Coating composition and coating film forming method
By using a combination of hydroxyl-containing resin, polyisocyanate compound, zinc compound and amidine compound catalyst and phosphate ester group in the coating composition, the problems of toxicity and insufficient pot life of organotin compounds are solved, and low-temperature and short-time curing and High pot life coating compositions that provide excellent cure performance and finished product appearance.
Patent Information
- Application Number
- CN202380021573.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-18
- Filing Date
- 2023-02-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-17
AI Technical Summary
In the existing technology, hydroxyl/isocyanate-based cross-linked coating compositions require the use of organotin compounds as catalysts during low-temperature and short-time curing processes. However, their toxicity issues and insufficient pot life make it difficult to meet higher performance requirements.
Using a hydroxyl-containing resin, a polyisocyanate compound, an organometallic catalyst formed from a zinc compound and an amidine compound, and a compound containing a phosphate group to form a new coating composition that can be cured at low temperature and in a short time, and can be cured without use In the case of organotin compounds, the pot life is increased.
The coating composition achieves excellent curing performance at low temperatures and in a short time, while extending the pot life, avoiding the toxicity issues of organotin compounds, and providing better finished product appearance and weather resistance.
Smart Images

Figure BDA0004990714690000231 
Figure BDA0004990714690000241 
Figure BDA0004990714690000251
Abstract
Description
Technical Field
[0001] The present invention relates to a coating composition and a coating film forming method. Background Art
[0002] In the painting of automobile bodies and the like, in recent years, developments to shorten the baking and curing steps have been actively conducted from the viewpoints of energy conservation and reduction of environmental load.
[0003] In shortening the baking curing step, there is an increasing demand for lowering the temperature in the curing step and shortening its time period. As a coating composition that meets such low temperature and short time curing requirements, a hydroxyl / isocyanate crosslinked coating composition has been studied, in which a hydroxyl-containing resin is cured by using a polyisocyanate compound as a curing agent.
[0004] Organic tin compounds are generally used as catalysts for accelerating the curing reaction of the above-mentioned hydroxyl / isocyanate group crosslinking coating composition (Patent Document 1).
[0005] However, despite the extremely high catalytic performance of organotin compounds, their toxicity has become a problem in recent years. Therefore, there is a need for catalysts that can replace organotin compounds.
[0006] In addition, a hydroxyl / isocyanate crosslinking coating composition is generally used by mixing a main agent containing a hydroxyl-containing resin and a curing agent containing a polyisocyanate compound. In order to ensure the working time after mixing, an excellent pot life is required.
[0007] In Patent Document 2, it is described that a coating composition having the following characteristics can achieve excellent low temperature and short time curing and pot life, and can provide a cured coating film with excellent finished product appearance: the composition contains (A) a secondary hydroxyl-containing acrylic resin, which is a copolymer of monomer components formed by 20% to 50% by mass of (a) a polymerizable unsaturated monomer containing a secondary hydroxyl group and 50% to 80% by mass of (b) any other polymerizable unsaturated monomer, (B) a polyisocyanate compound, and (C) an organic metal catalyst formed by (C1) a metal compound and (C2) an amidine compound, the metal of the metal compound being one selected from the following: zinc; tin; zirconium; bismuth; lead; cobalt; manganese; titanium; aluminum; and molybdenum; and the equivalent ratio (NCO / OH) of the isocyanate group in the polyisocyanate compound (B) to the hydroxyl group in the secondary hydroxyl-containing acrylic resin (A) falls within the range of 0.8 to 1.8. However, in recent years, it has been desired that the coating composition has a more excellent pot life.
[0008] Reference List
[0009] Patent Literature
[0010] PTL 1:JP 2002-338885 A
[0011] PTL 2: WO 2013 / 04720A1 Summary of the invention
[0012] Technical issues
[0013] An object to be achieved by the present invention is to provide a coating composition which has excellent low-temperature and short-time curability and has an excellent pot life without using any organic tin compound.
[0014] Solution to the problem
[0015] To achieve the above object, the inventors of the present invention have conducted extensive studies and found that the above object can be achieved by a coating composition comprising: (A) a hydroxyl-containing resin; (B) a polyisocyanate compound; (C) an organic metal catalyst formed by a zinc compound and an amidine compound; and (D) a compound containing a phosphate group.
[0016] According to the present invention, there are provided a coating composition and a coating film forming method including the following aspects.
[0017] Item 1. A coating composition comprising: (A) a hydroxyl-containing resin; (B) a polyisocyanate compound; (C) an organic metal catalyst formed from a zinc compound and an amidine compound; and (D) a compound containing a phosphate group.
[0018] Item 2. The coating composition according to Item 1, wherein the hydroxyl-containing resin (A) contains a hydroxyl-containing acrylic resin (A1).
[0019] Item 3. The coating composition according to Item 2, wherein the hydroxyl-containing acrylic resin (A1) contains a primary hydroxyl-containing acrylic resin (A11).
[0020] Item 4. The coating composition according to any one of Items 1 to 3, wherein the phosphate group-containing compound (D) contains an alkyl phosphate (D1) and / or a phosphate group-containing resin (D2).
[0021] Item 5. A method for forming a coating film, comprising: coating a top portion of an object to be coated with the coating composition described in any one of Items 1 to 4 to form a coating film; and then heating the coating film to cure the coating film.
[0022] Advantageous Effects of the Invention
[0023] The coating composition of the present invention has excellent low-temperature and short-time curing properties and has an excellent pot life without using any organic tin compound. Specific implementation plan
[0024] In this specification, except for the case where it is clearly described separately in this specification or the case where there is an obvious contradiction in the context, the singular form (for example, a, an or the) includes the singular form and the plural form. The coating composition of the present invention (hereinafter sometimes referred to as "the coating") is described in more detail below.
[0025] The coating composition of the present invention is a coating composition comprising: (A) a hydroxyl group-containing resin; (B) a polyisocyanate compound; (C) an organic metal catalyst formed of a zinc compound and an amidine compound; and (D) a phosphate group-containing compound.
[0026] Hydroxyl-containing resin (A)
[0027] The hydroxyl-containing resin (A) is a resin having at least one hydroxyl group in its molecule. Various known resins can be used as the hydroxyl-containing resin (A), and examples thereof include resins such as acrylic resins having hydroxyl groups, polyester resins having hydroxyl groups, acrylic modified polyester resins having hydroxyl groups, polyether resins having hydroxyl groups, polycarbonate resins having hydroxyl groups, polyurethane resins having hydroxyl groups, epoxy resins having hydroxyl groups, and alkyd resins having hydroxyl groups. These resins can be used alone or in combination. In particular, from the viewpoint of water resistance of the coating film to be formed, the hydroxyl-containing resin (A) preferably contains a hydroxyl-containing acrylic resin (A1).
[0028] Hydroxyl-containing acrylic resin (A1)
[0029] The hydroxy-containing acrylic resin (A1) can be obtained by, for example, copolymerizing a hydroxy-containing polymerizable unsaturated monomer and any other polymerizable unsaturated monomer (a polymerizable unsaturated monomer other than the hydroxy-containing polymerizable unsaturated monomer).
[0030] The above-mentioned hydroxyl-containing polymerizable unsaturated monomer is a compound having one or more hydroxyl groups and one or more polymerizable unsaturated bonds in its molecule. Examples of hydroxyl-containing polymerizable unsaturated monomers may include: (meth) acrylic acid and monoester compounds of diols each having 2 to 8 carbon atoms, such as (meth) acrylic acid 2-hydroxyethyl ester, (meth) acrylic acid 2-hydroxypropyl ester, (meth) acrylic acid 3-hydroxypropyl ester and (meth) acrylic acid 4-hydroxybutyl ester; (meth) acrylic acid and ε-caprolactone-modified products of monoester compounds of diols each having 2 to 8 carbon atoms; (meth) acrylic acid and adducts of epoxy group-containing compounds (e.g., "CARDURAE10P" (product name), manufactured by Hexion, Inc., neodecanoic acid glycidyl ester); N-hydroxymethyl (meth) acrylamide; allyl alcohol; and (meth) acrylic acid esters each having a polyoxyethylene chain having a hydroxyl group at its molecular end.
[0031] For example, the monomers described in the following items (1) to (6) can each be used as other polymerizable unsaturated monomers copolymerizable with the above-mentioned hydroxyl-containing polymerizable unsaturated monomer. These polymerizable unsaturated monomers can be used alone or in combination.
[0032] (1) Acid group-containing polymerizable unsaturated monomers
[0033] The polymerizable unsaturated monomer containing an acid group is a compound having one or more acid groups and one or more polymerizable unsaturated bonds in its molecule. Examples of monomers may include: carboxyl-containing monomers, such as (meth) acrylic acid, crotonic acid, itaconic acid, maleic acid and maleic anhydride; and sulfonic acid-containing monomers, such as vinyl sulfonic acid and (meth) 2-sulfoethyl acrylate. These monomers may be used alone or in combination. When using a polymerizable unsaturated monomer containing an acid group, its amount is set so that the acid value of the hydroxy-containing acrylic resin (A1) may be preferably 0.5 mgKOH / g to 15 mgKOH / g, more preferably 1 mgKOH / g to 12 mgKOH / g.
[0034] (2) Ester compounds of acrylic acid or methacrylic acid and a monohydric alcohol having 1 to 20 carbon atoms
[0035] The ester compound of acrylic acid or methacrylic acid and a monohydric alcohol having 1 to 20 carbon atoms may specifically be, for example, methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, isostearyl acrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., product name), lauryl (meth)acrylate, tridecyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, cyclohexyl (meth)acrylate or isobornyl (meth)acrylate.
[0036] (3) Aromatic vinyl monomers
[0037] The aromatic vinyl monomer may specifically be, for example, styrene, α-methylstyrene or vinyltoluene.
[0038] When an aromatic vinyl monomer is used as a component, the glass transition temperature of the resin to be obtained increases, and a hydrophobic coating film having a high refractive index can be obtained. Therefore, an effect of improving the appearance of the finished product by improving the gloss of the coating film can be obtained.
[0039] When an aromatic vinyl monomer is used as a component, the mixing ratio thereof is preferably in the range of 3% by mass to 50% by mass, more preferably in the range of 5% by mass to 40% by mass, relative to the total amount of the monomer components.
[0040] (4) Glycidyl-containing polymerizable unsaturated monomers
[0041] The glycidyl group-containing polymerizable unsaturated monomer is a compound having one or more glycidyl groups and one or more polymerizable unsaturated bonds in its molecule. Specific examples thereof may include glycidyl acrylate and glycidyl methacrylate.
[0042] (5) Compounds containing a nitrogen atom and containing a polymerizable unsaturated bond
[0043] The nitrogen atom-containing compound containing a polymerizable unsaturated bond may be, for example, (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-[3-(dimethylamino)propyl](meth)acrylamide, N-butoxymethyl(meth)acrylamide, diacetone(meth)acrylamide, N,N-dimethylaminoethyl(meth)acrylate, vinylpyridine, vinylimidazole, acrylonitrile or methacrylonitrile.
[0044] (6) Other vinyl compounds
[0045] Any other vinyl compound may be, for example, vinyl acetate, vinyl propionate, vinyl chloride or vinyl versatate. Examples of vinyl versatate may include commercial products "VeoVa 9" and "VeoVa 10" (which are product names, manufactured by Hexion, Inc.).
[0046] The term "polymerizable unsaturated monomer" as used herein refers to a monomer having one or more (e.g., 1 to 4) polymerizable unsaturated groups. The term "polymerizable unsaturated group" means an unsaturated group that can undergo free radical polymerization. Examples of such polymerizable unsaturated groups include vinyl, (meth)acryloyl, (meth)acrylamide, vinyl ether, allyl, propenyl, isopropenyl, and maleimide.
[0047] In addition, the term "(meth)acrylate" used herein means acrylate or methacrylate. The term "(meth)acrylic acid" means acrylic acid or methacrylic acid. In addition, the term "(meth)acryloyl" means acryl or methacryloyl. In addition, the term "(meth)acrylamide" means acrylamide or methacrylamide.
[0048] The hydroxy value of the hydroxy-containing acrylic resin (A1) is preferably within a range of 20 to 200 mg KOH / g, more preferably 25 to 180 mg KOH / g, and particularly preferably 30 to 160 mg KOH / g, from the viewpoints of pot life, low temperature and short time curing properties of the coating composition, and the like.
[0049] Furthermore, from the viewpoint of pot life, low temperature and short time curability of the coating composition, etc., the weight average molecular weight of the above hydroxyl-containing acrylic resin (A1) falls within the range of preferably 2,000 to 50,000, more preferably 3,000 to 40,000, particularly preferably 4,000 to 30,000.
[0050] The term "weight average molecular weight" used herein refers to the value calculated from the molecular weight of a chromatogram measured by a gel permeation chromatograph relative to standard polystyrene. "HLC-8120GPC" (manufactured by Tosoh Corporation) is used as a gel permeation chromatograph. Four columns "TSKgel G-4000HXL", "TSKgel G-3000HXL", "TSKgel G-2500HXL" and "TSKgel G-2000HXL" (all manufactured by Tosoh Corporation, product names) are used as columns, and measurements are performed under the following conditions: tetrahydrofuran is used as a mobile phase; the measurement temperature is set to 40°C; the flow rate is set to 1cc / min; and an RI detector is used as a detector.
[0051] Furthermore, from the viewpoint of the hardness and final appearance of the coating film to be formed, the glass transition temperature of the hydroxyl-containing acrylic resin (A1) preferably falls within the range of -30 to 85°C, more preferably -10 to 80°C, particularly preferably 10 to 75°C.
[0052] In this specification, the glass transition temperature (° C.) of the acrylic resin is calculated by the following equation.
[0053] 1 / Tg(K)=(W1 / T1)+(W2 / T2)+……(1)
[0054] Tg (℃)=Tg (K)-273 (2)
[0055] In the corresponding equations, W1, W2, ... represent the corresponding mass fractions of the monomers used for copolymerization, and T1, T2, ... represent the Tg (K) of the homopolymers of the corresponding monomers.
[0056] T1, T2, ... are values according to "Polymer Handbook (Second Edition, edited by J. Brandup and EH Immergut)" III, pages 139-179. In addition, when the Tg of the homopolymer of the monomer is unclear, the static glass transition temperature is used as the glass transition temperature (°C). For example, the sample is loaded into the measuring cup of a differential scanning calorimeter "DSC-220U" (manufactured by Seiko Instruments Inc.), and vacuum suction is performed to completely remove the solvent, and then the change in heat is measured with a calorimeter in the range of -20°C to +200°C at a heating rate of 3°C / min. The first baseline change point at a lower temperature is used as the static glass transition temperature.
[0057] The copolymerization method for obtaining the hydroxyl-containing acrylic resin (A1) by copolymerization of the above-mentioned monomer mixture is not particularly limited, and copolymerization methods known per se can each be used. In particular, a solution polymerization method involving polymerization in an organic solvent in the presence of a polymerization initiator can be suitably used.
[0058] Examples of the organic solvent used in the solution polymerization method may include: aromatic solvents such as toluene, xylene and SWASOL 1000 (manufactured by Maruzen Petrochemical Co., Ltd., product name, high boiling point petroleum-based solvent); ester-based solvents such as ethyl acetate, butyl acetate, propyl propionate, butyl propionate, 1-methoxy-2-propyl acetate, 2-ethoxyethyl propionate, 3-methoxybutyl acetate, ethylene glycol ethyl ether acetate and propylene glycol methyl ether acetate; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone and methyl amyl ketone; and alcohol-based solvents such as isopropyl alcohol, n-butanol, isobutyl alcohol and 2-ethylhexanol.
[0059] Although these organic solvents may be used alone or in combination, an ester-based solvent or a ketone-based solvent is preferably used in terms of solubility of the acrylic resin. In addition, further, an aromatic solvent may be suitably used in combination therewith.
[0060] Examples of the polymerization initiator that can be used for the copolymerization of the hydroxyl-containing acrylic resin (A1) may include known free radical polymerization initiators such as 2,2′-azobisisobutyronitrile, benzoyl peroxide, di-tert-butyl peroxide, di-tert-amyl peroxide, tert-butyl peroctoate, 2,2′-azobis(2-methylbutyronitrile) and 2,2′-azobis(2,4-dimethylvaleronitrile).
[0061] The hydroxyl-containing acrylic resin (A1) can be used alone or in combination.
[0062] The hydroxyl-containing acrylic resin (A1) preferably includes a primary hydroxyl-containing acrylic resin (A11) from the viewpoints of low temperature and short-time curing properties and the like.
[0063] The above-mentioned primary hydroxyl-containing acrylic resin (A11) can be prepared, for example, by using a primary hydroxyl-containing polymerizable unsaturated monomer as a hydroxyl-containing polymerizable unsaturated monomer in the above-mentioned method for producing the hydroxyl-containing acrylic resin (A1).
[0064] Examples of the above-mentioned polymerizable unsaturated monomers containing primary hydroxyl groups include: polymerizable unsaturated monomers having primary hydroxyl groups, wherein the alkyl group of the ester portion has 2 to 8, preferably 2 to 6, more preferably 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth) acrylate, 3-hydroxypropyl (meth) acrylate, or 4-hydroxybutyl (meth) acrylate; and adducts of (meth) acrylic acid and epoxy group-containing compounds (e.g., "CARDURA E10P" (product name), manufactured by Hexion, Inc., neodecanoic acid glycidyl ester). These monomers can be used alone or in combination. In particular, from the perspective of the hardness of the coating to be formed, 2-hydroxyethyl (meth) acrylate can be suitably used.
[0065] From the viewpoint of low-temperature and short-time curing properties of the coating film to be formed, etc., in the production of the above-mentioned primary hydroxyl-containing acrylic resin (A11), the amount of the above-mentioned primary hydroxyl-containing polymerizable unsaturated monomer used preferably falls within the range of 10% by mass to 60% by mass relative to the total amount of the monomer components to be copolymerized, and more preferably falls within the range of 5% by mass to 50% by mass relative thereto.
[0066] Furthermore, in the above-mentioned primary hydroxyl group-containing acrylic resin (A11), from the viewpoints of low temperature and short time curing properties, etc., the content of the above-mentioned primary hydroxyl group-containing polymerizable unsaturated monomer in the total amount of hydroxyl group-containing polymerizable unsaturated monomers preferably falls within the range of 50 mass % to 100 mass %, more preferably falls within the range of 55 mass % to 100 mass %, and still more preferably falls within the range of 60 mass % to 100 mass %.
[0067] From the viewpoints of pot life, low temperature and short time curing properties of the coating composition, etc., the content of the above-mentioned hydroxyl-containing acrylic resin (A1) in the coating composition of the present invention is preferably 40% by mass to 85% by mass, more preferably 45% by mass to 75% by mass, and still more preferably 50% by mass to 70% by mass relative to the resin solid content of the coating composition.
[0068] Polyisocyanate compound (B)
[0069] The polyisocyanate compound (B) is a compound having at least two isocyanate groups in its molecule, and examples thereof may include aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds, aromatic-aliphatic polyisocyanate compounds, aromatic polyisocyanate compounds, and derivatives of polyisocyanate compounds.
[0070] Examples of the aliphatic polyisocyanate compound may include aliphatic diisocyanate compounds such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 1,2-butylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate or 2,2,4-trimethylhexamethylene diisocyanate, dimer acid diisocyanate, and 2,6- Methyl diisocyanatohexanoate (common name: lysine diisocyanate); and aliphatic triisocyanate compounds, such as 2-isocyanatoethyl 2,6-diisocyanatohexanoate, 1,6-diisocyanato-3-isocyanatomethylhexane, 1,4,8-triisocyanatooctane, 1,6,11-triisocyanatoundecane, 1,8-diisocyanato-4-isocyanatomethyloctane, 1,3,6-triisocyanatohexane, and 2,5,7-trimethyl-1,8-diisocyanato-5-isocyanatomethyloctane.
[0071] Examples of the alicyclic polyisocyanate compound may include: alicyclic diisocyanate compounds such as 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexyl diisocyanate (common name: hydrogenated TDI), 2-methyl-1,3-cyclohexyl diisocyanate (common name: hydrogenated TDI), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 4-methyl-1,3-cyclohexyl diisocyanate (common name: hydrogenated TDI), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 3-isocyanatomethyl-1,3-cyclohexyl diisocyanate (common name: hydrogenated TDI), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diisocyanate), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl iso ... isophorone diisocyanate), 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (common name: isophorone diiso diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane or 1,4-bis(isocyanatomethyl)cyclohexane (common name: hydrogenated xylylene diisocyanate) or a mixture thereof, methylenebis(4,1-cyclohexanediyl)diisocyanate (common name: hydrogenated MDI), and norbornane diisocyanate; and alicyclic triisocyanate compounds such as 1,3,5-triisocyanatocyclohexane, 1,3,5-trimethylisocyanatocyclohexane , 2-(3-isocyanatopropyl)-2,5-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 2-(3-isocyanatopropyl)-2,6-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 3-(3-isocyanatopropyl)-2,5-bis(isocyanatomethyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo Cyclo(2.2.1)heptane, 6-(2-isocyanatoethyl)-2-isocyanatomethyl-3-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, 5-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane, and 6-(2-isocyanatoethyl)-2-isocyanatomethyl-2-(3-isocyanatopropyl)-bicyclo(2.2.1)heptane.
[0072] Examples of the aromatic-aliphatic polyisocyanate compound may include: an aromatic-aliphatic diisocyanate compound such as methylenebis(4,1-phenylene)diisocyanate (common name: MDI), 1,3-xylylene diisocyanate or 1,4-xylylene diisocyanate or a mixture thereof, ω,ω′-diisocyanato-1,4-diethylbenzene, and 1,3-bis(1-isocyanato-1-methylethyl)benzene or 1,4-bis(1-isocyanato-1-methylethyl)benzene (common name: tetramethylxylylene diisocyanate) or a mixture thereof; and an aromatic-aliphatic triisocyanate compound such as 1,3,5-triisocyanatomethylbenzene.
[0073] Examples of the aromatic polyisocyanate compound may include: an aromatic diisocyanate compound such as m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4′-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 2,4-tolylene diisocyanate (common name: 2,4-TDI) or 2,6-tolylene diisocyanate (common name: 2,6-TDI) or a mixture thereof, 4,4′-toluidine diisocyanate, and 4,4′-diphenyl ether diisocyanate; an aromatic triisocyanate compound such as triphenylmethane-4,4′,4″-triisocyanate, 1,3,5-triisocyanatobenzene, and 2,4,6-triisocyanatotoluene; and an aromatic tetraisocyanate compound such as 4,4′-diphenylmethane-2,2′,5,5′-tetraisocyanate.
[0074] In addition, examples of derivatives of the polyisocyanate compounds may include dimers, trimers, biuret, allophanate, uretdione, uretimine, isocyanurate, oxadiazinetrione, polymethylene polyphenyl polyisocyanate (crude MDI and polymeric MDI), and crude TDI of the above polyisocyanate compounds.
[0075] The above-mentioned polyisocyanate compounds and derivatives thereof may be used alone or in combination.
[0076] From the viewpoint of weather resistance of the coating film to be formed, it is preferred to use at least one selected from aliphatic polyisocyanate compounds, alicyclic polyisocyanate compounds and derivatives thereof as the polyisocyanate compound (B), and from the viewpoint of the final appearance of the coating film to be formed by the coating composition to be obtained, it is more preferred to use aliphatic polyisocyanate compounds and / or derivatives thereof.
[0077] In particular, from the viewpoints of, for example, the final appearance, curability and weather resistance of the coating film to be formed, an aliphatic diisocyanate compound and / or its isocyanurate form among those mentioned above is preferably used as the above-mentioned aliphatic polyisocyanate compound and / or its derivative, and hexamethylene diisocyanate and / or its isocyanurate form is more preferably used.
[0078] The content of the polyisocyanate compound (B) in the coating composition of the present invention is preferably 5% by mass to 60% by mass, more preferably 10% by mass to 55% by mass, still more preferably 15% by mass to 50% by mass, relative to the resin solid content of the coating composition, from the viewpoints of, for example, pot life, low temperature and short time curability of the coating composition.
[0079] Organometallic catalyst (C) formed from a zinc compound and an amidine compound
[0080] The organometallic catalyst (C) composed of the zinc compound and the amidine compound has both a catalyst function for accelerating the curing reaction of the coating when heated and a blocker function for the catalytic ability at room temperature.
[0081] This may be due to the following reasons. The organometallic catalyst (C) formed by the zinc compound and the amidine compound forms a complex structure, and the amidine compound is used as a blocking agent. The amidine compound used as a blocking agent dissociates at low temperatures, and after the amidine compound dissociates, the inherent catalytic ability of the zinc compound, that is, the ability to improve low-temperature curing, becomes active. Therefore, the low-temperature and short-time curing and application period of the coating can be achieved.
[0082] Examples of the above zinc compound may include carboxylic acid zinc compounds and acetylacetonate zinc complexes. In particular, carboxylic acid zinc compounds may be suitably used.
[0083] Specific examples of the above-mentioned zinc carboxylate compound may include zinc 2-ethylhexanoate, zinc acetate, zinc naphthenate, zinc octoate, zinc stearate, zinc neodecanoate and zinc oleate. In particular, zinc octoate may be suitably used because zinc octoate has excellent catalytic activity and is easily available industrially.
[0084] The amidine compound is an organic compound having a structure represented by the following formula (1).
[0085] R 1 -C(=NR 2 )-NR 3 R 4 …(1)
[0086] In formula (1), one nitrogen atom is bonded to the carbon (C) atom via a double bond, and the other nitrogen atom is bonded thereto via a single bond.
[0087] R 1 represents a hydrogen atom, an organic group which may be substituted, or an amine group, and specifically represents, for example, a hydrocarbon group which may be substituted or a hydroxyl group which may be etherified.
[0088] R 2 and R 3 Each independently represents a hydrogen atom or an organic group, or represents a heterocycle having a structure in which heterocycles are bonded to each other (the heterocycles are each a monocycle having one, two or more heteroatoms, or a bonded bicycle having one, two or more heteroatoms).
[0089] R 4 represents a hydrogen atom, an organic group which may be substituted, or a hydroxyl group which may be etherified, and may preferably represent, for example, a hydrocarbon group having 8 or more carbon atoms which may be substituted.
[0090] When R 1 or R 4 When an organic group is indicated, the group may be, for example, a group having 1 to 40 carbon atoms, or a polymer group having, for example, a molecular weight of 500 to 50,000.
[0091] By R 1 , R 2 , R 3 and R 4 The groups represented may each independently contain an alcoholic hydroxyl group as a substituent.
[0092] Where R 2 and R 3 Specific examples of the amidine compounds represented by formula (1) which are not bonded to each other may include N′-cyclohexyl-N,N-dimethylformamidine, N′-methyl-N,N-di-n-butylacetamidine, N′-octadecyl-N,N-dimethylformamidine, N′-cyclohexyl-N,N-dimethylpentamidine, 1-methyl-2-cyclohexyliminopyrrolidine, 3-butyl-3,4,5,6-tetrahydropyrimidine, N-(hexyliminomethyl)morpholine, N-(α-(decyliminoethyl)ethyl)pyrrolidine, N′-decyl-N,N-dimethylformamidine, N′-decyl-N,N-dimethylformamidine, and N′-cyclohexyl-N,N-acetamidine.
[0093] In addition, the following amidine compounds are included in the amidine compounds: 2 -R 3 In its amidine structure, a five- to seven-membered ring containing two nitrogen atoms is formed, and R 1 -R 3 or R 1 -R 4 An amidine compound in which a five- to nine-membered ring structure having one nitrogen atom and a plurality of carbon atoms is formed in the amidine structure.
[0094] Specific examples of the amidine compound having such a structure may include 1,5-diazabicyclo(4.3.0)non-5-ene, 1,8-diazabicyclo(5.4.0)undec-7-ene, 1,4-diazabicyclo(3.3.0)oct-4-ene, 2-methyl-1,5-diazabicyclo(4.3.0)non-5-ene, 2,7,8-trimethyl-1,5-diazabicyclo(4.3.0)non-5-ene, 2-butyl-1,5-diazabicyclo(4.3.0)non-5-ene, and 1,9-diazabicyclo(6.5.0)tridec-8-ene.
[0095] In addition, examples of the amidine compound may include: 2 and R 3Heterocyclic compounds of structures bonded to each other, such as imidazole, imidazoline, tetrahydropyrimidine, dihydropyrimidine, and pyrimidine ring-containing compounds.
[0096] Specific examples of the imidazole compound may include N-(2-hydroxyethyl)imidazole, N-(3-aminopropyl)imidazole, 4-(hydroxymethyl)imidazole, 1-(tert-butoxycarbonyl)imidazole, imidazole-4-propionic acid, 4-carboxyimidazole, 1-butylimidazole, 1-methylimidazole, 2-methyl-4-imidazolecarboxylic acid, 4-formylimidazole, 1-(ethoxycarbonyl)imidazole, a reaction product of propylene oxide with imidazole and 2-methylimidazole, 1-trimethylsilylimidazole, 4-(hydroxymethyl)imidazole hydrochloride, 1-chloro-2,3-propylene oxide with imidazole copolymers of, 1-(p-toluenesulfonyl)imidazole, 1,1-carbonylbisimidazole, 1-(2-cyanoethyl)-2-ethyl-4-methylimidazole, 2-phenyl-2-imidazoline pyromellitate, 4-(hydroxymethyl)imidazole picrate, 2-acrylic acid with disodium salt of 4,5-dihydro-2-nonyl-1H-imidazole-1-ethanol and 2-heptyl-4,5-dihydro-1H-imidazole-1-ethanol, 1-(cyanoethyl)-2-undecylimidazole trimellitate, 1-(2-hydroxypropyl)imidazole formate, sodium imidazole, and silver imidazole.
[0097] The amidine compounds may be used alone or in combination.
[0098] Specifically, in the coating material, the organic metal catalyst formed of a zinc compound and an amidine compound is a metal complex, and the complex can be prepared by, for example, heating one mole of zinc carboxylate and two moles of the amidine compound in a solvent such as methanol.
[0099] In the above production, the metal complex can be produced by keeping the mixture at about 50° C. for about 2 hours until the mixture becomes a transparent solution state. The transparent solution is filtered and dried. From the viewpoints of the pot life, low temperature and short time curing of the coating composition, the molar ratio of the amidine compound to the zinc compound (the ratio of the number of moles of the amidine compound to the number of moles of the zinc compound) is preferably set in the range of 1.3 to 8.0, more preferably in the range of 1.6 to 5.0, and still more preferably in the range of 1.8 to 4.0.
[0100] The organometallic catalyst formed by the zinc compound and the amidine compound can be used by dissolving in a solvent. The solvent is not particularly limited, but examples thereof may include the following solvents: alcohol compounds such as ethylene glycol, diethylene glycol, dipropylene glycol, propylene glycol, and butanediol; hydrocarbons such as toluene, xylene, mineral turpentine, and mineral spirits; ester compounds such as ethyl acetate, butyl acetate, methyl glycol acetate, and cellosolve acetate; ketone compounds such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; glycol ether compounds such as ethyl 3-ethoxypropionate and 3-methoxybutyl acetate; organic solvents of amide compounds such as N,N-dimethylformamide and N,N-dimethylacetamide; β-diketone compounds such as acetylacetone and fluorine-substituted products thereof; and ketoester compounds such as methyl acetoacetate and ethyl acetoacetate.
[0101] From the viewpoints of pot life, low temperature and short time curability of the coating composition, etc., the content of the organometallic catalyst (C) formed of the zinc compound and the amidine compound preferably falls within the range of 0.01 to 5 parts by mass, more preferably within the range of 0.03 to 4 parts by mass, and still more preferably within the range of 0.05 to 3 parts by mass, relative to 100 parts by mass of the resin solid content of the coating composition of the present invention.
[0102] Phosphate group-containing compound (D)
[0103] The compound (D) containing a phosphate group has a function of inhibiting the catalytic ability of the organic metal catalyst (C) composed of a zinc compound and an amidine compound at ordinary temperature.
[0104] Examples of the compound (D) containing a phosphate group may include: phosphoric acid; monoalkyl phosphoric acids such as mono-n-propyl phosphoric acid, mono-isopropyl phosphoric acid, mono-n-butyl phosphoric acid, mono-isobutyl phosphoric acid, mono-tert-butyl phosphoric acid, mono-octyl phosphoric acid and mono-decyl phosphoric acid; dialkyl phosphoric acids such as di-n-propyl phosphoric acid, di-isopropyl phosphoric acid, di-n-butyl phosphoric acid, di-isobutyl phosphoric acid, di-tert-butyl phosphoric acid, di-octyl phosphoric acid and didecyl phosphoric acid; monoalkyl phosphorous acids such as mono-n-propyl phosphoric acid, mono-isopropyl phosphoric acid, mono-n-butyl phosphoric acid, mono-isobutyl phosphoric acid, mono-tert-butyl phosphoric acid, mono-octyl phosphoric acid and mono-decyl phosphoric acid; dialkyl phosphorous acids such as di-n-propyl phosphoric acid, di-isopropyl phosphoric acid, di-n-butyl phosphoric acid, di-isobutyl phosphoric acid, di-tert-butyl phosphoric acid, di-octyl phosphoric acid and didecyl phosphoric acid; alkyl ether phosphoric acids; polyoxyethylene alkyl ether phosphoric acids; alkyl phosphates (D1); and resins (D2) containing a phosphate group. In particular, it is preferred to incorporate alkyl phosphate (D1) and / or a phosphate group-containing resin (D2), and more preferably to incorporate alkyl phosphate (D1). These compounds may be used alone or in combination.
[0105] In the present invention, the resin containing a phosphate group and a hydroxyl group is not included in the hydroxyl group-containing resin (A) but is included in the phosphate group-containing compound (D).
[0106] The alkyl phosphate (D1) may be, for example, a compound having a chemical structure represented by the following formula (2).
[0107] O=P(OR) n (OH) 3-n ……Formula (2)
[0108] In the formula, R represents an alkyl group having 4 or more, preferably 6 to 20 carbon atoms. The alkyl group may be linear or branched, preferably branched. In addition, "n" represents an integer of 1 to 3. In addition, "n" Rs may be the same or different from each other.
[0109] Commercial products that can be used as the above-mentioned alkyl phosphate (D1) are, for example, NACURE 4054J (product name, manufactured by King Industries, Inc.), Korantin SMK (product name, manufactured by BASF SE), NIKKOL PHOSTEN HLP (product name, manufactured by Nikko Chemicals Co., Ltd.), PHOSPHANOL RS-410, PHOSPHANOL RS-610, PHOSPHANOL RS-710, PHOSPHANOL RD-510Y, PHOSPHANOL RD-720, PHOSPHANOL RB-410, PHOSPHANOL RL-210, PHOSPHANOL RL-310, PHOSPHANOL ML-200, PHOSPHANOL ML-220, PHOSPHANOL RE-410, PHOSPHANOL PE-510, PHOSPHANOL PHOSPHANOL RE-610, PHOSPHANOL RE-960, PHOSPHANOL RM-410, PHOSPHANOL RM-510, PHOSPHANOL RM-710, PHOSPHANOL RE-210, PHOSPHANOL RP-710, or PHOSPHANOL SM-172 (all are product names, manufactured by TOHO Chemical Industry Co., Ltd.), or PLYSURF A212C, PLYSURF A215C, PLYSURF A208B, PLYSURF A219B, PLYSURF A210G, PLYSURF A208F, or PLYSURF A212E (all are product names, manufactured by DKS Co. Ltd.). Each of these products may be used as it is or as a salt neutralized with an alkali metal or an organic base. Furthermore, two or more of them may be used in combination.
[0110] From the viewpoints of pot life, low temperature and short time curability of the coating composition, etc., when the coating composition of the present invention includes the above-mentioned alkyl phosphate (D1) as the phosphate group-containing compound (D), its content preferably falls within the range of 0.01 to 3 parts by mass, more preferably within the range of 0.05 to 2.5 parts by mass, and still more preferably within the range of 0.1 to 2 parts by mass relative to 100 parts by mass of the resin solid content of the coating composition of the present invention.
[0111] Examples of the above-mentioned phosphoric acid ester group-containing resin (D2) may include phosphoric acid ester group-containing acrylic resin (D21), phosphoric acid ester group-containing polyester resin, phosphoric acid ester group-containing polyether resin, phosphoric acid ester group-containing polycarbonate resin, phosphoric acid ester group-containing polyurethane resin and phosphoric acid ester group-containing epoxy resin. In particular, phosphoric acid ester group-containing acrylic resin (D21) is preferred from the viewpoints of the pot life, low temperature and short time curing of the coating composition.
[0112] The phosphate group-containing acrylic resin (D21) can be synthesized by copolymerizing a polymerizable unsaturated monomer having a phosphate group and any other polymerizable unsaturated monomer by a conventional method.
[0113] Examples of the polymerizable unsaturated monomer having a phosphate group may include acidic phosphooxyethyl (meth)acrylate, acidic phosphooxypropyl (meth)acrylate, acidic phosphooxypoly (oxyethylene) glycol (meth)acrylate, and acidic phosphooxypoly (oxypropylene) glycol (meth)acrylate.
[0114] Examples of other polymerizable unsaturated monomers may include the compounds listed in the section of "hydroxyl-containing acrylic resin (A1)".
[0115] In the phosphate group-containing acrylic resin (D21), the polymerizable unsaturated monomer having a phosphate group preferably accounts for 1 to 50% by mass, particularly preferably 5 to 40% by mass, of the total amount of the corresponding monomer components used to form the phosphate group-containing acrylic resin (D21).
[0116] The weight average molecular weight of the phosphate group-containing acrylic resin (D21) falls within the range of preferably 3,000 to 30,000, more preferably 5,000 to 25,000, particularly preferably 7,000 to 20,000, from the viewpoint of final appearance and coating film properties.
[0117] From the viewpoints of the pot life, low temperature and short time curing properties of the coating composition, etc., when the coating composition of the present invention includes the above-mentioned phosphate group-containing acrylic resin (D21) as the phosphate group-containing compound (D), its content is preferably 0.01% by mass to 3% by mass, more preferably 0.05% by mass to 2.5% by mass, and still more preferably 0.1% by mass to 2% by mass relative to the resin solid content of the coating composition.
[0118] From the viewpoints of the pot life, low temperature and short time curability of the coating composition, etc., when the coating composition of the present invention includes a phosphate group-containing compound other than the above-mentioned alkyl phosphate (D1) and the above-mentioned phosphate group-containing acrylic resin (D21) as the phosphate group-containing compound (D), its content preferably falls within the range of 0.01 to 3 parts by mass, more preferably within the range of 0.05 to 2.5 parts by mass, and still more preferably within the range of 0.1 to 2 parts by mass relative to 100 parts by mass of the resin solid content of the coating composition of the present invention.
[0119] From the viewpoints of the pot life, low temperature and short time curing properties of the coating composition, etc., in terms of the molar ratio of the organic metal catalyst (C) formed of a zinc compound and an amidine compound to the compound (D) containing a phosphate group, in the coating composition of the present invention, the content ratio of the organic metal catalyst (C) formed of a zinc compound and an amidine compound to the compound (D) containing a phosphate group preferably falls within the range of 1 / 0.1 to 1 / 10, more preferably falls within the range of 1 / 0.3 to 1 / 8, and still more preferably falls within the range of 1 / 0.5 to 1 / 5.
[0120] Other components
[0121] The coating composition of the present invention may further optionally include, for example, a resin other than the hydroxyl-containing resin (A), a crosslinking agent other than the polyisocyanate compound (B), a curing catalyst other than the organic metal catalyst (C) formed of a zinc compound and an amidine compound, a pigment, a matting agent, an organic solvent, a dispersant, an anti-settling agent, a defoaming agent, a thickener, an ultraviolet absorber, a light stabilizer, a surface conditioner, or a scratch resistance improving agent.
[0122] Examples of the resin other than the above-mentioned hydroxyl-containing resin (A) may include hydroxyl-free acrylic resins, hydroxyl-free polyester resins, hydroxyl-free polyurethane resins, hydroxyl-free polyether resins, hydroxyl-free polycarbonate resins, and hydroxyl-free epoxy resins.
[0123] Examples of the pigment may include coloring pigments, gloss pigments, and extender pigments. The pigments may be used alone or in combination.
[0124] Examples of the coloring pigment may include titanium oxide, zinc spangles, carbon black, cadmium red, molybdenum red, chrome yellow, chromium oxide, Prussian blue, cobalt blue, azo pigments, phthalocyanine pigments, quinacridone pigments, isoindoline pigments, threne-based pigments, and perylene pigments.
[0125] Examples of the luster pigment may include aluminum powder, mica powder, and mica powder coated with titanium oxide.
[0126] Examples of the extender pigment may include talc, clay, kaolin, barium oxide, barium sulfate, barium carbonate, calcium carbonate, and aluminum oxide white.
[0127] The above corresponding pigments may be used alone or in combination.
[0128] When the coating composition of the present invention is used as a clear coating and includes a pigment, the blending amount of the pigment is preferably an amount that does not impair the transparency of the coating film to be obtained. For example, the blending amount preferably falls within the range of 0.1% to 20% by mass relative to the total amount of the resin solid content in the coating composition, more preferably falls within the range of 0.3% to 10% by mass, and particularly preferably falls within the range of 0.5% to 5% by mass.
[0129] Furthermore, when the coating composition of the present invention is used as a colored coating and includes a pigment, the blending amount of the pigment relative to the total amount of the resin solid content in the coating composition preferably falls within the range of 1% by mass to 200% by mass, more preferably falls within the range of 2% by mass to 100% by mass, and particularly preferably falls within the range of 5% by mass to 50% by mass.
[0130] Examples of the matting agent include silica particles, alumina particles, titania particles, zirconia particles, zircon particles, tin oxide particles, magnesium oxide particles, polymethyl methacrylate (PMMA) resin beads, MMA-ethylene glycol dimethacrylate (EGDM) copolymer resin beads, nylon resin beads, and polytetrafluoroethylene resin beads.
[0131] When the coating composition of the present invention is used as a matting coating and includes a matting agent, for example, the blending amount of the matting agent preferably falls within the range of 1% by mass to 30% by mass, more preferably falls within the range of 2% by mass to 25% by mass, and particularly preferably falls within the range of 3% by mass to 20% by mass relative to the total amount of the resin solid content in the coating composition.
[0132] Examples of organic solvents may include aromatic solvents such as toluene, xylene, and "SWASOL 1000" (manufactured by Maruzen Petrochemical Co., Ltd., product name, aromatic organic solvent); ester-based solvents such as ethyl acetate, butyl acetate, propyl propionate, butyl propionate, 1-methoxy-2-propyl acetate, 2-ethoxyethyl propionate, ethyl 3-ethoxypropionate, 3-methoxybutyl acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monoethyl ether acetate, and propylene glycol monomethyl ether acetate; ketone-based solvents such as methyl ethyl ketone, methyl isobutyl ketone, and methyl amyl ketone; and alcohol-based solvents such as isopropyl alcohol, n-butanol, isobutyl alcohol, and 2-ethylhexanol. These solvents may be used alone or in combination.
[0133] Hitherto known thickeners can be used as the thickener, and examples thereof may include clay minerals (e.g., metal silicates or montmorillonite), acrylic resins (e.g., acrylic resins containing a structure formed of a polymer or oligomer of acrylate or methacrylate in its molecule, or non-aqueous dispersion resins), polyolefins (e.g., polyethylene or polypropylene), amides (e.g., higher fatty acid amides, polyamides or oligomers), polycarboxylic acids (including derivatives having at least two or more carboxyl groups in its molecule), cellulose (including various derivatives such as nitrocellulose, acetyl cellulose and cellulose ether), carbamates (e.g., polymers or oligomers having a carbamate structure in its molecule), ureas (e.g., polymers or oligomers having a urea structure in its molecule), and carbamate ureas (e.g., polymers or oligomers having a carbamate structure and a urea structure in its molecule).
[0134] Hitherto known ultraviolet absorbers can be used as the ultraviolet absorber, and examples thereof may include ultraviolet absorbers such as benzotriazole-based absorbers, triazine-based absorbers, salicylic acid derivative-based absorbers, and benzophenone-based absorbers. These absorbers may be used alone or in combination.
[0135] When the coating composition of the present invention contains an ultraviolet absorber, the blending amount of the ultraviolet absorber relative to the total amount of solid content in the coating composition preferably falls within the range of 0.1 mass % to 10 mass %, more preferably falls within the range of 0.2 mass % to 8 mass %, particularly preferably falls within the range of 0.3 mass % to 6 mass %.
[0136] A hitherto known light stabilizer may be used as the light stabilizer, and may be, for example, a hindered amine-based light stabilizer.
[0137] From the viewpoint of pot life, a hindered amine-based light stabilizer having low basicity can be suitably used as the hindered amine-based light stabilizer. Examples of such hindered amine-based light stabilizers may include acylated hindered amines and aminoether-based hindered amines, and specific examples thereof may include "HOSTAVIN 3058" (product name, manufactured by Clariant AG), "TINUVIN 123" (product name, manufactured by BASF SE), and "HALS292" (product name, manufactured by BASF SE).
[0138] There is no particular limitation on the coating method of the coating composition of the present invention, and examples thereof include coating methods such as air spraying, airless spraying, rotary atomization coating and curtain coating. Each of these methods can form a wet coating film. In each of these coating methods, electrostatic application can be optionally performed. Among them, air spraying or rotary atomization coating is particularly preferred. The coating amount of the coating is preferably set to an amount such that its cured thickness is 5 μm to 50 μm, and the amount is particularly preferably set to an amount such that the cured thickness is 10 μm to 40 μm.
[0139] In addition, when each of air spraying, airless spraying and rotary atomization spraying is performed, it is preferred to appropriately adjust the viscosity of the coating with a solvent such as an organic solvent and a thickener within a viscosity range suitable for coating, and the viscosity range is generally 5 seconds to 20 seconds, particularly 8 seconds to 15 seconds at 20° C. in an ANESTIWATA viscosity cup NK2.
[0140] Coating film forming method
[0141] The coating composition of the present invention can be suitably used in a coating film forming method comprising: coating the top of an object to be coated with the coating composition of the present invention to form a coating film; and then heating the coating film to cure the coating film.
[0142] The coating composition of the present invention can be used in various industrial applications. The composition can be suitably used as a coating composition for automobile outer panels or parts, and can be particularly suitably used as a clear coat coating composition.
[0143] Preferred aspects of the above-mentioned coating film forming method may include the following methods (A) to (D).
[0144] Method (A)
[0145] A coating film forming method comprising:
[0146] Step (A1): a step of coating the top of an object with the coating composition of the present invention to form a clear coating film; and
[0147] Step (A2): a step of heating the clear coating film formed in step (A1) to cure the film.
[0148] Method (B)
[0149] A coating film forming method comprising:
[0150] Step (B1): a step of coating the top of the object with the base coating composition to form a base coating film;
[0151] Step (B2): a step of coating the top of the base coating film with the coating composition of the present invention to form a clear coating film; and
[0152] Step (B3): a step of heating the base coating film formed in step (B1) and the clear coating film formed in step (B2) separately or simultaneously to cure the coating films.
[0153] Method (C)
[0154] A coating film forming method comprising:
[0155] Step (C1): a step of coating the top of the object with a first base coating composition to form a first base coating film;
[0156] Step (C2): a step of coating the top of the first base coating film with a second base coating composition to form a second base coating film;
[0157] Step (C3): a step of coating the top of the second base coating film with the coating composition of the present invention to form a clear coating film; and
[0158] Step (C4): a step of separately or simultaneously heating the first base coating film formed in step (C1), the second base coating film formed in step (C2), and the clear coating film formed in step (C3) to cure the coating films.
[0159] Method (D)
[0160] A coating film forming method comprising:
[0161] Step (D1): a step of coating the top of the object with a primer coating composition to form a primer coating film;
[0162] Step (D2): a step of coating the top of the primer coating film with a first base coating composition to form a first base coating film;
[0163] Step (D3): a step of coating the top of the first base coating film with a second base coating composition to form a second base coating film;
[0164] Step (D4): a step of coating the top of the second base coating film with the coating composition of the present invention to form a clear coating film; and
[0165] Step (D5): A step of separately or simultaneously heating the primer coating film formed in step (D1), the first base coating film formed in step (D2), the second base coating film formed in step (D3) and the clear coating film formed in step (D4) to cure the coating films.
[0166] The above-mentioned coated object is not particularly limited, and examples thereof may include: outer panel portions of automobile bodies for passenger cars, trucks, motorcycles, buses, etc.; automobile parts; and outer panel portions of household appliances such as mobile phones or audio equipment. Among them, outer panel portions of automobile bodies and automobile parts are preferred.
[0167] The material of the coated object is not particularly limited. Examples thereof may include: metal materials such as iron, aluminum, brass, copper, tin-plated iron, stainless steel, galvanized steel, and steel plated with zinc alloys (e.g., Zn-Al, Zn-Ni, or Zn-Fe); resins such as polyethylene resins, polypropylene resins, acrylonitrile-butadiene-styrene (ABS) resins, polyamide resins, acrylic resins, vinylidene chloride resins, polycarbonate resins, polyurethane resins, and epoxy resins; plastic materials such as various FRPs; inorganic materials such as glass, cement, and concrete; wood; and fiber materials such as paper and cloth. Among them, metal materials and plastic materials are preferred.
[0168] In addition, the surface of the object to which the coating film is applied may be a surface obtained by subjecting the metal surface of, for example, a metal substrate (for example, a metal substrate of a steel sheet used to form each of the outer panel portion and the inner panel portion of an automobile body, automobile parts, and household appliances) to a surface treatment such as a phosphate treatment, a chromate treatment, or a composite oxide treatment.
[0169] A coating film may be further formed on the object which has been subjected to or has not been subjected to the surface treatment. For example, the following steps may be performed: the object to be coated serving as a substrate is optionally subjected to the surface treatment, and an undercoating film is formed thereon. For example, when the object to be coated is an automobile body, the undercoating film may be formed by using a coating material for undercoating which is known per se and is generally used for automobile body painting.
[0170] For example, an electrodeposition paint, preferably a cationic electrodeposition paint, can be used as an undercoat paint for forming the undercoat coating film.
[0171] The product obtained by converting the following materials into a coating together with a pigment, a thickener and any other optional ingredients: a base resin such as a polyolefin resin, an acrylic resin having a crosslinkable functional group (such as a carboxyl group or a hydroxyl group), a polyester resin, an alkyd resin, a urethane resin and an epoxy resin; and a crosslinking agent such as an amino resin (such as a melamine resin urea resin), or a polyisocyanate compound that may be blocked can be used as the above-mentioned primer coating composition.
[0172] A product obtained by converting the following materials into a coating together with a pigment, a thickener and any other optional ingredients can be used as each of the above-mentioned first base coating composition and second base coating composition: a base resin such as an acrylic resin, a polyester resin, an alkyd resin, a urethane resin, or an epoxy resin having a crosslinkable functional group (such as a carboxyl group or a hydroxyl group); and a crosslinking agent such as an amino resin (such as a melamine resin or a urea resin), or a polyisocyanate compound that can be blocked.
[0173] Heating can be performed by known means, and a drying furnace such as a hot air furnace, an electric furnace or an infrared induction heating furnace can be applied. The heating temperature falls within the range of 50° C. to 110° C., preferably 60° C. to 90° C. Although the heating time is not particularly limited, the time falls within the range of preferably 5 minutes to 40 minutes, more preferably 10 minutes to 35 minutes.
[0174] Example
[0175] The present invention is described in more detail below by way of Examples and Comparative Examples. However, the present invention is not limited to these Examples. The terms "parts" and "%" mean "parts by mass" and "% by mass", respectively.
[0176] Production of hydroxyl-containing acrylic resin (A1)
[0177] Production Example 1
[0178] 27 parts of "SWASOL 1000" (product name, manufactured by Maruzen Petrochemical Co., Ltd., aromatic organic solvent) and 5 parts of propylene glycol monomethyl ether acetate were charged into a reaction vessel including a thermometer, a thermostat, a stirring device, a reflux condenser, a nitrogen inlet tube and a dripping device. While nitrogen was blown into the reaction vessel, the loaded liquid was stirred at 150°C, and a monomer mixture formed by 20 parts of styrene, 24.8 parts of isobutyl methacrylate, 24 parts of ethyl acrylate, 30 parts of 2-hydroxyethyl methacrylate, 1.2 parts of acrylic acid and 4.5 parts of di-tert-amyl peroxide (polymerization initiator) was added dropwise thereto at a constant rate over 4 hours. Thereafter, the mixture was aged at 150°C for 1 hour and then cooled. In addition, 21 parts of isobutyl acetate were added to dilute the cooled product. Thus, a solution of a primary hydroxyl-containing acrylic resin (A11-1) having a solid content concentration of 65% by mass was obtained. The obtained primary hydroxyl-containing acrylic resin (A11-1) had an acid ester of 9.3 mgKOH / g, a hydroxyl value of 129 mgKOH / g, a weight average molecular weight of 6,000, and a glass transition temperature of 39°C.
[0179] Production of an organic metal catalyst (C) composed of a zinc compound and an amidine compound
[0180] Production Example 2
[0181] 47 parts of ethyl 3-ethoxypropionate and 81.6 parts of "NIKKA OCTHIX ZINC" (product name, zinc octoate, manufactured by Nihon Kagaku Sangyo Co., Ltd., zinc content: 8% by mass) were charged into a reaction vessel comprising a stirrer, a condenser, a temperature controller, a nitrogen inlet tube and a dropping funnel. The interior of the reaction vessel was purged with nitrogen and heated to 50°C. Subsequently, 16.4 parts of 1-methylimidazole were dropped into the mixture under stirring, and after the dropwise addition was completed, the reaction was maintained at a temperature of 50°C for 2 hours to complete the reaction. The resulting organometallic catalyst (C-1) formed from the zinc compound and the amidine compound was a liquid having a zinc content of 4.5% by mass.
[0182] Preparation Examples 3 to 10
[0183] Organometallic catalysts (C-2) to (C-9) each formed of a zinc compound and an amidine compound were each obtained in the same manner as in Production Example 2 except that the mixed composition in Production Example 2 was set to the composition shown in Table 1.
[0184] Table 1
[0185]
[0186]
[0187] "Zinc naphthenate" (Note 1): Zinc content: 10.1%, manufactured by Tokyo Chemical Industry Co., Ltd.
[0188] "Zinc acetylacetonate" (Note 2): Zinc content: 25%, manufactured by Showa Chemical Co., Ltd.
[0189] DBN (Note 3): 1,5-diazabicyclo[4.3.0]non-5-ene, and
[0190] DBU (Note 4): 1,8-diazabicyclo[5.4.0]undec-7-ene.
[0191] Manufacture of other organometallic catalysts (E)
[0192] Production Example 11
[0193] 364 parts of ethyl 3-ethoxypropionate and 83.6 parts of "K-KAT 348" (product name, bismuth octoate, bismuth content: 25%, manufactured by King Industries, Inc.) were loaded into a reaction vessel comprising a stirrer, a condenser, a temperature controller, a nitrogen inlet tube and a dropping funnel. The interior of the reaction vessel was purged with nitrogen and heated to 50°C. Subsequently, 16.4 parts of 1-methylimidazole were dropped into the mixture under stirring, and after the dropwise addition was completed, the reaction was maintained at a temperature of 50°C for 2 hours to complete the reaction. The resulting other organometallic catalyst (E-1) was a liquid having a bismuth content of 4.5% by mass.
[0194] Preparation Example 12 and Preparation Example 13
[0195] Other organometallic catalysts (E-2) and (E-3) were each obtained in the same manner as in Production Example 11, except that the mixed composition was set to the composition shown in Table 2 in Production Example 11.
[0196] Table 2
[0197]
[0198] "NIKKAOCTHIX COBALT" (Note 5): product name, cobalt octoate, cobalt content: 8%, manufactured by Nippon Chemical Industry Co., Ltd., and
[0199] "NIKKAOCTHIX MANGANESE" (Note 6): Product name, manganese octoate, manganese content: 8%, manufactured by Nippon Chemical Industry Co., Ltd.
[0200] Production of resin containing phosphate groups (D2)
[0201] Production Example 14
[0202] A mixed solvent containing 27.5 parts of methoxypropanol and 27.5 parts of isobutyl alcohol was charged into a reaction vessel comprising a thermometer, a thermostat, a stirrer, a reflux condenser and a dripping device, and heated to 110°C. Subsequently, 121.5 parts of a mixture formed by 25 parts of styrene, 27.5 parts of n-butyl methacrylate, 20 parts of "isostearyl acrylate" (product name, manufactured by Osaka Organic Chemical Industry Ltd., branched acrylic acid higher alkyl ester), 7.5 parts of 4-hydroxybutyl acrylate, 15 parts of the following polymerizable monomers containing phosphate groups, 12.5 parts of 2-methacryloyloxyethyl acid phosphate, 10 parts of isobutyl alcohol and 4 parts of tert-butyl peroxyoctanoate were added to the above-mentioned mixed solvent within 4 hours. In addition, a mixture formed by 0.5 parts of tert-butyl peroxyoctanoate and 20 parts of isopropyl alcohol was added to the resulting mixture for 1 hour. After that, the resulting mixture was stirred and aged for 1 hour to provide a phosphate group-containing acrylic resin solution (D21-1) having a solid content concentration of 50%. The resin had an acid value of phosphate group of 83 mgKOH / g, a hydroxyl value of 29 mgKOH / g, and a weight average molecular weight of 10,000.
[0203] Polymerizable monomer containing phosphate group: 57.5 parts of monobutyl phosphoric acid and 41 parts of isobutyl alcohol were charged into a reaction vessel including a thermometer, a thermostat, a stirrer, a reflux condenser and a dripping device, and the temperature of the mixture was increased to 90°C. Thereafter, 42.5 parts of glycidyl methacrylate were added dropwise to the mixture over 2 hours, and then the whole was further stirred and aged for 1 hour. Thereafter, 59 parts of isopropanol were added to the aged product to provide a solution of a polymerizable monomer containing a phosphate group having a solid content concentration of 50%. The acid value of the phosphate group of the obtained monomer was 285 mgKOH / g.
[0204] Production of coating compositions
[0205] Examples 1 to 11 and Comparative Examples 1 to 6
[0206] The hydroxyl-containing acrylic resin obtained in the above-mentioned Preparation Example 1, the organometallic catalyst formed of a zinc compound and an amidine compound obtained in the above-mentioned Preparation Examples 2 to 10, the other organometallic catalysts obtained in the above-mentioned Preparation Examples 11 to 13, the phosphate group-containing resin obtained in the above-mentioned Preparation Example 14, and the raw materials shown in Table 3 shown later were used, and these materials were stirred and mixed with a blade stirrer according to the recipe shown in Table 3 shown later. In addition, butyl acetate was added to the mixture to adjust its viscosity measured at 20° C. with an ANEST IWATA viscosity cup NK2 to 11 seconds. Thus, coating compositions No. 1 to No. 17 were obtained. The recipe of each of the coating compositions shown in Table 3 is the solid content mass ratio between the corresponding components.
[0207] Table 3
[0208]
[0209]
[0210]
[0211] Table 3 (Continued-1)
[0212]
[0213]
[0214] Table 3 (Continued-2)
[0215]
[0216]
[0217] (Note 7) "SUMIDUR N3300": product name, manufactured by Sumika Covestro Urethane Co., Ltd., isocyanurate form of hexamethylene diisocyanate, solid content: 100%, and
[0218] (Note 8) "NACURE 4054J": product name, manufactured by King Industries, Inc., 2-ethylhexyl phosphate.
[0219] Applicable period
[0220] The pot life of each of coating compositions No. 1 to No. 17 was evaluated by measuring the viscosity of coating compositions No. 1 to No. 17 at 20° C. after standing at 20° C. for 6 hours using an ANEST IWATA viscosity cup NK2. The measurement results are summarized in Table 3. The viscosity after 6 hours of 13 seconds or less was considered acceptable.
[0221] Fabrication of test panels
[0222] A tinplate was air-sprayed with each of coating compositions No. 1 to No. 17 so that its cured thickness became about 30 μm. The plate was heated at 80° C. for 30 minutes to cure the composition, and then allowed to stand in a thermostatic chamber at 20° C. for 24 hours. Thus, a corresponding test plate was obtained.
[0223] NCO reaction ratio (%)
[0224] The NCO reaction ratio was evaluated as follows: the isocyanate peak intensity immediately after the coating was prepared was measured by the liquid film method using an FT-IR apparatus "FT / IR-420" (manufactured by JASCO Corporation); and the isocyanate peak intensity on the surface of the test plate was measured by the ATR method. The corresponding isocyanate peak intensity (2,271 cm -1 ), and the NCO reaction ratio (%) was determined by calculating the ratio between these intensities by the following equation. An NCO reaction ratio (%) of 80% or more was considered acceptable. The measurement results are summarized in Table 3.
[0225] NCO reaction ratio (%) = 100 - NCO remaining ratio (%)
[0226] NCO residual ratio (%) = (isocyanate peak intensity of the test plate) / (isocyanate peak intensity immediately after the coating is prepared) × 100
[0227] Knoop hardness
[0228] The Knoop hardness of the coating was measured with TUKON (manufactured by American Chain & Cable Company, Inc., a microhardness tester). Knoop hardness indicates the hardness of the coating read by the size of the diamond indentation produced by pressing a quadrangular pyramid diamond indenter into the test surface of the material under a constant test load. A larger value means a higher hardness. A Knoop hardness of 10 or more is considered acceptable. The measurement results are summarized in Table 3.
[0229] The embodiments and examples of the present invention have been specifically described above. However, the present invention is not limited to the above-described embodiments, and various modifications based on the technical idea of the present invention are possible.
[0230] For example, the configurations, methods, steps, shapes, materials, numerical values, etc. listed in the above-mentioned embodiments and examples are merely examples, and configurations, methods, steps, shapes, materials, numerical values, etc. different therefrom may be optionally used.
Claims
1. A coating composition comprising: (A) a hydroxyl-containing resin; (B) a polyisocyanate compound; (C) an organometallic catalyst formed from a zinc compound and an amidine compound; and (D) Compounds containing a phosphate group. 2 . The coating composition according to claim 1 , wherein the hydroxyl-containing resin (A) contains a hydroxyl-containing acrylic resin (A1). 3 . The coating composition according to claim 2 , wherein the hydroxyl-containing acrylic resin (A1) contains a primary hydroxyl-containing acrylic resin (A11). 4 . The coating composition according to claim 1 , wherein the phosphate group-containing compound (D) contains an alkyl phosphate (D1) and / or a phosphate group-containing resin (D2).
5. A coating film forming method comprising: Applying the coating composition according to any one of claims 1 to 4 to the top of the object to be coated to form a coating film; as well as The coating film is then heated to cure the coating film.
Citation Information
Patent Citations
Method for forming coating film and coated article
CN103842095A
Polyurethane coating agent compositions, multi-stage coating methods
CN104487473A
Polyisocyanate composition, paint composition and coating
JP2016037539A
Coating composition
WO2015087920A1