combination thereof (see Figure 3A , 3B and 3C).
[0272] The details of the light emitting layer are the same as for the patterned film comprising the first region described herein. The details of the first solvent are the same as described herein.
[0273] The first electrode 1 or the second electrode 5 may include an anode or a cathode. In one embodiment, the first electrode may include a cathode (or an anode), and the second electrode may include an anode (or a cathode). In one embodiment, the second electrode includes a cathode. In the electroluminescent device of the embodiment, the first electrode 10 or the second electrode 50 may be disposed on a (transparent) substrate 100. The transparent substrate may be a light extraction surface. (See Figure 3B and 3C ). The light-emitting layer may be disposed in a pixel in a display device.
[0274] In the electroluminescent device, the first electrode 10 or the second electrode 50 may be disposed on a (transparent) substrate 100. Figure 3B and Figure 3C In the light emitting (e.g., electroluminescent) device of the embodiment, the light emitting layer 30 may be disposed between a first electrode (e.g., an anode) 10 and a second electrode (e.g., a cathode) 50. The cathode 50 may include an electron injection conductor. The anode 10 may include a hole injection conductor. The work functions of the electron / hole injection conductors included in the cathode and the anode may be appropriately adjusted and are not particularly limited. For example, the cathode may have a small work function, and the anode may have a relatively large work function, or vice versa.
[0275] The electron / hole injection conductor may include a metal-based material (e.g., a metal, a metal compound, an alloy, or a combination thereof) (e.g., aluminum, magnesium, tungsten, nickel, cobalt, platinum, palladium, calcium, LiF, etc.), a metal oxide such as indium gallium oxide or indium tin oxide (ITO), or a conductive polymer (e.g., having a relatively high work function) such as polyethylenedioxythiophene, but is not limited thereto.
[0276] The first electrode, the second electrode or a combination thereof may be a light-transmitting electrode or a transparent electrode. In an embodiment, both the first electrode and the second electrode may be light-transmitting electrodes. The electrode may be patterned. The first electrode, the second electrode or a combination thereof may be disposed on a (e.g., insulating) substrate. The substrate may be optically transparent (e.g., may have the following light transmittance: greater than or equal to about 50%, greater than or equal to about 60%, greater than or equal to about 70%, greater than or equal to about 80%, greater than or equal to about 85%, or greater than or equal to about 90% and, for example, less than or equal to about 99%, or less than or equal to about 95%). The substrate may include an area for blue pixels, an area for red pixels, an area for green pixels or a combination thereof. A thin film transistor may be disposed in each area of the substrate, and one of the source and drain of the thin film transistor may be electrically connected to the first electrode or the second electrode.
[0277] The light-transmitting electrode may be disposed on a (eg insulating) transparent substrate. The substrate may be a rigid or flexible substrate. The substrate may include plastic or an organic material such as a polymer, an inorganic material such as glass, or a metal.
[0278] The light-transmitting electrode may be made of, for example, a transparent conductor such as indium tin oxide ("ITO") or indium zinc oxide ("IZO"), gallium indium tin oxide, zinc indium tin oxide, titanium nitride, polyaniline, LiF / Mg:Ag, etc., or a single-layer or multi-layer metal film, but is not limited thereto. If one of the first electrode and the second electrode is an opaque electrode, the opaque electrode may be made of an opaque conductor such as aluminum (Al), lithium-aluminum (Li:Al) alloy, magnesium-silver (Mg:Ag) alloy, or lithium fluoride-aluminum (LiF:Al) compound.
[0279] The thickness of each of the electrodes (the first electrode, the second electrode, or each of the first electrode and the second electrode) is not particularly limited and can be appropriately selected in consideration of device efficiency. For example, the thickness of the electrode may be greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 20 nm, greater than or equal to about 30 nm, greater than or equal to about 40 nm, or greater than or equal to about 50 nm. For example, the thickness of the electrode may be less than or equal to about 100 micrometers (μm), less than or equal to about 90 μm, less than or equal to about 80 μm, less than or equal to about 70 μm, less than or equal to about 60 μm, less than or equal to about 50 μm, less than or equal to about 40 μm, less than or equal to about 30 μm, less than or equal to about 20 μm, less than or equal to about 10 μm, less than or equal to about 1 μm, less than or equal to about 900 nm, less than or equal to about 500 nm, or less than or equal to about 100 nm.
[0280] The method of forming the electrode is not particularly limited and may be appropriately selected depending on the material. In an embodiment, the electrode may be formed by deposition, coating, or a combination thereof, but is not limited thereto.
[0281] The light-emitting layer 3, 30, QD disposed between the first electrode 1 and the second electrode 5 (e.g., the anode 10 and the cathode 50) may include semiconductor nanoparticles (e.g., blue light-emitting nanoparticles, red light-emitting nanoparticles, green light-emitting nanoparticles, or a combination thereof). The light-emitting layer may include a patterned semiconductor nanocrystal film as described herein.
[0282] For example, the first area of the patterned film of the embodiment can be set to correspond to the first pixel in the display device described herein. For example, the second area of the patterned film of the embodiment can be set to correspond to the second pixel in the display device described herein. For example, the third area of the patterned film of the embodiment can be set to correspond to the third pixel in the display device described herein. Each of the regions can be separated from an adjacent region (e.g., optically) by a partition wall. The partition wall may include a light blocking element such as a black matrix. In an embodiment, a partition wall may be set between the first region, the second region, and the third region. In an embodiment, the first region, the second region, and the third region are each optically isolated. (See Figure 1C )
[0283] For example, on the light-emitting layer, an electron auxiliary layer disposed between the second electrode and the light-emitting layer may be included. The electron auxiliary layer may include an electron transport layer based on an organic material. The types of organic materials are described herein. The electron auxiliary layer may include an electron transport layer based on zinc oxide nanoparticles. The electron transport layer may include zinc oxide nanoparticles. In an embodiment, a separate electron injection layer may be provided between the second electrode and the electron transport layer, but is not limited thereto. The electron transport layer may be provided adjacent to the light-emitting layer (e.g., directly above the light-emitting layer). In an embodiment, the electron transport layer may contact the light-emitting layer.
[0284] The zinc oxide (nanoparticles) may include: zinc; and optionally a Group IIA metal, Zr, W, Li, Ti, Y, Al, gallium, indium, tin (Sn), cobalt (Co), vanadium (V) or a combination thereof. The zinc oxide (nanoparticles) may include zinc, a Group IIA metal, and optionally an alkali metal.
[0285] The metal oxide may include zinc oxide, zinc magnesium oxide, or a combination thereof. The metal oxide may include Zn 1- x M x O, wherein M is Mg, Ca, Zr, W, Li, Ti, Y, Al or a combination thereof and 0≤x≤0.5. In the formula, x may be greater than or equal to about 0.01, greater than or equal to about 0.03, greater than or equal to about 0.05, greater than or equal to about 0.07, greater than or equal to about 0.1, greater than or equal to about 0.13, greater than or equal to about 0.15, greater than or equal to about 0.17, greater than or equal to about 0.2, greater than or equal to about 0.23, or greater than or equal to about 0.25. In the formula, x may be less than or equal to about 0.47, less than or equal to about 0.45, less than or equal to about 0.43, less than or equal to about 0.4, less than or equal to about 0.37, less than or equal to about 0.35, or less than or equal to about 0.3. The metal oxide (or zinc oxide) may further include magnesium. In an embodiment, the electron auxiliary layer (or the zinc oxide) may include Zn 1-x Mg x O (wherein x is greater than 0 and less than or equal to about 0.5, and x is the same as described herein), ZnO, or a combination thereof. The zinc oxide may further contain magnesium.
[0286] The zinc oxide nanoparticles may have a particle size (e.g., an average particle size) of about 1 nm or more, about 2 nm or more, about 2.5 nm or more, about 3 nm or more, or about 3.5 nm or more and about 10 nm or less, about 9 nm or less, about 8 nm or less, about 7 nm or less, about 6 nm or less, about 5 nm or less, or about 4.5 nm or less.
[0287] In an embodiment, the zinc oxide nanoparticles may be prepared by any suitable method, which is not particularly limited. The preparation of the zinc oxide nanoparticles may include a sol-gel reaction. In an embodiment, the zinc oxide (e.g., zinc magnesium oxide) nanoparticles may be prepared by placing a zinc compound (e.g., an organic zinc compound such as zinc acetate dihydrate) and optionally another metal compound (e.g., another organic metal compound such as magnesium acetate tetrahydrate) in an organic solvent (e.g., dimethyl sulfoxide) in a flask to have a desired molar ratio, and heating it at a predetermined temperature (e.g., about 40°C to about 120°C, or about 60°C to about 100°C) (e.g., in air), and adding a precipitation promoter solution (e.g., a solution of tetramethylammonium hydroxide pentahydrate and ethanol) at a predetermined rate while stirring (e.g., while stirring). The prepared zinc oxide nanoparticles (e.g., ZnO) may be recovered from the reaction solution. 1-x Mg x O nanoparticles), for example via centrifugation.
[0288] In an embodiment, the electron-assisting layer or the electron-transporting layer may be prepared by a solution process. In an embodiment, the electron-assisting layer or the electron-transporting layer may be prepared by dispersing a plurality of metal oxide nanoparticles in an organic solvent (e.g., a polar solvent, a non-polar solvent, or a combination thereof) to obtain an electron-transporting layer precursor dispersion, which is then applied to a surface to form a film. The electron-transporting layer precursor dispersion may be applied to the light-emitting layer. The solution process may further include removing an organic solvent from the formed film, for example by evaporation. The organic solvent may include a C1 to C10 alcohol solvent or a combination thereof.
[0289] In an embodiment, the electron auxiliary layer 4 or 40 may further include an electron injection layer, a hole blocking layer or a combination thereof. The electron injection layer, the hole blocking layer or a combination thereof may be disposed between the electron transport layer and the second electrode. In an embodiment, the hole blocking layer may be disposed between the light emitting layer and the electron transport layer. The thickness of the electron injection layer, the hole blocking layer or a combination thereof is not particularly limited and may be appropriately selected. The thickness of the electron injection layer, the hole blocking layer, or a combination thereof may be greater than or equal to about 5 nm, greater than or equal to about 6 nm, greater than or equal to about 7 nm, greater than or equal to about 8 nm, greater than or equal to about 9 nm, greater than or equal to about 10 nm, greater than or equal to about 11 nm, greater than or equal to about 12 nm, greater than or equal to about 13 nm, greater than or equal to about 14 nm, greater than or equal to about 15 nm, greater than or equal to about 16 nm, greater than or equal to about 17 nm, greater than or equal to about 18 nm, greater than or equal to about 19 nm, or greater than or equal to about 20 nm, and less than or equal to about 120 nm, less than or equal to about 110 nm, less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 30 nm, or less than or equal to about 25 nm.
[0290] In embodiments, materials for the electron transport layer, the electron injection layer, the hole blocking layer, or a combination thereof may include 1,4,5,8-naphthalenetetracarboxylic dianhydride ("NTCDA"), bathocuproin ("BCP"), tris[3-(3-pyridyl)-mesityl]borane ("3TPYMB"), LiF, tris(8-hydroxyquinoline)aluminum "(Alq 3 ”), tris(8-hydroxyquinoline)gallium” (Gaq 3 ”), tris(8-hydroxyquinoline)indium” (Inq 3 ”), bis(8-hydroxyquinoline)zinc (“Znq 2 ”), bis[2-(2-hydroxyphenyl)benzothiazole]zinc (“Zn(BTZ) 2 ”), bis(10-hydroxybenzo[H]quinolinolato)beryllium (“BeBq 2 ”), 8-(4-(4,6-di(naphthalen-2-yl)-1,3,5-triazin-2-yl)phenyl)quinolone (“ET204”), 8-hydroxyquinolate lithium (“Liq”), 2,2′,2″-(1,3,5-phenyltriyl)-tris(1-phenyl-1-H-benzimidazole) (“TPBi”), n-type metal oxides (e.g. ZnO, HfO 2etc.), 8-(4-(4,6-di(naphthalen-2-yl)-1,3,5-triazin-2-yl)phenyl)quinolone:8-hydroxyquinoline lithium ("ET204:Liq"), or a combination thereof, but not limited thereto.
[0291] In an embodiment, the electroluminescent device may further include a hole auxiliary layer. The hole auxiliary layer 2, 20 may be disposed between the first electrode 1, 10 and the light-emitting layer 3, 30. The hole auxiliary layer 2, 20 may include a hole injection layer, a hole transport layer, an electron blocking layer or a combination thereof. The hole auxiliary layer 2, 20 may be a single layer or a multilayer structure in which adjacent layers include different components. The hole auxiliary layer 2, 20 may be a single component layer or a multilayer structure in which adjacent layers include different components. The hole transport layer may include a hole transport material and may not include semiconductor nanoparticles.
[0292] The hole auxiliary layer 2, 20 may have a HOMO energy level that can match the HOMO energy level of the light-emitting layer 3 or the quantum dot layer 30 to enhance the mobility of holes transferred from the hole auxiliary layer 2, 20 to the light-emitting layer 3 or the quantum dot layer 30. In an embodiment, the hole auxiliary layer 2, 20 may include a hole injection layer close to (e.g., adjacent to) the first electrode 1, 10 and a hole transport layer close to (e.g., adjacent to) the light-emitting layer 3 or the quantum dot layer 30.
[0293] In an embodiment, the material included in the hole auxiliary layer 2, 20 (e.g., a hole transport layer, a hole injection layer, or an electron blocking layer) is not particularly limited, and may include, for example, poly(9,9-dioctyl-fluorene-co-N-(4-butylphenyl)-diphenylamine) ("TFB"), polyarylamine (polyarylamine), poly(N-vinylcarbazole), poly(3,4-ethylenedioxythiophene) ("PEDOT"), poly(3,4-ethylenedioxythiophene):polystyrene sulfonate ("PEDOT:PSS"), polyaniline, polypyrrolidone, polyvinyl ... pyrrole, N,N,N',N'-tetrakis(4-methoxyphenyl)-benzidine ("TPD"), 4,4'-bis[N-(1-naphthyl)-N-phenyl-amino]biphenyl ("α-NPD"), m-MTDATA (4,4',4"-tri[phenyl(m-tolyl)amino]triphenylamine), 4,4',4"-tri(N-carbazolyl)-triphenylamine ("TCTA"), 1,1-bis[(di-4-tolylamino)phenyl]cyclohexane ("TAPC"), p-type metal oxides (e.g., NiO, WO 3 、MoO 3 etc.), carbon-based materials such as graphene oxide, or combinations thereof, but are not limited thereto.
[0294] In the hole auxiliary layer, the thickness of each layer may be appropriately selected. For example, the thickness of each layer may be greater than or equal to about 5 nm, greater than or equal to about 10 nm, greater than or equal to about 15 nm, or greater than or equal to about 20 nm and less than or equal to about 100 nm, less than or equal to about 90 nm, less than or equal to about 80 nm, less than or equal to about 70 nm, less than or equal to about 60 nm, less than or equal to about 50 nm, less than or equal to about 40 nm, less than or equal to about 35 nm, or less than or equal to about 30 nm, but is not limited thereto.
[0295] The manufacture of the electroluminescent device according to the embodiment may include forming a hole auxiliary layer on a first electrode or a substrate on which the first electrode is formed (e.g., by vapor deposition or coating), and forming a light-emitting layer on the substrate or the hole auxiliary layer. The light-emitting layer is formed as described above. An electron auxiliary layer is formed on the light-emitting layer according to the selection, and a second electrode is formed thereon to manufacture an electroluminescent device. The method for forming the electrode and the hole auxiliary layer is not particularly limited, and may be selected depending on the electrode or the hole auxiliary layer material (e.g., formed by vapor deposition or coating).
[0296] Embodiments relate to patterned semiconductor nanocrystal films or electronic devices including electroluminescent devices including the same. Embodiments relate to patterned semiconductor nanocrystal films or display devices including electroluminescent devices including the same.
[0297] The display device or electronic device may include (or may be) a handheld terminal, a monitor, a laptop computer, a television, an electronic display board, a camera, or a component for an automatic (such as self-driving) vehicle (for example, a component of an automatic (such as self-driving) vehicle).
[0298] Hereinafter, the embodiments are described in more detail with reference to Examples. However, these Examples are exemplary, and the scope of the present invention is not limited thereto.
[0299] Example
[0300] Analytical methods
[0301] 1. Photoluminescence Analysis
[0302] The relative photoluminescence quantum yield (PLQY) and photoluminescence (PL) emission spectrum of each emissive nanomaterial film and solution were measured by integrating sphere and fluorescence spectrometer (JASCO FP-8550). For PL emission spectrum measurement, the solution was placed in a quartz sample cell (transparent small container, cuvette) and measured. In order to measure the PLQY of the solution, a mother solvent such as toluene can be placed in a PLQY quartz sample cell (2mm liquid cell 2x 10mm path length, 400μL sample volume) and the baseline is recorded. Next, the emissive nanomaterial dispersed in the mother solvent is placed in the same sample cell and the PL emission spectrum is measured again. From these two measurement data, the fluorescence spectrometer peak integral value (I 原始 ), the peak integral value of the sample by fluorescence spectrometer (I 样品 ) and the PL emission peak integral value of the sample (I 发射 ). The excitation wavelength for PL measurement is 360 nm, and the emission wavelength range for measurement is 300 to 800 nm. The relative PLQY is then calculated by the following equation:
[0303] Relative PLQY = I 发射 / (I 原始 -I 样品 )x100%.
[0304] 2. Optical and Scanning Microscopy Analysis
[0305] An optical microscope (Olympus BS51M) or a scanning microscope was used to obtain optical micrographs of the fabricated patterns.
[0306] 3.XPS analysis
[0307] X-ray photoelectron spectroscopy (XPS) spectra were measured in a nitrogen atmosphere by using a SigmaProbe (Thermo VG Scientific) with an Al (1486.7 eV) source. All data were calibrated to 284.8 eV by the C1s peak.
[0308] 4. Raman spectroscopy analysis
[0309] Raman measurement on LabRAM HR Evolution Visible_NIR (HORIBA), 3000-200cm -1 , resolution 2cm -1 The measurement was performed by using a 1064 nm infrared (IR) laser.
[0310] 5. TRPL Analysis
[0311] Time-resolved photoluminescence (TrPL) measurements of PeNC films were performed on a Fluorolog-QM (HORIBA).
[0312] Synthesis Example 1-1:
[0313] In a three-necked round-bottom flask, 0.5 g of Cs 2 CO 3 , 1.6 mL of oleic acid (OA) and 14 mL of 1-octadecene (ODE), and degassed at 60° C. for 1 hour. After degassed, the temperature of the mixture was increased to 120° C. to produce a clear Cs-oleate solution. Then, the Cs-oleate solution was maintained in a nitrogen atmosphere.
[0314] In a three-necked round-bottom flask, mix 700 mg of PbBr 2 , 1400 mg ZnBr 2 , 6 mL of OA, 7 mL of oleylamine (OLA) and 40 mL of ODE to form lead bromide PbBr 2 Solution. The lead bromide PbBr 2 The solution was degassed at 120°C for 1 hour. Then, the lead bromide PbBr 2 The solution was kept in a nitrogen atmosphere and its temperature was increased to 180°C. 2 When the temperature of the solution reaches 180°C (i.e., the reaction temperature), 3 mL of the Cs-oleate solution is quickly injected. After a reaction time of about 30 seconds to 1 minute, the reaction mixture is cooled to room temperature, and a non-solvent (e.g., acetone) is injected to promote the precipitation of nanoparticles. The reaction mixture is then centrifuged to obtain cesium lead bromide (CsPbBr 3 ) semiconductor nanoparticles. It was confirmed that the manufactured semiconductor nanoparticles emitted green light having an emission peak wavelength of about 510 nm.
[0315] Synthesis Example 1-2
[0316] In the same manner as in Synthesis Example 1-1, cesium lead bromide (CsPbBr 3 ) of semiconductor nanoparticles, except for the PbBr 2 The temperature of the solution was increased to over 80° C. It was confirmed that the prepared semiconductor nanoparticles could emit blue light.
[0317] Synthesis Example 2
[0318] Cadmium oxide (CdO), octadecylphosphonic acid and trioctylamine were placed in a reactor and heated at 150° C. under vacuum with stirring. 2After flowing into the reactor, the temperature was raised to 300°C to form a cadmium (Cd) solution. Selenium powder and trioctylphosphine (TOP) were reacted to form Se-TOP, which was then rapidly injected into the Cd solution at 300°C and reacted to prepare CdSe cores. The prepared cores were dispersed in toluene. Zinc acetate, oleic acid and trioctylamine were placed in a reaction flask and vacuum treated at 150°C. While N 2 After flowing into the reaction flask, the temperature is raised to 300°C. Sulfur powder and trioctylphosphine (TOP) react to obtain S-TOP. The toluene dispersion of the prepared CdSe core and S-TOP are then injected into the reaction flask and reacted. A non-solvent (ethanol) is added to promote the precipitation of nanoparticles, and the obtained precipitate is subjected to centrifugation to provide CdSe / ZnS semiconductor nanoparticles. Confirm that the prepared semiconductor nanoparticles emit blue light (peak emission wavelength: 470nm).
[0319] Synthesis Example 3
[0320] Indium acetate, palmitic acid and 1-octadecene were placed in a reactor and heated to 120°C under vacuum. After one hour, the atmosphere in the reactor was switched to nitrogen. After heating to 280°C, tris(trimethylsilyl)phosphine (TMS 3 InP semiconductor nanocrystal is provided in the reactor.The mixed solution of 1% tantalum (P) and trioctylphosphine is injected in the reactor rapidly and reacted 20 minutes.Reaction soln is cooled to room temperature rapidly, and adds acetone to it to promote the precipitation of nanoparticle, and the precipitate obtained thus is centrifugal to provide InP semiconductor nanocrystal.Described InP semiconductor nanocrystal is dispersed in toluene.
[0321] Zinc acetate, oleic acid and trioctylamine were placed in a reaction flask and vacuum treated at 120°C for 10 minutes. 2 After replacement, the temperature was raised to 220° C. The toluene dispersion of the InP semiconductor nanocrystal prepared above and S / TOP were placed in the reaction flask, and the temperature was raised to 280° C., and the reaction was allowed to proceed for 30 minutes. After the reaction was complete, the reaction solution was rapidly cooled to room temperature, a non-solvent (ethanol) was added to promote the precipitation of the reaction product, and centrifugation was performed to obtain InP / ZnS semiconductor nanoparticles.
[0322] The fabricated semiconductor nanoparticles emitted red light (peak emission wavelength: 620 nm).
[0323] Example 1: Patterning method
[0324] The cesium lead bromide semiconductor nanoparticles prepared in Synthesis Example 1 were washed three times with an acetate solvent (e.g., methyl acetate) and then dispersed in toluene to obtain a dispersion of 20 to 30 mg / mL semiconductor nanoparticles (hereinafter, PeNC). As a thiol compound, pentaerythritol tetrakis (3-mercaptopropionate) (hereinafter, PTMP) was dissolved in toluene to obtain a 0.025 M additive solution.
[0325]
[0326] As a pattern forming composition, a clear patternable ink was obtained by mixing 0.025 M of the additive solution and the semiconductor nanoparticle dispersion in an amount of 10 wt % of the semiconductor nanoparticles, and filtering the resulting mixture with a filter.
[0327] The obtained film-forming composition (patternable ink) was spin-coated on a glass or silicon substrate at a speed of 2000 rpm for about 30 seconds to produce a film. The film was then coated with a UV lamp (wavelength: 365 nm, power density 41 mW / cm 2 ) irradiates the fabricated film for about 10 seconds or less, and then removes the unexposed portion by contacting toluene to obtain a patterned film including the first region. An optical micrograph of the obtained patterned film is shown in Figure 4A and 4B In. From Figure 4A and 4B As a result, it was confirmed that a pattern having a line width of 10 μm or less could be obtained.
[0328] Without wishing to be bound by any theory, it is believed that rather than the formation of disulfide bonds, the thiol-ene reaction between the alkenyl groups in the ligand and the thiol groups in the additive is the primary pattern formation mechanism for photocatalytic patterning according to embodiments.
[0329] Evaluation Examples 1 to 3:
[0330] Raman spectroscopy analysis and XPS analysis were performed on the dispersion of semiconductor nanoparticles obtained in Example 1 and the film during the pattern formation process, and the results are shown in Figure 7 and 8 TRPL analysis was performed on the dispersion of semiconductor nanoparticles obtained in Example 1 and the film during the pattern formation process, and the results are shown in Fig. 9 middle.
[0331] Figure 7 Showing PeNC-PTMP thin films, CsPbBr patterned by direct photocatalytic patterning 3 Raman spectra of PeNC films (patterned PeNC), and Figure 8 For the original CsPbBr3 PeNC film (pristine NC), PeNC-PTMP film (formulated), UV-irradiated PeNC-PTMP film (UV-exposed), and patterned CsPbBr by direct photocatalytic patterning method 3 XPS S2p spectrum of PeNC film (developed).
[0332] In the Raman spectrum, the presence of PeNC is confirmed by the presence of -1 The presence of PTMP is indicated by a strong band at 2574 cm -1 The band at 1737 cm-1 (stretching mode of SH of thiol group) and -1 The other band at (stretching mode of carbonyl group (C=O)) is indicated. After UV irradiation and development, the intensity of thiol and ene stretching modes decreased significantly; this change confirmed that the thiol-ene reaction had proceeded. The reduced intensity of thiol and carbonyl stretching modes during development means that almost all unreacted PTMP molecules were removed due to its high solubility in toluene. The weak carbonyl stretching mode remaining after development is attributed to the residual PTMP molecules used as a cross-linking agent.
[0333] XPS S2p spectra confirmed the change in the form of the thiol group of PTMP. The S2p spectrum showed no signal in the original PeNC film, but appeared in the PeNC-PTMP blend film due to PTMP. After deconvolution of each S2p peak, the PeNC-PTMP blend showed a peak at 164.53 and 163.25 eV (S2p 1 / 2 and S2p 3 / 2 ), indicating the presence of PTMP. After UV exposure, the thiol-ene reaction leads to the formation of CSC bonds, resulting in a peak shift to lower binding energies (for S2p 1 / 2 and S2p 3 / 2 During the development process, the unreacted PTMP is removed, resulting in a decrease in the intensity of the S2p peak. Therefore, only the PTMP involved in cross-linking remains, and the binding energy is reduced (for S2p 1 / 2 and S2p 3 / 2 These results provide evidence that PTMP is retained in the patterned films as a cross-linking agent.
[0334] Based on the TRPL results, the average lifespan (τ average) is shown in Table 1 below.
[0335] Table 1
[0336] Classification τ average Original PeNC 3.53ns Patterned 6.26ns
[0337] As can be seen from Table 1, the pattern may have a significantly increased average lifetime compared to nanoparticles without the additive. These results indicate that in the presence of the additive, UV light irradiation does not destroy the structure of the nanoparticles, and instead may contribute to the preservation of their optical properties.
[0338] Embodiment 2:
[0339] A patterned film including semiconductor nanoparticles was prepared according to the same method as in Example 1, except that the CdSe / ZnS blue light-emitting semiconductor nanoparticles prepared in Synthesis Example 2 were used as the light-emitting material. An optical micrograph image of the prepared film pattern is shown in Figure 5 In. From Figure 5 As a result, it was confirmed that a pattern having a line width of 10 μm or less could be obtained.
[0340] Embodiment 3:
[0341] A patterned film including semiconductor nanoparticles was prepared according to the same method as Example 1, except that the InP / ZnS red light-emitting semiconductor nanoparticles prepared in Synthesis Example 3 were used as the light-emitting material. By optical microscopy analysis, it was confirmed that a pattern having a line width of 10 μm or less could be obtained.
[0342] Evaluation Example 4:
[0343] [1] In Example 1, PLQY was measured for each of the film obtained from the cesium lead bromide toluene dispersion (original), the formulation obtained from the composition for pattern formation, the film after exposure (UV-exposure), and the developed film after development, and the relative PLQY is summarized in Table 2 below.
[0344] Table 2
[0345] Classification Relative PLQY (%) Original 100 Preparation 106.9 UV-exposure 108.8 Developing 105.1
[0346] As confirmed from the above table, the pattern obtained by the method of the embodiment can show an increased PLQY compared to the PLQY in the semiconductor nanoparticle film state.
[0347] [2] In Example 3, the PLQY of the film obtained from the toluene dispersion solution of InP / ZnS nanocrystal particles, the film formulation obtained from the pattern forming composition, the film after exposure (UV-exposure) and the developed film after development were measured, and the relative PLQY is summarized in Table 3 below.
[0348] Table 3
[0349] Classification Relative PLQY (%) Original 100 Preparation 116.6 UV-exposure 117.1 Developing 115.1
[0350] As confirmed from Table 3, the pattern obtained by the method of the embodiment can show an increased PLQY compared to the PLQY in the semiconductor nanoparticle film state.
[0351] [2] In Example 1, the photostability was measured for a film obtained from a cesium lead bromide toluene dispersion (original NC) and a film pattern obtained from the composition for pattern formation, and the results are shown in Figure 6 The photostability measurement was performed to monitor the change in PLQY when the sample was irradiated with UV light having a high power wavelength of 365 nm.
[0352] Depend on Figure 6 It is confirmed that the film obtained by the method of the embodiment can show improved light stability.
[0353] Example 4
[0354] A patterned film of green-light-emitting PeNC was obtained in substantially the same manner as in Example 1 (ink composition preparation - film formation - exposure - development). A patterned film of red-light-emitting InP / ZnS was provided to the non-patterned portion of the obtained patterned film of PeNC nanoparticles in substantially the same manner as in Example 3. The results are shown in Fig.10 middle.
[0355] Fig.10 Results showing orthogonal patterning of green-emitting PeNC and red-emitting InP / ZnS nanoparticles. Fig.10 The results confirm that improved quality patterns are provided by continuous patterning without damaging adjacent patterns.
[0356] Example 5
[0357] A patterned QD-LED device with the following structure was fabricated:
[0358] Indium tin oxide (145nm) / poly(3,4-ethylenedioxythiophene):poly(styrene sulfonate) (40nm) / poly[(9,9-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine)] / PeNC patterned light-emitting layer (30nm) / 2,2',2"-(1,3,5-benzenetriyl)-tri(1-phenyl-1-H-benzimidazole) (50nm) / LiF (1nm) / Al (100nm).
[0359] Using the toluene dispersion of pristine PeNC and additives, a PeNC patterned light-emitting layer was patterned in the same manner as in Example 1. It was confirmed that the patterned device exhibited electroluminescence, which may indicate that the charge transport properties of the pattern may be substantially the same as the pristine PeNC film.
[0360] While the present disclosure has been described in connection with what are presently considered to be practical example embodiments, it is to be understood that the invention is not limited to the disclosed embodiments, but, on the contrary, is intended to cover various modifications and equivalent arrangements within the spirit and scope of the appended claims.
Claims
1. A method of manufacturing a patterned film having a first region configured to emit a first light, the method include: forming a first film including semiconductor nanoparticles and an additive, wherein the additive includes a polythiol compound including at least two thiol groups, and the semiconductor nanoparticles are configured to emit a first light, the semiconductor nanoparticles include an organic ligand, and the organic ligand includes a first functional group and a carbon-carbon unsaturated bond bonded to a surface of the semiconductor nanoparticle; exposing a portion of the first film corresponding to the first region to radiation to cause a change in the solubility of the semiconductor nanoparticles in the exposed area relative to the first solvent to form a radiation-treated film; as well as The radiation treated film is contacted with the first solvent to remove at least a portion of the unexposed area of the radiation treated film to obtain a patterned film having the first region. 2 . The method according to claim 1 , wherein the semiconductor nanoparticles are photocatalysts for a reaction between the organic ligand and the polythiol compound. 3 . The method according to claim 1 , wherein the polythiol compound comprises a dithiol compound, a trithiol compound, a tetrathiol compound, or a combination thereof.
4. The method according to claim 1, wherein the polythiol compound has a molecular weight of 50 g / mol to 5,000,000 g / mol, and Optionally, the polythiol compound further includes -O-, -CO-, -COO-, -NR-, -CONR-, a substituted or unsubstituted C1 to C20 alkylene group, a substituted or unsubstituted C2 to C20 alkenylene group, a substituted or unsubstituted C2 to C20 alkynylene group, or a combination thereof, and wherein R in -NR- and -CONR- is independently hydrogen or a C1 to C10 hydrocarbon group.
5. The method of claim 1, wherein the semiconductor nanoparticles comprise a II-VI group compound, a III-V group compound, a IV-VI group compound, a group IV element or a compound thereof, a II-III-VI group compound, a I-III-VI group compound, a I-II-IV-VI group compound, a metal halide perovskite compound, a transition metal chalcogenide perovskite compound, or a combination thereof, and wherein the first light has a red spectrum, a green spectrum or a blue spectrum, and optionally wherein a half width of the first light is greater than or equal to 1 nanometer and less than or equal to 55 nanometers.
6. The method according to claim 1, wherein the first functional group comprises a carboxyl group, a thiol group, an amine group, a phosphine group, a phosphine oxide group, an ester group, a hydroxyl group or a combination thereof, and The carbon-carbon unsaturated bond includes a carbon-carbon double bond.
7. The method of claim 1, wherein the organic ligand comprises a C1 to C50 aliphatic moiety.
8. The method according to claim 1, wherein in the first film, the amount of the semiconductor nanoparticles is greater than or equal to 60 wt % to less than or equal to 99.99 wt % based on the total weight of the first film, and The amount of the additive is greater than or equal to 0.01 wt % to less than or equal to 40 wt % based on the total weight of the first film.
9. The method according to claim 1, wherein in the first film, the amount of the polymerizable monomer is less than 10 wt % based on the total weight of the first film, and the polymerizable monomer is a (meth)acrylic monomer including two or more carbon-carbon double bonds, a (meth)acrylic oligomer including a carbon-carbon double bond, a vinyl monomer, or a combination thereof. 10 . The method of claim 9 , wherein in the first film, the amount of the polymerizable monomer is less than 1 wt % based on the total weight of the first film.
11. The method of claim 1 , wherein the first film does not include an organic compound containing two or more azide groups; an organic polymer having an acid value greater than or equal to 50 mg KOH / gram of organic polymer and soluble in an alkaline aqueous solution; an organic compound containing an oxetane group and an aromatic hydrocarbon group; or a combination thereof.
12. The method of claim 1, wherein the radiation is light having a peak emission wavelength greater than or equal to 150 nm and less than or equal to 450 nm, and The radiation dose is greater than or equal to 0.1 mJ / cm 2 And less than or equal to 5000mJ / cm 2 .
13. The method of claim 1, wherein the first solvent comprises an organic solvent capable of dispersing the semiconductor nanoparticles, and the organic solvent disperses the semiconductor nanoparticles in unexposed areas of the radiation-treated film.
14. The method of claim 1, wherein the patterned film has a relative luminous efficiency greater than or equal to 100% and less than or equal to 200% defined by the following equation: Relative luminous efficiency (%) = A / B x 100 where A is the quantum efficiency of the patterned film, and B is the quantum efficiency of a film comprising the semiconductor nanoparticles without the additive.
15. Electroluminescent devices, include: a first electrode and a second electrode, and a light-emitting layer between the first electrode and the second electrode, and a hole transport layer between the light-emitting layer and the first electrode, wherein the light emitting layer comprises a patterned film, the patterned film comprises a first region configured to emit a first light, wherein the first region is arranged to correspond to a first pixel of the electroluminescent device, wherein the first region of the patterned film comprises semiconductor nanoparticles and portions containing carbon-sulfur bonds, wherein the semiconductor nanoparticles are configured to emit the first light and exhibit resistance to dissolution by a first solvent, wherein the first solvent comprises toluene, octane, hexane, chlorobenzene, dichlorobenzene, chloroform, xylene or a combination thereof, and The hole transport layer includes a hole transport material but does not include the semiconductor nanoparticles.
16. The electroluminescent device of claim 15, wherein the moiety containing a carbon-sulfur bond connects two or more semiconductor nanoparticles, wherein the semiconductor nanoparticles include a II-VI group compound, a III-V group compound, a IV-VI group compound, a IV group element or a compound thereof, a II-III-VI group compound, a I-III-VI group compound, a I-II-IV-VI group compound, a metal halide perovskite compound, a transition metal chalcogenide perovskite compound, or a combination thereof, and The first light has a red spectrum, a green spectrum or a blue spectrum. 17 . The electroluminescent device according to claim 15 , wherein the light-emitting layer has a carbon content greater than or equal to 1 wt % and less than or equal to 50 wt % based on the total weight of the light-emitting layer.
18. The electroluminescent device of claim 15, wherein the light-emitting layer does not include a chemical substance formed by a reaction between an azide group and an alkyl group; an organic polymer having an acid value greater than or equal to 50 mg KOH / gram of organic polymer and soluble in an alkaline aqueous solution; or a combination thereof.
19. The electroluminescent device of claim 15, wherein the electroluminescent device further comprises an electron transport layer between the light emitting layer and the second electrode, and the electron transport layer comprises zinc oxide nanoparticles.
20. A display device comprising the electroluminescent device according to any one of claims 15 to 19.