Metal material and surface treatment method thereof
Through the imidazole ionic liquid electrolyte system and finely controlled electroplating parameters, the problem of difficulty in controlling the thickness of the zinc-cobalt alloy coating is solved, a uniform, smooth and highly corrosion-resistant coating is achieved, and the corrosion resistance and color effect of the coating are significantly improved. .
Patent Information
- Application Number
- CN202411089648.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-10-25
AI Technical Summary
In the existing technology, it is difficult to control the thickness of the pickling plating solution, resulting in uneven thickness of the zinc-cobalt alloy coating and insufficient corrosion resistance and color.
The imidazole ionic liquid electrolyte system is used to achieve precise control of the thickness of the zinc-cobalt alloy coating by controlling the deposition time and electroplating parameters. It combines mechanical grinding, water washing, chemical degreasing, pickling and passivation to prepare a uniform, smooth and durable coating. Coating with excellent corrosion resistance and color resistance.
The thickness uniformity and corrosion resistance of the zinc-cobalt alloy coating have been significantly improved. The thickness fluctuation of the coating is less than 0.5 μm. The corrosion resistance is significantly better than that of conventional zinc-cobalt coating, and the color effect is good.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal surface treatment, and in particular relates to a colorful corrosion-resistant metal material and a preparation method thereof. Background Art
[0002] As modern industry's requirements for material performance increase, people's requirements for material surface corrosion resistance and decorative properties are gradually increasing. Metal alloy coatings with high corrosion resistance and excellent decorative properties are gaining more and more attention, especially in the application range of mobile phone cases, metal accessories, automobiles, shipbuilding, electromechanical and other industries.
[0003] Compared with pure zinc coating, the binary alloy electroplating layer formed by zinc-based iron metals can greatly improve the corrosion resistance of steel substrates. The zinc-cobalt alloy coating electroplated on the surface of the steel substrate is an anodic protective coating, which has both mechanical and electrochemical protection for the substrate, and its corrosion resistance is significantly improved compared with pure zinc coating. There are four systems for zinc-cobalt alloy electroplating currently used: chloride system, sulfate system, chloride-sulfate mixed system and alkaline zincate system. Among them, the chloride system is more studied and applied, but the chloride system has the disadvantages of insufficient electroplating thickness, poor all-over plating ability and insufficient stability of the electroplating solution. The alkaline zincate system has the advantages of simple plating solution composition, excellent plating solution dispersion ability and coverage, and the obtained zinc-cobalt alloy coating has the advantages of fine and bright crystals and easy passivation. In recent years, there have been many literature reports on zinc-cobalt alloy electroplating in the alkaline zincate system suitable for electroplating of more complex parts, but most of the research focuses on the optimization of electroplating process, the improvement of plating solution performance and the corrosion resistance of zinc-cobalt alloy coatings.
[0004] In the prior art, such as CN102260889B Guangzhou Haikeshun Surface Treatment Co., Ltd. discloses a highly corrosion-resistant, bright, and soft zinc-cobalt alloy electroplating process. Its process flow is workpiece surface pretreatment, zinc-cobalt alloy plating, and workpiece surface posttreatment. The surface pretreatment is as follows: alkaline chemical degreasing → water washing → alkaline anode electrolytic degreasing → water washing × 2 → pickling (30% HCl) → water washing → final electrolytic defilming (anode) → water washing → activation (10% HCl) → water washing and other processes; the zinc-cobalt alloy electroplating uses an alkaline zinc-cobalt alloy electroplating solution; the workpiece surface posttreatment is as follows: water washing × 2 → light (0.25% nitric acid) → water washing → passivation → water washing × 2 → sealing → drying. The biggest feature of the present invention is strong anti-rust performance. The trivalent chromium passivation is combined with a zinc plating sealer. The neutral salt spray can reach 240 hours without white rust and 1000 hours without red rust. The alloy composition is uniform, the operating range is wide, and the cost is low.
[0005] For example, CN103320821B Guiyang Huake Electroplating Co., Ltd. discloses an alkaline zinc-cobalt alloy electroplating solution, characterized in that: by weight, the following substances are included in 1000 parts of the electroplating solution: 7-20 parts of zinc oxide, 130-170 parts of sodium hydroxide, 3-12 parts of cobalt sulfate, 15-25 parts of triethanolamine, 5-10 parts of citric acid, 30-35 parts of tartaric acid, 0.1-0.6 parts of sodium benzylpyridinium carboxylate, 0.1-0.5 parts of sodium phytate, 2-5 parts of dimethylamine, 0.3-0.5 parts of thiourea, 0.02-0.05 parts of jasminaldehyde, and the rest is water. According to the applicant's test, the electroplated product obtained by the electroplating solution formula of the present invention does not produce white rust in a neutral salt spray test for 300 hours. Compared with the prior art, it has the advantages of easy control of the cobalt content of the alloy component, good deep plating ability and throwing ability of the plating solution, convenient operation, and stable plating solution.
[0006] CN110760906B China University of Geosciences (Wuhan) discloses a nano zinc-cobalt alloy coating based on double pulse electrodeposition and its preparation method. A preparation method of a nano zinc-cobalt alloy coating based on double pulse electrodeposition, using a zinc plate as an anode and a low carbon steel sheet as a cathode, and electroplating a nano zinc-cobalt alloy coating in a plating solution using a double pulse electrodeposition process, wherein the pH of the plating solution is 4-5, the concentration of zinc ions is 0.64-0.70 mol / L, the concentration of cobalt ions is 0.1-0.16 mol / L, the electrodeposition time is 20min, the forward current density is 1.5-3.0A / dm2, the forward duty cycle is 30-70%, the forward cycle is 30-70ms, the reverse current density is 0.2-0.4A / dm2, the reverse duty cycle is 30-70%, the forward working time is 100ms, the reverse working time is 12ms, and the reverse cycle is 1ms. The nano zinc-cobalt alloy coating prepared by a preparation method of a nano zinc-cobalt alloy coating based on double pulse electrodeposition has a bright and smooth surface, uniform and dense crystals, good bonding strength with a substrate, and excellent corrosion resistance. Summary of the invention
[0007] Based on the above, it can be known that it is difficult to achieve thick zinc-cobalt alloy plating in the pickling plating solution in the prior art, and it is difficult to control the thickness. Based on the above, the present invention provides a new electroplating electrolyte, which can effectively control the relationship between the coating thickness and time in the electroplating system. The obtained coating has uniform and flat thickness, good bonding with the substrate, and has excellent corrosion resistance and color after passivation treatment.
[0008] Specifically: A method for preparing a colorful corrosion-resistant metal material comprises mechanical grinding, water washing, chemical degreasing, water washing, primary pickling, water washing, secondary pickling, water washing, electroplating, water washing, tertiary pickling, water washing, passivation and drying.
[0009] Furthermore, the chemical degreasing solution is composed of 30-40 g / L sodium hydroxide, 20-25 g / L sodium carbonate, 12-15 g / L trisodium phosphate, 5-7 g / L sodium silicate and 1-2 g / L O emulsifier and deionized water, the temperature is 80-90° C., and the degreasing method is immersion.
[0010] Further, the pickling solution is composed of 25wt%H 3 PO 4 , 0.2wt% thiourea, 3wt% ethylene glycol butyl ether and deionized water, and the temperature is 55°C.
[0011] Furthermore, the secondary pickling solution is 40 mL / L HCl at room temperature.
[0012] Furthermore, the solution for the three acid washes is 3 vol% HNO 3 .
[0013] Furthermore, the passivation solution used in the passivation includes 5g / LCrO 3 , 3mL / L HNO 3 and 0.5mL / LH2SO 4 , time is 25s, temperature is 20-30℃.
[0014] Furthermore, the substrate of the metal material is selected from stainless steel, aluminum alloy or copper alloy.
[0015] Furthermore, the electroplating is electroplating zinc-cobalt alloy on the metal surface, and the zinc-cobalt alloy electroplating solution is prepared by the following steps: (1) Under stirring conditions at room temperature, butyl chloride and 1-methylimidazole in a molar ratio of 1.3:1 were mixed in toluene solvent and introduced into a reactor; argon gas was introduced into the reactor as a protective gas, and then the temperature of the reactor was controlled to 83°C using an oil bath, and the temperature was continuously stirred for 52 hours at a constant temperature and a stirring speed of 500 rpm. After naturally cooling to room temperature, the reactants were taken out; (2) removing the excess toluene solvent and butyl chloride by vacuum distillation once, then extracting with 20 mL of ethyl acetate three times and recrystallizing, then removing the excess ethyl acetate by vacuum distillation twice, and then vacuum drying at 75 ° C for 24 h to collect the product for later use; (3) 18 g of the product prepared in step 2, 14 g of zinc chloride and 6 g of cobalt chloride were placed in a reaction kettle, and under argon protection, an oil bath was heated at 75°C to obtain a viscous liquid.
[0016] (4) Take 120 g / L of the viscous liquid prepared in step (3), 35 g / L of boric acid, 10 g / L of ethanol, 5 g / L of quaternized polyvinyl imidazole, 0.2 g / L of fatty alcohol polyoxyethylene ether sodium sulfate AES, 0.15 g / L of benzyl nicotinate and deionized water, and adjust the pH to 4.3±0.2 with ammonia water to obtain a zinc-cobalt alloy electroplating solution.
[0017] Furthermore, the electroplating parameters are: temperature 35°C, constant current mode 5.7A / dm 2 , time t: 0 <t<35min。
[0018] Furthermore, the time and coating thickness satisfy the following formula: δ=a*t b ; where δ is thickness, a=0.0292±0.0067, 0 <t<35min,b=1.8238±0.0668。
[0019] Furthermore, the zinc-cobalt alloy coating thickness is less than 20 μm, and the thickness fluctuation range is less than 0.5 μm.
[0020] Beneficial technical effects: (1) The imidazolium ionic liquid electrolyte system is used to effectively realize zinc-cobalt co-deposition; (2) Under this electrolyte system, the thickness of the coating can be accurately controlled by controlling the deposition time, and the thickness fluctuation is controlled to be less than 1 μm; (3) The relative relationship between the thickness of the zinc-cobalt coating and time is fitted for the first time, which has practical guiding significance; (4) After other pre- and post-treatments, a coating with excellent corrosion resistance and color is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Attached Figure 1 Morphology of coating at different time periods.
[0022] Attached Figure 2 Variation of coating thickness with time at different periods. DETAILED DESCRIPTION Example 1
[0023] A method for preparing a colorful corrosion-resistant metal material comprises mechanical grinding, water washing, chemical degreasing, water washing, primary pickling, water washing, secondary pickling, water washing, electroplating, water washing, tertiary pickling, water washing, passivation and drying.
[0024] The chemical degreasing solution is composed of 35g / L sodium hydroxide, 22.5g / L sodium carbonate, 13.5g / L trisodium phosphate, 6g / L sodium silicate and 1-2g / LOP emulsifier and deionized water, the temperature is 85°C, and the degreasing method is immersion.
[0025] The primary pickling solution consists of 25wt% H 3 PO 4, 0.2wt% thiourea, 3wt% ethylene glycol butyl ether and deionized water, and the temperature is 55°C.
[0026] The secondary pickling solution is 40 mL / L HCl at room temperature.
[0027] The electroplating is to electroplating zinc-cobalt alloy on the metal surface, and the zinc-cobalt alloy electroplating solution is prepared by the following steps: (1) Under stirring conditions at room temperature, butyl chloride and 1-methylimidazole in a molar ratio of 1.3:1 were mixed in toluene solvent and introduced into a reactor; argon gas was introduced into the reactor as a protective gas, and then the temperature of the reactor was controlled to 83°C using an oil bath, and the temperature was continuously stirred for 52 hours at a constant temperature and a stirring speed of 500 rpm. After naturally cooling to room temperature, the reactants were taken out; (2) removing the excess toluene solvent and butyl chloride by vacuum distillation once, then extracting with 20 mL of ethyl acetate three times and recrystallizing, then removing the excess ethyl acetate by vacuum distillation twice, and then vacuum drying at 75 ° C for 24 h to collect the product for later use; (3) 18 g of the product prepared in step 2, 14 g of zinc chloride and 6 g of cobalt chloride were placed in a reaction kettle, and under argon protection, an oil bath was heated at 75°C to obtain a viscous liquid.
[0028] (4) Take 120 g / L of the viscous liquid prepared in step (3), 35 g / L of boric acid, 10 g / L of ethanol, 5 g / L of quaternized polyvinyl imidazole, 0.2 g / L of fatty alcohol polyoxyethylene ether sodium sulfate AES, 0.15 g / L of benzyl nicotinate and deionized water, and adjust the pH to 4.3±0.2 with ammonia water to obtain a zinc-cobalt alloy electroplating solution.
[0029] The electroplating parameters are: temperature 35°C, constant current mode 5.7A / dm 2 .
[0030] The solution for the third pickling is 3 vol% HNO 3 .
[0031] The passivation solution used for passivation includes 5g / LCrO 3 , 3mL / L HNO 3 and 0.5 mL / LH 2 SO 4 , time is 25s, temperature is 20-30℃. Example 2
[0032] A metal surface treatment method, the surface treatment method is electroplating zinc-cobalt alloy on the metal surface, the zinc-cobalt alloy electroplating solution is prepared by the following steps: (1) Under stirring conditions at room temperature, butyl chloride and 1-methylimidazole in a molar ratio of 1.3:1 were mixed in toluene solvent and introduced into a reactor; argon gas was introduced into the reactor as a protective gas, and then the temperature of the reactor was controlled to 83°C using an oil bath, and the temperature was continuously stirred for 52 hours at a constant temperature and a stirring speed of 500 rpm. After naturally cooling to room temperature, the reactants were taken out; (2) removing the excess toluene solvent and butyl chloride by vacuum distillation once, then extracting with 20 mL of ethyl acetate three times and recrystallizing, then removing the excess ethyl acetate by vacuum distillation twice, and then vacuum drying at 75 ° C for 24 h to collect the product for later use; (3) 18 g of the product prepared in step 2, 14 g of zinc chloride and 6 g of cobalt chloride were placed in a reaction kettle, and under argon protection, an oil bath was heated at 75°C to obtain a viscous liquid.
[0033] (4) Take 120 g / L of the viscous liquid prepared in step (3), 35 g / L of boric acid, 10 g / L of ethanol, 5 g / L of quaternized polyvinyl imidazole, 0.2 g / L of fatty alcohol polyoxyethylene ether sodium sulfate AES, 0.15 g / L of benzyl nicotinate and deionized water, and adjust the pH to 4.3±0.2 with ammonia water to obtain a zinc-cobalt alloy electroplating solution.
[0034] Electroplating parameters: temperature 35°C, constant current mode 5.7A / dm 2 , time t: 0 <t<35min。
[0035] The time variation of Example 2 was used as a variable to characterize its morphology. Figure 1 , thickness changes over time, see Appendix Figure 2 , the parameters are fitted, and the time and coating thickness satisfy the following formula: δ=a*t b ; where δ is thickness, a=0.0292±0.0067, 0 <t<35min,b=1.8238±0.0668。
[0036] Comparative Example 1. A metal surface treatment method, the surface treatment method is to electroplate zinc-cobalt alloy on the metal surface, the zinc-cobalt alloy electroplating solution has the following composition: 100 g / L zinc sulfate, 50 g / L cobalt sulfate, 30 g / L boric acid and deionized water, the electroplating parameters are: temperature 35°C, constant current mode 5.7 A / dm 2 , time t: 20min.
[0037] The coating thickness values of Example 2 and Comparative Example 2 were tested. The electrodeposition time for both was 17 min. The average thickness of Example 2 was 5.14 μm, and the thickness of Comparative Example 2 was only 2.7 μm. It can be seen that the deposition effect of Comparative Example 2 is not as good as that of Example 2. The main reason lies in the plating solution system and the plating solution additives. Specifically, Example 2 tests different positions of the same coating material, and the coating thicknesses are 5.22 μm, 5.29 μm, 5.14 μm, 4.98 μm, 4.93 μm, 5.09 μm, 5.13 μm, 5.24 μm, 5.18 μm, and 5.20 μm, respectively. By calculating the standard deviation, it can be concluded that the standard deviation of the coating is 0.11 3725. In comparison, the coating thicknesses at different positions of the same coating material in Comparative Example 1 are 1.91 μm, 2.03 μm, 3.21 μm, 2.78 μm, 1.98 μm, 3.41 μm, 2.64 μm, 2.98 μm, 3.14 μm and 2.99 μm respectively. By calculating the standard deviation, it can be concluded that the standard deviation of the coating is 0.54987. The smaller the standard deviation, the higher the corresponding data concentration and the smaller the fluctuation. That is, the larger the quasi-deviation, the higher the corresponding data discreteness and the larger the fluctuation. That is, the coating prepared in Example 2 shows more deposition and more uniform thickness in the coating effect, which is significantly better than Comparative Example 2, that is, better than the conventional zinc-cobalt plating solution.
[0038] Then, the corrosion resistance test of the passivated material prepared in Example 1 was carried out. The corrosion resistance of the zinc-cobalt coating material after passivation was significantly improved, and the corrosion current density was 2.969*10 -8 A / cm 2 The corresponding corrosion potential is -1.013V, which is significantly better than that of conventional zinc-cobalt coating materials. It can be inferred that the coating itself has a dense structure and uniform coating thickness, and the corresponding passivation film is also more uniform and stable, thus showing excellent corrosion resistance.
[0039] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A metal surface treatment method, characterized in that Including mechanical grinding, water washing, chemical degreasing, water washing, primary pickling, water washing, secondary pickling, water washing, electroplating, water washing, tertiary pickling, water washing, passivation, and drying; The electroplating is to electroplating zinc-cobalt alloy on the metal surface, and the zinc-cobalt alloy electroplating solution is prepared by the following steps: (1) Under stirring conditions at room temperature, butyl chloride and 1-methylimidazole in a molar ratio of 1.3:1 were mixed in toluene solvent and introduced into a reactor; argon gas was introduced into the reactor as a protective gas, and then the temperature of the reactor was controlled to 83°C using an oil bath, and the temperature was continuously stirred for 52 hours at a constant temperature and a stirring speed of 500 rpm. After naturally cooling to room temperature, the reactants were taken out; (2) removing the excess toluene solvent and butyl chloride by vacuum distillation once, then extracting with 20 mL of ethyl acetate three times and recrystallizing, then removing the excess ethyl acetate by vacuum distillation twice, and then vacuum drying at 75 ° C for 24 h to collect the product for later use; (3) 18 g of the product prepared in step 2, 14 g of zinc chloride and 6 g of cobalt chloride were placed in a reaction kettle, and under argon protection, an oil bath was set at 75°C to obtain a viscous liquid; (4) Take 120 g / L of the viscous liquid prepared in step (3), 35 g / L of boric acid, 10 g / L of ethanol, 5 g / L of quaternized polyvinyl imidazole, 0.2 g / L of fatty alcohol polyoxyethylene ether sodium sulfate AES, 0.15 g / L of benzyl nicotinate and deionized water, and adjust the pH to 4.3±0.2 with ammonia water to obtain a zinc-cobalt alloy electroplating solution.
2. A metal surface treatment method as claimed in claim 1, characterized in that The electroplating parameters are: temperature 35°C, constant current mode 5.7A / dm 2 , time t: 0 <t<35min。 3. A metal surface treatment method as claimed in claim 2, characterized in that The time and coating thickness satisfy the following formula: δ=a*t b ; where δ is thickness, a=0.0292±0.0067, 0 <t<35min,b=1.8238±0.0668。 4. A metal surface treatment method as claimed in claim 3, characterized in that The zinc-cobalt alloy coating thickness is less than 20 μm.
5. A metal surface treatment method as claimed in claim 1, characterized in that The chemical degreasing solution is composed of 30-40g / L sodium hydroxide, 20-25g / L sodium carbonate, 12-15g / L trisodium phosphate, 5-7g / L sodium silicate and 1-2g / LOP emulsifier and deionized water. The temperature is 80-90°C, and the degreasing method is immersion.
6. A metal surface treatment method as claimed in claim 1, characterized in that The solution for the first pickling is composed of 25wt% H3PO4, 0.2wt% thiourea, 3wt% ethylene glycol butyl ether and deionized water, and the temperature is 55°C; the solution for the second pickling is 40mL / L HCl, at room temperature; the solution for the third pickling is 3vol% HNO3.
7. A metal surface treatment method as claimed in claim 1, characterized in that The passivation solution used in the passivation includes 5g / L CrO3, 3mL / L HNO3 and 0.5mL / L H2SO4, the time is 25s, and the temperature is 20-30°C.
8. A metal material, characterized in that A metal material obtained by the metal surface treatment method according to any one of claims 1 to 7.
9. A metal material as claimed in claim 8, characterized in that The substrate of the metal material is selected from stainless steel, aluminum alloy or copper alloy.