Metal organic framework (MOF) glass composites comprising metal halide perovskite

By combining MOF glass with metal halide titanite, a stable MOF glass composite material is formed, which solves its decomposition and stability problems in moisture, heat, light and polar solvents, improves mechanical and optical properties, and achieves Long-term stability in water and organic solvents.

CN118829643APending Publication Date: 2024-10-22THE UNIVERSITY OF QUEENSLAND +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202280072122.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2021-08-31
Filing Date
2022-08-30
Publication Date
2024-10-22

AI Technical Summary

Technical Problem

Metal halide perovskites face problems such as decomposition, toxic ion leaching, deep trap electronic states, and polymorphic transitions in applications, resulting in poor stability in moisture, heat, light, and polar solvents, and the mechanical properties of composite materials Stability and functionality are limited.

Method used

Using metal-organic framework (MOF) glass composites, MOF glass is combined with metal halide perovskites to form amorphous MOF glass through sintering and quenching steps, providing chemical, optoelectronic, thermal and morphological stability, and through interfacial interactions Passivated surface defects in metal halide titanites.

Benefits of technology

It significantly inhibits the decomposition and toxic ion leaching of metal halide titanite, improves the mechanical stability and optical activity of the composite material, extends the photoluminescence lifetime, and remains stable in water and organic solvents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118829643A_ABST
    Figure CN118829643A_ABST
Patent Text Reader

Abstract

The invention relates to a metal organic framework (MOF) glass composite material containing metal halide perovskite and a preparation method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to composite materials, and more particularly to a composite material comprising metal halide perovskite. Background Art

[0002] Metal halide perovskites have attracted much attention for applications in photovoltaics, light-emitting diodes, radiation detection, and thermometry due to their attractive optoelectronic properties. In this regard, metal halide perovskites exhibit tunable bandgaps, long charge carrier lifetimes, and narrow-band and bright photoluminescence (PL). These properties make metal halide perovskites more attractive as active materials in optoelectronic devices compared to conventional binary II-VI, III-V, and IV-VI semiconductors.

[0003] However, the practical application of metal halide perovskites faces formidable obstacles, which are mainly related to the following tendencies of metal halide perovskites: (i) to easily decompose upon exposure to moisture, heat, light, oxygen, and polar solvents; (ii) to leach toxic heavy metal ions; (iii) to exhibit a high concentration of deep-trapped electronic states; and (iv) to have inherent polymorphism in the crystal structure.

[0004] To minimize the adverse effects of the above limitations, stabilization strategies based on forming a protective shell of organic ligands around the metal halide perovskite microparticle core have been reported. However, while providing a passivating shell helps maintain the optoelectronic integrity of the metal halide perovskite core, the stabilization effect is short-lived, the fabrication process is complex, and the processing performance is limited.

[0005] Other strategies include fabricating composites in which metal halide perovskites are fixed on a passivating substrate. However, the inherent ionic nature of metal halide perovskites is not conducive to composite fabrication. The functionality of the composites can be severely affected, including aggregation / decomposition of metal halide perovskites, poor mechanical stability of the composites due to weak interfacial bonding with the chosen matrix, and the formation of a high concentration of electronic defects (trap states).

[0006] Therefore, there is still opportunity to develop metal halide perovskite-based materials that can address the limitations of existing technologies. Summary of the invention

[0007] The present invention provides a metal organic framework (MOF) glass composite material comprising metal halide perovskite.

[0008] By "MOF glass" is meant that the MOF is a solid amorphous MOF (also referred to herein as "aMOF"). Thus, the MOF glass used and the MOF glass forming part of the composite material exhibits the thermally induced solid-liquid transition associated with an amorphous MOF.

[0009] The so-called MOF glass is a "composite material", which means that MOF glass is combined with metal halide perovskite. For example, the MOF glass composite material of the present invention can be in the form of a solid amorphous MOF matrix in which metal halide perovskite particles are distributed.

[0010] It has been advantageously discovered that providing the metal halide perovskite with the MOF glass in a composite form prevents or at least significantly inhibits the occurrence of one or more of the following: (i) decomposition of the metal halide perovskite upon long-term exposure to moisture, heat, light, and polar solvents; (ii) leaching of toxic heavy metal ions; (iii) formation of deep-trapped electronic states; and (iv) polymorphic transformation of the metal halide perovskite to an optically inactive crystalline phase.

[0011] Surprisingly, it was found that MOF glass can provide excellent chemical, optoelectronic, thermal and morphological stability for metal halide perovskites compared to other supports such as crystalline MOFs. In addition, MOF glass provides higher molecular and morphological flexibility relative to crystalline material stars, which is beneficial for the use of macroscopic devices. Therefore, amorphous MOF can more effectively passivate the surface defects of metal halide perovskites.

[0012] For example, compared to their crystalline MOF counterparts, MOF glass is not hindered by rigid structural constraints and can be easily deformed around the morphological features of perovskites. As a result, the surface passivation of metal halide perovskites is more effective. In addition, the stronger and more extensive interfacial interactions between MOF glass and metal halide perovskites also significantly improve the mechanical stability of the composites.

[0013] Therefore, the present invention can also be understood to relate to a MOF glass composite material, which includes a MOF glass matrix in which metal halide perovskite is encapsulated.

[0014] In some embodiments, the MOF glass is a zeolitic imidazolate framework (ZIF) glass. Therefore, in these embodiments, the amorphous component of the MOF glass composite is a solid amorphous ZIF (also referred to herein as "aZIF"). Due to its chemical stability, aZIF can effectively protect metal halide perovskites from erosion by water and organic solvents, as well as ensure the mechanical and thermal stability of the prepared glass composite. In addition, the high processability of aZIF makes it an ideal candidate material for large-scale production of ZIF-perovskite glass composites.

[0015] The special interfacial interaction between aZIF and metal halide perovskites can not only stabilize the metastable and optically active polycrystalline perovskite phase, but also passivate the Lewis acid and base surface defects of the perovskite, allowing electron transport in this heterostructure. In addition, the interfacial interaction between amorphous ZIF and metal halide perovskites is also observed to effectively passivate the under-coordinated metal or halide sites and negatively charged metal halide anti-sites on the metal halide perovskite surface.

[0016] Due to its structural flexibility, the MOF glass described herein has been found to be an effective passivation support for various metal halide perovskites. Therefore, the composite material of the present invention may include a metal halide perovskite, which is one or more of a lead halide perovskite, a tin halide perovskite, a germanium halide perovskite, and a double perovskite (such as a silver bismuth halide double perovskite). In some embodiments, the metal halide perovskite is selected from one or more of the following: CsPbI3, CsPbBr3, CsPbCl2Br, CsPbCl 1.5 Br 1.5 , MAPbI3, MAPbBr3, FAPbI3, (C4H9NH3)2PbBr4, CsPbCl2Br, CsPbCl 1.5 Br 1.5 、CsPbClBr2、CsPbCl 0.75 Br 2.25 、CsPbCl 0.5 Br 2.5 、CsPbBr 2.5 I 0.5 、CsPbBr 2.25 I 0.75 、CsPbBr2I、CsPbBr 1.5 I 1.5 、CsPbBrI2、CsPbBr4 4- 、(MAPbI3) 0.95 (FAPbI3) 0.05 and 2D perovskites, where MA is methylammonium and FA is formamidine.

[0017] The present invention also provides a method for manufacturing a MOF glass composite material containing metal halide perovskite, the method comprising the following steps: (a) mixing MOF and metal halide perovskite to obtain a precursor mixture; (b) sintering the precursor mixture so that the MOF is liquefied and covers the metal halide perovskite; (c) quenching the sintered precursor mixture to vitrify the liquefied MOF and form a MOF glass composite material.

[0018] The combination of the proposed method steps promotes the formation of an amorphous MOF, which effectively passivates the guest perovskite. The MOF is embedded in the metal halide perovskite by sintering the precursor mixture to form a liquefied MOF around the metal halide perovskite. As the sintered mixture is quenched, the liquefied MOF vitrifies and solidifies in an amorphous form, forming the final structure of the MOF glass composite.

[0019] By promoting the sintering and subsequent vitrification of MOFs, the proposed method overcomes the inherent limitations of attempting to encapsulate perovskites in crystalline MOFs. Since vitrified MOFs do not have the rigid microstructure of the corresponding crystalline MOFs, there are no structural constraints that limit the range and morphology of metal halide perovskites that can be encapsulated within the MOFs. Therefore, an advantage of the present method is that a large number of MOFs can now be combined with a wide range of metal halide perovskites.

[0020] As long as the sintering and quenching steps can form MOF glass, the MOF used in the precursor mixture can be a crystalline MOF, a MOF glass, or both. In some embodiments, the MOF in the precursor mixture includes at least one of a crystalline MOF and a MOF glass. For example, the precursor mixture may include at least one of crystalline MOF particles and MOF glass particles. In some embodiments, the precursor mixture is mainly composed of MOF glass particles.

[0021] Advantageously, the combination of sintering and quenching also effectively reduces bulk crystal defects of metal halide perovskites in the resulting MOF glass composites. This is reflected in the significantly improved crystallinity of the perovskites used in the proposed method. In this regard, it has been observed that higher quenching rates reduce the defect density in the crystal structure of metal halide perovskites. Combining sintering and quenching also allows to obtain and stabilize optically active crystalline phases of metal halide perovskites (which are themselves metastable) in vitrified MOF glasses.

[0022] In some embodiments, the sintering temperature of the precursor mixture is at least 100° C. These sintering temperatures have been shown to be particularly advantageous for achieving effective liquefaction of MOFs, as well as amorphization when using crystalline MOFs in the mixing step. More advantageously, the proposed sintering temperatures can also obtain optically active crystalline phases of metal halide perovskites.

[0023] In some embodiments, the quenching rate of the sintered precursor mixture is at least 20° C. / minute. These conditions are particularly advantageous for minimizing the crystal structure defect density of the metal halide perovskite in the resulting MOF glass composite.

[0024] Vitrified MOF glass is a strong host material that can provide an effective and potential microporous physical barrier to protect the metal halide perovskite host from external interference or degradation. Therefore, the MOF glass composite material of the present invention represents a step towards large-scale practical application of metal halide perovskite-based materials in application fields such as optoelectronics, catalysis, sensing and data encryption. Due to its structural and chemical stability, vitrified MOF glass can effectively protect metal halide perovskites from organic solvents (e.g., non-polar solvents, polar-protic solvents, polar-aprotic solvents), heat, water and mechanical stress.

[0025] Other aspects and / or embodiments of the invention are discussed in more detail below. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Embodiments of the present invention will now be described with reference to the following non-limiting drawings:

[0027] Figure 1 CsPbI3 as a pure compound or as (CsPbI3) (a g Schematic diagram of the crystallization phase transition of the guest phase in the ZIF-62 composite material and the corresponding transition temperature;

[0028] Figure 2 Shown are (CsPbI3) sintered at increasing sintering temperatures up to 350°C measured at room temperature 0.25 (a g ZIF-62) 0.75 In situ powder X-ray diffraction (XRD) of the composite material. Some non-overlapping peaks belonging to PbI2 and δ-CsPbI3 are highlighted in the figure;

[0029] Figure 3 Shown with the corresponding (CsPbI3) (a g Zoomed PL emission spectra of the (ZIF-62) (25 / 75) precursor mixture measured before sintering (peaks on the left concentrated in the 400-600 nm wavelength region) compared to (CsPbI3) sintered at increasing sintering temperatures from 150°C to 350°C 0.25 (a g ZIF-62) 0.75 Photoluminescence (PL) emission spectra of the composites;

[0030] Figure 4 The results are shown for the corresponding (CsPbI3) sintered to 150 °C (a g ZIF-62) (25 / 75) precursor mixture, (CsPbI3) fabricated at different sintering temperatures ranging from 200°C to 350°C 0.25 (a gZIF-62) 0.75 Ultraviolet-visible (UV-vis) absorption spectra of glass composites;

[0031] Figure 5 Shown (CsPbI3) 0.25 (a g ZIF-62) 0.75 Phase distributions of γ-phase and δ-phase of CsPbI3 in glass composite samples as mapped by (A) annular dark field-scanning transmission electron microscopy (ADF-STEM), (b) scanning electron diffraction-scanning transmission electron microscopy (SED-STEM); and (C) shown in the corresponding CsPbI3 crystal phase classification.

[0032] Figure 6 Shown are (E) the cathodoluminescence-scanning transmission electron microscopy (CL-STEM) integrated CL intensity map (scale bar, 70 nm), (F) the CL spectra acquired at each STEM probe position, and the sum of the CL spectra for the entire area in (E);

[0033] Figure 7 The microstructural evolution of the MOF glass composites of the embodiments during sintering and subsequent quenching is shown, in particular, (a) for (CsPbI3) sintered up to 350°C and then quenched (a g Temperature-resolved in situ powder XRD measurements of ZIF-62) (25 / 75) precursor blends, with the signature Bragg peak hkl of α-CsPbI3 (Pm-3m) as reference; (b) Evolution of the corresponding average size of α-CsPbI3c crystals calculated from powder XRD;

[0034] Figure 8 (D) shows the temperature-resolved second derivative in situ THz-FIR spectrum of the powder mixture during the first heating from 25°C to 300°C (at 20°C / min) under argon, (E) (CsPbI3) (a g ZIF-62) (25 / 75) powder mixture and (CsPbI3) 0.25 (a g ZIF-62) 0.75 of 133 Cs MAS NMR spectrum (in the figure, the symbol * indicates the rotating sideband, Indicates weak signal of CsI);

[0035] Fig. 9 Shown (CsPbX3) 0.25 (a g ZIF-62) 0.75Normalized photoluminescence (PL) emission spectra of glass composites, X is different halides or mixed halides, top to bottom in the inset list corresponds to the emission spectra from left to right;

[0036] Fig.10 (C) PL intensity of MOF glass composites before exposure to solvent, (CsPbI3) 0.25 (a g ZIF-62) 0.75 PL peak intensity of glass composites after sonication in different types of solvents for about 20 h, and (D) time evolution of PL intensity of glass composites before immersion in Milli-Q water, (CsPbI3) 0.25 (a g ZIF-62) 0.75 Temporal evolution of PL intensity of glass composites immersed in Milli-Q water;

[0037] Fig.11 (F) shows a sintered to 325 °C g ZIF-62 and (CsPbI3) 0.25 (a g ZIF-62) 0.75 CO2 adsorption isotherm at 273 K, where the adsorption and desorption data points are shown as closed and open symbols, respectively; and

[0038] Fig.12 Schematic diagram showing (G) an embodiment MOF glass composite material used as a photocatalytic material, and (H) relative to (CsPbI3) 0.25 (a g ZIF-62) 0.75 Glass composite samples were prepared by using pure a g Inductively coupled plasma-optical emission spectroscopy (ICP-OES) of ZIF-62 measured Ag after photodeposition test + / Zn + Concentration ratio (%). DETAILED DESCRIPTION

[0039] The invention provides a metal organic framework (MOF) glass composite material.

[0040] It is well known that MOF is a mixed coordination structure formed by metal clusters composed of metal ions (such as metal ions or metal oxides) coordinated with multifunctional organic ligands. The one-dimensional, two-dimensional or three-dimensional structure formed thereby can be porous.

[0041] The traditional MOF field is dominated by crystalline MOFs, in which metal clusters are coordinated by multifunctional organic ligands to form highly ordered crystal structures and patterns, thereby forming materials with ultra-high specific surface areas. In contrast, as "MOF glass", MOF is a solid-state amorphous MOF (also referred to as "aMOF" here).

[0042] Solid-state amorphous MOFs (also called "aMOFs") retain the basic building blocks and connectivity of their crystalline counterparts, but lack any long-range periodic order. In amorphous MOFs, metal clusters and multifunctional organic ligands form a framework with no detectable spatial order. Due to the non-periodic arrangement of atoms, the X-ray diffraction patterns produced by aMOFs do not exhibit the typical sharp Bragg diffraction peaks as in crystalline diffraction patterns, but are dominated by broad "humps" caused by diffusion. Therefore, aMOFs are largely indistinguishable from each other by XRD diffraction measurements.

[0043] The presence of inorganic and organic domains in aMOFs provides multiple opportunities to tailor the physicochemical properties of the MOF glass composites of the present invention, such as porosity, phase transition behavior, affinity, mechanical rigidity / toughness, and optical properties.

[0044] Amorphous MOFs suitable for use in the present invention undergo a reversible solid-liquid transition when heated below their thermal decomposition point, similar to the transition observed in amorphous silica, etc. The thermally induced solid-liquid transition in aMOF is caused by at least partial rupture of the metal-ligand coordination bonds, but this rupture maintains the integrity of the inorganic and organic building blocks in the liquid phase. From a macroscopic perspective, the solid-liquid transition exhibited by aMOF is associated with the transformation of the MOF into a soft, flowable liquid state before thermal decomposition.

[0045] Examples of metal ions that form part of the aMOF structure suitable for use in the present invention include Zn 2+ 、Co 3+ 、Co 2+ 、Ni 2+ , Pd 4+ , Pd 2+ , Pt 4+ , Pt 2+ , Cu 2+ , Cu + 、Na + , Fe 3+ , Fe 2+ , Os 2+ , Ir 2+ 、Ag + and combinations thereof.

[0046] Examples of multifunctional organic ligands that form part of an aMOF structure suitable for use in the present invention include imidazolate, 2-methylimidazolate, 2-nitroimidazolate, 5-chlorobenzimidazole, 4-methyl-5-nitroimidazolate, imidazolate-2-carbaldehyde, imidazole-4,5-dicarboxylate, benzene-1,4-dicarboxylate, 1,3,5-tris(4'-carboxyphenyl)benzene, 2,4,6-tris(4-pyridyl)triazine, and combinations thereof.

[0047] Further examples of amorphous MOFs suitable for use in the present invention and corresponding synthesis methods include those described in Bennett et al., Nature Reviews Materials, Vol. 3, pp. 431-440 (2018) and Bennett et al., Accounts of Chemical Research, Vol. 47, pp. 1555-1562 (2014) .

[0048] In some embodiments, the MOF is a mixed component MOF (also called a "mixed ligand" MOF). A mixed component MOF has a structural feature of containing more than one organic ligand and / or metal.

[0049] In some embodiments, aMOF is an amorphous zeolitic imidazolate framework (aZIF). Structurally, amorphous ZIF is a non-crystalline three-dimensional framework made of tetrahedral monovalent, divalent or trivalent transition metal ions connected by imidazolate-based ligands. Therefore, the amorphous ZIF used in the present invention includes a ZIF having the above structure and being able to show thermally induced reversible solid-liquid transition below its decomposition temperature.

[0050] Examples of ZIFs suitable for the present invention include ZIFs having an amorphous structure in which tetrahedral Zn 2+ or Co 2+ Coordinated by imidazolate-based bridging units. For example, amorphous ZIFs suitable for the present invention include tetrahedral Zn 2+ or Co 2+ Those ZIFs coordinated by a bridging unit, such as an imidazolate ("Im", C3H3N2 - ), 2-methylimidazolate ("mIm", C4H5N3 - )、2-nitroimidazole salt ("nIm", C3H2N3O2 - ), benzimidazole salt ("bIm", C7H5N2- ), 5-chlorobenzimidazole salt ("cbIm", C7H4N2Cl - ), 5-methylbenzimidazolate (“5-mbIm”, C8H7N2 - ), 4-methyl-5-nitroimidazole ester ("mnIm", C4H4N3O2 - ), imidazolate-2-carboxaldehyde ("ICA", C4H3N2O - ) or imidazole-4,5-dicarboxylate ("ImDC", C5HN2O4 - ).

[0051] In some embodiments, the amorphous ZIF is selected from aZIF-1, aZIF-3, aZIF-4, aCo-ZIF-4, aZIF-8, aZIF-62, aZIF-76, aZIF-69, aZIF-UC-2, aZIF-UC-3, aZIF-UC-4, aZIF-UC-5, and combinations thereof known in the art.

[0052] In some embodiments, the aZIF is aZIF-4. The aZIF undergoes a reversible solid-liquid transition at a temperature of about 292°C, and thus has high processability. Structurally, aZIF-4 is characterized by Zn 2+ The center is coordinated with four imidazole ligands to form a continuous random network topology that is different from the corresponding crystals and similar to amorphous silica.

[0053] In some embodiments, aZIF is aZIF-62. Structurally, aZIF-62 is characterized by Zn 2+ The center is connected to the benzimidazole ligand ("bIm", C7H5N2 - ) to form Zn(Im) 1.75 (bIm) 0.25 Skeleton. Similar to aZIF-4, aZIF-62 has high processability due to its inherent low reversible solid-liquid transition temperature (about 430°C). In addition, aZIF-62 has a large temperature range and the resulting liquid is stable before decomposing at around 550°C. Another benefit of using aZIF-62 is that aZIF-62 has extremely high crystallization stability, which is attributed to the high viscosity of its liquid phase. These properties make ZIF-62 particularly useful in the composite materials of the present invention to achieve effective surface passivation and protection of metal halide perovskites.

[0054] In some embodiments, the aZIF is a mixed ligand aZIF. In a mixed ligand aZIF, the metal center is coordinated by at least two different types of multifunctional organic ligands. It may be particularly advantageous to use a mixed ligand aZIF. By changing the properties and relative amounts of the organic ligands, the solution-liquid transition temperature of the MOF glass composite can be adjusted. Examples of mixed ligand aZIFs suitable for the present invention include those obtained by replacing a portion of conventional ligands of a given aZIF with functionalized ligands (e.g., halogenated ligands). The halogenated ligand can be a ligand derived from a benzimidazole ester. The ligand derived from a benzimidazole ester can be selected from 5-chlorobenzimidazole ester ("5-ClbIm", C7H4N2Cl - ), 5-chloro-2-methylbenzimidazole ester ("5-Cl-2-mbIm", C8H6N2Cl - ), 5-fluorobenzimidazole ester ("5-FbIm", C7H4N2F - ) and 6-chloro-5-fluorobenzimidazole ester ("6-Cl-5-FbIm", C7H3N2ClF - ).

[0055] In some embodiments, the aZIF is a mixed ligand aZIF based on aZIF-62, wherein a portion of the benzimidazole ester ligands in aZIF-62 are replaced by a benzimidazole ester-derived ligand, such as 5-chlorobenzimidazole ester (“5-ClbIm”, C7H4N2Cl - ), 5-chloro-2-methylbenzimidazole ester ("5-Cl-2-mbIm", C8H6N2Cl - ), 5-fluorobenzimidazole ester ("5-FbIm", C7H4N2F - ) and 6-chloro-5-fluorobenzimidazole ester ("6-Cl-5-FbIm", C7H3N2ClF - ). Examples of such mixed-ligand aZIFs and corresponding synthesis methods are described in Hou et al., "Halogenated Metal-Organic Framework Glasses and Liquids", Journal of the American Chemical Society 2020, 142, 3880-3890, the contents of which are incorporated herein in their entirety.

[0056] The composite materials of the present invention include metal halide perovskites.

[0057] The term "perovskite" is used herein according to its ordinary meaning in the art to refer to the "perovskite crystal structure" of certain metal halides, rather than specifically to perovskite material (CaTiO3).

[0058] Therefore, for the purposes of this specification, the expression "metal halide perovskite" should be understood to include any crystalline material having the same crystal structure as CaTiO3 and the general stoichiometry AMX3 (three-dimensional structure perovskite) or A2MX4 (two-dimensional structure or layered perovskite), wherein A is a monovalent cation, M is a divalent Group IVA metal cation, and X is a halide anion. A can be an inorganic cation (such as Cs + or Sn + ) or organic cations (such as CH3NH3 + 、C4H9NH3 + or C6H5–C2H4NH2 + ), M is a divalent IVA group metal cation (such as Pb 2+ Sn 2+ Or Ge 2+ ), X can be a halide anion. The halide anion can be an anion of a halide element (such as F - , Cl - Br - or I - ), or a mixed halide anion, in which case the X3 or X4 component in the above formula is composed of two or more halide elements in appropriate proportions (e.g., Cl2Br 3- , Cl 1.5 Br 1.5 3- 、ClBr2 3- , Cl 0.75 Br 2.25 3- , Cl 0.5 Br 2.5 3- Br 2.5 I 0.5 3- Br 2.25 I 0.75 3- Br2I 3- Br 1.5 I 1.5 3- BrI2 3- or Br4 4- ).

[0059] In some embodiments, the metal halide perovskite is a lead halide perovskite (LHP). In these cases, M is lead (Pb). Lead halide perovskites are particularly attractive due to their many potential applications, including solar cells, photovoltaics, lasers, light emitting diodes (LEDs), water separation, and laser cooling. Examples of LHPs suitable for use in the present invention include CsPbI3, CsPbBr3, CsPbCl2Br, CsPbCl 1.5 Br 1.5 、MAPbI3(MA=methylammonium), MAPbBr3、FAPbI3(FA=formamidinium), (C4H9NH3)2PbBr4、CsPbCl2Br、CsPbCl 1.5 Br 1.5 、CsPbClBr2、CsPbCl 0.75 Br 2.25 、CsPbCl 0.5 Br 2.5 、CsPbBr 2.5 I 0.5 、CsPbBr 2.25 I 0.75 、CsPbBr2I、CsPbBr 1.5 I 1.5 、CsPbBrI2、CsPbBr4 4- One or more of .

[0060] In some embodiments, the metal halide perovskite is a tin halide perovskite. In these cases, M is tin (Sn). Examples of suitable tin halide perovskites include those corresponding to those listed herein in which Pb is replaced by Sn in lead halide perovskites. Using Sn instead of Pb has obvious advantages, which can reduce toxicity and facilitate handling. Examples of tin halide perovskites suitable for the present invention include methylammonium tin iodide (CH3NH3SnI3, or MASnI3), formamidine tin triiodide (CH(NH2)2SnI3, or FASnI3) and CH3NH3SnIBr2 (MASnIBr2).

[0061] In some embodiments, the metal halide perovskite is a composite metal halide perovskite composed of metal halide perovskites with different cations A. Examples of suitable metal halide perovskites include (MAPbI3) 0.95 (FAPbI3) 0.05 .

[0062] As is known to those skilled in the art, metal halide perovskites are susceptible to polymorphic transformations upon heating. As temperature increases, they transform from an optically inert and commercially irrelevant crystalline phase (hexagonal or pseudo-hexagonal delta phase, also known as the "yellow" phase) to an optically active and commercially relevant phase (i.e., α-phase, β-phase, and / or γ-phase, also known as the "black" phase). However, while the "black" phases can be obtained by thermal annealing, they are metastable in nature and tend to readily transform to the more thermodynamically stable yellow phase when the material returns to room temperature, especially when exposed to moisture.

[0063] Due to the stabilizing effect of the amorphous MOF, the metal halide perovskite in the composite material of the present invention can be stabilized at room temperature in any of its photoactive cubic or quasi-cubic black phases (i.e., α-phase, β-phase and / or γ-phase, when any phase is available, depending on the specific metal halide perovskite).

[0064] Thus, in some embodiments, the metal halide perovskite includes one or more of α-phase, β-phase, and γ-phase metal halide perovskites. For example, the metal halide perovskite may include one or more of α-phase, β-phase, and γ-phase CsPbI3 perovskites, or a similar crystalline phase mixture of FAPbI3 perovskites.

[0065] The MOF glass composite material of the present invention is a combination of a solid amorphous MOF and a metal halide perovskite. Functionally, the interfacial interaction between the amorphous MOF and the metal halide perovskite can effectively stabilize the metastable phase of the perovskite and passivate the surface defects of the perovskite so that it maintains an optically active state. Therefore, the optical activity of the metal halide perovskite in the MOF glass composite material is much higher than that in the absence of the amorphous MOF.

[0066] Therefore, from a morphology point of view, metal halide perovskites can be provided in any form that is favorable for passivation by amorphous MOF surfaces.

[0067] For example, metal halide perovskites can exist in particle form. In this case, the MOF glass composite can be viewed as a solid distribution of discrete metal halide perovskite particles in an amorphous MOF as a dispersion medium. Figure 5 An example of such a dispersion is shown in (a)-5(c).

[0068] Therefore, the present invention can also be said to provide a MOF glass composite material comprising a MOF glass matrix in which metal halide perovskite particles are distributed.

[0069] Under the premise of achieving surface passivation, there is no particular restriction on the shape and size of the metal halide perovskite particles.

[0070] In some embodiments, the metal halide perovskite particles have a major dimension ranging from about 2.5 nm to about 1 μm, from about 5 nm to about 750 nm, from about 5 nm to about 500 nm, from about 5 nm to about 250 nm, from about 5 nm to about 150 nm, from about 5 nm to about 100 nm, from about 5 nm to about 50 nm, from about 5 nm to about 25 nm, from about 5 nm to about 10 nm. In some embodiments, the metal halide perovskite is provided in the form of particles having a major dimension ranging from about 2.5 nm to about 50 nm.

[0071] In some embodiments, the metal halide perovskite is provided in the form of a two-dimensional structure having lateral dimensions of 200 nm to about 1 μm and a thickness of 1 nm to 50 nm.

[0072] Under the premise of achieving surface passivation, the MOF glass composite material may include a metal halide perovskite, and the amount thereof is not particularly limited. For example, relative to the total weight of the MOF glass composite material, the MOF glass composite material may include the metal halide perovskite in an amount of at least about 1 wt%, at least about 5 wt%, at least about 10 wt%, at least about 25 wt%, at least about 50 wt%, at least about 75 wt%.

[0073] In some embodiments, the MOF glass composite comprises the metal halide perovskite in an amount of about 1 wt % to about 75 wt %, about 5 wt % to about 50 wt %, about 15 wt % to about 50 wt %, about 25 wt % to about 50 wt %, relative to the total weight of the MOF glass composite.

[0074] In some embodiments, the MOF glass composite includes the metal halide perovskite in an amount of about 25 wt %, relative to the total weight of the MOF glass composite.

[0075] The present invention also provides a method for manufacturing a MOF glass composite material. The MOF glass composite material may be the MOF glass composite material described herein.

[0076] The method includes the step of mixing the MOF and the metal halide perovskite to obtain a precursor mixture.

[0077] The nature of the MOF used in this step is not limited, as long as the MOF (i) can be mixed with the metal halide perovskite and (ii) exhibits a solid-liquid transition below its decomposition temperature. Therefore, as long as (i) and (ii) are satisfied, the MOF can be a crystalline MOF or an amorphous MOF.

[0078] In some embodiments, the MOF is at least one of an amorphous MOF and a crystalline MOF. In some embodiments, the MOF is an amorphous MOF. One skilled in the art will be aware of available procedures for providing an amorphous MOF. For example, an amorphous MOF can be provided by amorphization of a crystalline MOF, which can be achieved by applying high pressure, heat treatment, or mechanical grinding (such as ball milling) to the crystalline framework.

[0079] In some embodiments, the MOF used in the methods of the present invention is a MOF described herein.

[0080] The nature and morphology of the metal halide perovskite suitable for use in the method of the present invention are not particularly limited as long as the metal halide perovskite can be mixed with the MOF.

[0081] In some embodiments, the metal halide perovskite is a metal halide perovskite described herein.

[0082] Typically, synthesized MOFs and metal halide perovskites are granular solids at room temperature, i.e., assemblies of discrete solid particles whose sizes can vary from nanometers to millimeters. Therefore, mixing MOFs and metal halide perovskites would be understood as a solid mixing process.

[0083] The MOF and the metal halide perovskite can be mixed by any method known to the skilled person. For the purposes of the present invention, mixing can include diffusion mixing, convection mixing, and shear mixing. Therefore, in some embodiments, the MOF and the metal halide perovskite are provided in a specific form and mixed by one or more of a drum mixer, a ribbon mixer, a paddle mixer, a plough mixer, a screw mixer, and a drum mixer.

[0084] In some embodiments, the mixing is high energy mixing. For example, high energy mixing can be achieved by ball milling. Advantageously, ball milling can simultaneously perform grinding and mixing, thereby obtaining a highly uniform precursor mixture in which the MOF and the metal halide perovskite are present in the form of fine particles. Those skilled in the art can easily determine appropriate operating conditions for ball milling the MOF and the metal halide perovskite for the purposes of the present invention.

[0085] The method of the present invention further comprises sintering the precursor mixture to liquefy the MOF.

[0086] Since MOFs "liquefy", sintering should be understood as heating the precursor mixture within the temperature range where the MOF undergoes a solid-liquid transition, but the temperature should be below the decomposition temperature of the MOF. Therefore, for a given MOF, a person skilled in the art will be able to determine a suitable range of usable sintering temperatures, for example based on the solid-liquid transition temperature of the specific MOF available in the literature.

[0087] When designing an appropriate sintering temperature, one skilled in the art may make additional considerations. As explained herein, metal halide perovskites readily undergo polymorphic transformations when heated. As temperature increases, they transform from a photo-inactive and commercially irrelevant phase (the hexagonal delta phase, also known as the "yellow" phase) to a photo-active and commercially relevant phase (i.e., the α-phase, β-phase, and / or the γ-phase, also known as the "black" phase). Therefore, for a given metal halide perovskite, the sintering temperature may also be adjusted to ensure that the perovskite transforms to any of the optically active α-phase, β-phase, and / or γ-phase.

[0088] In addition, those skilled in the art may also note that the sintering temperature affects the grain size of the metal halide perovskite. In general, the higher the sintering temperature, the larger the grain size of the metal halide perovskite. Since the optoelectronic properties of metal halide perovskites are also related to the grain size, the electronic band gap of the metal halide perovskite can be adjusted by selecting the sintering temperature. For example, it has been observed that higher sintering temperatures cause the concentration maximum of the metal halide perovskite to red-shift. For a specific metal halide perovskite, those skilled in the art are able to determine a specific sintering temperature designed to produce a specific electronic band gap value.

[0089] The considerations made in this article on the effects of sintering temperature on the structures of MOFs and metal halide perovskites can provide guidance for determining suitable combinations of MOFs and metal halide perovskites. For example, the target crystalline phase and / or grain size of the metal halide perovskite may determine the range of sintering temperatures. Therefore, a suitable MOF should be one that exhibits a solid-liquid transition within a temperature window that overlaps with the sintering temperature range.

[0090] In some embodiments, the sintering temperature of the precursor mixture is at least about 100° C. For example, the precursor mixture can be sintered to a sintering temperature of at least about 125° C., at least about 150° C., at least about 175° C., at least about 200° C., at least about 225° C., at least about 250° C., at least about 275° C., at least about 300° C., at least about 325° C., at least about 350° C., at least about 375° C., at least about 400° C., at least about 425° C., or at least about 450° C. In some embodiments, the precursor mixture is sintered to a sintering temperature of about 150° C. to about 500° C., for example, about 150° C. and 350° C.

[0091] As the MOF liquefies, it coats the metal halide perovskite. This ensures a continuous MOF-perovskite interface around the metal halide perovskite, allowing for effective surface passivation and stabilization. Since the MOF is in liquid form, it can wrap around the metal halide perovskite, promoting extensive and tight bonding at the interface. As a result, surface passivation of metal halide perovskites is more effective than using previously proposed substrates, including crystalline MOFs.

[0092] The method of the present invention also requires quenching the sintered precursor mixture to vitrify the liquefied MOF and form a MOF glass composite material.

[0093] As used herein, the term "quenching" is understood to be rapid cooling at a rate sufficient to ensure vitrification of the liquefied MOF. In this context, the term "vitrification" and corresponding terms such as "vitrification" refer to the process by which the liquid-solid transition promoted by quenching causes the molecularly disordered nature of the liquid phase to solidify into a solid amorphous glass phase. This is to be understood as the reverse process of the liquid-solid transition promoted by cooling leading to crystallization.

[0094] Those skilled in the art will be able to easily determine the minimum quenching rate for solidifying the liquid MOF into a solid amorphous MOF. As long as the quenching can promote the vitrification of the liquid MOF, the quenching rate is not particularly limited.

[0095] However, the quenching rate can also be tuned to maximize the surface passivation of metal halide perovskites. In this regard, it has been observed that higher quenching rates are correlated with lower electron trap state density in metal halide perovskites. This correlation can be used, for example, to tailor the photoluminescence properties of metal halide perovskites. In this regard, higher quenching rates lead to higher quantum yields and longer exciton lifetimes in metal halide perovskites.

[0096] For example, in the method of the present invention, the sintering precursor mixture may be quenched at a quenching rate of at least 20° C. / min.

[0097] In some embodiments, the sintering precursor mixture may be quenched at a quench rate of at least about 50°C / min, at least about 100°C / min, at least about 250°C / min, at least about 500°C / min, or at least about 1000°C / min.

[0098] As long as the quenching can achieve the vitrification of the liquid MOF, there is no particular restriction on how to perform the quenching. For example, the quenching can be a low temperature quenching. As is well known to those skilled in the art, low temperature quenching is to immerse the sintered precursor mixture in a liquid bath of a low temperature liquid (such as liquid argon, helium or nitrogen). Low temperature quenching has been shown to be particularly effective in minimizing the density of electron trap states in metal halide perovskites.

[0099] According to the MOF glass composite material provided by the present invention, the best combination point is found between MOF and metal halide perovskite, two related functional materials, and several key obstacles in the practical application and development of metal halide perovskite are solved. The MOF glass composite material disclosed herein has both the robustness of the inorganic matrix and the processability of the polymer substrate, and its liquid phase reactivity can easily passivate the surface defects of the metal halide perovskite.

[0100] It is noteworthy that the MOF glass composite material of the present invention can show bright exciton emission, a wide color gamut, and has remarkable chemical, morphological and mechanical stability when exposed to aggressive external conditions. For example, the MOF glass composite material of the present invention can stably emit light in water for more than 10,000 hours.

[0101] When metal halide perovskites are present in the form of polydisperse particles, the overall light scattering and outcoupling efficiency of MOF-glass composites are improved, which is useful for applications such as down-conversion layers in liquid crystal displays.

[0102] In addition, the proposed mechanochemical method for preparing MOF glass composites is simple and flexible. This method can also prepare MOF glass composites with stoichiometric, cheap and moderately pure precursors, consuming only a very small amount of solvent. Therefore, the proposed method is easy to mass-produce.

[0103] Specific embodiments and various aspects of the present invention will now be described with reference to the following non-limiting examples.

[0104] Example

[0105] Example 1 - Synthesis of ZIFs and Perovskites as Glass Precursors

[0106] Unless otherwise stated, all chemicals were purchased from Sigma Aldrich and used without further purification. Cesium chloride (CsCl, 99.9%), cesium bromide (CsBr, 99.9%), cesium iodide (CsI, 99.9%), lead (II) chloride (PbCl2, 99.999%), lead (II) bromide (PbBr2, 99.999%), and lead (II) iodide (PbI2, 99%) were used for the fabrication of inorganic lead halide perovskites. Iodoformamide (FAI, 99% from Greatcell Solar Materials Pty Ltd) was used for the fabrication of hybrid perovskites. Zinc oxide (ZnO, nanopowder <100 nm), zinc acetate (Zn(OAc)2, 99.99%), cobalt(II) nitrate hexahydrate (Co(NO3)2-6H2O, 98%), imidazole (Im, >99%), and benzimidazole (bIm, 98%) were used for the synthesis of zinc and cobalt ZIFs. N,N-dimethylformamide (DMF, >99.8%), dimethyl sulfoxide (DMSO, >99.7%), diethyl ether (>99.7%), toluene (anhydrous, 99.8%), chloroform (>99.5%), and ethanol (>99.5%) were used as solvents. AgNO3 (>99.0%) was used for the photodeposition of silver. All gases were provided by Coregas Pty Ltd.

[0107] ZIF-62 crystal powder

[0108] In order to prepare ZIF-62[Zn(Im) 1.95 (bIm) 0.05 ], 162.8mg (2.00mmol) zinc oxide, 265.6mg (3.90mmol) imidazole and 11.8mg (0.10mmol) benzimidazole were added to the ball mill. Then 150μL DMF and 15mg (0.19mmol) NH4NO3, as well as 16g zirconium oxide balls were added. The mixture was ball milled at 600RPM for 1 hour using a planetary ball mill, and other ZIF crystals with Im:bIm stoichiometric ratios were prepared using the corresponding number of ligands. The obtained ZIF-62 crystals were briefly rinsed with methanol, dried in an oven at 80°C for 24 hours, and then used again.

[0109] Co-ZIF-62 crystal powder

[0110] Cobalt nitrate hexahydrate (1.15 g, 3.95 mmol) and imidazole (891 mg, 13.09 mmol) were dissolved in 90 mL DMF and stirred for 1 hour (2). 12 mg (0.10 mmol) of benzimidazole was then added to the solution and heated to 130° C. for 72 hours. The product was cooled to room temperature and the crystals were collected by centrifugation. Three wash-redispersion cycles were performed in DMF to remove all unreacted ligands. The sample was then dried in an oven at 150° C. overnight. It should be noted that complete desolventization was not performed in order to minimize amorphization during subsequent ball milling mixing.

[0111] Inorganic lead halide perovskite

[0112] CsPbCl3, CsPbBr3, CsPbI3, and mixed-ion perovskites were made by a solvent-free mechanochemical process. For example, in the synthesis of CsPbI3, a total of 400 mg of a stoichiometric mixture of CsI (144.17 mg) and PbI2 (255.83 mg) was added to a ball mill jar, along with 16 g of zirconia balls. Ball milling was performed at 600 RPM for 1 hour using a planetary ball mill, and then the solid sample was recovered from the jar and stored under ambient conditions before further testing. All other inorganic perovskites were prepared similarly, with a total amount of 400 mg of precursors.

[0113] Differential scanning calorimetry (DSC) measurements confirmed the expected “yellow” / “black” phase transition to be reversible at approximately 325°C and 250°C with an enthalpy change of 23.7 J / g ( Figure 1 The thermogravimetric analysis (TGA) curve of CsPbI3 showed no features before decomposition at about 460°C (not shown).

[0114] Mixed lead halide perovskites

[0115] FAPbI3 was also made by a mechanochemical process. 108.7 mg of FAI and 291.3 mg of PbI2 were mixed in a ball mill, and then 200 μL of hexane and 12 g of zirconia grinding balls were added. The mechanochemical reaction was carried out at 800 RPM for 15 minutes under an argon environment. The solid sample was then collected and stored under ambient conditions for further testing.

[0116] Example 2 - Manufacture of MOF Glass Composites

[0117] The manufacture of ZIF glass composite material can use ZIF-62 crystal or ZIF-62 amorphous glass. Using ZIF crystal as the manufacturing object, ZIF glass (amorphous glass) is melted at the corresponding melting temperature of ZIF-62 crystal in a tube furnace under argon (Ar) protection. g ZIF-62). In a typical procedure, 50 mg of CsPbI3 perovskite was mixed with 150 mg of a g ZIF-62 was mixed by ball milling at a rate of 600 RPM for 1 hour. The resulting mixture was called (CsPbI3)(a g ZIF-62) (25 / 75), where 25 and 75 are the mass percentages of each component.

[0118] The resulting mixture was then placed in a tube furnace and heat treated at a heating rate of 20°C / min under flowing argon. Once the sample reached the specified temperature, the entire tube was immediately removed from the furnace and quenched in low temperature (liquid nitrogen) under argon protection, unless otherwise stated. The composite material thus obtained is called (Perovskite)X(a g Glass)Y, such as (CsPbI3) 0.25 (a g ZIF-62) 0.75 Pure perovskite samples were also subjected to the same ball milling and heat treatment procedures as a benchmark.

[0119] In order to minimize thermal decomposition, CsPbI3 and ZIF-62 glass powder (denoted as a g ZIF-62) instead of ZIF-62 crystals. Compared with crystalline ZIF-62, a g ZIF-62 requires lower temperatures to enter the intrinsic ZIF liquid phase. In addition, during liquid phase sintering, it is often observed that the mixed powders form a liquid-solid mixture above the solid phase temperature, which is usually much lower than the T of the two constituent compounds. m / T g .

[0120] CsPbI3 and a g ZIF-62[Zn(Im) 1.95 (bIm) 0.05 ](T m About 375.0℃, T g is about 303.8℃) and the resulting mixture is called (CsPbI3) (a g ZIF-62)(X / Y), where X and Y are the mass percentages of the respective components. The mixture was sintered at a rate of 20°C / min to different temperatures (up to 350°C) and then quenched at low temperatures in an argon atmosphere. The resulting composite material is called (CsPbI3) X (a g ZIF-62) Y .

[0121] Example 3 - XRD Characterization

[0122] Room temperature powder XRD analysis data were collected using a Bruker D8 Advance MKII diffractometer using Cu Kα radiation with divergence (Bragg-Brentano) geometry. The 2θ range was 5 to 50°, the step length was 0.024°, and the step rate was 10 seconds. Temperature-resolved in-situ powder XRD was performed in a nitrogen environment using a PANalyticalX'Pert Pro MPD equipped with an Anton Paar XRD900 furnace. Cu Kα radiation with divergence (Bragg-Brentano) geometry was used. The heating rate was 20°C / min, the 2θ range was 5 to 50°, the step length was 0.05°, and the step rate was 10 seconds.

[0123] In the in situ powder X-ray diffraction (XRD), (CsPbI3) (a g ZIF-62)(25 / 75) shows Bragg peaks from PbI2 and δ-CsPbI3 ( Figure 2 ) In the case of (CsPbI3) sintered at a higher temperature 0.25 (a g ZIF-62) 0.75 The newly emerged peaks are believed to be the metastable phase of γ-CsPbI3, which is the only phase identified after quenching at 350 °C ( Figure 2 ). TGA showed negligible weight loss during sintering (not shown). During sintering, the endoplasmic reaction (20.3 J / g) was more pronounced than the phase change of 25 wt% CsPbI3, indicating an endothermic effect between the two phases. g Compared with ZIF-62, (CsPbI3) 0.25 (ag ZIF-62) 0.75 T g Even lower, at 282.5°C.

[0124] In situ synchrotron X-ray scattering data were collected at the (SAXS / WAXS) beamline at the Australian Synchrotron. Detector calibration was performed on a Dectris PILATUS3 X2M using a silver behenate standard. Scattering intensity normalization was performed using a diode embedded in the beam stop. Scattering data were collected at a wavelength of (11.000keV) with a q range of (Detector distance 7600mm) and (Detector distance 700 mm). Temperature resolved SAXS data were collected using a temperature calibrated Linkam furnace. The heating rate was 20°C / min under a flowing nitrogen environment.

[0125] The data were reduced to one-dimensional data using the in-house developed Scatterbrain software package. The SAXS data were fitted with a minimal Monte Carlo regression using the McSAS software package.

[0126] Example 4 - Thermogravimetric and thermal analysis

[0127] Thermogravimetric analysis (TGA) was performed using a Mettler Toledo 1STARe system. The samples were placed in an alumina crucible and heated at a heating rate of 20°C / min under a flowing (20 mL / min) nitrogen environment.

[0128] Calorimetric characteristics were determined using an independent Mettler Toledo Differential Scanning Calorimetry (DSC) 1STARe system. For each measurement, approximately 10 mg of sample was placed in an aluminum crucible and heated under flowing nitrogen (20 mL / min). To determine the melting point (T m ) and thermal decomposition (T d ) and the crystal phase transition temperature, the sample was heated to the target temperature at a heating rate of 20 °C / min. In order to determine the solid-liquid transition temperature (T g ), the sample was heated above its melting temperature at a rate of 20°C / min, then cooled to 40°C at a rate of 10°C / min, and then heated at a rate of 10°C / min in a second upscan.

[0129] Example 5 - Optical Characterization

[0130] Photoluminescence measurement

[0131] Photoluminescence (PL) and time-resolved fluorescence emission spectra were collected at room temperature using an Edinburgh Instrument FLSP-900 fluorescence spectrophotometer. Steady PL spectra were measured using a monochromatic Xe lamp light source, while time-resolved PL (TRPL) decays were measured using a 375 nm pulsed diode laser excitation light source.

[0132] As for the optical properties, due to photon reabsorption, the CsPbI3, i.e. (CsPbI3) (a g After mixing ZIF-62) (25 / 75), a g The broad PL emission of ZIF-62 was quenched. After quenching at 150 °C, the composite began to show narrow red PL emission, confirming that the metastable δ-CsPbI3 remained in (CsPbI3) 0.25 (a g ZIF-62) 0.75 The strongest PL was obtained at 275℃, which is comparable to (CsPbI3)(a g Compared with ZIF-62)(25 / 75), the Figure 3 ). Higher sintering temperature causes the PL maximum after quenching to red-shift, consistent with the reduced band gap in the UV-Vis absorption spectrum ( Figure 4 ). (CsPbI3) 0.25 (a g ZIF-62) 0.75 The absolute PL quantum yield (QY) can reach more than 50%.

[0133] The sintering process reduces the defect density of γ-CsPbI3, makes the trap states shallower, and enhances the uniformity, as evidenced by the gradually reduced PL full width at half maximum (FWHM) and longer lifetime of photogenerated excitons. In addition, this suggests that the reduction in PL intensity above 275°C stems from the enhancement of the interface interaction within the composite; it effectively improves the charge separation of the heterojunction, thereby suppressing the radiative recombination of excitons.

[0134] In a series of parallel tests, (CsPbI3) produced with a slower quenching rate (20°C / min) 0.25 (a g ZIF-62) 0.75 The composite material showed very similar trends. However, the lower PLQY and shorter exciton lifetime indicated an increase in the number of trap states formed. Therefore, low-temperature quenching was used in subsequent studies.

[0135] UV-Vis Absorption

[0136] A Jasco V-650 UV-visible spectrophotometer was used to measure the gUV-visible absorption spectra of ZIF-62 powder mixtures and composites.

[0137] Example 6 - Microphase structure and distribution

[0138] Scanning electron microscopy (SEM)

[0139] The surface morphology and atomic density information near the surface were studied using a JEOL JSM-7100F high-resolution scanning electron microscope in secondary electron and backscattering mode (8.0KV accelerating voltage). All samples were dried at 30°C and then briefly plasma cleaned. The surface was treated with platinum coating before imaging.

[0140] Scanning electron microscopy (SEM) in secondary electron (SE) and backscattering (BSE) modes confirmed the uniform distribution of heavy atom nanoparticles within the composite. g The quenching started at the solid-liquid transition temperature of ZIF-62 (about 285 °C) and showed continuous surface uniformity, indicating that the liquid formation temperature is greatly reduced, which is a common phenomenon in the liquid phase sintering process.

[0141] Transmission Electron Microscopy (TEM)

[0142] The SED data were collected using a JEOL ARM300CF equipped with an ultra-high resolution pole piece, a cold field emission gun, and aberration correctors in the probe forming and image forming optics (Diamond Light Source, UK). The instrument was operated at 200 kV. The nanobeam configuration was obtained by turning off the aberration corrector in the probe forming optics and using a 10 μm condenser aperture to obtain a convergence half-angle of <1 mrad and a diffraction-limited probe diameter of approximately 5 nm. The probe current measured using a Faraday cup was approximately 3.5 pA and the exposure time for each probe position was 1 ms. Assuming the probe is disk-shaped, the electron flux is estimated to be approximately Diffraction patterns were acquired at each probe position using a Merlin-Medipix hybrid counting direct electron detector (QuantumDetectors, UK) with 512 × 512 pixels, but in these experiments the direct beam was positioned close to the center of a single 256 × 256 quadrant. Annular dark field STEM images were acquired from the same area with a dedicated ADF detector after SED acquisition. X-ray energy dispersive spectroscopy (EDS) images were also acquired from the same selected areas after SED acquisition. For EDS images, a 150 μm condenser aperture was used to obtain a larger detection current in order to generate sufficient X-ray counts.

[0143] The SED data were processed using pyxem-0.10.0. The active quadrants were cropped from the full data set. The calibration of the scan step size and the pixel size of the diffraction patterns was performed using a 500 nm gold diffraction grating (Ted Pella) replicated with latex spheres under the same conditions as for the composite samples. The SED data were processed using the open source pyXem Python library to find the diffraction peaks in each measured diffraction pattern using the Gaussian difference method, i.e., subtracting the blurred version of the diffraction pattern from the less blurred version of the diffraction pattern. The EDS data were processed using the open source HyperSpy Python library to generate spectra for each relevant X-ray emission line, which were extracted by integrating over energy windows. The crossed grating data were also used to determine the residual elliptical deformation of the diffraction pattern due to the post-specimen optics.

[0144] Electron tomography and point diffraction experiments were acquired using a FEI Titan3 Themis (Thermo Fisher) equipped with an “X-FEG” high-brightness electron source and a OneView (Gatan) CMOS camera (University of Leeds, UK). The instrument was operated at 300 kV. A nanobeam configuration was used in microprobe mode with a 50 μm condenser aperture to obtain an estimated convergence half-angle of ∼0.6 mrad. The probe current was 7 pA measured on a phosphor screen and the diffraction patterns were acquired with an exposure time of 0.5 s. ADF STEM image was acquired by taking a series of point diffraction patterns, then blanking the beam, positioning the beam at the selected point position, unblank, record, and re-blank the beam to minimize other beam exposures. After acquiring the point diffraction data, an ADF-STEM image was acquired again to assess the drift of the sample position for registration of the selected point. Subsequently, a tilt series was acquired from −70° to +70° in 1° increments using the same optical configuration.

[0145] Point diffraction data were similarly processed using pyxem-0.10.0. Diffraction data from a replica of the 462.9 nm (2160 lines / mm) gold cross grating were collected under point diffraction conditions, but with an extended camera while manually moving the beam through the sample to record the polycrystalline ring pattern. Calibration of the STEM scan step size and diffraction pattern pixel size as well as ellipticity correction were performed according to the procedures used for SED and were adjusted to accommodate the beam stop inserted when performing point diffraction experiments on the OneView camera. The diffraction patterns were re-binned and characteristic d-spacings were determined to distinguish the crystal phases of individual CsPbI3 grains.

[0146] All tomography data were preprocessed in the HyperSpy Python library. For ADF-STEM tomography, micrographs were combined into tilt-series data stacks and aligned using Numpy and the cross-correlation method in the SciKit-Image Python library. Tilt axis shift and rotation adjustments were performed using tools in the SciKit-Image Python library. Reconstruction was performed using total variation (TV) regularization and the primal-dual hybrid gradient (PDHG) algorithm implemented in Python using the ASTRA toolbox from Projector.

[0147] STEM-CL experiments were performed on a Nion Hermes 200 ("ChromaTEM") electron microscope at the Solid State Physics Laboratory of Université Paris-Saclay, Orsay, France, equipped with an electron monochromator and a cold field emission gun electron source. The accelerating voltage of the microscope was 100 kV, and the beam convergence half angle was about 15 mrad. The sample stage was cooled to about 150 K using a liquid nitrogen cooling system. The CL signal was obtained using an Attolight The data were collected by a 4107STEM-CL system equipped with an optical spectrometer with a 150-groove / mm diffraction grating and a wavelength of 500 nm. While scanning the sample, each pixel records a complete CL spectrum, thereby obtaining a hyperspectral image. The typical dwell time per pixel is 20 ms. The spectral resolution of the spectrometer CCD is 0.33 nm / pixel.

[0148] Application of TEM to (CsPbI3) 0.25 (a g ZIF-62) 0.75 The microstructure of the sintered steel (sintered to 300°C) was further examined. Annular dark field (ADF)-STEM images showed good mass-thickness contrast between the two phases, and their distribution was consistent with the expected elemental distribution based on energy dispersive X-ray spectroscopy (STEM-EDS) ( Figure 5 (a)). The crystalline and amorphous regions are determined by scanning electron diffraction patterns (SED), which are obtained by summing the number of Bragg diffraction disks in the electron diffraction pattern recorded for each probe position. The crystalline region corresponds to the distribution of the CsPbI3 phase ( Figure 5 (b)).

[0149] Further convolutional neural network (CNN) classification of the SED patterns identified the main γ-CsPbI3 phase in the composite. The individual grains were mostly single crystals, although a few grains appeared as fuzzy spots during the classification process, which may be caused by crystal structure deformation at the interface or out-of-plane stacking of different grains ( Figure 5 (c)). For (CsPbI3) 0.25 (a g ZIF-62) 0.75 Further investigation of the sintered samples (sintered at 275 °C) showed similar behavior with a slightly lower ratio of γ-CsPbI3 pixels, which is in good agreement with the in situ XRD results ( Figure 2 ).

[0150] ADF-STEM tomography was used to reconstruct (CsPbI3) 0.25 (a g ZIF-62) 0.75 (sintered to 300°C) to explore the three-dimensional crystal phase distribution. The atomic density of the composite material is represented by different colors: yellow represents CsPbI3, purple represents a g ZIF-62. Composites fabricated by liquid phase sintering often contain voids, which can be observed from cross-sectional structural reconstructions. Subsequent SED data identified non-perovskite δ-CsPbI3 near the voids and γ-CsPbI3 in densely packed regions. This suggests a correlation between interfacial contacts and CsPbI3 phase control.

[0151] Cathodoluminescence (CL-STEM) detected strong narrow luminescence from isolated grains (<40 nm) and slight inter-particle emission wavelength shifts (<4 nm). The variation of CL intensity can be attributed to the depth of CsPbI3 from the composite surface ( Figure 6 (a) and 6(b)). It is worth noting that although large particles were observed in STEM, the average particle size of CsPbI3 was about 30 nm, which can be easily further reduced by extended ball milling before sintering.

[0152] SED phase identification

[0153] The convolutional neural network used for X-ray diffraction classification was adapted from Bennett et al., “Melt-Quenched Glasses of Metal–Organic Frameworks,” Journal of the American Chemical Society 138, 3484–3492 (2016). This network architecture is robust to peak disappearance and peak intensity variations [A], which are inherent properties of SED data because diffraction is recorded from a single orientation for each pixel. The neural network was then implemented in TensorFlow (2.1.0) using Keras to solve the binary classification problem required to distinguish γ-CsPbI3 from δ-CsPbI3 in SED data. Simulated 2D spot patterns were generated in pyxem 0.11.0 (17) and then converted to 1D patterns by azimuthal integration for training and testing the neural network. The training data was generated by uniformly sampling the crystal orientations, excluding rotations about the azimuthal integration axis. Test data were generated by randomly sampling directions, simulating the unknown and possible random directions found in experimental composites. Random direction sampling of the training data yielded comparable results. To ensure a consistent intensity range for the training, test, and experimental data, all data were normalized by setting the maximum intensity to 1 for each pattern. The power law was fitted to the A*kb type (where k is the magnitude of the scattering vector). A and b are fitting parameters), the experimental patterns were cropped to exclude the direct beam, and the background was subtracted to remove the diffuse scattered intensity. The fit was performed using the diffuse intensity tails at low and high scattering angles outside the scattering vector window showing the Bragg diffraction spot, and the A parameter was constrained to be non-negative. In order to match the mutual spatial calibration between the simulated patterns and the experimental data, the calibration was first determined by fitting an annular pattern of polycrystalline gold obtained under the same experimental conditions, and then further refined using image registration (Matlab, MathWorks) of the simulated patterns with the near-zone axis patterns of γ-CsPbI3 and δ-CsPbI3 identified after an initial neural network classification of the experimental data set. The direct beam was not included in the simulated spot pattern, and the one-dimensional pattern was cropped to the same k range as the experimental data.

[0154] The neural network architecture was optimized for electron diffraction data by evaluating the effect of the amount of training data, hidden layer depth, filter size, kernel size, step size, activation function, optimizer, and number of epochs used in network training on the performance. The performance of the network was evaluated using the classification accuracy of simulated test data, and the parameters were varied until a high point in network performance was observed. The optimized method (network accuracy > 98% with 1000 patterns as test data) used 1000 simulated patterns as training data (500 for each crystal phase), four 1D convolutional layers, a filter size of 32 for each of the four convolutional layers, kernel size and step size set to (8,5,3,3), Adam optimizer, and 100 training epochs. In the experimental application, pixels containing Bragg scattering were isolated by applying a threshold to the crystallinity map. The patterns were then classified and a phase map was generated at the original pixel location using the probability prediction (0-1) determined by the neural network. For visualization purposes, pixels excluded from crystal classification were set to different intensity and color values, i.e., assigned as vacuum, carbon film, or a g Pixels of ZIF-62.

[0155] The neural network classification was validated by summing the normalized patterns of all pixels in each class. The resulting average pattern corresponded to the expected differences (unique scattering vectors) between the γ-CsPbI3 and δ-CsPbI3 phases. Additional inspection of the experimental patterns near the axes of high symmetry regions further confirmed the classification results by manually indexing high confidence. Some spots were observed in the crystal phase map, and inspection of these areas showed that these spots corresponded to crystal directions with fewer Bragg scattering points, which led to inherently ambiguous classifications. Manual inspection of the SED data pixel by pixel showed that all crystals showed single crystal diffraction patterns with no obvious changes in the orientation or phase of individual grains.

[0156] Example 7 - Structural evolution during sintering

[0157] (CsPbI3)(a g Temperature-resolved in situ powder X-ray diffraction (XRD) patterns of ZIF-62 (25 / 75) were collected. Figure 7 (a)). The peak at about 150°C indicates the formation of α-CsPbI3 (Pm-3m). The higher the sintering temperature, the stronger the peak. The calculated α-CsPbI3 crystal size increases with increasing sintering temperature ( Figure 7 (b)), and STEM results ( Figure 5 and Figure 6 ) is consistent. In the quenching stage ( Figure 7 (a)), about 35° The diffraction peak at 200°C gradually disappears, indicating that [PbI6] 4- The octahedron tilted and formed γ-CsPbI3(Pbnm).

[0158] In situ synchrotron small angle X-ray scattering (SAXS) measurements (0.5-1.2A -1 ), similar crystal structure evolution with temperature was also observed. In particular, SAXS (0.002-0.5A -1 ) shows that small CsPbI3 (<10 nm) gradually coarsens from about 160 °C, which is the main scattering phase in the composite ( Figure 7 (c)). In contrast, pure a g The coarsening of ZIF-62 or CsPbI3 is negligible before 300 °C. Moreover, a rapid densification of the composites is observed above 175 °C, which may be due to the presence of a liquid-solid mixture above the solidus temperature during the liquid phase sintering process.

[0159] During the sintering of the composite, a series of CsPbI3 crystal structure transformations and grain coarsening occurred. The viscous liquid-solid mixture above the solidus temperature increases the surface energy of δ-CsPbI3, which is conducive to the phase transition to the α phase, which is similar to the case of solvent-modulated or ligand-terminated CsPbI3 quantum dots. For smaller grains, the interfacial energy plays a greater role, so the phase transition occurs at lower temperatures. Larger grains require higher temperatures to reduce the phase transition energy barrier and achieve intimate interfacial contact with the viscous liquid. The presence of the liquid phase also allows CsPbI3 grains to diffuse and agglomerate, but due to the large diffusion resistance, the diffusion and agglomeration of small particles are mainly the case.

[0160] Therefore, the composites show a sintering temperature-dependent α-phase grain size distribution and a tunable band gap after quenching due to quantum confinement effects. We anticipate that intimate interfacial contact is essential for phase control: in [Zn(Im) 1.55 (bIm) 0.45 ]a g In ZIF-62, probably due to the higher intrinsic T g (about 309.3℃) and the viscosity caused by the looser bIm ligands, there are still a lot of δ-CsPbI3 and PbI2 in the final composite material.

[0161] Example 8 - Dynamic Properties and Interface Bonding

[0162] Synchrotron Tera-Hz Far-Infrared (THz / Far-IR) Absorption Spectroscopy

[0163] THz / far-infrared absorption spectra were collected at the THz / far-infrared beamline at the Australian Synchrotron using a Bruker IFS125 / HR Fourier transform (FT) spectrometer. The bolometer was kept at cryogenic conditions with liquid helium to improve the signal-to-noise ratio and a 6 μm thick multilayer Mylar beam splitter was used.

[0164] The measurement was performed using the attenuated total reflectance (ATR) technique. The sample was mounted on the surface of a diamond crystal window and fixed in position by applying pressure. Temperature-resolved in-situ spectra were collected using an ATR heating stage, and the sample was placed in flowing argon (about 20 mL / min). For data processing, the extended ATR correction algorithm in OPUS 8.0 software, as well as the NumPy module v1.15 and Python v3.5 were used for spectral data correction and peak fitting.

[0165] Computer calculation of vibration behavior

[0166] Standard computational chemistry calculations were performed using Gaussian 16. We used molecular species to simulate the key components in the material system. As in previous studies, they include complexes of zinc with three imidazolium anions and a benzimidazolium anion derivative; in addition, we studied similar complexes of zinc with three imidazolium anions and an iodide. The overall charge of these complexes is negative two, corresponding to that of Zn(II) species. The geometries of these molecular models were optimized using the B3-LYP method with the 6-31+G(d,p) basis set for all elements except iodine, for which the def2-SVP basis set was used. Harmonic vibrational frequencies were obtained at the same level of theory. The simulated infrared spectra were obtained by assuming a half-width of 10 cm for each peak. -1 Multiple conformations of the iodide complex were sampled, and the reported spectrum is equivalent to the average of the spectra of these conformations.

[0167] X-ray Photoelectron Spectroscopy

[0168] The surface chemistry of the samples was investigated using a Kratos Axis Ultra XPS at 150 W (15 kV, 10 mA) and single Al Kα (1486.6 eV). The instrument was equipped with a 165 mm hemispherical electron energy analyzer. The C1s peak position was set at 284.8 eV and used as an internal standard.

[0169] Raman spectroscopy

[0170] Raman spectra were measured using a Renishaw Raman microscope and spectrometer. All samples were excited using a 785nm laser beam. Five cycles of data acquisition were performed to reduce the influence of background noise caused by strong fluorescence.

[0171] Solid-state NMR

[0172] Solid-state NMR experiments were performed on a 600 MHz Varian NMR system using a 1.6 mm HXY FastMAS probe and a 3.2 mm HX CPMAS probe. Zn[(Im) 1.95 (bIm) 0.05 ] series samples. Unless otherwise stated, the sample rotation frequency was 20 kHz. 133 The Cs MAS NMR spectra were measured with short excitation pulses of 1 μs; the number of scans was 1000-1500 and the repetition delay was 60 seconds. The 207Pb MAS NMR spectra were recorded with a Hahn echo pulse sequence; an interpulse delay of one rotation period was used and the repetition delay was 1 second.

[0173] When using a 1.6mm probe, the rotation frequency was 32kHz, the π / 2 pulse length was 2.2μs, and the number of scans was 226,000. When using a 3.2mm probe, the rotation frequency was 20kHz, the π / 2 pulse length was 2.9μs, and the number of scans was 100,000. The 1H-13C cross-polarization (CP) MAS experiment included proton excitation using a 2.6μs π / 2 pulse, a 4ms CP block, and signal acquisition using high-power XiX proton decoupling. A total of about 10,000 to 50,000 scans were accumulated with a repetition delay of 1 second. In the 1H-15N CP MAS experiment, the CP block length was 3ms, the repetition delay was 0.5s, and the number of scans was 450,000. The Larmor frequencies of 13C, 15N, 133Cs and 207Pb are 150.72 MHz, 60.76 MHz, 78.62 MHz and 125.40 MHz, respectively. The corresponding spectral axes are referenced to the signals of tetramethylsilane, nitromethane, cesium nitrate and tetramethyllead, respectively.

[0174] Results and Discussion

[0175] Molecular Lewis acids / bases and imidazolium ion compounds can enhance the phase stability of LHPs and passivate surface defects by forming surface bonds. Therefore, we conducted a series of studies to understand the 0.25 (a g ZIF-62) 0.75 Temperature-resolved synchrotron tera-Hz (THz) far-infrared vibrational spectroscopy can directly probe the dynamic properties of ZIF and CsPbI3 phonon modes. For (CsPbI3) 0.25 (a g ZIF-62) 0.75 The secondary diffraction spectrum of the ZIF in the Zn matrix shows the fine vibration modes of the Zn tetrahedron ( Figure 8 (a)).

[0176] Density functional theory (DFT) suggests that the -1 The vibration mode at about 135 cm is the Zn-N vibration in the Zn(Im)2(bIm)I tetrahedron. This vibration mode increases with increasing temperature starting from 150°C (dotted line). -1 The peaks appearing at 100°C also align with the Zn-I stretching vibrations in DFT. Moreover, these newly emerged features remain largely unchanged during the cooling and second heating cycles, suggesting the formation of interfacial bonds between CsPbI3 and liquid ZIF above the solidus temperature (about 150°C).

[0177] During sintering, the interfacial bonds also begin to destroy the intrinsic phonon modes of CsPbI3 (Pb-I-Pb bending and Pb-I stretching) starting from about 150°C, while these phonon modes of pure CsPbI3 are retained even after sintering to 300°C. In situ X-ray photoelectron spectroscopy (XPS) and Raman spectroscopy also confirmed the possible interfacial bonds formed by sintering, showing peak shifts for all elements (Cs, Pb, I, Zn, and N in XPS) and imidazole vibrations (about 1170 cm in Raman spectroscopy). -1 ) peak broadened.

[0178] Due to its isotopic specificity, NMR spectroscopy can selectively provide insight into different species in powder mixtures and composites. 13 C and 15 The NNMR spectrum showed a broader signal, indicating the presence of additional disorder in the ZIF glass.

[0179] a g Effect of sintering conditions and solid-liquid transition temperature of ZIF-62 on the composite 207 Pb NMR spectrum is less affected, but 133 The Cs MASNMR spectra are highly dependent on these conditions. The spectra of the powder mixtures all show narrow signals of δ-CsPbI3 (260 ppm), CsI (290 ppm) and a low broad signal extending between 0 and 350 ppm, which belongs to poorly crystallized, highly defective CsPbI3. In the case of the composites, the broad contribution and CsI peaks are weakened, with the main signal coming from γ-CsPbI3. The different δ- / γ-phase ratios between the two composite samples are consistent with the above-mentioned sintering temperature and a g The γ-CsPbI3 peak in the composite material shows a significant shoulder peak between 160ppm and 80ppm, indicating that there is a significant distribution of the chemical environment within the γ-CsPbI3 particles of the composite material, which may be related to the huge influence of the interface that can be propagated to the interior of the γ-CsPbI3 particles.

[0180] to a g ZIF-62, (CsPbI3) (a g ZIF-62)(25 / 75) and (CsPbI3) 0.25 (a g ZIF-62) 0.75 The X-ray total scattering patterns of the samples were studied. The relatively weak Bragg diffraction peaks of the powder mixture were enhanced after the composite was formed. After data correction and inverse Fourier transformation of the structure factor S(Q), the X-ray PDF, D(r) was extracted. The a g Short-range to long-range oscillations of ZIF-62 and simulated γ-CsPbI3. This indicates that the intrinsic structure of the bulk phase is preserved in the composite and the changes in the chemical environment mainly occur in the interface region.

[0181] The pseudo-cubic phase of CsPbI3 has a double-well phonon mode at the center of the Brillouin zone, which drives the phase transition to δ-CsPbI3 in a consistent phononic manner. The interface bonding destroys the local Pb-I sublattice phonon modes and vibrational harmonics, thus avoiding harmonic order-disorder entropy. In addition, due to the low ionic charge and large interatomic distance, CsPbI3 has a low lattice energy but can obtain higher energy from the interface bonds. Together with the physical confinement effect provided by the matrix, these aspects prevent the complete reorganization of atomic coordination. The strong driving force for the γ-phase transition to the δ-phase transition is therefore offset and the metastable γ-CsPbI3 is maintained in the composite material.

[0182] Although LHP is highly tolerant to structural defects, a large number of Schottky-type cesium sites and halide vacancies can be expected due to its low formation energy, leading to non-radiative exciton recombination. Sintering can effectively reduce bulk crystal defects, as indicated by the improvement of crystallinity. Interfacial interactions can further passivate under-coordinated Pb / halide sites and negatively charged Pb halide anti-sites on the CsPbI3 surface.

[0183] ZIF-62 liquid has Lewis base ligands (imidazolium and benzimidazolium salts with p-conjugation) and Lewis acid sites (undercoordinated Zn nodes) to passivate Lewis acid and base defects in CsPbI3. In addition, Zn-I interactions can alleviate interstitial defects caused by halide pp antibonding states; the lower s orbital energy level of Zn can lead to shallower defects and promote hole decapture rates after Shockley-Read-Hall statistics.

[0184] Example 9 - ZIF Glass Composite

[0185] The versatility of liquid phase sintering was examined using CsPbX3 (X = Cl, Br and mixed halide ions).

[0186] The composite material exhibited a wide color gamut and narrow PL peaks (half-height width: 20.4-45.1 nm, Fig. 9 ). CsPbCl3, CsPbCl2Br and CsPbCl 1.5 Br 1.5 The presence of the shoulder of the composite material can be attributed to a g Emission from ZIF-62. For all CsPbX3 composites with 25 wt% loading, the absolute PL intensity is at least two orders of magnitude higher than that of the corresponding pure CsPbX3 samples, both as synthesized and after the same ball milling and sintering to 275 °C treatment. The broad, asymmetric PL peak of pure CsPbX3 indicates halide ion segregation, which is also suppressed in the composites. The composite fabrication can be extended to hybrid LHP: Co-based g ZIF-62 can retain the metastable black phase of FAPbI3 (FA: formamidine) under ambient conditions, showing PL emission in the red to infrared region.

[0187] Example 10 - Practical Application

[0188] Hydrophobicity, mechanical robustness g ZIF-62 can provide satisfactory protection for perovskite. Due to the suppression of unfavorable light-induced ion migration, (CsPbI3) 0.25 (a g ZIF-62) 0.75 The PL spectra remained essentially unchanged over 100 repeated measurement cycles. The composite material could withstand long-term (about 20 h) ultrasonic treatment in various nonpolar, polar protic, and polar aprotic organic solvents, even though the polypropylene cap showed a certain degree of swelling ( Fig.10 (a)), and even after 10,000 h of immersion, the composites exhibited resistance to water chemicals ( Fig.10 (b)).

[0189] Mild heating also has little effect on the composite: repeated heating to 100°C in argon or 80°C in air for 1000 cycles does not significantly affect its optical properties. The processable rigid substrate allows the composite to be molded into different macrostructures. Therefore, CGC is promising for the fabrication of stable PL LEDs.

[0190] a g Microscopic properties of ZIF-62 ( Fig.11 ) to make it Pb 2+ The adsorption capacity of (CsPbI3) is 10 times its weight.0.25 (a g ZIF-62) 0.75 The glass composite material showed its own lead chelation effect, and after 10,000 hours of immersion test, the Pb in the water phase 2+ The concentration was below the detection limit of 0.5 ppm by inductively coupled plasma-optical emission spectrometry (ICP-OES).

[0191] Water stability and safety bring great opportunities for liquid photocatalysis. As a demonstration, (CsPbI3) 0.25 (a g ZIF-62) 0.75 Under the excitation of visible light with a wavelength of >520nm, Ag ions in water can be effectively reduced, while pure glass has no photoactivity under this low excitation energy ( Fig.12 (a) and 12(b)).

[0192] Throughout this specification and the appended claims, unless the context requires otherwise, the word "comprise" and variations such as "comprises" and "comprising", will be understood to imply the inclusion of a specified integer or step or group of integers or steps but not the exclusion of any other integer or step or group of integers or steps.

[0193] Reference in this specification to any previous publication (or information obtained therefrom) or any known matter is not to be taken as an admission or acquiescence, or any form of implication, that the previous publication (or information obtained therefrom) or known matter forms part of the common general knowledge in the field relevant to this specification.

Claims

1. A metal organic framework (MOF) glass composite material comprising a metal halide perovskite.

2. The composite material according to claim 1, wherein The MOF is a zeolitic imidazolate framework (ZIF).

3. The composite material according to claim 1 or 2, wherein: ZIF is a mixed ligand ZIF.

4. The composite material according to claim 2 or 3, wherein: ZIF is a mixed ligand halogenated ZIF.

5. The composite material according to any one of claims 1 to 4, wherein The MOF is selected from ZIF-4, ZIF-62, ZIF-76, ZIF-UC-2, ZIF-UC-3, ZIF-UC-4, ZIF-UC-5, and combinations thereof.

6. The composite material according to any one of claims 1 to 5, wherein The metal halide perovskite is one or more of lead halide perovskite, tin halide perovskite, germanium halide perovskite and silver bismuth halide double perovskite.

7. The composite material according to any one of claims 1 to 6, wherein The metal halide perovskite is a mixed halide metal halide perovskite.

8. The composite material according to any one of claims 1 to 7, wherein The metal halide perovskite includes one or more of α-phase, β-phase and γ-phase metal halide perovskite.

9. The composite material according to any one of claims 1 to 8, wherein The metal halide perovskite is a lead halide perovskite.

10. The composite material according to any one of claims 1 to 9, wherein The metal halide perovskite is CsPbI3, CsPbBr3, CsPbCl2Br, CsPbCl 1.5 Br 1.5 , MAPbI3, MAPbBr3, FAPbI3, (C4H9NH3)2PbBr4, CsPbCl2Br, CsPbCl 1.5 Br 1.5 、CsPbClBr2、CsPbCl 0.75 Br 2.25 、CsPbCl 0.5 Br 2.5 、CsPbBr 2.5 I 0.5 、CsPbBr 2.25 I 0.75 、CsPbBr2I、CsPbBr 1.5 I 1.5 、CsPbBrI2、CsPbBr4 4- 、(MAPbI3) 0.95 (FAPbI3) 0.05 , MASnI3, FASnI3 and MASnIBr2, wherein MA is methylammonium and FA is formamidine.

11. The composite material according to any one of claims 1 to 10, wherein The metal halide perovskite includes one or more of α-phase, β-phase and γ-phase CsPbI3 perovskite.

12. The composite material of any one of claims 1-11, comprising at least about 1 wt% of a metal halide perovskite relative to the total weight of the MOF glass composite.

13. The composite material according to any one of claims 1 to 12, comprising about 25 wt% of metal halide perovskite relative to the total weight of the MOF glass composite material.

14. A method for manufacturing a MOF glass composite material comprising a metal halide perovskite, the method comprising the following steps: mixing the MOF and the metal halide perovskite to obtain a precursor mixture; Sintering the precursor mixture to liquefy the MOF and coat the metal halide perovskite; as well as The sintered precursor mixture is quenched to vitrify the liquefied MOF and form the MOF glass composite material.

15. The method according to claim 14, wherein: The MOF in the mixing step is at least one of a crystalline MOF and a MOF glass.

16. The method according to claim 14 or 15, wherein: The MOF in the mixing step is a zeolitic imidazolate framework (ZIF).

17. The method according to claim 16, wherein: The ZIF is a ZIF as defined in any one of claims 3-5.

18. The method according to any one of claims 14 to 17, wherein: The metal halide perovskite is the metal halide perovskite defined in any one of claims 6-11.

19. The method according to any one of claims 14 to 18, wherein: The precursor mixture contains at least 1 wt % of a metal halide perovskite.

20. The method according to any one of claims 14 to 19, wherein: The precursor mixture contains about 25 wt % of the metal halide perovskite.

21. The method according to any one of claims 14 to 20, wherein: The precursor mixture is sintered to a sintering temperature of at least 150°C.

22. The method according to any one of claims 14 to 21, wherein: The sintered precursor mixture is quenched at a quenching rate of at least 20° C. / min.

23. The method according to any one of claims 14 to 22, wherein: The quenching is low temperature quenching.

24. The method according to claim 23, wherein: The low temperature quenching includes immersing the sintered precursor mixture in liquid argon.

Citation Information

Cited By

  • MOF glass as well as preparation method and application thereof

    CN120423781A