Display system, display method, display body, and method for manufacturing display body
By optimizing the light path configuration and optical characteristics of the display system, and using display elements, reflective polarizing components and λ/4 components, the problem of lightweight and high definition of the VR goggles display system is solved, and efficient image display and visual effects are achieved. .
Patent Information
- Application Number
- CN202380025226.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-28
- Filing Date
- 2023-03-08
- Publication Date
- 2024-10-22
AI Technical Summary
The display system of existing VR goggles is difficult to achieve lightweight and high definition, and the thickness and phase difference characteristics of the optical components cannot meet the needs of efficient display.
A display system consisting of a display element, a reflective polarizing component, a half-reflecting mirror, and first and second λ/4 components is used to optimize the optical path configuration and optical characteristics to ensure that the polarization direction and phase difference of light meet specific conditions to achieve image efficient display.
It achieves lightweight and high-definition display of VR goggles, reduces light leakage and ghosting, and improves visual effects.
Smart Images

Figure CN118829933A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a display system, a display method, a display body, and a method for manufacturing the display body. Background Art
[0002] Image display devices, typified by liquid crystal displays and electroluminescent (EL) displays (e.g., organic EL displays), are rapidly gaining popularity. To achieve image display and improve image display performance, these devices typically use optical components such as polarizers and phase shifters (e.g., see Patent Document 1).
[0003] In recent years, new applications for image display devices have been developed. For example, goggles with displays (VR goggles) for implementing Virtual Reality (VR) have begun to be commercialized. The use of VR goggles in various applications is under review, leading to demands for lightweighting and higher resolution. Lightweighting can be achieved, for example, by thinning the lenses used in VR goggles. Furthermore, there is also a desire to develop optical components suitable for display systems using thin lenses.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: (Japanese) Patent Application Publication No. 2021-103286 Summary of the Invention
[0007] Technical problem to be solved by the invention
[0008] In view of the above, the main object of the present invention is to provide a display system that can achieve lightweight and high-definition VR goggles.
[0009] Technical solutions to technical problems
[0010] 1. A display system according to an embodiment of the present invention displays an image to a user, comprising: a display element having a display surface that emits light displaying the image forward via a polarizing element; a reflecting portion disposed in front of the display element and including a reflective polarizing element, the reflecting portion reflecting light emitted from the display element; a first lens portion disposed in an optical path between the display element and the reflecting portion; a half mirror disposed between the display element and the first lens portion, the half mirror transmitting light emitted from the display element and reflecting light reflected by the reflecting portion toward the reflecting portion; a first λ / 4 element disposed in an optical path between the display element and the half mirror; and a second λ / 4 element disposed in an optical path between the half mirror and the reflecting portion; wherein the absolute value of the difference between the in-plane phase difference (a) of the first λ / 4 element and the in-plane phase difference (b) of the second λ / 4 element is 3.5 nm or less.
[0011] 2. In the display system of 1 above, the in-plane phase difference (a) of the first λ / 4 element and the in-plane phase difference (b) of the second λ / 4 element may also satisfy the following formula (I):
[0012] ((a)-(b)) / ((a)+(b) / 2)≤0.02···(I).
[0013] 3. In the display system according to 1 or 2 above, the ISC values of the first λ / 4 member and the second λ / 4 member may each be 50 or less.
[0014] 4. In the display system according to any one of 1 to 3 above, each of the first λ / 4 member and the second λ / 4 member may have a thickness of 100 μm or less.
[0015] 5. In the display system according to any one of 1 to 4 above, each of the first λ / 4 member and the second λ / 4 member may have a thickness deviation of 1 μm or less.
[0016] 6. In the display system according to any one of 1 to 5 above, the ISC value per unit thickness of the first λ / 4 member and the second λ / 4 member may each be 1 or less.
[0017] 7. In the display system according to any one of 1 to 6 above, the polarization direction of the light emitted through the polarizing element and the reflection axis of the reflective polarizing element may be substantially orthogonal to each other.
[0018] 8. In the display system of any one of items 1 to 7 above, the angle formed by the absorption axis of the polarizing component contained in the above display element and the slow axis of the above first λ / 4 component may also be 40° to 50°, and the angle formed by the absorption axis of the polarizing component contained in the above display element and the slow axis of the above second λ / 4 component may also be 40° to 50°.
[0019] 9. A display according to an embodiment of the present invention includes the display system according to any one of 1 to 8 above.
[0020] 10. A method for manufacturing a display according to an embodiment of the present invention is a method for manufacturing a display including the display system according to any one of 1 to 8 above.
[0021] 11. The display method of an embodiment of the present invention has the following steps: a step of passing light of a display image emitted through a polarizing component through a first λ / 4 component; a step of passing the light passing through the above-mentioned first λ / 4 component through a half-reflecting mirror and a first lens portion; a step of passing the light passing through the above-mentioned half-reflecting mirror and the above-mentioned first lens portion through a second λ / 4 component; a step of causing the light passing through the above-mentioned second λ / 4 component to be reflected toward the above-mentioned half-reflecting mirror at a reflecting portion including a reflective polarizing component; and a step of allowing the light reflected by the above-mentioned reflecting portion and the above-mentioned half-reflecting mirror to pass through the above-mentioned reflecting portion through the above-mentioned second λ / 4 component; and the absolute value of the difference between the in-plane phase difference (a) of the above-mentioned first λ / 4 component and the in-plane phase difference (b) of the above-mentioned second λ / 4 component is less than 3.5nm.
[0022] Effects of the Invention
[0023] According to the display system of the embodiment of the present invention, VR goggles can be made lighter and more precise. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention.
[0025] Figure 2 In the example, (a) indicates Figure 1 (b) is a schematic diagram illustrating an example of light flow in the display system shown; Figure 1 Schematic diagram of an example of changes in the polarization state of light in the display system shown.
[0026] Figure 3 This is a diagram for explaining the method of measuring thickness deviation.
[0027] Figure 4 This is a diagram for explaining the method of measuring the ISC value. DETAILED DESCRIPTION
[0028] The following describes embodiments of the present invention with reference to the accompanying drawings, but the present invention is not limited to these embodiments. To clarify the drawings, the widths, thicknesses, shapes, and other aspects of various components may be schematically illustrated compared to the embodiments. However, these are merely examples and are not intended to limit the present invention. Furthermore, in the drawings, identical or equivalent elements may be designated by the same reference numerals, and repeated descriptions may be omitted.
[0029] (Definition of Terms and Symbols)
[0030] The definitions of terms and symbols in this specification are as follows.
[0031] (1) Refractive index (nx, ny, nz)
[0032] "nx" is the refractive index in the direction where the in-plane refractive index reaches a maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), and "nz" is the refractive index in the thickness direction.
[0033] (2) In-plane retardation (Re)
[0034] "Re(λ)" is the in-plane retardation measured at 23°C using light of a wavelength of λ nm. For example, "Re(550)" is the in-plane retardation measured at 23°C using light of a wavelength of 550 nm. Re(λ) is calculated using the formula: Re(λ) = (nx - ny) × d, assuming a layer (thin film) thickness of d (nm).
[0035] (3) Retardation in the thickness direction (Rth)
[0036] "Rth(λ)" is the retardation in the thickness direction measured at 23°C using light of a wavelength of λ nm. For example, "Rth(550)" is the retardation in the thickness direction measured at 23°C using light of a wavelength of 550 nm. For a layer (film) thickness of d (nm), Rth(λ) is calculated using the formula: Rth(λ) = (nx - nz) × d.
[0037] (4) Nz coefficient
[0038] The Nz coefficient is obtained by Nz=Rth / Re.
[0039] (5) Angle
[0040] When referring to angles in this specification, unless otherwise specified, the angles include both clockwise and counterclockwise directions relative to a reference direction. Thus, for example, "45°" means ±45°. Furthermore, in this specification, "substantially parallel" includes a range of 0°±10°, preferably 0°±5°, more preferably 0°±3°, and even more preferably 0°±1°. "Substantially orthogonal" includes a range of 90°±10°, preferably 90°±5°, more preferably 90°±3°, and even more preferably 90°±1°.
[0041] Figure 1 This is a schematic diagram showing a schematic configuration of a display system according to one embodiment of the present invention. Figure 1 The schematic diagram illustrates the arrangement and shape of the components of the display system 2. The display system 2 includes a display element 12, a reflective unit 14 including a reflective polarizing element, a first lens unit 16, a half mirror 18, a first phase difference element 20, a second phase difference element 22, and a second lens unit 24. The reflective unit 14 is disposed on the display surface 12a side of the display element 12, i.e., in front of the display surface 12a, and reflects light emitted from the display element 12. The first lens unit 16 is disposed in the optical path between the display element 12 and the reflective unit 14, and the half mirror 18 is disposed between the display element 12 and the first lens unit 16. The first phase difference element 20 is disposed in the optical path between the display element 12 and the half mirror 18, and the second phase difference element 22 is disposed in the optical path between the half mirror 18 and the reflective unit 14.
[0042] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying images. Light emitted from the display surface 12a passes through a polarizing member (typically a polarizing film) that the display element 12 may include, and then is emitted as first linearly polarized light.
[0043] The first phase difference member 20 is a λ / 4 member that converts the first linearly polarized light incident on the first phase difference member 20 into the first circularly polarized light (hereinafter, the first phase difference member may be referred to as the first λ / 4 member). Alternatively, the first phase difference member 20 may be integrally provided on the display element 12.
[0044] The half mirror 18 transmits light emitted from the display element 12 and reflects light reflected by the reflection portion 14 toward the reflection portion 14. The half mirror 18 is integrally provided on the first lens portion 16.
[0045] The second phase difference member 22 is a λ / 4 member that allows light reflected by the reflector 14 and the half mirror 18 to pass through the reflector 14 including the reflective polarizing member (hereinafter, the second phase difference member may be referred to as the second λ / 4 member). Alternatively, the second phase difference member 22 may be integrally provided on the first lens portion 16.
[0046] The first circularly polarized light emitted from the first λ / 4 element 20 passes through the half mirror 18 and the first lens unit 16, and is converted into second linearly polarized light by the second λ / 4 element 22. The second linearly polarized light emitted from the second λ / 4 element 22 does not pass through the reflective polarizing element included in the reflecting section 14 and is reflected toward the half mirror 18. At this time, the polarization direction of the second linearly polarized light entering the reflective polarizing element included in the reflecting section 14 is aligned with the reflection axis of the reflective polarizing element. Therefore, the second linearly polarized light entering the reflecting section 14 is reflected by the reflective polarizing element.
[0047] The second linearly polarized light reflected by the reflective portion 14 is converted into second circularly polarized light by the second λ / 4 element 22. The second circularly polarized light emitted from the second λ / 4 element 22 passes through the first lens portion 16 and is reflected by the half mirror 18. The circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into third linearly polarized light by the second λ / 4 element 22. The third linearly polarized light passes through the reflective polarizing element included in the reflective portion 14. At this time, the polarization direction of the third linearly polarized light entering the reflective polarizing element included in the reflective portion 14 is aligned with the transmission axis of the reflective polarizing element. Therefore, the third linearly polarized light entering the reflective polarizing element 14 passes through the reflective polarizing element.
[0048] The light transmitted through the reflective portion 14 passes through the second lens portion 24 and enters the user's eye 26 .
[0049] For example, the absorption axis of the polarizing element included in the display element 12 and the reflection axis of the reflective polarizing element included in the reflective portion 14 can be arranged to be substantially parallel to each other or substantially orthogonal to each other. The angle formed by the absorption axis of the polarizing element included in the display element 12 and the slow axis of the first phase difference element 20 is, for example, 40° to 50°, 42° to 48°, or approximately 45°. The angle formed by the absorption axis of the polarizing element included in the display element 12 and the slow axis of the second phase difference element 22 is, for example, 40° to 50°, 42° to 48°, or approximately 45°.
[0050] The in-plane retardation Re(550) of the first phase difference member 20 may be, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm.
[0051] The first phase difference member 20 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The Re(450) / Re(550) ratio of the first phase difference member 20 is, for example, less than 1, and may be 0.95 or less, further less than 0.90, and further may be 0.85 or less. The Re(450) / Re(550) ratio of the first phase difference member 20 is, for example, 0.75 or greater.
[0052] In one embodiment, the first phase difference member 20 satisfies all of Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. The first phase difference member 20 preferably satisfies at least one selected from the following, more preferably satisfies at least two, and more preferably satisfies all: 0.65<Re(400) / Re(550)<0.80 (preferably 0.7<Re(400) / Re(550)<0.75), 1.0<Re(650) / Re(550)<1.25 (preferably 1.05<Re(650) / Re(550)<1.20), and 1.05<Re(750) / Re(550)<1.40 (preferably 1.08<Re(750) / Re(550)<1.36).
[0053] The first phase difference member 20 preferably exhibits a refractive index characteristic exhibiting the relationship nx>ny≥nz. Here, "ny=nz" encompasses not only the case where ny and nz are identical but also the case where they are substantially identical. Therefore, a situation where ny<nz is acceptable without impairing the effects of the present invention is permitted. The Nz coefficient of the first phase difference member 20 is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0054] The ISC value of the first phase difference member 20 is, for example, 50 or less, preferably 40 or less, more preferably 30 or less, and more preferably 20 or less. By satisfying the ISC value of the first phase difference member 20, a display system with excellent visual recognition can be achieved. For example, by satisfying the ISC value, the uniformity of the in-plane phase difference can be improved, and as a result, light leakage in the reflective portion described later can be suppressed. The ISC value can serve as an indicator of smoothness or unevenness.
[0055] The thickness deviation of the first phase difference member 20 is preferably 1 μm or less, more preferably 0.8 μm or less, more preferably 0.6 μm or less, and more preferably 0.4 μm or less. According to the thickness deviation, for example, the above-mentioned ISC value can be well achieved. Here, the thickness deviation can be calculated by measuring the thickness of the first portion located in the surface of the phase difference member and the thickness of the position from the first portion to any direction (for example, up, down, left and right) through a predetermined interval (for example, 5 mm to 15 mm).
[0056] The ISC value per unit thickness of the first phase difference member 20 is preferably 1 or less, more preferably 0.7 or less, and further preferably 0.5 or less. The ISC value per unit thickness can be calculated by, for example, dividing the thickness (unit: μm) by the ISC value.
[0057] The first phase difference member 20 is formed of any appropriate material that can meet the above characteristics. The first phase difference member 20 can be, for example, a stretched film of a resin film or a directional solidified layer of a liquid crystal compound. In addition, a stretched film of a resin film is sometimes referred to as a phase difference film.
[0058] The resin contained in the above-mentioned resin film can be listed as follows: polycarbonate resin, polyester carbonate resin, polyester resin, polyvinyl acetal resin, polyarylate resin, cyclic olefin resin, cellulose resin, polyvinyl alcohol resin, polyamide resin, polyimide resin, polyether resin, polystyrene resin, acrylic resin, etc. These resins can be used alone or in combination (for example, blending, copolymerization). When the first phase difference member 20 exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate resin or a polyester carbonate resin (hereinafter sometimes referred to as simply a polycarbonate resin) can be preferably used.
[0059] Any appropriate polycarbonate resin can be used as long as the effects of the present invention are achieved. For example, the polycarbonate resin comprises: a structural unit derived from a fluorene-based dihydroxy compound; a structural unit derived from an isosorbide-based dihydroxy compound; and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanols, di-, tri-, or polyethylene glycols, and alkylene glycols or spiroglycerol. The polycarbonate resin preferably comprises: a structural unit derived from a fluorene-based dihydroxy compound; a structural unit derived from an isosorbide-based dihydroxy compound; a structural unit derived from an alicyclic dimethanol; and / or a structural unit derived from di-, tri-, or polyethylene glycol; more preferably comprises: a structural unit derived from a fluorene-based dihydroxy compound; a structural unit derived from an isosorbide-based dihydroxy compound; and a structural unit derived from di-, tri-, or polyethylene glycol. The polycarbonate resin may also contain structural units derived from other dihydroxy compounds as needed. In addition, the details of the polycarbonate resin that can be preferably used for the first phase difference component and the method for forming the first phase difference component are recorded in, for example, (Japan) Patent Gazette No. 2014-10291, (Japan) Patent Gazette No. 2014-26266, (Japan) Patent Gazette No. 2015-212816, (Japan) Patent Gazette No. 2015-212817, and (Japan) Patent Gazette No. 2015-212818, and this specification cites the records of these gazettes as reference.
[0060] The oriented solidified layer of the liquid crystal compound is a layer in which the liquid crystal compound is oriented in a predetermined direction within the layer and its oriented state is fixed. In addition, the concept of "oriented solidified layer" includes an oriented hardened layer obtained by hardening the liquid crystal monomer as described later. For the first phase difference component, it represents that the upper rod-shaped liquid crystal compound is oriented (oriented along the surface) in a state where it is arranged in the slow axis direction of the first phase difference component. Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the liquid crystal compound can be polymerized after orientation, thereby fixing the oriented state of the liquid crystal compound.
[0061] The above-mentioned oriented solidified layer of liquid crystal compound (liquid crystal oriented solidified layer) can be formed by the following method: applying an orientation treatment to the surface of a predetermined substrate, and applying a coating liquid containing a liquid crystal compound to the surface, so that the liquid crystal compound is oriented in the direction corresponding to the above-mentioned orientation treatment, and fixing the orientation state. The orientation treatment can adopt any appropriate orientation treatment. Specifically, mechanical orientation treatment, physical orientation treatment, and chemical orientation treatment can be mentioned. Specific examples of mechanical orientation treatment include friction treatment and stretching treatment. Specific examples of physical orientation treatment include magnetic field orientation treatment and electric field orientation treatment. Specific examples of chemical orientation treatment include oblique evaporation method and light orientation treatment. The processing conditions of various orientation treatments can adopt any appropriate conditions according to the purpose.
[0062] The liquid crystal compound can be aligned by treating the liquid crystal compound at a temperature that allows it to exhibit a liquid crystal phase, depending on the type of the liquid crystal compound. The temperature treatment causes the liquid crystal compound to enter a liquid crystal state, and the liquid crystal compound is aligned in the direction of the alignment treatment on the substrate surface.
[0063] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound. When the liquid crystal compound is polymerizable or cross-linkable, the alignment state is fixed by subjecting the aligned liquid crystal compound to a polymerization treatment or a cross-linking treatment.
[0064] The above-mentioned liquid crystal compound can use any appropriate liquid crystal polymer and / or liquid crystal monomer. The liquid crystal polymer and liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for preparing liquid crystal directional solidification layers are described in, for example, Japanese Patent Application Publication No. 2006-163343, Japanese Patent Application Publication No. 2006-178389, and International Publication No. 2018 / 123551. This specification cites the records of these publications as reference.
[0065] The thickness of the first phase difference member 20 is preferably 100 μm or less. Specifically, the thickness of the first phase difference member 20 formed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, more preferably 10 μm to 60 μm, and even more preferably 20 μm to 50 μm. Furthermore, the thickness of the first phase difference member 20 formed of a liquid crystal oriented solidification layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and even more preferably 1 μm to 4 μm.
[0066] The in-plane retardation Re(550) of the second phase difference member 22 may be, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm.
[0067] The second phase difference member 22 preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The Re(450) / Re(550) ratio of the second phase difference member 22 is, for example, less than 1, and may be 0.95 or less, further less than 0.90, and further may be 0.85 or less. The Re(450) / Re(550) ratio of the second phase difference member 22 is, for example, 0.75 or greater.
[0068] In one embodiment, the second phase difference member 22 satisfies all of Re(400) / Re(550)<0.85, Re(650) / Re(550)>1.03, and Re(750) / Re(550)>1.05. The second phase difference member 22 preferably satisfies at least one selected from the following, more preferably satisfies at least two, and more preferably satisfies all: 0.65<Re(400) / Re(550)<0.80 (preferably 0.7<Re(400) / Re(550)<0.75), 1.0<Re(650) / Re(550)<1.25 (preferably 1.05<Re(650) / Re(550)<1.20), and 1.05<Re(750) / Re(550)<1.40 (preferably 1.08<Re(750) / Re(550)<1.36).
[0069] The second phase difference member 22 preferably exhibits a refractive index characteristic exhibiting the relationship nx>ny≥nz. "ny=nz" here encompasses not only situations where ny and nz are identical but also situations where they are substantially identical. Therefore, a situation where ny<nz is acceptable without impairing the effects of the present invention is permitted. The Nz coefficient of the second phase difference member 22 is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0070] The ISC value of the second phase difference member 22 is, for example, 50 or less, preferably 40 or less, more preferably 30 or less, and more preferably 20 or less. By satisfying the ISC value of the second phase difference member 22, a display system with excellent visual discernibility can be achieved. For example, by satisfying the ISC value, the uniformity of the in-plane phase difference can be improved, and as a result, light leakage in the reflective portion described later can be suppressed. The ISC value can serve as an indicator of smoothness or unevenness.
[0071] The thickness deviation of the second phase difference member 22 is preferably 1 μm or less, more preferably 0.8 μm or less, further preferably 0.6 μm or less, and further preferably 0.4 μm or less. With such thickness deviation, for example, the above-mentioned ISC value can be well achieved.
[0072] The ISC value per unit thickness of the second phase difference member 22 is preferably 1 or less, more preferably 0.7 or less, and further preferably 0.5 or less.
[0073] The second phase difference member 22 is formed of any appropriate material that can satisfy the above-mentioned characteristics. The second phase difference member 22 can be, for example, an extended film of a resin film or a directional solidified layer of a liquid crystal compound. Regarding the second phase difference member 22 composed of an extended film of a resin film or a directional solidified layer of a liquid crystal compound, the same description as the first phase difference member 20 can be applied. The first phase difference member 20 and the second phase difference member 22 can be members of the same composition (forming material, thickness, optical properties, etc.), or they can be members of different compositions.
[0074] The thickness of the second phase difference member 22 is preferably 100 μm or less. Specifically, the thickness of the second phase difference member 22 formed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, more preferably 10 μm to 60 μm, and even more preferably 20 μm to 50 μm. Furthermore, the thickness of the second phase difference member 22 formed of a liquid crystal oriented solidification layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and even more preferably 1 μm to 4 μm.
[0075] The absolute value of the difference between the in-plane phase difference (a) of the first phase difference member and the in-plane phase difference (b) of the second phase difference member is 3.5 nm or less, preferably 3.0 nm or less, more preferably 2.5 nm or less, more preferably 2.0 nm or less, particularly preferably 1.5 nm or less, and most preferably 1.0 nm or less. In one embodiment, (a) and (b) are values of Re(590).
[0076] The in-plane phase difference (a) of the first phase difference member and the in-plane phase difference (b) of the second phase difference member preferably satisfy the following formula (I):
[0077] ((a)-(b)) / ((a)+(b) / 2)≤0.02···(I).
[0078] More preferably, ((a)-(b)) / ((a)+(b) / 2)≤0.015,
[0079] More preferably, ((a)-(b)) / ((a)+(b) / 2)≤0.01.
[0080] In addition to the reflective polarizing element, the reflective portion 14 may also include an absorptive polarizing element. The absorptive polarizing element may be positioned in front of the reflective polarizing element. The reflection axis of the reflective polarizing element and the absorption axis of the absorptive polarizing element may be positioned substantially parallel to each other, and the transmission axis of the reflective polarizing element and the transmission axis of the absorptive polarizing element may be positioned substantially parallel to each other. When the reflective polarizing element 14 includes the absorptive polarizing element, the reflective polarizing element 14 may also include a laminated structure comprising the reflective polarizing element and the absorptive polarizing element.
[0081] The above-mentioned reflective polarizing member can transmit polarized light (typically linear polarized light) parallel to its transmission axis while maintaining its polarization state, and reflect light in other polarization states. The orthogonal transmittance (Tc) of the reflective polarizing member can be, for example, 0.01% to 3%. The single transmittance (Ts) of the reflective polarizing member can be, for example, 43% to 49%, preferably 45% to 47%. The polarization degree (P) of the reflective polarizing member can be, for example, 92% to 99.99%. The reflective polarizing member is typically composed of a film having a multilayer structure (sometimes referred to as a reflective polarizing film). Commercially available reflective polarizing films include, for example, the trade names "DBEF" and "APF" manufactured by 3M and the trade name "APCF" manufactured by Nitto Denko Corporation.
[0082] The absorption-type polarizing member may typically include a resin film containing a dichroic substance (sometimes referred to as an absorption-type polarizing film). The thickness of the absorption-type polarizing film may be, for example, 1 μm to 20 μm, 2 μm to 15 μm, 12 μm to 10 μm, 8 μm to 8 μm, or 5 μm to 5 μm.
[0083] The above-mentioned absorption-type polarizing film can be made of a single layer of resin film or a laminate of two or more layers.
[0084] When produced from a single-layer resin film, for example, an absorption-type polarizing film can be obtained by dyeing a hydrophilic polymer film such as a polyvinyl alcohol (PVA) film, a partially formalized PVA film, or a partially saponified ethylene-vinyl acetate copolymer film with a dichroic substance such as iodine or a dichroic dye, or by stretching the film. Among these, an absorption-type polarizing film obtained by dyeing a PVA film with iodine and then uniaxially stretching the film is preferred.
[0085] The iodine dyeing described above can be performed, for example, by immersing the PVA film in an aqueous iodine solution. The uniaxial stretching ratio is preferably 3 to 7 times. Stretching can be performed after dyeing or while dyeing is taking place. Furthermore, dyeing can be performed after stretching. The PVA film can be subjected to swelling treatment, crosslinking treatment, washing treatment, drying treatment, etc., as needed.
[0086] When the laminated body is produced using the above-mentioned two or more layers, the following laminated bodies can be cited: a laminated body of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate; or a laminated body of a resin substrate and a PVA-based resin layer formed by coating the resin substrate. The absorption-type polarizing film obtained by using the laminated body of the resin substrate and the PVA-based resin layer formed by coating the resin substrate can be produced, for example, by the following steps: applying a PVA-based resin solution to the resin substrate and drying it to form a PVA-based resin layer on the resin substrate to obtain a laminated body of the resin substrate and the PVA-based resin layer; and stretching and dyeing the laminated body to make the PVA-based resin layer into an absorption-type polarizing film. In this embodiment, it is preferred to form a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin on one side of the resin substrate. Stretching typically includes immersing the laminated body in a boric acid aqueous solution for stretching. Furthermore, as required, the stretching may further include stretching the laminate in the air at a high temperature (e.g., above 95°C) before stretching in a boric acid aqueous solution. Furthermore, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment, wherein the drying shrinkage treatment is to heat the laminate while conveying it in the longitudinal direction so that it shrinks by more than 2% in the width direction. Typically, the manufacturing method of this embodiment includes sequentially performing an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, the crystallinity of the PVA can be improved even when the PVA is coated on a thermoplastic resin, thereby achieving high optical properties. Furthermore, by simultaneously improving the orientation of the PVA in advance, problems such as a reduction in orientation or dissolution of the PVA can be prevented when the PVA is immersed in water in a subsequent dyeing step or stretching step, thereby achieving high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and reduction in orientation of the polyvinyl alcohol molecules can be further suppressed compared to the case where the PVA-based resin layer does not contain a halide. Thus, the optical properties of the absorption-type polarizing film obtained by immersing the laminate in a liquid through a dyeing process and an underwater stretching process can be improved. In addition, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage process. The obtained resin substrate / absorption-type polarizing film laminate can be used directly (that is, the resin substrate can be used as a protective layer for the absorption-type polarizing film), or it can be used by laminating any appropriate protective layer that meets the purpose on the peeling surface after peeling the resin substrate from the resin substrate / absorption-type polarizing film laminate, or on the surface opposite to the peeling surface. The details of the method for manufacturing the absorption-type polarizing film are described in, for example, (Japan) Patent Gazette No. 2012-73580 and (Japan) Patent No. 6470455. The entire contents of these gazettes are cited in this specification as a reference.
[0087] The cross transmittance (Tc) of the absorptive polarizing element (absorptive polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The single-element transmittance (Ts) of the absorptive polarizing element (absorptive polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or greater. The degree of polarization (P) of the absorptive polarizing element (absorptive polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or greater.
[0088] Figure 2 It is an explanation Figure 1 Schematic diagram of an example of the flow of light and the change in polarization state of light in the display system shown. Figure 2 (a) is a schematic diagram illustrating an example of the flow of light in the display system. Figure 2 (b) is a schematic diagram illustrating an example of changes in the polarization state of light caused by transmission through or reflection by each member in the display system. Figure 2 , the solid arrow attached to the display element 12 indicates the absorption axis direction of the polarizing member contained in the display element 12, the arrows attached to the first phase difference member 20 and the second phase difference member 22 indicate the slow axis direction, the solid arrow attached to the reflective polarizing member 14a contained in the reflector 14 indicates the reflection axis direction, and the dotted arrows indicate the transmission axis direction of each polarizing member. In the example shown in the figure, the first phase difference member 20 and the second phase difference member 22 are arranged so that their slow axes are approximately parallel to each other. The absorption axis of the polarizing member contained in the display element 12 and the reflection axis of the reflective polarizing member 14a contained in the reflector 14 are arranged so as to be approximately parallel to each other. In other words, the polarization direction of the light emitted through the polarizing member contained in the display element 12 and the reflection axis of the reflective polarizing member 14a contained in the reflector 14 are made approximately orthogonal to each other.
[0089] The light L emitted from the display element 12 via the polarizing member in the form of first linear polarization is converted into first circular polarization by the first λ / 4 member 20. The first circular polarization passes through the half mirror 18 and the first lens unit 16 (at Figure 2 The second linearly polarized light is converted by the second λ / 4 element 22 into a second linearly polarized light having a polarization direction orthogonal to the first linearly polarized light. The polarization direction of the second linearly polarized light is aligned with (substantially parallel to) the reflection axis of the reflective polarizing element 14a included in the reflective portion 14. Therefore, the second linearly polarized light incident on the reflective portion 14 is reflected by the reflective polarizing element 14a toward the half mirror 18.
[0090] The second linearly polarized light reflected by the reflective portion 14 is converted into a second circularly polarized light by the second λ / 4 element 22. The rotation direction of the second circularly polarized light is the same as that of the first circularly polarized light. The second circularly polarized light emitted from the second λ / 4 element 22 passes through the first lens portion 16 and is reflected by the half mirror 18, where it is converted into a third circularly polarized light rotating in the opposite direction to the second circularly polarized light. The third circularly polarized light reflected by the half mirror 18 passes through the first lens portion 16 and is converted into a third linearly polarized light by the second λ / 4 element 22. The polarization direction of the third linearly polarized light is orthogonal to that of the second linearly polarized light and is in the same direction (approximately parallel) as the transmission axis of the reflective polarizing element 14a. Therefore, the third linearly polarized light can transmit through the reflective polarizing element 14a. Although not shown, if the reflective portion includes an absorptive polarizing element, it is arranged so that its absorption axis is approximately parallel to the reflection axis of the reflective polarizing element 14a. Therefore, the third linearly polarized light that transmits the reflective polarizing element 14a can directly transmit through the absorptive polarizing element.
[0091] Light passing through the reflector 14 passes through the second lens portion 24 and enters the user's eye 26. As described above, in the display system according to the embodiment of the present invention, the first linearly polarized light emitted from the display element 12 via the polarizing member passes through the λ / 4 member a total of four times before passing through the reflector 14. By setting the absolute value of the difference between the in-plane phase difference (a) of the first phase difference member 20 and the in-plane phase difference (b) of the second phase difference member 22 to 3.5 nm or less, light leakage from the reflector 14 can be preferably suppressed. As a result, it is possible to preferably suppress light that should be reflected or absorbed by the reflector 14 from being perceived by the user as a ghost.
[0092] Figure 2 In (a), when viewed from the display element 12 side, the slow axes of the first phase difference member 20 and the second phase difference member 22 are both arranged to form a 45° angle in the counterclockwise direction relative to the absorption axis of the polarizing member contained in the display element 12, but they can also be arranged to form a 45° angle in the clockwise direction. In this case, the same description as above can also be applied. In addition, Figure 2 In (a), the slow axis of the first phase difference member 20 and the slow axis of the second phase difference member 22 are arranged to be approximately parallel to each other, but can also be arranged to be approximately orthogonal. For example, one of the slow axis of the first phase difference member 20 and the slow axis of the second phase difference member 22 is arranged to form an angle of 45° in the counterclockwise direction relative to the absorption axis of the polarizing member contained in the display element 12, and the other is arranged to form an angle of 45° in the clockwise direction relative to the absorption axis of the polarizing member. In this case, Figure 2 Unlike the example shown in (a), the absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 a included in the reflecting portion 14 may be arranged to be substantially orthogonal to each other.
[0093] Example
[0094] The present invention is described in detail below using examples, but the present invention is not limited to these examples. The test and evaluation methods used in the examples are as follows. Furthermore, "parts" are "parts by weight" unless otherwise specified, and "%" are "% by weight" unless otherwise specified.
[0095] (1) Thickness
[0096] Thicknesses of 10 μm or less were measured using a scanning electron microscope (JEOL Ltd., product name “JSM-7100F”), and thicknesses greater than 10 μm were measured using a digital micrometer (Anritsu Ltd., product name “KC-351C”).
[0097] (2) In-plane phase difference Re(λ)
[0098] The retardation film was cut into squares with a width of 50 mm and a length of 50 mm, with the center and one of the two ends of the film parallel to the width of the film, to prepare samples. The in-plane retardation of the samples was measured at various wavelengths at 23°C using a Mueller matrix polarimeter (manufactured by Axometrics, product name "Axoscan").
[0099] (3) Single transmittance and polarization degree of polarizing film
[0100] The polarizing film's single transmittance (Ts), parallel transmittance (Tp), and cross transmittance (Tc) were measured using a spectrophotometer (LPF-200, manufactured by Otsuka Electronics Co., Ltd.). These values, Ts, Tp, and Tc, were measured using a 2-degree field of view (illuminant C) as per JIS Z8701 and corrected for visual sensitivity using the Y value. The polarization degree of the polarizing film was calculated from the obtained Tp and Tc using the following formula.
[0101] Polarization degree (%) = {(Tp - Tc) / (Tp + Tc)} 1 / 2 ×100
[0102] (4) Thickness deviation
[0103] Cut the phase difference film into a size of 100mm×100mm to prepare a measurement sample. Figure 3 As shown, the thickness of the measurement sample was measured at five points in total, namely, the center and four points 10 mm apart from the center in the upper, lower, left, and right directions. The difference between the maximum and minimum values was taken as the thickness deviation.
[0104] (5) ISC value
[0105] The ISC value of the retardation film was measured using EyeScale-4W manufactured by i-system Co., Ltd. Specifically, in accordance with the specifications of the measuring device, the in-plane unevenness was calculated as the ISC value using the ISC measurement mode of the 3CCD image sensor.
[0106] Figure 4 This figure is used to explain the method of measuring the ISC value. It is a schematic diagram showing the arrangement of the light source, retardation film, screen, and CCD camera as viewed from above. Figure 4 As shown, a light source L, a retardation film M, and a screen S are arranged in this order, and a transmitted image projected onto the screen S is measured by a CCD camera C. Furthermore, the retardation film M is attached to an alkali-free glass plate (1737, manufactured by Corning Incorporated) and is positioned so that the glass plate is on the side of the light source L for measurement.
[0107] The distance in the X-axis direction from the light source L to the retardation film M is 10 to 60 cm. The distance in the X-axis direction from the light source L to the screen S is 70 to 130 cm. The distance in the Y-axis direction from the CCD camera C to the retardation film M is 3 to 30 cm. The distance in the X-axis direction from the CCD camera C to the screen S is 70 to 130 cm.
[0108] [Manufacturing Example 1-1: Preparation of Retardation Film 1]
[0109] Into a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and a reflux cooler controlled at 100°C, 29.60 parts by weight (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by weight (0.200 mol) of isosorbide (ISB), 42.28 parts by weight (0.139 mol) of spiroglycerol (SPG), 63.77 parts by weight (0.298 mol) of diphenyl carbonate (DPC) and 1.19×10 -2 Parts by weight (6.78×10 -5mol). After the reactor was purged with nitrogen under reduced pressure, it was heated with a heat medium and stirring was initiated when the internal temperature reached 100°C. Forty minutes after the start of the temperature increase, the internal temperature was brought to 220°C. While maintaining this temperature, the pressure was reduced to 13.3 kPa over 90 minutes after reaching 220°C. Phenol vapor, a by-product of the polymerization reaction, was introduced into a 100°C reflux cooler. A small amount of monomer components contained in the phenol vapor were returned to the reactor, and uncondensed phenol vapor was recovered in a 45°C condenser. Nitrogen was introduced into the first reactor to temporarily return it to atmospheric pressure, and the oligomerized reaction liquid in the first reactor was transferred to the second reactor. Next, the temperature and pressure in the second reactor were increased and reduced, reaching an internal temperature of 240°C and a pressure of 0.2 kPa over 50 minutes. Polymerization was then continued until the desired stirring power was reached. Once the desired power was reached, nitrogen was introduced into the reactor to reduce the pressure. The resulting polyester carbonate resin was extruded into water, and the bundle was cut to obtain pellets.
[0110] The resulting polyester carbonate resin (pellets) was vacuum-dried at 80°C for 5 hours and then formed into a 130 μm thick long resin film using a film forming apparatus equipped with a uniaxial extruder (manufactured by Toshiba Machine Co., Ltd., cylinder set temperature: 250°C), a T-die (200 mm width, set temperature: 250°C), a cooling roll (set temperature: 120-130°C), and a winder. The resulting long resin film was then stretched in the width direction at a stretching temperature of 140°C and a stretching ratio of 2.7.
[0111] In the above manner, a retardation film 1 having a thickness of 47 μm, an Re(590) of 143 nm, and an Nz coefficient of 1.2 was obtained. The Re(450) / Re(550) ratio of the obtained retardation film 1 was 0.856. Table 1 shows the ISC value and thickness deviation of the retardation film 1.
[0112] [Manufacturing Example 1-2: Preparation of Phase Difference Film 2]
[0113] A retardation film 2 was obtained in the same manner as in Production Example 1-1, except that the stretching temperature was changed. The resulting retardation film 2 had a thickness of 47 μm, a Re(590) of 145 nm, an Nz coefficient of 1.2, and a Re(450) / Re(550) ratio of 0.856. Table 1 shows the ISC value and thickness variation of the retardation film 2.
[0114] [Manufacturing Example 1-3: Preparation of Phase Difference Film 3]
[0115] Retardation Film 3 was obtained in the same manner as in Production Example 1-1, except that the stretching temperature was changed. The resulting Retardation Film 3 had a thickness of 47 μm, a Re(590) of 147 nm, an Nz coefficient of 1.2, and a Re(450) / Re(550) ratio of 0.856. Table 1 shows the ISC value and thickness variation of Retardation Film 3.
[0116] [Table 1]
[0117]
[0118] [Manufacturing Example 2: Preparation of Polarizing Film]
[0119] A long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a Tg of approximately 75° C. was used as the thermoplastic resin substrate, and one surface of the resin substrate was corona treated.
[0120] 13 parts by weight of potassium iodide was added to 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Mitsubishi Chemical Co., trade name "GOHSENX Z410") in a ratio of 9:1, and the resulting mixture was dissolved in water to prepare a PVA aqueous solution (coating solution).
[0121] The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60° C. to form a PVA-based resin layer having a thickness of 13 μm, thereby producing a laminate.
[0122] The obtained layered product was uniaxially stretched to 2.4 times in the longitudinal direction (longitudinal direction) in an oven at 130° C. (in-flight auxiliary stretching treatment).
[0123] Next, the layered product was immersed in an insolubilization bath (a boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).
[0124] Next, the film is immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single body transmittance (Ts) of the final absorption-type polarizing film becomes the desired value (dyeing treatment).
[0125] Next, the film was immersed in a crosslinking bath (a boric acid aqueous solution prepared by adding 3 parts by weight of potassium iodide and 5 parts by weight of boric acid to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).
[0126] Then, while immersing the laminate in a boric acid aqueous solution (boric acid concentration 4 wt%, potassium iodide concentration 5 wt%) at a liquid temperature of 70°C, it is uniaxially stretched in the longitudinal direction (long side direction) between rollers with different peripheral speeds so that the total stretching ratio reaches 5.5 times (underwater stretching treatment).
[0127] Then, the layered product was immersed in a cleaning bath (an aqueous solution prepared by mixing 4 parts by weight of potassium iodide with respect to 100 parts by weight of water) at a liquid temperature of 20° C. (cleaning treatment).
[0128] Thereafter, the laminate was dried in an oven maintained at approximately 90° C. while being brought into contact with a SUS heating roll maintained at a surface temperature of approximately 75° C. (drying shrinkage treatment). The shrinkage rate in the width direction of the laminate after the drying shrinkage treatment was 5.2%.
[0129] Through the above steps, an absorption-type polarizing film with a thickness of about 5 μm was formed on the resin substrate.
[0130] A cycloolefin resin film (25 μm thick) was applied as a protective layer to the surface of the resulting absorption-type polarizing film (the surface opposite the resin substrate) via a UV-curable adhesive. Specifically, the curable adhesive was applied to a total thickness of approximately 1 μm and then bonded using a roll mill. UV light was then applied from the cycloolefin resin film side to cure the adhesive. The resin substrate was then peeled off.
[0131] Thus, a polarizing film having a structure of cycloolefin resin film / absorption-type polarizing film was obtained. The single-piece transmittance (Ts) of the polarizing film was 43.4%, and the degree of polarization was 99.993%.
[0132] [Example 1]
[0133] Four phase difference films 1 obtained in Manufacturing Example 1-1 are stacked together, and the polarizing film obtained in Manufacturing Example 2 is stacked together to obtain a laminate. Adjacent films are bonded together through an acrylic adhesive layer (manufactured by Nitto Denko Corporation, with a thickness of 5 μm). The four phase difference films are stacked in the form of λ / 4 component 1, λ / 4 component 2, λ / 4 component 3 and λ / 4 component 4 in the order shown in Table 2, starting from one side. Then, the polarizing film is stacked on the λ / 4 component 4. In addition, the angles shown in Table 2 are the axis angles of each component based on the absorption axis direction of the absorption-type polarizing film of the polarizing film when the laminate is viewed from the side of the λ / 4 component 1. "+" indicates the clockwise direction, and "-" indicates the counterclockwise direction.
[0134] [Table 2]
[0135]
[0136] [Example 2]
[0137] A laminate was obtained in the same manner as in Example 1 except that the retardation film 3 obtained in Production Example 1-3 was used instead of the retardation film 1 obtained in Production Example 1-1.
[0138] [Example 3]
[0139] A laminate was obtained in the same manner as in Example 1 except that the retardation film 2 obtained in Production Example 1-2 was used as the λ / 4 member 2 , the λ / 4 member 3 , and the λ / 4 member 4 .
[0140] [Example 4]
[0141] A laminate was obtained in the same manner as in Example 2 except that the retardation film 2 obtained in Production Example 1-2 was used as the λ / 4 member 2 , the λ / 4 member 3 , and the λ / 4 member 4 .
[0142] [Comparative Example 1]
[0143] A laminate was obtained in the same manner as in Example 1 except that the retardation film 3 obtained in Production Example 1-3 was used as the λ / 4 member 2 , the λ / 4 member 3 , and the λ / 4 member 4 .
[0144] [Comparative Example 2]
[0145] A laminate was obtained in the same manner as in Example 2 except that the retardation film 1 obtained in Production Example 1-1 was used as the λ / 4 member 2 , the λ / 4 member 3 , and the λ / 4 member 4 .
[0146] Evaluation
[0147] The single-unit transmittance and polarization degree of the laminated body of each Example and each Comparative Example were measured. Specifically, linear polarization with a polarization direction perpendicular to the absorption axis direction of the absorption-type polarizing film was incident on the surface of the λ / 4 member 1 side of the laminated body, and the single-unit transmittance Ts, parallel transmittance Tp, and orthogonal transmittance Tc at this time were measured using a spectrophotometer ("LPF-200" manufactured by Otsuka Electronics Co., Ltd.). These Ts, Tp, and Tc are Y values measured using a 2-degree field of view (light source C) in accordance with JIS Z8701 and corrected for visual sensitivity. The polarization degree of the laminated body was calculated from the obtained Tp and Tc using the formula described in (3) above.
[0148] The single-unit transmittance, cross transmittance, and polarization degree of the laminate are shown in Table 3. The laminates produced in the Examples and Comparative Examples serve as simplified evaluation models for display systems according to embodiments of the present invention. Specifically, light entering the laminate from the λ / 4 element 1 side and exiting from the polarizing film side was evaluated as follows: In a display system according to an embodiment of the present invention, first linearly polarized light emitted forward from the display element via the polarizing element sequentially transmits through the first and second phase difference elements, is reflected by the reflective portion and the half mirror, further transmits through the second phase difference element twice, and then transmits forward from the reflective portion.
[0149] [Table 3]
[0150]
[0151] In each embodiment, a high degree of polarization can be achieved, and light leakage can be preferably suppressed according to the display system.
[0152] The present invention is not limited to the above-described embodiments and can be modified in various ways. For example, the present invention can be replaced by a configuration that is substantially the same as the configuration shown in the above-described embodiments, a configuration that can exert the same effects, or a configuration that can achieve the same purpose.
[0153] Industrial applicability
[0154] The display system according to the embodiment of the present invention can be used for a display device such as VR goggles, for example.
[0155] Description of Reference Numerals
[0156] 2: Display system; 12: Display element; 14: Reflection unit; 14a: Reflective polarizing element; 16: First lens unit; 18: Half mirror; 20: First phase difference element; 22: Second phase difference element; 24: Second lens unit.
Claims
1. A display system for displaying images to a user, comprising: A display element having a display surface, the display surface emits light of a display image forward through a polarizing member; a reflective portion, disposed in front of the display element and comprising a reflective polarizing member, the reflective portion reflecting light emitted from the display element; A first lens portion, disposed on an optical path between the display element and the reflective portion; a half mirror disposed between the display element and the first lens portion, the half mirror transmitting light emitted from the display element and reflecting light reflected by the reflection portion toward the reflection portion; A first λ / 4 member is disposed on an optical path between the display element and the half mirror; and A second λ / 4 member is disposed on an optical path between the half mirror and the reflecting portion; The absolute value of the difference between the in-plane phase difference (a) of the first λ / 4 member and the in-plane phase difference (b) of the second λ / 4 member is 3.5 nm or less.
2. A display system as claimed in claim 1, The in-plane phase difference (a) of the first λ / 4 element and the in-plane phase difference (b) of the second λ / 4 element satisfy the following formula (I): ((a)-(b)) / ((a)+(b) / 2)≤0.02···(I).
3. The display system as claimed in claim 1, The ISC values of the first λ / 4 element and the second λ / 4 element are each 50 or less.
4. The display system as claimed in claim 1, The thickness of each of the first λ / 4 member and the second λ / 4 member is 100 μm or less.
5. The display system as claimed in claim 1, The first λ / 4 member and the second λ / 4 member each have a thickness deviation of 1 μm or less.
6. The display system as claimed in claim 1, The ISC values per unit thickness of the first λ / 4 member and the second λ / 4 member are each 1 or less.
7. The display system as claimed in claim 1, The polarization direction of the light emitted through the polarizing element and the reflection axis of the reflective polarizing element are substantially orthogonal to each other.
8. The display system as claimed in claim 1, The angle formed by the absorption axis of the polarizing member included in the display element and the slow axis of the first λ / 4 member is 40° to 50°, The angle formed by the absorption axis of the polarizing member included in the display element and the slow axis of the second λ / 4 member is 40° to 50°.
9. A display body, A display system according to any one of claims 1 to 8.
10. A method for manufacturing a display body, A method for manufacturing a display body having a display system according to any one of claims 1 to 8.
11. A display method comprising the following steps: The step of passing the light of the display image emitted through the polarizing member through a first λ / 4 member; The step of passing the light that has passed through the first λ / 4 member through a half mirror and a first lens portion; a step of passing the light that has passed through the half mirror and the first lens portion through a second λ / 4 member; a step of causing the light that has passed through the second λ / 4 member to be reflected toward the half mirror at a reflection portion including a reflective polarizing member; and A step of allowing the light reflected by the reflecting portion and the half mirror to pass through the reflecting portion through the second λ / 4 member; The absolute value of the difference between the in-plane phase difference (a) of the first λ / 4 member and the in-plane phase difference (b) of the second λ / 4 member is 3.5 nm or less.