Positive electrode material substrate and preparation method thereof, positive electrode plate and sodium ion battery
By adopting Na3V2(PO4)3 hollow pellet connection structure and double-layer CEI membrane technology, the problem of low conductivity and structural change of sodium vanadium phosphate cathode material is solved, the capacity and cycle performance of sodium ion battery are improved, and the electrochemical stability is ensured. Stability and rate performance.
Patent Information
- Application Number
- CN202410867454.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-25
AI Technical Summary
Sodium vanadium phosphate (NVP), as the cathode material of sodium-ion batteries, has low electronic conductivity and structural changes, resulting in poor battery performance, unstable electrode surface, and interfacial side reactions that consume active materials and affect cycle performance.
A lantern-like structure formed by connecting multiple Na3V2(PO4)3 hollow spheres is used as the cathode material matrix, and a double-layer CEI film is formed through a specific preparation method and electrolyte film-forming additives to optimize sodium ion transmission and electrode surface stability.
It improves the gram capacity and cycle performance of sodium-ion batteries, suppresses the volume expansion of the cathode material, enhances electrochemical stability and rate performance, and reduces side reactions between the electrolyte and the cathode material.
Smart Images

Figure BDA0004920629470000071 
Figure BDA0004920629470000081 
Figure BDA0004920629470000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, and in particular to a positive electrode material matrix and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Background Art
[0002] Sodium vanadium phosphate (Na3V2(PO4)3, abbreviated as NVP) has a sodium ion fast conductor structure and is considered to be a promising positive electrode material for sodium ion batteries. However, the low electronic conductivity of NVP and the large structural changes during the cycle process have hindered its commercial application process. Currently, the use of surface coating technology and morphology regulation is considered to be a simple and effective method to improve the performance of sodium vanadium phosphate positive electrode materials. But even so, sodium vanadium phosphate as a positive electrode material still faces the problem of electrode surface / interface chemical instability, such as residual alkali on the electrode surface, continuous consumption of active substances by interfacial side reactions, large interfacial impedance leading to poor battery performance during cycling, and changes in the CEI film during charging and discharging directly affecting the electrochemical reaction of the electrode and battery attenuation.
[0003] In view of this, it is indeed necessary to provide a technical solution to the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a positive electrode material matrix and a preparation method thereof, a positive electrode plate and a sodium ion battery in view of the deficiencies in the prior art, so as to improve the gram capacity and cycle performance of the sodium ion battery.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A positive electrode material matrix, wherein the interior of the positive electrode material matrix is a lantern-shaped structure formed by connecting a plurality of hollow spheres made of Na3V2(PO4)3.
[0007] In some embodiments, the pore size A of the hollow spheres is in the range of 0.03um≤A≤0.08um.
[0008] The present invention also aims to provide a method for preparing a positive electrode material matrix, comprising the following steps:
[0009] Step S1, dispersing polyvinyl pyrrolidone in ethylene glycol to obtain a first mixture that is uniformly mixed;
[0010] Step S2, adding a sodium source, a vanadium source, and a phosphorus source to the first mixture, reacting at 15° C.-30° C. with stirring for 8-12 hours, then placing the second mixture after the reaction in a high-pressure reactor, heating and reacting at 160-200° C. for 14-18 hours to obtain a first intermediate product;
[0011] Step S3, placing the first intermediate product in an air atmosphere and sintering at a high temperature of 500° C. to 700° C. to remove PVP, thereby obtaining a second intermediate product.
[0012] Step S4, placing the second intermediate product in an argon atmosphere and sintering at a high temperature of 900°C-100°C to obtain a black positive electrode material matrix with a lantern-shaped structure composed of multiple hollow spheres made of Na3V2(PO4)3 connected together.
[0013] In some embodiments, the stoichiometric ratio of the sodium source, the vanadium source, and the phosphorus source is: 1.5-3:1-2:3;
[0014] The concentration ratio of polyvinyl pyrrolidone to sodium acetate is 12-16:1;
[0015] The sodium source is selected from at least one of sodium nitrate, sodium acetate and Na2CO3;
[0016] The vanadium source is selected from at least one of vanadium pentoxide, vanadium acetylacetonate, and sodium metavanadate;
[0017] The phosphorus source is selected from at least one of phosphoric acid and diammonium phosphate.
[0018] In some embodiments, the concentration of polyvinyl pyrrolidone in step S1 is 0.5-1.0 mol / L;
[0019] The step S3 specifically comprises: placing the first intermediate product in an air atmosphere, heating the temperature to 500°C-700°C at a rate of 4°C-6°C / min, and then keeping the temperature for 1-3 hours to remove PVP, thereby obtaining a second intermediate product;
[0020] The step S4 is specifically as follows: placing the second intermediate product in an argon atmosphere, heating it to 900°C-1000°C at a rate of 4°C-6°C / min, and sintering it for 10-14h to obtain a black Na3V2(PO4)3 positive electrode material with a lantern-shaped structure formed by connecting multiple hollow spheres.
[0021] In some embodiments, after placing the second mixture after the reaction in a high pressure reactor and heating the reaction at 160-200° C. for 14-18 hours, the step S2 further comprises:
[0022] The product after the reaction is washed and dried to obtain the first intermediate product.
[0023] In the preparation method of the positive electrode material provided by the present invention, PVP is used as a soft template and a surfactant, and ethylene glycol is used as a cross-linking agent. First, PVP is converted into spherical micelles with carbonyl groups under the cross-linking effect of ethylene glycol, and then a plurality of spherical micelles with carbonyl groups are connected to each other to form a lantern shape. The acetylacetonato ligands in vanadium acetylacetonate are gradually replaced by hydroxyl groups in ethylene glycol to generate oligomeric vanadium glycolate. Finally, under the action of hydrogen bonds, the oligomeric vanadium glycolate is connected to the PVP spherical micelles for self-assembly, and a sodium source and a phosphorus source react with vanadium glycolate under high temperature and high pressure to generate a first intermediate product: a Na3V2(PO4)3 precursor. Finally, PVP is removed at high temperature, the hollow microspheres are retained, and the precursor is converted into a Na3V2(PO4)3 positive electrode material with a lantern-shaped structure formed by connecting a plurality of black hollow microspheres. In the process of preparing positive electrode materials, when the concentration ratio of PVP to sodium source is too high, a large number of individual PVPs will combine into spherical micelles with a larger radius. The sodium source content is insufficient to react with all the vanadium glycolate spheres to form precursor products. The generated Na3V2(PO4)3 precursor will face problems such as large size, easy to break, and holes. When the concentration ratio of PVP to sodium source is too low, due to the low content of PVP, the diameter of the spherical micelles formed becomes smaller, making the pore size of the generated Na3V2(PO4)3 precursor smaller and prone to agglomeration. Therefore, in the process of preparing positive electrode materials, it is necessary to control the concentration ratio of PVP to sodium source within an appropriate range: 12-16:1.
[0024] Another object of the present invention is to provide a positive electrode plate, which includes a current collector and a positive electrode slurry coated on the current collector; the positive electrode slurry contains the positive electrode material matrix described above.
[0025] The present invention also aims to provide a sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte, wherein the positive electrode sheet is the positive electrode sheet described above; the electrolyte comprises a sodium salt, an organic solvent and a film-forming additive, and the film-forming additive comprises: a first film-forming additive and a second film-forming additive;
[0026] The first film-forming additive is selected from one or two of tris(trimethylsilyl)borate phosphite and tris(trimethylsilyl)borate phosphate.
[0027] The second film-forming additive is selected from one of fluoroethylene carbonate, chloroether 1,2-bis(2-chloroethoxy)ethane, bromooctane, and 3-iodooxetane;
[0028] The pore size A of the positive electrode material matrix in the positive electrode plate and the first film-forming additive content N1 and the second film-forming additive content N2 satisfy the following relationship: 0.35≤(N1+N2) / 100×A≤1;
[0029] Wherein, N1 is the mass fraction of the first film-forming additive in the total amount of the electrolyte; N2 is the mass fraction of the second film-forming additive in the total amount of the electrolyte.
[0030] In some embodiments, the sodium salt includes NaPF6; the organic solvent includes dimethyl carbonate (DMC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC).
[0031] In some embodiments, the first film-forming additive accounts for 0.8-1.6 wt % of the total amount of the electrolyte; the second film-forming additive accounts for 1-2 wt % of the total amount of the electrolyte.
[0032] In the sodium ion battery of the present invention, during the first cycle, the first film-forming additive such as tri(trimethylsilyl)phosphite borate will oxidize and decompose to produce NaSiO3, and the residual alkaline substances on the surface of the positive electrode material Na3V2(PO4)3 matrix will be converted to NaPO3 in situ, thereby forming a first inorganic CEI film layer composed of NaSiO3 and NaPO3 on the surface of the positive electrode material Na3V2(PO4)3 matrix. In addition, the second film-forming additive such as 3-iodooxetane will decompose the produced NaI, and form a second mixed CEI film layer of inorganic and organic uniform mixture on the first inorganic CEI film layer with the sodium alkylate produced by the decomposition of the electrolyte. That is, during the first cycle of the sodium ion battery of the present invention, after the first film-forming additive and the second film-forming additive in the electrolyte are infiltrated and contacted with the positive electrode material, the first inorganic CEI film layer and the second mixed CEI film layer will be formed in sequence on the surface of the positive electrode material Na3V2(PO4)3 matrix.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The sodium ion battery provided by the present invention has a lantern-shaped structure formed by connecting a plurality of hollow spheres made of Na3V2(PO4)3 inside the cathode material matrix, which can shorten the sodium ion transmission path, widen the ion channel, and increase the sodium ion diffusion coefficient on the active material. It can inhibit the volume expansion of the cathode material during the sodium ion embedding process, thereby ensuring the capacity and electrochemical stability of the sodium ion battery.
[0035] Since the positive electrode material Na3V2(PO4)3 matrix inevitably reacts with water and carbon dioxide to generate residual alkaline substances during storage, the positive electrode material Na3V2(PO4)3 matrix in the present invention has a large number of pore structures to expose more specific surface areas. After assembling the battery, the mixed electrolyte and the positive electrode material are more fully infiltrated. During the charge and discharge process, the first film-forming additive tri(trimethylsilyl)phosphite reacts with the residual alkali in situ to generate a hard ion-conducting NaPO3 inorganic substance, thereby reducing the excessive loss of sodium salt and solvent in the electrolyte by the residual alkali in the positive electrode material.
[0036] At the same time, after the electrolyte used in the sodium ion battery of the present invention is infiltrated and contacted with the positive electrode sheet, a first layer of solid inorganic CEI film layer and a second layer of mixed CEI film layer will be sequentially generated on the surface of the positive electrode material Na3V2(PO4)3 matrix. This rigid and flexible double-layer CEI film can not only inhibit the electrolyte from directly contacting the positive electrode material during the charge and discharge process to produce side reactions, but also buffer the volume expansion of the positive electrode material when sodium is embedded, so that the sodium ion battery has good cycle stability and rate performance. This double-layer CEI film structure has good ion conductivity and mechanical properties at the same time, which can reduce the interface resistance and polarization phenomenon generated by the contact between the electrolyte and the positive electrode. DETAILED DESCRIPTION
[0037] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.
[0038] The preparation method of the positive electrode material matrix provided by the present invention is as follows:
[0039] Step S1, dispersing polyvinyl pyrrolidone in ethylene glycol to obtain a first uniform mixture;
[0040] Step S2, adding sodium acetate, vanadium acetylacetonate, and ammonium dihydrogen phosphate to the first mixture in a stoichiometric ratio of 3:2:3, stirring at T1 of 15°C-30°C for a reaction time of t1 of 8-12 hours, placing the second mixture after the reaction in a high-pressure reactor, heating the reaction at T2 of 160-200°C for a reaction time of t2 of 14-18 hours, washing and drying the product after the reaction, and obtaining the first intermediate product. The concentration ratio of polyvinyl pyrrolidone to sodium acetate is 12-16:1.
[0041] Step S3, placing the first intermediate product in an air atmosphere, heating it to T3 of 500°C-700°C at a rate of V1 of 4°C-6°C / min, and then keeping it at t3 for 1-3h to remove PVP to obtain a second intermediate product.
[0042] Step S4, placing the second intermediate product in an argon atmosphere, heating it at a rate of V2 of 4℃-6℃ / min to T4 of 900℃-1000℃, and sintering t4 for 10-14h to obtain a black positive electrode material matrix with a lantern-shaped structure composed of multiple hollow spheres made of Na3V2(PO4)3 connected inside.
[0043] The electrolyte used in the sodium ion battery provided by the present invention includes sodium salt, organic solvent and film-forming additive, wherein the film-forming additive includes: a first film-forming additive and a second film-forming additive; the first film-forming additive is selected from one or two of tris(trimethylsilyl) borate phosphite and tris(trimethylsilyl) borate phosphate; the second film-forming additive is selected from one of fluoroethylene carbonate, chloroether 1,2-bis(2-chloroethoxy)ethane, bromooctane and 3-iodooxetane; the sodium salt includes NaPF6; the organic solvent includes at least one of dimethyl carbonate (DMC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC). The first film-forming additive accounts for 0.8-1.6wt% of the total amount of the electrolyte; the second film-forming additive accounts for 1-2wt% of the total amount of the electrolyte.
[0044] Example 1
[0045] 1. Preparation of Na3V2(P04)3 cathode material
[0046] Disperse polyvinyl pyrrolidone (PVP) into 70 ml of ethylene glycol solvent and stir evenly to obtain a first mixed solution with a (PVP) concentration of 0.6 mol / L. Add sodium acetate, vanadium acetylacetonate, and ammonium dihydrogen phosphate to the first mixed solution in a stoichiometric ratio of 3:2:3 to obtain a second mixed solution, wherein the concentration ratio of PVP to sodium acetate is 15:1. The second mixed solution is reacted for 10 hours under stirring conditions of T1 at 25°C to obtain a third mixed solution. The third mixed solution is placed in a 100 ml high-pressure reactor and heated to react for 16 hours under high temperature conditions of T2 at 180°C to obtain a first intermediate product. The first intermediate product is centrifuged and washed with deionized water three times and with 95% ethanol once; after washing, it is placed in a 60°C temperature environment for drying. The dried first intermediate product was placed in a tubular furnace, heated to T3 = 600°C at a rate of V1 = 5°C / min under air atmosphere, and then kept warm for t3 = 2h to remove the PVP template; then argon atmosphere was introduced into the tubular furnace, heated to T4 = 950°C at a rate of V2 = 5°C / min, and kept warm for t4 = 12h to obtain a black lantern-shaped Na3V2(PO4)3 positive electrode material composed of multiple hollow spheres.
[0047] 2. Preparation of electrolyte
[0048] 0.8% by mass of the first film-forming additive: tris(trimethylsilyl)borate phosphite and 1.2% by mass of the second film-forming additive: 3-iodooxetane were added to an electrolyte in which the organic solvent was dimethyl carbonate (DMC), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) and the concentration of sodium salt NaPF6 was 1 mol / L to obtain the electrolyte of this embodiment 1.
[0049] 3. Preparation of positive electrode sheet
[0050] The lantern-shaped Na3V2(PO4)3 cathode material, acetylene black and polyvinylidene fluoride (PVDF) were placed in a 5 ml small jar at a mass ratio of 7:2:1 and 5% of the total mass of NMP solvent was added for mixing; the cathode slurry was obtained by ball milling at a speed of 300 rpm for 2 hours in a ball mill; the cathode slurry was coated on an aluminum foil, and the aluminum foil was dried under vacuum at 120°C for 12 hours; the dried aluminum foil was punched into discs with a diameter of 14 mm and an average load density of 1.0 mg cm -2 , and obtain the positive electrode sheet of this embodiment 1.
[0051] 4. Preparation of negative electrode sheet
[0052] Commercial graphite as negative electrode material, acetylene black and polyvinylidene fluoride (PVDF) were placed in a 5 ml small jar at a mass ratio of 8:1:1 and 5% of the total mass of NMP solvent was added for mixing; the positive electrode slurry was obtained by ball milling at a speed of 300 rpm for 2 hours in a ball mill; the positive electrode slurry was coated on aluminum foil, and the copper foil was placed under vacuum at 80°C for 12 hours; the dried electrode was punched into discs with a diameter of 16 mm, and the average load density was 2.0 mg cm -2 , and obtain the positive electrode sheet of this embodiment 1.
[0053] 5. Preparation of sodium-ion batteries
[0054] The positive electrode sheet, the separator, and the negative electrode sheet were stacked in order, 80 ul of electrolyte was added, and a button-type half-cell was assembled to obtain the sodium ion battery of this Example 1.
[0055] Examples 2 to 16
[0056] The steps of Example 1 were repeated according to the parameters PVP concentration, N1 and N2 specified in Examples 2 to 16 in Table 1. That is, the difference between Examples 2-16 and Example 1 is that the PVP concentration, the mass content N1 of the first film-forming additive, and the mass content N2 of the second film-forming additive are different, as shown in Table 1.
[0057] Table 1 shows some process parameters for preparing sodium ion batteries in Examples 1 to 16.
[0058]
[0059]
[0060] The preparation method of the positive electrode material provided by the present invention, in the specific embodiment, the following process conditions such as reaction temperature, reaction time, heating rate, sintering temperature, and sintering time are within the corresponding value range. T1 is within the range of 15°C-30°C; T2 is within the range of 160-200°C; T3 is within the range of 500°C-700°C; T4 is within the range of 900°C-100°C; V1 is within the range of 4°C-6°C / min; V2 is within the range of 4°C-6°C / min. t1 is within the range of 8-12 hours; t2 is within the range of 14-18h; t3 is within the range of 1-3h; t4 is within the range of 10-14h. The concentration ratio of polyvinyl pyrrolidone to sodium acetate can be set to 12:1, 13:1, 14:1, 15:1 or 16:1, specifically, as long as it is within the range of 12-16:1.
[0061] The first film-forming additive used in the electrolyte of the present invention may be tris(trimethylsilyl)borate of phosphite, tris(trimethylsilyl)borate of phosphite and tris(trimethylsilyl)borate of phosphate, or tris(trimethylsilyl)borate of phosphate. The second film-forming additive used in the electrolyte of the present invention may be one of fluoroethylene carbonate, chloroether 1,2-bis(2-chloroethoxy)ethane, and bromooctane, in addition to 3-iodooxetane.
[0062] In the above embodiments of the present invention, the negative electrode active material of the prepared negative electrode sheet of the sodium ion battery includes at least one of carbon material, sulfide, oxide, metal element, and alloy material. The negative electrode active material is a carbon-based material.
[0063] Comparative Examples 1 to 12
[0064] The steps of Example 1 were repeated according to the parameters PVP concentration, N1 and N2 specified in Comparative Examples 1 to 12 in Table 1. That is, the difference between Comparative Examples 1-12 and Example 1 is that the PVP concentration, the mass content N1 of the first film-forming additive, and the mass content N2 of the second film-forming additive are different, as shown in Table 1.
[0065] Comparative Example 11 uses commercially available irregularly shaped sodium vanadium phosphate as the positive electrode active material, and the preparation of its positive electrode pole piece is the same as the process of Example 14, and the electrolyte formula of Example 14 is used when assembling the battery; Comparative Example 12 uses the sodium vanadium phosphate in Example 14 as the positive electrode active material, and the preparation of its positive electrode pole piece is the same as the process of Example 14, and 1 mol / L NaPF6 (DMC / EC / EMC) reference electrolyte formula is used when assembling the battery.
[0066] Experimental method for performance testing:
[0067] The sodium ion batteries prepared in Examples 1-16 and Comparative Examples 1-12 were subjected to the following performance tests. The test results are shown in Table 2.
[0068] (1) Aperture test method
[0069] Through the gas adsorption method, which uses nitrogen as the adsorbent, the adsorption amount of nitrogen by porous sodium vanadium phosphate at different relative pressures is measured at liquid nitrogen temperature. The data is analyzed and processed by the BET equation and the Kelvin equation to obtain the specific surface area and pore size distribution of the material.
[0070] (2) Test on the proportion of inorganic components in CEI membrane
[0071] The half-cell was disassembled after 600 cycles, and the positive electrode was cleaned in dimethyl carbonate (DMC) solvent for 20 minutes to remove the residual electrolyte. The electrode was then cut into a size of 0.5cm*0.5cm and placed in an X-ray photoelectron spectrometer. X-rays were irradiated to the sample surface and reacted with sodium vanadium phosphate. The proportion of organic and inorganic components in the second layer CEI of sodium vanadium phosphate was calculated based on the peak area of the obtained photoelectron spectrum.
[0072] (3) Gram capacity test
[0073] The assembled button-type full battery was first charged to 4.1V at a rate of 1C on a blue battery tester, and then charged to 2.5V at a rate of 1C, and this cycle was repeated for 600 cycles.
[0074] (4) Cyclic performance test
[0075] The assembled button-type full battery was first charged to 4.1V at a rate of 1C on a blue battery tester, and then charged to 2.5V at a rate of 1C, and this cycle was repeated for 600 cycles.
[0076] Table 2: Performance test data results of sodium ion batteries prepared in Examples and Comparative Examples
[0077]
[0078]
[0079] Result analysis:
[0080] It can be seen from the above Tables 1-2 that compared with Comparative Examples 1-2, Example 1 does not contain the first film-forming additive in Comparative Example 1, and does not contain the second film-forming additive in Comparative Example 2, while the pore size A of the positive electrode active material is within the pore size range of the lantern-shaped Na3V2(PO4)3 positive electrode material prepared by the present invention, and the capacity retention rate of the prepared sodium ion half-cell is still poor. This shows that the electrolyte contains the first film-forming additive or the second film-forming additive alone, which cannot play a synergistic role, and the double-layer CEI film cannot be formed on the surface of the positive electrode plate when the sodium ion battery is cycled, resulting in poor cycle performance of the sodium ion battery.
[0081] Compared with Comparative Examples 3-4, Example 1 shows that the content of the first film-forming additive N1 in Comparative Example 3 is lower than 0.8%, and the sodium ion battery has poor cycle performance. This is because the residual alkali on the surface of the positive electrode plate has not reacted completely, and will have a side reaction with the electrolyte solvent. At the same time, the first layer of inorganic phase CEI film generated on its surface is not complete and not strong enough, resulting in a decrease in the stability of the sodium ion battery. In Comparative Example 4, the content of the first additive N1 is higher than 1.6%, and the sodium ion battery has poor cycle performance, indicating that there are too many inorganic phase substances in the first layer of CEI film formed on the surface of the positive electrode, the thickness is increased, and the flexibility is greatly reduced, causing the CEI film to be easily broken, thereby reducing the cycle performance of the sodium ion battery.
[0082] Comparison of Comparative Example 1 with Comparative Examples 5-6 shows that although N1, N2, and A satisfy the relationship 0<(N1+N2) / (100×A)<1, when the mass content of the second film-forming additive N2 is higher than 2%, it means that the content of the second film-forming additive is high, and there are more inorganic phase substances in the second CEI film, and its flexibility can be reduced, so that the sodium ions expand in volume when returning to the positive electrode, causing the CEI to fall off directly, and the cycle performance is reduced. When the mass content of the second film-forming additive N2 is lower than 1%, the second CEI film with both rigidity and flexibility cannot be formed at the interface of the positive electrode sheet, and the expansion of the positive electrode sheet cannot be alleviated, thereby reducing the cycle performance of the sodium ion battery.
[0083] Compared with Comparative Examples 7-8, when the pore size A of the positive active material is too high (pore size A is 0.1um in Comparative Example 7), the material will expose a large amount of specific surface area to direct contact with the electrolyte, and the solvent of the electrolyte will participate in the side reaction, resulting in more active sodium ions being lost, leading to an increase in the side reactions of the sodium ion battery and an increase in the battery impedance, thereby reducing the cycle performance of the sodium ion battery. When the pore size A of the positive active material is too small (pore size A of Comparative Example 8 is 0.02um), it is more difficult for the electrolyte to diffuse into the electrode, which will inhibit the infiltration process of the electrolyte on the electrode, and the sodium ion transmission path will become longer and the speed will become slower; at the same time, the smaller pore size will limit the escape of sodium ions, thereby reducing the cycle performance of the sodium ion battery.
[0084] Compared with Example 1 and Comparative Examples 9-10, although N1, N2, and A in Comparative Examples 9 and 10 are within the condition range, they do not satisfy the relationship 0.35<(N1+N2) / (100×A)<1, and the battery cycle performance is poor, indicating that the individual values of N1, N2, and A must not only satisfy the conditions, but also satisfy the relationship 0.35<(N1+N2) / (100×A)<1. Only when all the above conditions are met can the first additive consume the residual alkali on the surface of the positive electrode active material and generate a dense and stable The second additive then generates a flexible second phase CEI dominated by an inorganic phase, which improves the ion transport conductivity and flexibility, reduces the decomposition of the electrolyte, and alleviates the volume expansion of the positive electrode material. At the same time, the pore size of the positive electrode active material is limited, so that the electrolyte infiltration is more sufficient and the ion transmission distance is shorter. In addition, the first additive and the second additive work together to generate a rigid and flexible passivation film of appropriate thickness on the surface of the positive electrode particles, thereby improving the battery cycle performance.
[0085] Compared with Example 1 and Comparative Examples 11-12, since Example 11 uses commercial irregular sodium vanadium phosphate as the positive electrode active material, its surface has no porous structure, resulting in poor electrolyte infiltration effect, slow diffusion of sodium ions inside the material, and a certain volume expansion of the active material, resulting in poor battery performance. Comparative Example 12 uses a 1 mol / L NaPF6 (DMC / EC / EMC) reference electrolyte formula. After the cycle, the solvent of the electrolyte is excessively decomposed to form a large amount of loose, porous, and overly thick organic phase CEI, which cannot inhibit the dissolution of metal ions and has poor ion conductivity, ultimately resulting in poor battery performance.
[0086] According to the data comparison of Examples 1-16, it is obtained that only under the premise of satisfying the relationship 0.35<(N1+N2) / (100×A)<1, and the mass content N1 of the first film-forming additive is in the small range of 1.0-1.4%, the mass content N2 of the second film-forming additive is in the small range of 1.2-1.8%, and the positive electrode surface pore size A is in the small range of 0.03-0.07μm, under these conditions, the residual alkali on the surface of the positive electrode active material can be consumed and a suitable amount of solid first inorganic CEI film with uniform thickness can be formed, and the second film-forming additive will form a tough second mixed CEI film layer with an inorganic component accounting for 35-68% on the first inorganic CEI film. This multilayer CEI film structure has good flexibility and mechanical properties, so that the discharge capacity of the sodium ion battery and the room temperature cycle capacity retention rate are relatively high.
[0087] In summary, the sodium ion battery provided by the present invention can shorten the sodium ion transmission path, widen the ion channel, and improve the sodium ion diffusion coefficient on the active material because the Na3V2(PO4)3 positive electrode material is a lantern-shaped structure formed by connecting hollow spheres with multiple holes. The volume expansion of the positive electrode material can be suppressed during the embedding process of sodium ions, ensuring the gram capacity and electrochemical stability of the sodium ion battery. At the same time, the porous structure of the Na3V2(PO4)3 positive electrode material makes it easier for the electrolyte to fully infiltrate and contact the positive electrode material to form a CEI film. The electrolyte used in the sodium ion battery of the present invention is NaSiO3 produced by the oxidation and decomposition of tri(trimethylsilyl)borate phosphite during the first cycle; tri(trimethylsilyl)borate phosphite converts the residual alkaline substances on the surface of the positive electrode material Na3V2(PO4)3 matrix to generate NaPO3 in situ, thereby forming a first inorganic CEI film layer composed of NaSiO3 and NaPO3 on the surface of the Na3V2(PO4)3 matrix; the NaI produced by the decomposition of 3-iodooxetane and the sodium alkylated produced by the decomposition of the electrolyte form a second mixed CEI film layer of inorganic and organic uniform mixture on the first inorganic CEI film layer. This double-layer CEI film can inhibit the side reaction caused by the contact between the electrolyte and the positive electrode material, stabilize the structure of the positive electrode material, and make the sodium ion battery have good cycle stability and rate performance; reduce the side reaction between the residual alkali in the positive electrode material and the electrolyte. This double-layer CEI film structure has good ion conductivity and mechanical properties at the same time, and can reduce the interface resistance and polarization phenomenon caused by the contact between the electrolyte and the positive electrode.
[0088] Those skilled in the art may combine and associate different embodiments or examples and features of different embodiments or examples described in this specification without mutual contradiction.
[0089] The above description is only a partial or preferred embodiment of the present invention, and the text thereof cannot limit the scope of protection of the present invention. All equivalent structural transformations made using the contents of the present invention specification under the concept of an overall concept of the present invention, or direct / indirect application in other related technical fields are included in the scope of protection of the present invention.
Claims
1. A positive electrode material matrix, characterized in that: The interior of the positive electrode material matrix is a lantern-shaped structure formed by connecting multiple hollow spheres made of Na3V2(PO4)3.
2. The positive electrode material matrix according to claim 1, characterized in that: The value range of the pore diameter A of the hollow sphere is: 0.03um≤A≤0.08um.
3. A method for preparing a positive electrode material matrix, characterized in that: The following steps are involved: Step S1, dispersing polyvinyl pyrrolidone in ethylene glycol to obtain a first mixture that is uniformly mixed; Step S2, adding a sodium source, a vanadium source, and a phosphorus source to the first mixture, reacting at 15° C.-30° C. with stirring for 8-12 hours, then placing the second mixture after the reaction in a high-pressure reactor, heating and reacting at 160-200° C. for 14-18 hours to obtain a first intermediate product; Step S3, placing the first intermediate product in an air atmosphere and sintering at a high temperature of 500° C. to 700° C. to remove PVP, thereby obtaining a second intermediate product; Step S4, placing the second intermediate product in an argon atmosphere and sintering at a high temperature of 900°C-100°C to obtain a black Na3V2(PO4)3 positive electrode material matrix with a lantern-shaped structure formed by connecting a plurality of hollow spheres.
4. The method for preparing the positive electrode material matrix according to claim 3, characterized in that: The stoichiometric ratio of the sodium source, the vanadium source and the phosphorus source is 1.5-3:1-2:3; The concentration ratio of polyvinyl pyrrolidone to sodium acetate is 12-16:1; The sodium source is selected from at least one of sodium nitrate, sodium acetate and Na2CO3; The vanadium source is selected from at least one of vanadium pentoxide, vanadium acetylacetonate, and sodium metavanadate; The phosphorus source is selected from at least one of phosphoric acid and diammonium phosphate.
5. The method for preparing the positive electrode material matrix according to claim 3, characterized in that: The concentration of polyvinyl pyrrolidone in step S1 is 0.5-1.0 mol / L; The step S3 specifically comprises: placing the first intermediate product in an air atmosphere, heating the temperature to 500°C-700°C at a rate of 4°C-6°C / min, and then keeping the temperature for 1-3 hours to remove PVP, thereby obtaining a second intermediate product; The step S4 is specifically as follows: placing the second intermediate product in an argon atmosphere, heating it to 900°C-100°C at a rate of 4°C-6°C / min, and sintering it for 10-14h to obtain a black Na3V2(PO4)3 positive electrode material with a lantern-shaped structure formed by connecting multiple hollow spheres.
6. The method for preparing a cathode material matrix according to any one of claims 3 to 5, characterized in that: In the step S2, after placing the second mixture after the reaction in a high pressure reactor and heating the reaction at 160-200° C. for 14-18 hours, the step further comprises: The product after the reaction is washed and dried to obtain the first intermediate product.
7. A positive electrode sheet, characterized in that: The positive electrode plate comprises a current collector and a positive electrode slurry coated on the current collector; the positive electrode slurry comprises the positive electrode material matrix according to claim 1 or 2.
8. A sodium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator between the positive electrode sheet and the negative electrode sheet, and an electrolyte, characterized in that: The positive electrode sheet is the positive electrode sheet according to claim 7; the electrolyte comprises a sodium salt, an organic solvent and a film-forming additive, and the film-forming additive comprises: a first film-forming additive and a second film-forming additive; The first film-forming additive is selected from one or two of tris(trimethylsilyl)borate phosphite and tris(trimethylsilyl)borate phosphate; The second film-forming additive is selected from one of fluoroethylene carbonate, chloroether 1,2-bis(2-chloroethoxy)ethane, bromooctane, and 3-iodooxetane; The pore size A of the positive electrode material matrix in the positive electrode plate and the first film-forming additive content N1 and the second film-forming additive content N2 satisfy the following relationship: 0.35≤(N1+N2) / 100×A≤1; Wherein, N1 is the mass fraction of the first film-forming additive in the total amount of the electrolyte; N2 is the mass fraction of the second film-forming additive in the total amount of the electrolyte.
9. The sodium ion battery according to claim 8, characterized in that: The sodium salt includes NaPF6; the organic solvent includes dimethyl carbonate (DMC), ethylene carbonate (EC), and ethyl methyl carbonate (EMC).
10. The sodium ion battery according to claim 8 or 9, characterized in that: The first film-forming additive accounts for 0.8-1.6 wt % of the total amount of the electrolyte; the second film-forming additive accounts for 1-2 wt % of the total amount of the electrolyte.