Lithium metal negative electrode material, negative electrode plate, lithium metal secondary battery, electric device, preparation method and application
By coating the surface of the lithium metal anode with a dense and uniform polymer layer, the cycle life decay and lithium dendrite short circuit problems of lithium metal secondary batteries are solved, achieving high-efficiency charge-discharge cycle stability and safety of the battery.
Patent Information
- Application Number
- CN202310477613.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-28
AI Technical Summary
Existing lithium metal secondary batteries suffer from problems such as rapid degradation of cycle life and short circuits and safety risks caused by lithium dendrites.
A dense and uniform polymer layer is used to coat the lithium metal anode. The polymer layer contains fluorinated aliphatic chains and flexible EO blocks, which are tightly bonded to the lithium metal through chemical connection. This inhibits the contact reaction between the electrolyte and the lithium metal, promotes uniform lithium ion deposition, suppresses the formation of lithium dendrites, and adapts to the volume expansion on the anode side.
It extends battery cycle life, reduces electrolyte and lithium metal consumption, improves lithium-ion transfer efficiency, reduces interfacial polarization and interfacial impedance, and enhances battery energy density and safety performance.
Smart Images

Figure CN118867147A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of lithium metal secondary batteries, and in particular to lithium metal negative electrode materials, negative electrode sheets, lithium metal secondary batteries, electrical devices, preparation methods and applications. Background Art
[0002] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.
[0003] With the development of various electronic products such as smart phones, tablets, smart wearables, power tools and electric vehicles, lithium metal secondary batteries with high energy density are becoming more and more popular, and high energy density is an irreversible trend in the development of lithium metal secondary batteries in the future.
[0004] However, lithium metal secondary batteries currently on the market often have problems with rapid decay of cycle life and very serious lithium dendrite-induced short circuits and safety risks. Summary of the invention
[0005] In view of the above problems, the present application provides a lithium metal negative electrode material, a negative electrode sheet, a lithium metal secondary battery, an electrical device, a preparation method and an application. The lithium metal negative electrode material comprises a dense and uniform polymer layer firmly bonded to the lithium metal, the polymer layer has certain elasticity, flexibility and swelling properties, the polymer component in the polymer layer contains a fluorinated aliphatic chain and a flexible side chain, the polymer layer can effectively inhibit the contact reaction between the electrolyte and lithium, reduce the consumption of the electrolyte and lithium metal, extend the battery cycle life, and also inhibit the problem of lithium dendrites.
[0006] In the first aspect, the present application provides a lithium metal negative electrode material, which includes a lithium-containing metal and a polymer Poly bonded to the lithium metal in the lithium-containing metal, the polymer Poly having a linear carbon chain and a first side chain and a second side chain grafted to the side group of the linear carbon chain, the first side chain containing a fluorinated aliphatic chain Rf, the second side chain containing an EO block, and the structure of the EO block is *-(CH2CH2O) z -, z is a positive integer, and * represents a connection site pointing to the linear carbon chain.
[0007] The lithium metal negative electrode material provided in the present application has a dense and uniform polymer layer coated on the surface of the lithium-containing metal. The polymer layer can play the role of a protective layer at the negative electrode of the lithium metal secondary battery, effectively inhibit the contact reaction between the electrolyte and the lithium metal, reduce the consumption of the electrolyte and the lithium metal, and extend the battery cycle life; the linear carbon chain can give the polymer Poly and the polymer layer a certain flexibility; the polymer component Poly in the polymer layer has a stable chemical connection with the lithium-containing metal, so that the polymer layer is firmly bonded to the lithium-containing metal surface, and when the volume of the negative electrode side changes during the charge and discharge process, the polymer layer can be prevented from peeling off from the lithium-containing metal surface; the polymer Poly contains a fluorinated aliphatic chain Rf. On the one hand, the introduction of fluorine element can regulate the lithium ion Deposition, promote uniform deposition of lithium ions, improve the deposition morphology of lithium dendrites in lithium metal secondary batteries, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the negative electrode side of lithium metal. On the other hand, the presence of the fluorinated aliphatic chain Rf can give the polymer layer a certain elasticity, which is conducive to better fitting between the polymer layer and the lithium-containing metal and the separator; the polymer Poly also contains a flexible EO block, which can not only improve the flexibility of the polymer layer, enhance the close fit between the protective layer and the negative electrode substrate and between the protective layer and the separator side, and reduce the interface impedance, but also enhance the elasticity of the protective layer, so that the protective layer can better adapt to the larger volume expansion of the negative electrode side, thereby reducing or avoiding the rupture of the polymer layer, and then can play a protective role for a longer time. In addition, the dense and uniform polymer layer can also be swollen by the electrolyte, and can provide good ionic conductivity after swelling, so that lithium ions can be efficiently transferred in the polymer layer and at the lithium metal interface, the interface polarization caused by the introduction of the polymer layer is small, and the battery has good charge and discharge cycle stability. The above-mentioned characteristics of the polymer layer cooperate with each other to greatly improve the cycle life of the lithium metal secondary battery and suppress the lithium dendrite problem.
[0008] In some embodiments, in the structure of the polymer Poly, the number of the first side chains is m, and the number of the second side chains is n; wherein m and n are each independently an integer greater than or equal to 8;
[0009] Optionally, m and n are each independently an integer selected from 8-600.
[0010] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0011] The ratio of m to n satisfies 0.5≤m / n≤8, optionally, 1≤m / n≤5, further optionally, 1≤m / n≤3;
[0012] m is an integer selected from 50 to 250, optionally, m is an integer selected from 50 to 200;
[0013] n is an integer selected from 25 to 200, and optionally, n is an integer selected from 40 to 150.
[0014] The introduction of the second side chain containing the EO block can improve the flexibility and swelling rate of the polymer layer, and the presence of the first side chain containing the fluorinated aliphatic chain Rf is conducive to improving the elasticity of the polymer layer. Further, by controlling the number of the two copolymer units in the polymer Poly, the flexibility and elasticity of the polymer layer can be regulated at the same time, thereby regulating the elastic deformation of the polymer layer, and regulating the degree of fit between the polymer layer and the substrate and between the polymer layer and the isolation membrane; larger elastic deformation is conducive to better adapting to the larger volume expansion of the negative electrode side during charging, which can reduce or avoid the rupture of the protective layer and thus achieve a longer protective effect; better flexibility is conducive to the close fit between the polymer layer and the lithium metal and between the polymer layer and the isolation membrane, reducing the interface impedance, and is conducive to improving the energy density and power density of the battery.
[0015] By controlling the ratio of m / n, the elasticity, swelling rate and ionic conductivity of the polymer can be optimized. Through the comprehensive regulation of the polymer elasticity, swelling rate and ionic conductivity, the polymer protective layer on the negative electrode side can better and more permanently play the role of isolating the electrolyte contact and regulating lithium deposition.
[0016] In some embodiments, z is an integer selected from 2 to 10;
[0017] Optionally, z is an integer selected from 3-7.
[0018] By adjusting the size of z, that is, by adjusting the length of the EO block, the flexibility of the polymer layer can be adjusted.
[0019] In some embodiments, the polymer Poly comprises a repeating unit of the structure shown in formula (U1) and a repeating unit of the structure shown in formula (U2):
[0020]
[0021] in,
[0022] X1 and X2 are each independently H or an electron withdrawing group;
[0023] Y1 and Y2 are each independently a cyano group or a linking group formed by a cyano group bonded to the lithium metal in the lithium-containing metal;
[0024] A1 and A2 are each independently O, S or NR 11 ; Among them, R 11 H or C 1-3 alkyl;
[0025] Rd is a hydrocarbon group or a hydrocarbon group substituted by Q1, Q1 is selected from the following substituents: cyano, -C(=O)NH2, -OC(=O)NHR 6 and -S(=O)2F,R 6 H or C 1-6 alkyl;
[0026] Optionally, at least one of Y1 and Y2 is a linking group formed by a cyano group bonded to the lithium metal in the lithium-containing metal.
[0027] In some embodiments, in the structure of the polymer Poly, each occurrence of X1 and X2 is independently H or cyano, nitro or -NR 21 R 22 ; Among them, R 21 and R 22 Each independently is H or C 1-3 alkyl;
[0028] Optionally, R 21 and R 22 are each independently H or methyl;
[0029] Further optionally, R 21 and R 22 All are methyl.
[0030] In some embodiments, in the structure of the polymer Poly, each occurrence of A1 and A2 is independently O, S or NH;
[0031] Optionally, each occurrence of A1 and A2 is independently O or NH.
[0032] In some embodiments, Rd is C 1-4 Hydrocarbon;
[0033] Optionally, Rd is C 1-4 alkyl;
[0034] Further optionally, Rd is C 1-3 alkyl;
[0035] In a further alternative, Rd is methyl.
[0036] The polymer Poly may be a copolymer comprising a repeating unit of the structure shown in formula (U1) and a repeating unit of the structure shown in formula (U2). The aforementioned polymer Poly may form a chemical bond with metallic lithium through a large number of cyano groups located on the side groups of the main chain, thereby achieving a stable chemical connection between the polymer layer and the lithium-containing metal, and further forming a covalent bond.
[0037] An electron-withdrawing group can be introduced into at least one of X1 and X2 in the polymer Poly, which is beneficial to increase the reactivity of the carbon-carbon double bond in the cyanoacrylate derivative monomer (such as cyanoacrylic acid derivative monomer) during the formation of the polymer layer, promote the in-situ polymerization reaction, and facilitate the polymer layer to achieve a tighter and more uniform coating on the lithium-containing metal surface.
[0038] In addition, the fluorinated aliphatic chain Rf and the EO block can be independently grafted onto the linear carbon chain via ester bonds, amide bonds or thioester bonds, thereby flexibly selecting the corresponding polymerization monomers.
[0039] Functional substituents can also be introduced at the end of the EO block to better optimize the performance of the polymer layer and the lithium metal secondary battery as needed. For example, the introduction of a cyano group can further enhance the chemical bonding between the polymer Poly and the lithium metal; the introduction of a fluorosulfonyl group (-S(=O)2F) can induce uniform deposition of lithium ions; the introduction of an amide group (-C(=O)NH2) can enhance the elastic modulus of the protective layer; the introduction of a carbamate group (-OC(=O)-NHR 6 , where R 6 It can be H or alkyl), and the elasticity of the material can be improved by matching the soft and hard segments.
[0040] In some embodiments, the structure of the polymer Poly comprises m repeating units represented by formula (U1) and n repeating units represented by formula (U2); the definitions of m and n are consistent with those described above;
[0041] Optionally, m repeating units represented by formula (U1) and n repeating units represented by formula (U2) are arranged linearly;
[0042] Further optionally, the polymer Poly has a general structure as shown below:
[0043]
[0044] The first side chains can all be introduced via formula (U1), and the second side chains can all be introduced via formula (U2).
[0045] Furthermore, formula (U1) and formula (U2) can jointly participate in the formation of a linear carbon chain in the polymer Poly.
[0046] In formula (P1), m+n is numerically equal to the degree of polymerization of the polymer Poly. By controlling m+n, the molecular weight of the polymer Poly can be regulated.
[0047] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0048] The fluorine substitution rate in any Rf is independently ≥ 50%;
[0049] The number of fluorine atoms in any Rf is independently ≥ 4;
[0050] The mass percentage of fluorine element in the polymer Poly is 15% to 44%.
[0051] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0052] The fluorine substitution rate in any Rf is independently ≥55%;
[0053] The number of fluorine atoms in any Rf is independently ≥ 5, and optionally, the number of fluorine atoms in any Rf is independently 5 to 15;
[0054] The mass proportion of fluorine element in the polymer Poly is 15% to 41%, and optionally 20% to 41%.
[0055] By controlling the fluorine substitution rate in Rf, by controlling the number of fluorine atoms in Rf, and by controlling the mass proportion of fluorine element in the polymer Poly in one or more ways, it is possible to better promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, increase the cycle life of lithium ions and reduce the risk of short circuits, and alleviate the volume expansion of the lithium metal negative electrode side. In addition, it can also be beneficial to the application of the polymer layer in lithium metal secondary batteries that perform charge and discharge cycles at a high current density.
[0056] Taking controlling the mass proportion of fluorine in the polymer Poly as an example, it is beneficial to improve the deposition morphology of lithium dendrites in lithium metal batteries and alleviate the volume expansion of lithium metal negative electrodes, which is beneficial to the application of polymer layers in lithium metal secondary batteries that perform charge and discharge cycles at high current density.
[0057] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0058] Each Rf independently contains 2 to 10 main chain carbon atoms;
[0059] The number of carbon atoms in any one Rf is independently an integer selected from 2 to 10.
[0060] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0061] Any Rf independently contains 2 to 8 main chain carbon atoms, optionally, any Rf independently contains 3 to 8 main chain carbon atoms;
[0062] The number of carbon atoms in any Rf is independently an integer selected from 2 to 8. Alternatively, the number of carbon atoms in any Rf is independently an integer selected from 3 to 8.
[0063] The length of the Rf side chain can be adjusted by controlling the number of carbon atoms in Rf, thereby giving the polymer layer appropriate elasticity and preferably inhibiting the polymer layer from rupturing under large volume deformation.
[0064] In some embodiments, in the structure of the polymer Poly, one, more or all Rf independently contain one or more heteroatoms selected from the group consisting of iodine, nitrogen, oxygen, sulfur, silicon, boron and phosphorus;
[0065] Optionally, the number of heteroatoms in any one, more or all Rf is independently 1 or more;
[0066] Further optionally, the number of the heteroatoms in any one, multiple or all Rf is selected from 1 or 2-6.
[0067] In some embodiments, in the structure of the polymer Poly, one, more or all Rf satisfy one or more of the following characteristics:
[0068] The number of oxygen atoms in one, more than one or all Rf is 1, 2, 3, 4 or 5;
[0069] The number of nitrogen atoms in one, more than one or all Rf is 1, 2 or 3;
[0070] The number of sulfur atoms in one, more than one or all Rf is 1, 2 or 3;
[0071] The number of phosphorus atoms in one, more than one or all Rf is 1 or 2;
[0072] The number of iodine atoms in one, more or all Rf is 1, 2, 3, 4, 5 or 6;
[0073] The number of silicon atoms in one, more than one or all of Rf is 1 or 2; and
[0074] The number of boron atoms in one, more than one or all of Rf is 1 or 2.
[0075] In some embodiments, in the structure of the polymer Poly, one, more or all of the Rf contain one or more selected from iodine, -NR 12 -, -O-, -S-, -S(O)2-, >Si<, >B- and >P(=O)-, wherein R 12 H or C 1-3 alkyl;
[0076] Optionally, R12 is H or methyl;
[0077] Further optionally, R 12 For H.
[0078] In some embodiments, in the structure of the polymer Poly, one, more or all Rf contain one or more atoms or atomic groups selected from the group consisting of -O-, -S(O)2- and -(O=)P(O-)2;
[0079] Optionally, one, more or all of Rf contain one or more -O-;
[0080] Optionally, one, more or all of Rf contain -S(O)2F;
[0081] Optionally, one, more than one or all of Rf contain -(O=)P(O-)2.
[0082] By introducing other heteroatoms other than fluorine atoms into Rf, such as one or more heteroatoms of iodine, nitrogen, oxygen, sulfur, silicon, boron, phosphorus, etc., special properties can be given to the polymer layer. For example, phosphorus has a certain flame retardant effect. For another example, iodine can also play a certain role in regulating the deposition of lithium ions. For another example, fluorosulfonyl (-S(=O)2F) has a certain effect on improving the ionic conductivity of the polymer layer and promoting the uniform deposition of lithium ions.
[0083] In some embodiments, in the structure of the polymer Poly, any Rf is independently a linear structure or a branched structure.
[0084] The linear Rf is beneficial to improving the elasticity of the polymer material, while the side chain Rf is beneficial to improving the swelling capacity of the electrolyte membrane, thereby improving the ionic conductivity.
[0085] In some embodiments, in the structure of the polymer Poly, any Rf is independently a saturated structure or an unsaturated structure.
[0086] When the fluorine-substituted aliphatic chain has a saturated structure, it can give the polymer Poly molecular chain a higher mobility, which is beneficial for improving the elasticity regulation of the polymer layer. In addition, by introducing unsaturated bonds in Rf, the polymer layer can be cross-linked to enhance the elastic modulus of the polymer protective layer.
[0087] In some embodiments, in the structure of the polymer Poly, the structure of any Rf is independently represented by formula (III-1), formula (III-2) or formula (III-3):
[0088]
[0089] in,
[0090] In formula (III-1), m3 is an integer selected from 2 to 10; R 31 , R 32 and R 3 Each occurrence is independently H or F; the structure represented by formula (III-1) contains at least 4 F atoms;
[0091] In formula (III-2), m 4a and m 4b Each independently represents an integer selected from 1 to 9; R 41a , R 42a , R 4a , R 41b , R 42b and R 4b Each occurrence is independently H or F; the structure represented by formula (III-2) contains at least 4 F atoms;
[0092] In formula (III-3), m5 is an integer selected from 2 to 10; R 51 and R 52 Each occurrence is independently H or F; the structure represented by formula (III-3) contains at least 4 F atoms.
[0093] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0094] m3 is an integer selected from 3 to 10; alternatively, m3 is an integer selected from 3 to 8;
[0095] m 4a and m 4b are each independently an integer selected from 2 to 9; optionally, m 4a and m 4b are each independently an integer selected from 2 to 8; further optionally, m 4a and m 4b are each independently an integer selected from 3 to 8; further optionally, m 4a and m 4b Each independently is an integer selected from 3 to 6
[0096] m5 is an integer selected from 3 to 10; optionally, m5 is an integer selected from 3 to 8.
[0097] In some embodiments, in the structure of the polymer Poly, the structure of Rf is as shown in formula (III-1); or, the structure of Rf is as shown in formula (III-2); or, the structure of Rf is as shown in formula (III-3).
[0098] Among them, the structure of Formula III-1 is a linear saturated fluorinated aliphatic chain. On the one hand, it can give the polymer layer better elasticity, reduce or avoid the rupture of the polymer layer under large volume deformation. On the other hand, it can effectively promote the uniform deposition of lithium ions through the fluorine element, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium metal negative electrode side.
[0099] The structure of formula III-2 can introduce phosphorus elements. In addition, the phosphate group therein has a flame retardant effect, which is beneficial to improving the safety performance of the battery cell.
[0100] The structure of formula III-3 can introduce a fluorosulfonyl group, which has a certain positive effect on improving the ionic conductivity of the polymer layer.
[0101] In some embodiments, in the structure of the polymer Poly, each time formula (III-1) appears, the number of H atoms therein is 0, 1, 2, 3 or 4; each time formula (III-2) appears, the number of H atoms therein is 0, 1, 2, 3, 4, 5 or 6; each time formula (III-3) appears, the number of H atoms therein is 0, 1, 2, 3 or 4;
[0102] Optionally, the number of H atoms in formula (III-1) is 0;
[0103] Optionally, the number of H atoms in formula (III-2) is 0;
[0104] Optionally, the number of H atoms in formula (III-3) is 0.
[0105] By controlling the number of H atoms, the number of sites available for fluorine substitution can be controlled.
[0106] In some embodiments, in the structure of the polymer Poly, any Rf is independently any of the following structures:
[0107]
[0108] In some embodiments, the number average molecular weight of the polymer Poly is selected from 10 kDa to 200 kDa;
[0109] Optionally, the number average molecular weight of the polymer Poly is selected from 40 kDa to 100 kDa;
[0110] Further optionally, the number average molecular weight of the polymer Poly is selected from 50 kDa to 80 kDa.
[0111] By adjusting the degree of polymerization or molecular weight of the polymer Poly, the molecular chain length of the polymer Poly can be adjusted, which can not only achieve effective coating of lithium metal, but also maintain stable chemical connection, and can also affect the density and uniformity of the polymer layer.
[0112] In some embodiments, the lithium-containing metal comprises lithium or a lithium alloy;
[0113] Optionally, the lithium alloy contains lithium element and also contains one or more elements selected from the group consisting of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium.
[0114] In some embodiments, the amount of lithium metal in the lithium-containing metal relative to the polymer Poly is greater than or equal to the catalyst amount, calculated by molar ratio.
[0115] In the lithium metal negative electrode material provided in the present application, the lithium-containing metal only needs to provide a catalytic amount to successfully catalyze the in-situ polymerization reaction of cyano olefin carboxylic acid derivative monomers (such as cyanoacrylic acid derivative monomers) on the surface of the lithium-containing metal. The lithium metal only needs to be in contact with the polymer Poly in a catalytic amount to catalyze the in-situ polymerization reaction of cyano olefin carboxylic acid derivative monomers (such as cyanoacrylic acid derivative monomers) on the surface of the lithium metal.
[0116] In a second aspect, the present application provides a negative electrode plate, which includes a lithium-containing layer and a polymer layer stacked, and the negative electrode plate includes the lithium metal negative electrode material described in the first aspect of the present application;
[0117] The lithium-containing layer includes the lithium-containing metal in the lithium metal negative electrode material, and the polymer layer includes the polymer Poly in the lithium metal negative electrode material.
[0118] The negative electrode plate includes a lithium metal negative electrode material distributed in a lithium-containing layer and a polymer layer. On at least one side of the negative electrode plate, the lithium-containing layer is stably connected to a dense and uniform polymer layer by chemical bonding. The polymer layer has certain elasticity, flexibility and swelling properties, which can make the polymer layer and the lithium-containing layer, and the polymer layer and the isolation membrane fit firmly, tightly and durably. It can better adapt to the larger volume expansion of the negative electrode side during charging, and can play the role of a protective layer at the negative electrode of the lithium metal secondary battery for a long time. The polymer layer can effectively inhibit the contact reaction between the electrolyte and lithium metal, reduce the consumption of the electrolyte and lithium metal, improve the coulombic efficiency, and extend the cycle life. It can also utilize the fluorinated aliphatic chain Rf in the lithium metal negative electrode material to promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium metal negative electrode side. In addition, the elasticity, flexibility and swelling comprehensive performance of the polymer layer not only promote the close fit between the polymer layer and the lithium-containing layer, but also help to exert good ionic conductivity, reduce interface polarization, and reduce interface impedance, so that the lithium metal secondary battery can achieve higher energy density, power density, charge and discharge cycle stability and higher safety performance in the presence of the polymer layer.
[0119] In some embodiments, the lithium-containing layer consists essentially of the lithium-containing metal;
[0120] Optionally, the material of the lithium-containing layer is lithium element;
[0121] Alternatively, the material of the lithium-containing layer is a lithium alloy.
[0122] In some embodiments, the polymer layer further contains a first electrolyte, and the first electrolyte contains a lithium salt and a first electrolyte solvent.
[0123] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:
[0124] The lithium salt includes one or more of lithium hexafluorophosphate, tetrafluoroboric acid, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate and lithium bis(oxalate)borate;
[0125] The first electrolyte solvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, diphenyl carbonate, dibutyl carbonate, butylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, dioxolane, methyl nonafluoro-n-butyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, octafluoropentyl-tetrafluoroethyl ether, 1,2-bis(cyanoethoxy)ethane, diphenyl ether and 18-crown-6.
[0126] In some embodiments, the concentration of the lithium salt in the first electrolyte is selected from 0.2 mol / L to 8 mol / L;
[0127] Optionally, the concentration of the lithium salt in the first electrolyte is selected from 0.5 mol / L to 5 mol / L;
[0128] Further optionally, the concentration of the lithium salt in the first electrolyte is selected from 0.5 mol / L to 2 mol / L.
[0129] The polymer layer of the lithium metal negative electrode material contains an electrolyte (which can be recorded as the first electrolyte). The concentration of lithium salt in the first electrolyte can affect the deposition morphology of lithium ions. The concentration of lithium salt can change the Li +The solvation effect affects the composition of the solid electrolyte interface film (SEI film) and the deposition morphology of lithium ions. By controlling the lithium salt in the electrolyte at a more appropriate concentration, it is more conducive to promoting dense and uniform deposition of lithium ions and reducing the volume expansion of the negative electrode side. In addition, by controlling the lithium salt in the electrolyte at a more appropriate concentration, the polymer layer can also have more suitable mechanical properties, such as flexibility and elasticity, and can also achieve better lithium ion conductivity during charging and discharging. When the lithium salt concentration is too high, the mechanical properties of the polymer layer may deviate from the optimal range. When the lithium salt concentration is too low, the lithium ion conductivity during charging and discharging may deviate from the larger range.
[0130] In some embodiments, the mass proportion of the first electrolyte in the polymer layer is 20% to 80%;
[0131] Optionally, the mass proportion of the first electrolyte in the polymer layer is 30% to 60%;
[0132] Further optionally, the mass proportion of the first electrolyte in the polymer layer is 40% to 60%;
[0133] Further optionally, the mass percentage of the first electrolyte in the polymer layer is 40% to 55%.
[0134] In some embodiments, the mass ratio of the polymer Poly to the first electrolyte is 4:1 to 0.25:1;
[0135] Optionally, the mass ratio of the polymer Poly to the first electrolyte is 3:1 to 0.5:1;
[0136] Further optionally, the mass ratio of the polymer Poly to the first electrolyte is 2.5:1 to 1:1;
[0137] Further optionally, the mass ratio of the polymer Poly to the first electrolyte is 7:3 to 2:1.
[0138] By controlling the mass proportion of the first electrolyte in the polymer layer or controlling the mass ratio of the polymer Poly and the first electrolyte in the polymer layer within a more suitable range, the electrolyte can be adjusted to have a more suitable mass proportion in the polymer layer. The mass proportion of the electrolyte in the polymer layer can affect the elastic modulus and ionic conductivity of the protective layer. In the first electrolyte, the presence of a certain amount of lithium salt and solvent (referred to as the first electrolyte solvent) can plasticize the polymer layer and improve the elasticity of the polymer layer. In addition, in the process of forming a polymer layer by in-situ polymerization, the lithium salt and solvent in the first electrolyte can be incorporated into the polymer layer, so that the polymer layer has a sponge-like loose porous structure on a microscopic scale, and the pores are filled with electrolyte, which can provide a path for the subsequent transmission of lithium ions.
[0139] In some embodiments, based on the first electrolyte, the swelling rate of the polymer layer at 25° C. is 8% to 65%;
[0140] Further optionally, the swelling rate of the polymer layer at 25° C. is 15% to 55%;
[0141] Further optionally, the swelling rate of the polymer layer at 25° C. is 18% to 44%;
[0142] Further optionally, the swelling ratio of the polymer layer at 25° C. is 30% to 40%.
[0143] In some embodiments, based on the first electrolyte, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.001 mS / cm to 5 mS / cm;
[0144] Optionally, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.1 mS / cm to 5 mS / cm;
[0145] Alternatively, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.5 mS / cm to 5 mS / cm;
[0146] Alternatively, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.9 mS / cm to 4.8 mS / cm;
[0147] Alternatively, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.95 mS / cm to 2.6 mS / cm.
[0148] In some embodiments, the thickness of the polymer layer is 5 nm to 10 μm;
[0149] Optionally, the thickness of the polymer layer is 0.02 μm to 8 μm;
[0150] Further optionally, the thickness of the polymer layer is 0.05 μm to 8 μm;
[0151] Further optionally, the thickness of the polymer layer is 0.05 μm to 5 μm;
[0152] Further optionally, the thickness of the polymer layer is 0.1 μm to 5 μm.
[0153] The thickness of the polymer layer on the surface of the lithium-containing metal can be controlled at a thin nanoscale, which is more conducive to the assembled battery cell showing a smaller interface impedance.
[0154] In some embodiments, the elastic modulus of the polymer layer at 25° C. is 0.1 MPa to 65 MPa;
[0155] Optionally, the elastic modulus of the polymer layer at 25° C. is 0.5 MPa to 50 MPa;
[0156] Further optionally, the elastic modulus of the polymer layer at 25° C. is 10 MPa to 46 MPa;
[0157] Further optionally, the elastic modulus of the polymer layer at 25° C. is 18 MPa to 41 MPa;
[0158] Further optionally, the elastic modulus of the polymer layer at 25° C. is 29 MPa to 41 MPa.
[0159] In some embodiments, the elastic deformation range of the polymer layer at 25° C. is 55% to 350%;
[0160] Optionally, the elastic deformation range of the polymer layer at 25° C. is 150% to 350%;
[0161] Further optionally, the elastic deformation range of the polymer layer at 25° C. is 150% to 300%;
[0162] Further optionally, the elastic deformation range of the polymer layer at 25° C. is 168% to 280%.
[0163] By controlling parameters such as the elastic modulus and elastic deformation range of the polymer layer within a more appropriate range, it is beneficial to make the polymer layer have more appropriate elasticity, better promote close contact between the polymer layer and the lithium-containing metal layer, reduce interface impedance, and help achieve better energy density and power density.
[0164] In a third aspect, the present application provides a lithium metal secondary battery, which includes a positive electrode plate, a separator and the negative electrode plate described in the second aspect of the present application, the separator is arranged between the positive electrode plate and the negative electrode plate, and the polymer layer is arranged on the side of the negative electrode plate close to the separator.
[0165] The negative electrode plate in the lithium metal secondary battery includes a lithium metal negative electrode material distributed in a lithium-containing layer and a polymer layer. On at least one side of the negative electrode plate, the lithium-containing layer is stably connected to a dense and uniform polymer layer by chemical bonding. The polymer layer has certain elasticity, flexibility and swelling properties, which can make the polymer layer and the lithium-containing layer, and the polymer layer and the isolation membrane fit firmly, tightly and durably. It can better adapt to the larger volume expansion of the negative electrode side during charging, and can play the role of a protective layer at the negative electrode of the lithium metal secondary battery for a long time. The polymer layer can effectively inhibit the contact reaction between the electrolyte and lithium metal, reduce the consumption of the electrolyte and lithium metal, improve the coulombic efficiency, and extend the cycle life. It can also utilize the fluorinated aliphatic chain Rf in the lithium metal negative electrode material to promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium metal negative electrode side. In addition, the elasticity, flexibility and swelling comprehensive performance of the polymer layer not only promote the close fit between the polymer layer and the lithium-containing layer, but also help to exert good ionic conductivity, reduce interface polarization, and reduce interface impedance, so that the lithium metal secondary battery can achieve higher energy density, power density, charge and discharge cycle stability and higher safety performance in the presence of the polymer layer.
[0166] In addition, by inhibiting the contact reaction between the electrolyte and lithium metal and reducing the consumption of the electrolyte and lithium metal, the coulombic efficiency of the battery can also be improved.
[0167] In some embodiments, the lithium metal secondary battery further includes a second electrolyte, and the components of the second electrolyte and the first electrolyte in the polymer layer may be the same or different.
[0168] In a fourth aspect, the present application provides an electrical device, which includes the lithium metal secondary battery described in the third aspect of the present application.
[0169] In a fifth aspect, the present application provides an application of a monomer composition in preparing a negative electrode sheet or a lithium metal secondary battery, wherein the monomer composition comprises a first monomer represented by formula (M1) and a second monomer represented by formula (M2):
[0170]
[0171] wherein X1, X2, Y1, Y2, A1, A2, Rf and Rd are respectively as defined in the first aspect of the present application; z is as defined in the first aspect of the present application; at least one of Y1 and Y2 is cyano;
[0172] The negative electrode plate contains lithium metal;
[0173] The first monomer and the second monomer are used to form a polymer layer bonded to the lithium metal in the negative electrode plate.
[0174] The first monomer and the second monomer in the monomer composition are both cyanoacrylic acid derivatives, the cyano group therein can contact with the lithium in the outermost layer of the negative electrode plate matrix to form a chemical connection, and the carbon-carbon double bonds therein can undergo in-situ polymerization reaction under lithium catalysis, thereby preparing the lithium metal negative electrode material of the first aspect of the present application. At this time, a firmly connected, dense and uniform polymer layer can be formed on the surface of the lithium-containing layer of the negative electrode. The polymer layer has certain elasticity, flexibility and swelling properties, and can play the role of a protective layer for a long time.
[0175] In some embodiments, the application comprises the following steps: the first monomer and the second monomer are brought into contact with lithium metal in the lithium-containing layer to form the polymer layer through an in-situ polymerization reaction.
[0176] In some embodiments, the negative electrode plate is as defined in the second aspect of the present application, and the lithium metal secondary battery is as defined in the third aspect of the present application.
[0177] In a sixth aspect, the present application provides a method for preparing a negative electrode sheet, which comprises the following steps:
[0178] Providing a negative electrode substrate, wherein the outermost layer of at least one side of the negative electrode substrate is a lithium-containing layer, and the lithium-containing layer contains lithium metal; and also providing a reaction mixture containing a monomer composition and a first electrolyte;
[0179] The reaction mixture is coated on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, so that the monomer composition contacts at least a catalytic amount of lithium metal, and the monomer composition undergoes an in-situ polymerization reaction to form a polymer Poly bonded to the lithium metal in the lithium-containing layer;
[0180] Wherein, the monomer composition is as defined in the fifth aspect of the present application;
[0181] The first electrolyte is as defined in the second aspect of the present application.
[0182] In the presence of the first electrolyte, the cyano group in the monomer composition can contact the lithium in the outermost layer of the negative electrode sheet substrate to form a chemical connection (further, a covalent connection), and the carbon-carbon double bond therein can undergo an in-situ polymerization reaction under lithium catalysis to form the aforementioned polymer Poly, thereby preparing the lithium metal negative electrode material of the first aspect of the present application. At this time, a firmly connected, dense and uniform polymer layer can be formed on the surface of the lithium-containing layer of the negative electrode. The polymer layer has certain elasticity, flexibility and swelling properties, and can play a protective layer role for a long time. Compared with the polymer coating of the physical coating method in the conventional technology, the polymer layer formed in the present application is not only stably bonded to the surface of the lithium-containing layer through chemical connection, but also can reduce, avoid or effectively delay the polymer layer from falling off from the surface of the lithium-containing layer during the charge and discharge process. In addition, the polymer layer of the present application is dense and uniform, and the thickness of the polymer layer can be controlled at the nanoscale by in-situ polymerization, so that the assembled battery cell can exhibit a smaller interface impedance.
[0183] In some embodiments, the reaction temperature of the in-situ polymerization is selected from 30°C to 100°C;
[0184] Optionally, the reaction temperature of the in-situ polymerization is selected from 30°C to 60°C;
[0185] Alternatively, the reaction temperature of the in-situ polymerization is selected from 40°C to 80°C.
[0186] In some embodiments, the reaction time of the in-situ polymerization is selected from 0.1h to 24h;
[0187] Optionally, the reaction time of the in-situ polymerization is selected from 0.1h to 12h;
[0188] Further optionally, the reaction time of the in-situ polymerization is selected from 0.1h to 6h.
[0189] In some embodiments, the polymer layer described in the second aspect of the present application is formed on the surface of the negative electrode plate substrate.
[0190] In some embodiments, the negative electrode plate substrate is a pure lithium plate or a lithium alloy;
[0191] Optionally, the mass proportion of the lithium element in the lithium alloy is ≥50%.
[0192] When the negative electrode plate substrate is a pure lithium plate or a lithium alloy, the negative electrode plate of the battery may further introduce a negative electrode current collector to facilitate the assembly of the pole lug, or a pure lithium plate covered with a polymer layer may be used as the negative electrode plate.
[0193] In some embodiments, the negative electrode plate is as defined in the second aspect of the present application.
[0194] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS
[0195] In order to better describe and illustrate the embodiments or examples of those applications disclosed herein, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered as limiting the scope of any of the disclosed applications, the embodiments or examples currently described, and the best modes of these applications currently understood. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the accompanying drawings:
[0196] Figure 1 is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer is provided on one side of the negative electrode plate;
[0197] Figure 2 1 is a schematic diagram of the structure of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer and a negative electrode current collector are provided on one side of the negative electrode plate;
[0198] Figure 3 is a schematic structural diagram of a negative electrode sheet according to an embodiment of the present application, wherein a second negative electrode active material layer is provided between the lithium-containing layer and the negative electrode current collector;
[0199] Figure 4 is a schematic structural diagram of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer is provided on both sides of the negative electrode plate;
[0200] Figure 5 1 is a schematic diagram of the structure of a negative electrode plate according to an embodiment of the present application, wherein a polymer layer is provided on both sides of the negative electrode plate, and a second negative electrode active material layer is provided between the lithium-containing layer and the negative electrode current collector on both sides;
[0201] Figure 6 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0202] Figure 7 yes Figure 6 An exploded view of a secondary battery according to an embodiment of the present application is shown;
[0203] Figure 8 FIG. 1 is a schematic diagram of an electrical device using a secondary battery as a power source according to an embodiment of the present application.
[0204] Explanation of the reference numerals: 100, negative electrode sheet substrate; 110, negative electrode current collector; 120, second negative electrode active material layer; 130, lithium-containing layer; 200, polymer layer; 5, secondary battery; 51, shell; 52, electrode assembly; 53, cover plate; 6, power-consuming device. DETAILED DESCRIPTION
[0205] Below, some embodiments of the lithium metal negative electrode material, negative electrode sheet, lithium metal secondary battery, electrical device, preparation method and application of the present application are described in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0206] Numerical value " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be including end value or excluding end value, and any end value can be included or not included independently, and can be combined arbitrarily, that is, any lower limit can form a scope with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 listed, and if the maximum range value 3,4 and 5 are also listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc. For example, when a parameter is expressed as an integer selected from "2-10", it is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0207] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0208] If there is no special explanation, all steps of the present application may be performed sequentially or randomly, and may preferably be performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0209] If there is no special explanation, the words "have", "include", "contain" and "include" mentioned in this application can each independently represent an open or closed form. For example, the words "include" and "include" can also mean that other members or timing characteristics that are not listed can also be included or included, or can only include or include the listed members or timing characteristics. Members include materials or components, structures, elements, instruments, etc.; non-limiting examples of timing characteristics include actions, conditions for the occurrence of actions, timing, states, etc.
[0210] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". Further, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0211] In this application, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.
[0212] In the present application, unless otherwise specified, the features or solutions corresponding to "and / or" include any one of two or more related listed items, and also include any and all combinations of the related listed items, wherein the arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. For example, "A and / or B" means a group consisting of A, B, and "a combination of A and B". Among them, "comprising A and / or B" can mean "comprising A, comprising B, and comprising A and B", and can also mean "comprising A, comprising B, or comprising A and B", which can be properly understood according to the sentence in which it is located.
[0213] In this application, "multiple", "multiple", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two. It is understood that when "any number" of items are involved, it refers to any suitable combination of multiple items, that is, the combination of "any number" of items is performed in a manner that does not conflict and can implement this application.
[0214] As used herein, "combination thereof", "any combination thereof", "any combination thereof" etc. include all suitable combinations of any two or more of the listed items.
[0215] Herein, the “suitable” mentioned in “suitable combination”, “suitable method”, “any suitable method”, etc., shall be based on the technical solution that can implement the present application.
[0216] Herein, "preferred", "better", and "more preferred" are only used to describe implementation methods or examples with better effects, and it should be understood that they do not constitute a limitation on the scope of protection of this application. If multiple "preferred" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "preferred" item is independent.
[0217] In this application, "optionally", "optional", and "optional" mean optional or dispensable, that is, any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0218] In the present application, "further", "further", "particularly" and the like are used for descriptive purposes to indicate the differences in content between different technical solutions, but should not be construed as limiting the scope of protection of the present application.
[0219] In the present application, the terms "first", "second", "third", "fourth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0220] In this application, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left endpoint and the right endpoint are the same. For example, 3~5h or 3-5h both mean that the units of the left endpoint "3" and the right endpoint "5" are both h (hours).
[0221] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Furthermore, the weight described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0222] In the present application, the term "hydrocarbon group" refers to a monovalent group composed of two elements, carbon and hydrogen. The hydrocarbon group can be in the form of an alkyl group, an alkenyl group, an alkynyl group, etc.
[0223] In this application, the term "alkyl" refers to a monovalent residue formed by the loss of a hydrogen atom from a saturated hydrocarbon containing a primary carbon atom, a secondary carbon atom, a tertiary carbon atom, a quaternary carbon atom, or a combination thereof. Phrases containing this term, for example, "C1- 10 "Alkyl" refers to an alkyl group containing 1 to 10 carbon atoms, each occurrence of which can be independently C1 alkyl, C2 alkyl, C3 alkyl, C4 alkyl, C5 alkyl, C6 alkyl, C7 alkyl, C8 alkyl, C9 alkyl or C 10Alkyl. Examples of suitable alkyl groups include, but are not limited to, methyl (Me, -CH3), ethyl (Et, -CH2CH3), 1-propyl (n-Pr, n-propyl, -CH2CH2CH3), 2-propyl (i-Pr, i-propyl, -CH(CH3)2), 1-butyl (n-Bu, n-butyl, -CH2CH2CH2CH3), 2-methyl-1-propyl (i-Bu, i-butyl, -CH2CH(CH3)2), 2-butyl (s-Bu, s-butyl, -CH (CH3)CH2CH3), 2-methyl-2-propyl (t-Bu, t-butyl, -C(CH3)3), 1-pentyl (n-pentyl, -CH2CH2CH2CH2CH3), 2-pentyl (-CH(CH3)CH2CH2CH3), 3-pentyl (-CH(CH2CH3)2), 2-methyl-2-butyl (-C(CH3)2CH2CH3), 3-methyl-2-butyl (-CH(CH3)CH(CH3)2), 3-methyl-1-butyl ( -CH2CH2CH(CH3)2), 2-methyl-1-butyl (-CH2CH(CH3)CH2CH3), 1-hexyl (-CH2CH2CH2CH2CH2CH3), 2-hexyl (-CH(CH3)CH2CH2CH2CH3), 3-hexyl (-CH(CH2CH3)(CH2CH2CH3)), 2-methyl-2-pentyl (-C(CH3)2CH2CH2CH3), 3-methyl-2-pentyl (-CH(CH3)CH (CH3)CH2CH3), 4-methyl-2-pentyl (-CH(CH3)CH2CH(CH3)2), 3-methyl-3-pentyl (-C(CH3)(CH2CH3)2), 2-methyl-3-pentyl (-CH(CH2CH3)CH(CH3)2), 2,3-dimethyl-2-butyl (-C(CH3)2CH(CH3)2), 3,3-dimethyl-2-butyl (-CH(CH3)C(CH3)3 and octyl (-(CH2)7CH3).
[0224] As used herein, the term "alkenyl" refers to a group containing at least one unsaturated site (i.e., a carbon-carbon sp 2 A monovalent residue formed by the loss of a hydrogen atom from a hydrocarbon having a double bond. Phrases containing this term, for example, "C2~C 10 "Alkenyl" or "C 2-10 "Alkenyl" refers to an alkenyl group containing 2 to 10 carbon atoms, and each occurrence can be independently C2 alkenyl, C3 alkenyl, C4 alkenyl, C5 alkenyl, C6 alkenyl, C7 alkenyl, C8 alkenyl, C9 alkenyl or C 10Suitable examples include, but are not limited to, vinyl (-CH=CH2), allyl (-CH2CH=CH2), cyclopentenyl (-C5H7), and 5-hexenyl (-CH2CH2CH2CH2CH=CH2).
[0225] In the present application, the term "alkynyl" refers to a monovalent residue formed by the loss of a hydrogen atom from a hydrocarbon having at least one unsaturated site, i.e., a carbon-carbon sp triple bond. Phrases containing this term, for example, "C2-C 10 "Alkynyl" refers to an alkynyl group containing 2 to 10 carbon atoms, and each occurrence can be independently C2 alkynyl, C3 alkynyl, C4 alkynyl, C5 alkynyl, C6 alkynyl, C7 alkynyl, C8 alkynyl, C9 alkynyl or C 10 Suitable examples include, but are not limited to, ethynyl (-C≡CH) and propargyl (-CH2C≡CH).
[0226] In the present application, fluorosulfonyl corresponds to -S(=O)2F, and nitro corresponds to -NO2.
[0227] High energy density is an irreversible trend in the development of lithium metal batteries in the future. It has high specific capacity (3860mAh / g), extremely low potential (-3.04V vs.H2 / H + ) has therefore received widespread attention in the industry, but the high reactivity of lithium metal and the problem of dendrite short-circuiting have greatly restricted its further development. Lithium metal has high reactivity and is prone to side reactions with the electrolyte, consuming the electrolyte and lithium metal, producing a thick passivation layer, and causing the battery cycle life to decay rapidly. In addition, during the charging process, lithium ions are unevenly deposited due to regional differences in ion flow and electron flow, resulting in dendrites. On the one hand, lithium dendrites have a high specific surface area, which will aggravate the consumption of electrolyte and even cause battery diving; on the other hand, the rapid growth of lithium dendrites will penetrate the diaphragm and bring the risk of battery short circuit.
[0228] It has been reported that the protective layer is attached to the surface of lithium metal by physical coating. The protective layer and lithium metal are bonded by intermolecular van der Waals forces, which are weak. Due to the volume change on the negative electrode side during long cycles, it is easy to lose contact with lithium metal; the functional groups contained in the protective layer have no regulatory effect on lithium deposition. In addition, if the protective layer is obtained independently in advance and then attached between the lithium metal and the diaphragm, the operation is complicated and the flatness of the thin layer is not good; in order to improve the wettability of the lithium metal surface, a highly viscous polymer solution is used to coat the lithium metal surface, but the resulting protective layer is thicker.
[0229] In response to the above-mentioned common technical problems, in a first aspect, the present application provides a lithium metal negative electrode material.
[0230] The lithium metal negative electrode material provided in the first aspect of the present application includes a polymer layer with both flexibility and high elasticity, which has lithium ion transmission and regulation functions and is tightly combined with lithium metal by chemical connection, and can be used as a protective layer for lithium metal, which is expected to alleviate or solve the above technical problems. First, the presence of the polymer layer can reduce the direct contact between the electrolyte and the lithium metal, inhibit the occurrence of side reactions, and reduce the consumption of the electrolyte and lithium metal; secondly, a higher ionic conductivity and functional group design can be introduced into the polymer layer, which can not only promote the effective transfer of lithium ions inside the polymer layer and at the interface with the lithium metal, but also promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, reduce the consumption of electrolyte, and greatly inhibit the problem of dendrites piercing the diaphragm and short-circuiting; furthermore, the close combination between the polymer layer and the lithium metal can better adapt to the volume change of the negative electrode side during the charging and discharging process, and can avoid peeling from the lithium metal surface as much as possible; in addition, the elastic polymer layer is conducive to the volume expansion of the lithium metal side during the charging process, is not easy to break, and can play a protective role for a long time.
[0231] In some embodiments, the present application provides a lithium metal negative electrode material, which includes a lithium-containing metal and a polymer Poly bonded to the lithium metal in the lithium-containing metal, the polymer Poly having a linear carbon chain and a first side chain and a second side chain grafted to the linear carbon chain side group, the first side chain containing a fluorinated aliphatic chain Rf, the second side chain containing an EO block, and the structure of the EO block is *-(CH2CH2O) z -, z is a positive integer, and * indicates a connection site pointing to the linear carbon chain.
[0232] In the present application, unless otherwise specified, the term "lithium-containing metal" may be substantially composed of lithium (Li) metal, may be a lithium alloy, or may be a composition comprising lithium metal and lithium alloy. The lithium-containing metal "substantially composed of lithium metal" means that the weight proportion of metallic lithium is very high, and the proportion described by "substantially" here is, for example, greater than or equal to 80%, greater than or equal to 85%, greater than or equal to 90%, greater than or equal to 95%, greater than or equal to 96%, greater than or equal to 97%, greater than or equal to 98%, greater than or equal to 99%, equal to 100%, etc.
[0233] In the present application, unless otherwise specified, the term "lithium metal" or "metallic lithium" refers to lithium in a metallic state.
[0234] In the present application, the term "lithium" used independently, unless otherwise specified, refers to lithium in a metallic state, for example, "lithium" in lithium-containing metals.
[0235] In this application, unless otherwise specified, the term "lithium alloy" refers to an alloy containing lithium. In addition to lithium, lithium alloys may also contain one or more other types of metals. All lithium alloys reported to be used as negative electrode active materials in lithium metal batteries fall within the scope of this application. For example, a lithium alloy may be an alloy of lithium and one or more metals selected from silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium. Non-limiting examples of lithium alloys include lithium-magnesium alloys and lithium-aluminum alloys.
[0236] In the present application, unless otherwise specified, "polymer" refers to at least one type of polymer having an average molecular weight greater than 1000 Da, for example, at least one of a number average molecular weight and a weight average molecular weight greater than 1000 Da.
[0237] In this application, unless otherwise specified, "linear carbon chain" refers to a linear chain carbon skeleton composed of carbon atoms connected in sequence, such as the following structure "...CCCCC...". The positions where non-hydrogen atoms or groups are connected to carbon atoms at non-end points of the linear carbon chain can be called "side chains". The side chains involved in this application include a first side chain and a second side chain. The "first" and "second" here are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features.
[0238] In the present application, unless otherwise specified, the structural description "grafted" involved in the structure of an organic compound, such as a polymer Poly, indicates a chemical connection method, and further, unless otherwise specified, indicates a covalent connection method.
[0239] In this application, unless otherwise specified, the term "aliphatic chain" may also be referred to as "aliphatic group", which refers to a group containing at least one carbon atom and no aromatic group, and when the aliphatic chain contains only one carbon atom, the carbon atom is connected to four adjacent atoms by four single bonds, that is, methylene groups substituted by carbonyl atoms or groups are excluded. The aliphatic chain is allowed to contain one or more heteroatoms. When there are multiple heteroatoms, the types of heteroatoms can be one or more; heteroatoms refer to non-carbon, non-hydrogen atoms, and examples of heteroatoms may include but are not limited to fluorine, iodine, nitrogen, oxygen, sulfur, silicon, boron and phosphorus. The aliphatic chain may be an aliphatic hydrocarbon group, an aliphatic hydrocarbon group in which one or more hydrogen atoms are independently replaced by non-fluorine heteroatoms, or an aliphatic hydrocarbon group in which one or more carbon atoms are independently replaced by heteroatoms. It is allowed that hydrogen atoms are replaced and carbon atoms are replaced at the same time.
[0240] In the present application, unless otherwise specified, "EO block" refers to a segment having one or more EO units; wherein the EO unit is a unit having a structure of -CH2CH2O-.
[0241] In the present application, the “*” mark at different structures or positions may have different meanings.
[0242] The lithium metal negative electrode material provided in the present application has a dense and uniform polymer layer coated on the surface of the lithium-containing metal. The polymer layer can play the role of a protective layer at the negative electrode of the lithium metal secondary battery, effectively inhibit the contact reaction between the electrolyte and the lithium metal, reduce the consumption of the electrolyte and the lithium metal, and extend the battery cycle life; the linear carbon chain can give the polymer Poly and the polymer layer a certain flexibility; the polymer component Poly in the polymer layer has a stable chemical connection with the lithium-containing metal, so that the polymer layer is firmly bonded to the lithium-containing metal surface, and when the volume of the negative electrode side changes during the charge and discharge process, the polymer layer can be prevented from peeling off from the lithium-containing metal surface; the polymer Poly contains a fluorinated aliphatic chain Rf. On the one hand, the introduction of fluorine element can regulate the lithium ion Deposition, promote uniform deposition of lithium ions, improve the deposition morphology of lithium dendrites in lithium metal secondary batteries, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the negative electrode side of lithium metal. On the other hand, the presence of the fluorinated aliphatic chain Rf can give the polymer layer a certain elasticity, which is conducive to better fitting between the polymer layer and the lithium-containing metal and the separator; the polymer Poly also contains a flexible EO block, which can not only improve the flexibility of the polymer layer, enhance the close fit between the protective layer and the negative electrode substrate and between the protective layer and the separator side, and reduce the interface impedance, but also enhance the elasticity of the protective layer, so that the protective layer can better adapt to the larger volume expansion of the negative electrode side, thereby reducing or avoiding the rupture of the polymer layer, and then can play a protective role for a longer time. In addition, the dense and uniform polymer layer can also be swollen by the electrolyte, and can provide good ionic conductivity after swelling, so that lithium ions can be efficiently transferred in the polymer layer and at the lithium metal interface, the interface polarization caused by the introduction of the polymer layer is small, and the battery has good charge and discharge cycle stability. The above-mentioned characteristics of the polymer layer cooperate with each other to greatly improve the cycle life of the lithium metal secondary battery and suppress the lithium dendrite problem.
[0243] In some embodiments, in the structure of the polymer Poly, the number of the first side chains is m, and the number of the second side chains is n; wherein m and n are each independently an integer greater than or equal to 8.
[0244] In some embodiments, m and n are each independently an integer selected from 8 to 600, for example, any of the following values or an interval consisting of any two of the following values: 8, 9, 10, 11, 12, 15, 16, 18, 20, 22, 24, 25, 30, 40, 50, 60, 70, 80, 100, 150, 200, 250, 300, 400, 500, 600, 700, 800, etc., and m and n can also be each independently selected from any of the following suitable ranges: 8 to 300, 8 to 250, 8 to 200, 8 to 180, 10 to 300, 10 to 250, 10 to 200, 10 to 180, 20 to 300, 20 to 250, 20 to 200, ,20~180,25~300,25~250,25~200,25~180,30~300,30~250,30~200,30~180,50~300,50~250,50~200,50~180,60~300,60~250,60~200,60~180,80 ~300, 80~250, 80~200, 80~180, 8~150, 10~150, 20~150, 25~150, 30~150, 35~150, 36~150, 8~125, 10~125, 20~125, 25~125, 30~125, 35~125, 36~125, etc.
[0245] In some embodiments, m is an integer selected from 8 to 300, and can also be selected from any suitable range: 8-300, 8-250, 8-200, 8-180, 10-300, 10-250, 10-200, 10-180, 20-300, 20-250, 20-200, 20-180, 25-300, 25-250, 25-200, 25-180, 30-300, 30-250, 30-200, 30-180, 50-300, 50-250, 50-200, 50-180, 60-300, 60-250, 60-200, 60-180, 80-300, 80-250, 80-200, 80-180, etc.
[0246] In some embodiments, m is an integer selected from 50-250, optionally, m is an integer selected from 50-200.
[0247] In some embodiments, n is an integer selected from 8 to 300, and may also be selected from any suitable range: 8 to 300, 8 to 250, 8 to 200, 8 to 180, 10 to 300, 10 to 250, 10 to 200, 10 to 180, 20 to 300, 20 to 250, 20 to 200, 20 to 180, 25 to 300, 25 to 250, 25 to 200, 25 to 180, 30 to 300, 30 to 250, 30 to 200, 30 to 180, 50 to 300. 00, 50-250, 50-200, 50-180, 60-300, 60-250, 60-200, 60-180, 80-300, 80-250, 80-200, 80-180, 8-150, 10-150, 20-150, 25-150, 30-150, 35-150, 36-150, 8-125, 10-125, 20-125, 25-125, 30-125, 35-125, 36-125, etc.
[0248] In some embodiments, n is an integer selected from 25-200, optionally, n is an integer selected from 40-150.
[0249] The value ranges of m and n can be combined in any suitable manner. In some embodiments, m is an integer selected from 50 to 250, and n is an integer selected from 25 to 200. In other embodiments, m is an integer selected from 50 to 200, and n is an integer selected from 40 to 150.
[0250] In some embodiments, the ratio of m to n (denoted as m / n) satisfies 0.5≤m / n≤8, optionally, 1≤m / n≤5, and further optionally, 1≤m / n≤3. m / n can be any of the following values or an interval consisting of any two of the following values: 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, etc. m / n can also be selected from any of the following suitable ranges: 1 to 8, 2 to 8, 2 to 5, etc.
[0251] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0252] The ratio of m to n satisfies 0.5≤m / n≤8, optionally, 1≤m / n≤5, further optionally, 1≤m / n≤3;
[0253] m is an integer selected from 50 to 250, optionally, m is an integer selected from 50 to 200;
[0254] n is an integer selected from 25 to 200, and optionally, n is an integer selected from 40 to 150.
[0255] The introduction of the second side chain containing the EO block can improve the flexibility and swelling rate of the polymer layer, and the presence of the first side chain containing the fluorinated aliphatic chain Rf is conducive to improving the elasticity of the polymer layer. Further, by controlling the number of the two copolymer units in the polymer Poly, the flexibility and elasticity of the polymer layer can be regulated at the same time, thereby regulating the elastic deformation of the polymer layer, and regulating the degree of adhesion between the polymer layer and the substrate and between the polymer layer and the isolation membrane; larger elastic deformation is conducive to better adapting to the larger volume expansion of the negative electrode side during charging, which can reduce or avoid the rupture of the protective layer and thus achieve a longer protective effect; better flexibility is conducive to the close adhesion between the polymer layer and the lithium metal and between the polymer layer and the isolation membrane, reducing the interface impedance, and is conducive to improving the energy density and power density of the battery.
[0256] By controlling the ratio of m / n, the elasticity, swelling rate and ionic conductivity of the polymer can be optimized. Through the comprehensive regulation of the polymer elasticity, swelling rate and ionic conductivity, the polymer protective layer on the negative electrode side can better and more permanently play the role of isolating the electrolyte contact and regulating lithium deposition.
[0257] In some embodiments, in the EO block structure, z is a positive integer. Further, z is a positive integer ≤ 10. z can also be an integer selected from 2 to 10; further optionally, z is an integer selected from 3 to 7. z can also be 2, 3, 4, 5, 6, 7, 8, 9 or 10, and z can also be selected from an interval consisting of any two of the aforementioned integers, such as 2 to 8, 3 to 7, etc.
[0258] In some embodiments, in the polymer Poly, each occurrence of z is independently 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10.
[0259] In some embodiments, in the polymer Poly, each occurrence of z is independently 2, 3, 4, 5, 6, 7, 8, 9 or 10.
[0260] In some embodiments, in the polymer Poly, each occurrence of z is independently 2, 3, 4, 5, 6, 7 or 8.
[0261] In some embodiments, in the polymer Poly, each occurrence of z is independently 3, 4, 5, 6 or 7.
[0262] The z in the EO block structure reflects the number of EO units (ethylene oxide units) with the structure of "CH2CH2O" in the EO block. By adjusting the size of z, that is, by adjusting the length of the EO block, the flexibility of the polymer layer can be adjusted, and then the elastic deformation of the polymer layer and the degree of fit between the polymer layer and the substrate and the diaphragm can be regulated. By controlling z in a more suitable range or size, it can also work synergistically with other structural units of the polymer Poly (such as the Rf chain) to achieve the aforementioned multi-dimensional comprehensive excellent effects. When the polymer Poly is prepared by in-situ polymerization, by controlling z in a more suitable range or size, it is possible to more effectively adjust the flexibility of the polymer layer while maintaining a high reaction rate and an effective grafting density, thereby maintaining a high density of the polymer layer.
[0263] In the present application, if there is no other explanation, "maintain" means at least still having a beneficial effect relative to the reference solution, and it is understood that it does not require strict equality in numerical values.
[0264] In some embodiments, the polymer Poly comprises a repeating unit of the structure shown in formula (U1) and a repeating unit of the structure shown in formula (U2):
[0265]
[0266] in,
[0267] X1 and X2 are each independently H or an electron withdrawing group;
[0268] Y1 and Y2 are each independently a cyano group or a linking group formed by a cyano group bonded to the lithium metal in the lithium-containing metal;
[0269] A1 and A2 are each independently O, S or NR 11 ; Among them, R 11 H or C 1-3 alkyl;
[0270] Rd is a hydrocarbon group or a hydrocarbon group substituted by Q1, Q1 is selected from the following substituents: cyano, -C(=O)NH2, -OC(=O)NHR 6 and -S(=O)2F,R 6 is H or alkyl; optionally, R 6 H or C 1-6 Alkyl; further optionally, R 6 H or C 1-3 alkyl.
[0271] In some embodiments, at least one of Y1 and Y2 is a linker formed by a cyano group bonded to the lithium metal in the lithium-containing metal. In the present application, the asterisk "*" in the repeating unit of the structure shown in formula (U1) and the repeating unit of the structure shown in formula (U2) is a conventional representation method in the art, and the position marked by "*" represents the connection site between adjacent, identical or different repeating units.
[0272] In the present application, the “bonding” mode or “chemical connection” between cyano group and lithium refers to covalent connection unless otherwise specified.
[0273] In the main chain of the polymer Poly, at least one of the main chain carbon atoms connected to the Rf side group and the main chain carbon atoms connected to the EO block can be connected to a cyano group at the same time. At this time, the cyano group at this position is conducive to the polymerization reaction of the cyanoacrylic acid derivative monomer. This is because the cyano group is an electron-withdrawing group. During the polymerization reaction, the carbon atom connected to the cyano group can form a relatively stable anion active center, and then continue the chain growth until the chain terminates. On the other hand, the cyano group at this position can react with the lithium metal in the lithium metal to form a stable chemical connection between the polymer Poly and the lithium-containing metal. As a non-limiting example, at least one of Y1 and Y2 is a cyano group. In some embodiments, Y1 and Y2 are both cyano groups. As a non-limiting example, at least one of Y1 and Y2 is a cyano group. In some embodiments, Y1 and Y2 are both cyano groups. As a non-limiting example, at least one of Y1 and Y2 is a cyano group bonded to the lithium metal in the lithium-containing metal to form a connecting group. As a non-limiting example, at least one of Y1 and Y2 is a linking group formed by a cyano group bonded to a lithium metal in the lithium-containing metal.
[0274] In this application, the term "cyanoacrylic acid derivative monomer" refers to The derivatives of the skeleton shown are used as monomers for the in-situ polymerization reaction in the present application, and the ends marked with asterisks "*" can be connected to the aforementioned Rf or EO blocks through ester groups, amide groups, etc. Wherein, for A1 and A2, O corresponds to an ester bond connection mode, S corresponds to a thioester bond connection mode, and NH corresponds to an amide bond connection mode.
[0275] In this application, the term "C 1-3 "Alkylene" refers to an alkylene group containing 1, 2 or 3 carbon atoms, suitable examples of which are methylene (-CH2-), ethylene (-CH2CH2- or -CH(CH3)-), propylene (-CH2CH2CH2-, -CH2CH(CH3)- or -C(CH3)2-).
[0276] The polymer Poly may be a copolymer comprising a repeating unit of the structure shown in formula (U1) and a repeating unit of the structure shown in formula (U2). The aforementioned polymer Poly may form a chemical bond with metallic lithium through a large number of cyano groups located on the side groups of the main chain, thereby achieving a stable chemical connection between the polymer layer and the lithium-containing metal.
[0277] In some embodiments, in the structure of the polymer Poly, each occurrence of X1 and X2 is independently H or cyano, nitro or -NR 21 R 22 ; Among them, R 21 and R 22 Each independently is H or C 1-3 Alkyl. 21 and R 22 Can be H or methyl each independently. In some embodiments, R 21 and R 22 All are methyl.
[0278] An electron-withdrawing group can be introduced into at least one of X1 and X2 in the polymer Poly, which is beneficial to increase the reactivity of the carbon-carbon double bond in the cyanoacrylate derivative monomer (such as cyanoacrylic acid derivative monomer) during the formation of the polymer layer, promote the in-situ polymerization reaction, and facilitate the polymer layer to achieve a tighter and more uniform coating on the lithium-containing metal surface.
[0279] In some embodiments, in the structure of the polymer Poly, each occurrence of A1 and A2 is independently O, S or NH. In some embodiments, each occurrence of A1 and A2 is independently O or NH. In some embodiments, A1 is O. In some embodiments, A1 is NH. In some embodiments, A2 is O. In some embodiments, A2 is NH. In some embodiments, A1 and A2 are both O. In some embodiments, A1 and A2 are both NH.
[0280] The fluoroaliphatic chain Rf and the EO block can be independently grafted onto the linear carbon chain through ester bonds, amide bonds or thioester bonds, thereby flexibly selecting the corresponding polymerization monomers.
[0281] In the present application, a polymerizable monomer refers to a monomer that can be used for a polymerization reaction. If there is no other explanation, it refers to a monomer that can form the polymer Poly described in the present application through a polymerization reaction.
[0282] In some embodiments, Rd is C 1-4 Hydrocarbyl; optionally, Rd is C 1-4 Alkyl can be methyl, ethyl, propyl or butyl; further optionally, Rd is C 1-3The alkyl group may be methyl, ethyl or propyl; further optionally, Rd is methyl.
[0283] In some embodiments, Rd is a hydrocarbon group substituted by Q1, and Q1 can be selected from the following substituents: cyano, -C(=O)NH2, -OC(=O)NHR 6 and -S(=O)2F,R 6 It can be H or an alkyl group.
[0284] In some embodiments, Rd is C substituted with Q1 1-4 In some embodiments, Rd is a C substituted by Q1 1-4 Alkyl; here substituted C 1-4 The alkyl group may further be methyl, ethyl, propyl or butyl, and may further be C 1-3 Alkyl (such as methyl, ethyl or propyl). In some embodiments, Rd is methyl substituted by Q1.
[0285] In some embodiments, Q1 is cyano, -C(=O)NH2, -OC(=O)NHR 6 or -S(=O)2F,R 6 It can be H or alkyl. In some embodiments, R 6 is H. In some embodiments, R 6 is an alkyl group, which may further be C 1-6 Alkyl, further can be C 1-3 Alkyl, further can be methyl, ethyl or propyl. In some embodiments, R 6 It is methyl.
[0286] Functional substituents can be introduced at the end of the EO block to better optimize the performance of the polymer layer and the lithium metal secondary battery as needed. For example, the introduction of cyano groups can further enhance the chemical bonding between the polymer Poly and lithium metal; the introduction of fluorosulfonyl groups (-S(=O)2F) can induce uniform deposition of lithium ions; the introduction of amide groups (-C(=O)NH2) can enhance the elastic modulus of the protective layer; the introduction of carbamate groups (such as -OC(=O)-NHR 6 , where R 6 It can be H or alkyl), and the elasticity of the material can be improved by matching soft and hard segments
[0287] In some embodiments, the structure of the polymer Poly comprises m repeating units represented by formula (U1) and n repeating units represented by formula (U2).
[0288] By controlling the number of the two repeating units represented by formula (U1) and formula (U2) in the polymer Poly, the flexibility and elasticity of the polymer layer can be regulated at the same time, thereby regulating the elastic deformation of the polymer layer and regulating the degree of fit between the polymer layer and the substrate and between the polymer layer and the isolation membrane; larger elastic deformation is conducive to better adapting to the larger volume expansion of the negative electrode side during charging, which can reduce or avoid rupture of the protective layer and thus achieve a longer protective effect; better flexibility is conducive to close fit between the polymer layer and the lithium metal and between the polymer layer and the isolation membrane, reducing interface impedance, which is conducive to improving the energy density and power density of the battery.
[0289] In some embodiments, in the structure of the polymer Poly, m repeating units represented by formula (U1) and n repeating units represented by formula (U2) are arranged linearly. In this case, the two repeating units represented by formula (U1) and formula (U2) form a linear carbon chain with good flexibility, which is more beneficial for the flexibility regulation of the polymer Poly.
[0290] In some embodiments, formula (U1) and formula (U2) jointly participate in the formation of a linear carbon chain in the polymer Poly.
[0291] In some embodiments, the polymer Poly has a general structure as shown in formula (P1):
[0292] The definitions of m and n are the same as above.
[0293] In the present application, the asterisks "*" on both sides of the general structure of formula (P1) are conventional notations in the art, indicating the end groups of the linear carbon chain of the polymer Poly. In the present application, the end groups of the polymer Poly, unless otherwise specified, refer to the end groups formed by the polymerization reaction of carbon-carbon double bonds, and their types are related to factors such as the initiator used and the end-capping group in the termination reaction. When "*" is used to describe the end groups of the polymer Poly, it can be understood in conjunction with the relevant description of the polymerization reaction in the present application, and those skilled in the art can correctly understand the structure of the polymer Poly.
[0294] In formula (P1), m+n is numerically equal to the degree of polymerization of the polymer Poly. By controlling m+n, the molecular weight of the polymer Poly can be regulated. By controlling m / n, the ratio of the number of two repeating units in the polymer Poly can be regulated. The polymer Poly shown in formula (P1) has a controllable number of repeating units shown in formula (U1) and repeating units shown in formula (U2), and has a flexible linear carbon chain, which is more conducive to the flexible regulation of the polymer Poly, and is also more conducive to the cyanide group of the main chain side group to fully contact the metallic lithium in the lithium-containing metal, so that the polymer Poly and the lithium-containing metal fit more closely, have more chemical bonding sites, and are more firmly bonded.
[0295] In some embodiments, the first side chains in the polymer Poly are introduced by formula (U1). In this case, Rf only exists in the repeating unit shown in formula (U1).
[0296] In some embodiments, the second side chains in the polymer Poly are introduced by formula (U2). In this case, the EO block only exists in the repeating unit shown in formula (U2).
[0297] In some embodiments, in the polymer Poly, the first side chains are introduced through formula (U1), and the second side chains are introduced through formula (U2).
[0298] In some embodiments, in the polymer Poly, the fluorine substitution rate in any Rf is independently ≥50%. In the polymer Poly, the fluorine substitution rate in any Rf can also be independently any of the following percentages, or independently selected from the interval consisting of any of the following percentages and 100%, or independently selected from the interval consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 90%, 95%, 96%, 97%, 98%, 99%. The interval consisting of any percentage and 100% is, for example, 50% to 100%, 55% to 100%, 60% to 100%, 65% to 100%, 70% to 100%, 80% to 100%, etc. Non-limiting examples of the interval consisting of any two percentages are 50% to 99%, 55% to 99%, etc. In some embodiments, in the polymer Poly, the fluorine substitution rate in at least one Rf is 100%. In some embodiments, in the polymer Poly, the fluorine substitution rate in any Rf is 100%.
[0299] In some embodiments, in the polymer Poly, the fluorine substitution rate in any Rf is independently ≥55%.
[0300] In the present application, the "fluorine substitution rate in Rf" is the molar percentage of fluorine atoms, based on the number of replaceable hydrogen atoms in the Rf group. The "number of replaceable hydrogen atoms" can be understood as the number of replaceable sites in the Rf group, that is, the maximum number of hydrogen atoms that can be connected to carbon atoms and possible heteroatoms (such as phosphorus atoms, nitrogen atoms, sulfur atoms, etc.), and the hydrogen atoms can also be replaced by other elements (in this case, the sites occupied by other elements are also included in the base number).
[0301] As a non-limiting example of Rf, The fluorine substitution rate in is 8 / 11, about 72.7%; The fluorine substitution rate in is 100%; The fluorine substitution rate in is 13 / 17, about 76.5%; The fluorine substitution rate in is 6 / 9, about 66.7%; The fluorine substitution rate in is 8 / 14, about 57.1%; The fluorine substitution rate in is 100%.
[0302] In some embodiments, at least 50% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥80%, or ≥90%.
[0303] In some embodiments, at least 60% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥70%, or ≥80%, or ≥90%.
[0304] In some embodiments, at least 70% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥60%, or ≥70%, or ≥80%, or ≥90%.
[0305] In some embodiments, at least 80% of the Rf in the polymer Poly satisfies a fluorine substitution rate of ≥50%, or ≥60%, or ≥70%, or ≥80%, or ≥90%.
[0306] In this application, for percentage intervals defined by "≥", such as ≥50%, ≥60%, unless otherwise specified, the upper limit is 100%, that is, ≥50%, ≥60% have the same meanings as 50% to 100%, 60% to 100%, respectively. This definition is applicable to, but not limited to, the range of values of fluorine substitution rate.
[0307] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently ≥ 4. In the polymer Poly, the number of fluorine atoms in any Rf can also be independently any of the following values, or independently greater than or equal to any of the following values, or independently an interval consisting of any two of the following values: 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19 and 20. Non-limiting examples of the interval consisting of any two of the above values are 4-20, 4-16, 4-15, 4-13, 5-20, 5-16, 5-15, 5-13, 6-20, 6-16, 6-15, 6-13, 8-20, 8-16, 8-15, 8-13, 4-10, etc.
[0308] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently ≥5.
[0309] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently an integer selected from 4 to 20.
[0310] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently an integer selected from 4 to 16.
[0311] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently an integer selected from 4 to 15.
[0312] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently an integer selected from 5 to 15.
[0313] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently an integer selected from 4 to 13.
[0314] In some embodiments, in the polymer Poly, the number of fluorine atoms in any Rf is independently an integer selected from 4 to 10.
[0315] In some embodiments, the mass proportion of fluorine element in the polymer Poly is 15% to 44%. The mass proportion of fluorine element in the polymer Poly can also be any of the following percentages or an interval consisting of any two of the following percentages: 15%, 20%, 25%, 30%, 35%, 40%, 44%. Non-limiting examples of the interval consisting of any two percentages are 15% to 44%, 20 to 44%, 25% to 44%, 30% to 44%, 15% to 41%, 20 to 41%, 25% to 41%, 30% to 41%, etc.
[0316] In some embodiments, the mass percentage of fluorine element in the polymer Poly is 15% to 41%.
[0317] In some embodiments, the mass percentage of fluorine element in the polymer Poly is 20% to 41%.
[0318] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0319] The fluorine substitution rate in any Rf is independently ≥ 50%;
[0320] The number of fluorine atoms in any Rf is independently ≥ 4;
[0321] The mass percentage of fluorine element in the polymer Poly is 15% to 44%.
[0322] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0323] The fluorine substitution rate in any Rf is independently ≥55%;
[0324] The number of fluorine atoms in any Rf is independently ≥ 5, and optionally, the number of fluorine atoms in any Rf is independently 5 to 15;
[0325] The mass proportion of fluorine element in the polymer Poly is 15% to 41%, and optionally 20% to 41%.
[0326] By controlling the fluorine substitution rate in Rf, by controlling the number of fluorine atoms in Rf, and by controlling the mass proportion of fluorine element in the polymer Poly in one or more ways, it is possible to better promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, increase the cycle life of lithium ions and reduce the risk of short circuits, and alleviate the volume expansion of the lithium metal negative electrode side. In addition, it can also be beneficial to the application of the polymer layer in lithium metal secondary batteries that perform charge and discharge cycles at a high current density.
[0327] Taking controlling the mass proportion of fluorine in the polymer Poly as an example, it is beneficial to improve the deposition morphology of lithium dendrites in lithium metal batteries and alleviate the volume expansion of lithium metal negative electrodes, which is beneficial to the application of polymer layers in lithium metal secondary batteries that perform charge and discharge cycles at high current density.
[0328] In some embodiments, in the polymer Poly, any Rf independently contains 2 to 10 main chain carbon atoms, that is, in the polymer Poly, the number of main chain carbon atoms contained in any Rf independently is 2 to 10. In the polymer Poly, the number of main chain carbon atoms contained in any Rf can also independently be any of the following values or independently selected from the interval consisting of any two of the following values: 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0329] In some embodiments, in the polymer Poly, any Rf independently contains 2 to 8 main chain carbon atoms.
[0330] In some embodiments, in the polymer Poly, any Rf independently contains 3 to 8 main chain carbon atoms.
[0331] In some embodiments, in the polymer Poly, any Rf independently contains 3, 4, 5, 6, 7 or 8 main chain carbon atoms.
[0332] In some embodiments, in the polymer Poly, the number of carbon atoms in any Rf is independently an integer selected from 2 to 10. In the polymer Poly, the number of carbon atoms in any Rf can also be independently any of the following values or independently selected from the interval consisting of any two of the following values: 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0333] In some embodiments, in the polymer Poly, the number of carbon atoms in any Rf is independently an integer selected from 2 to 8.
[0334] In some embodiments, in the polymer Poly, the number of carbon atoms in any Rf is independently an integer selected from 3 to 8.
[0335] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0336] Each Rf independently contains 2 to 10 main chain carbon atoms;
[0337] The number of carbon atoms in any one Rf is independently an integer selected from 2 to 10.
[0338] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0339] Any Rf independently contains 2 to 8 main chain carbon atoms, optionally, any Rf independently contains 3 to 8 main chain carbon atoms;
[0340] The number of carbon atoms in any Rf is independently an integer selected from 2 to 8. Alternatively, the number of carbon atoms in any Rf is independently an integer selected from 3 to 8.
[0341] In some embodiments, at least one Rf can be independently fluorinated C 2-10 In some embodiments, any one of Rf can be independently fluorinated C 2-10 Further, based on any of the above embodiments, the number of carbon atoms of any Rf can also be independently any of the following values or independently selected from the interval consisting of any two of the following values: 2, 3, 4, 5, 6, 7, 8, 9 and 10.
[0342] In some embodiments, C 2-10The alkyl group may be, for example, but is not limited to, ethylpropyl, butyl, pentyl, hexyl, heptyl, octyl, isopropyl, isobutyl, tert-butyl, isopentyl, tert-pentyl, neopentyl, 2-methylpentyl, 3-methylpentyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 2-methylhexyl, 3-methylhexyl, 2,2-dimethylpentyl, 3,3-dimethylpentyl, 2,3-dimethylpentyl, 2,4-dimethylpentyl, 3-ethylpentyl, 2,2,3-trimethylbutyl, 2-methylheptyl, 3-methylheptyl, 4- Methylheptyl, 2,2-dimethylhexyl, 3,3-dimethylhexyl, 2,3-dimethylhexyl, 2,4-dimethylhexyl, 2,5-dimethylhexyl, 3,4-dimethylhexyl, 3-ethylhexyl, 2,2,3-trimethylpentanyl, 2,2,4-trimethylpentanyl, 2,3,3-trimethylpentanyl, 2,3,4-trimethylpentanyl, 2-methyl-3-ethylpentanyl, 3-methyl-3-ethylpentanyl, 2,2,3,3-tetramethylbutanyl, nonanyl, decyl, and the like.
[0343] The length of the Rf side chain can be adjusted by controlling the number of carbon atoms in Rf, thereby giving the polymer layer appropriate elasticity and preferably inhibiting the polymer layer from rupturing under large volume deformation.
[0344] In some embodiments, in the structure of the polymer Poly, one, more or all Rf independently contains one or more heteroatoms selected from the group consisting of iodine, nitrogen, oxygen, sulfur, silicon, boron and phosphorus. Optionally, the number of heteroatoms in any one, more or all Rf is independently 1 or more. Further optionally, the number of heteroatoms in any one, more or all Rf is selected from 1 or 2 to 6. Further optionally, the number of heteroatoms in any one, more or all Rf is selected from 1 or 2 to 5. In some embodiments, the number of oxygen atoms in one, more or all Rf is 1, 2, 3, 4 or 5. In some embodiments, the number of nitrogen atoms in one, more or all Rf is 1, 2 or 3. In some embodiments, the number of sulfur atoms in one, more or all Rf is 1, 2 or 3. In some embodiments, the number of phosphorus atoms in one, more or all Rf is 1 or 2. In some embodiments, the number of iodine atoms in one, more or all Rf is 1, 2, 3, 4, 5 or 6. In some embodiments, the number of silicon atoms in one, more or all Rf is 1 or 2. In some embodiments, the number of boron atoms in one, more or all Rf is 1 or 2.
[0345] In some embodiments, in the structure of the polymer Poly, one, more or all Rf satisfy one or more of the following characteristics:
[0346] The number of oxygen atoms in one, more than one or all Rf is 1, 2, 3, 4 or 5;
[0347] The number of nitrogen atoms in one, more than one or all Rf is 1, 2 or 3;
[0348] The number of sulfur atoms in one, more than one or all Rf is 1, 2 or 3;
[0349] The number of phosphorus atoms in one, more than one or all Rf is 1 or 2;
[0350] The number of iodine atoms in one, more or all Rf is 1, 2, 3, 4, 5 or 6;
[0351] The number of silicon atoms in one, more than one or all of Rf is 1 or 2; and
[0352] The number of boron atoms in one, more than one or all of Rf is 1 or 2.
[0353] In some embodiments, in the structure of the polymer Poly, one, more or all of the Rf contain one or more selected from iodine, -NR 12 -, -O-, -S-, -S(O)2-, >Si<, >B- and >P(=O)-, wherein R 12 H or C 1-3 Alkyl. Optionally, R 12 is H or methyl. Further optionally, R 12 For H.
[0354] In some embodiments, in the structure of the polymer Poly, one, more or all Rf contains one or more atoms or atomic groups selected from the group consisting of -O-, -S(O)2- and -(O=)P(O-)2. In some embodiments, one, more or all Rf contains one or more -O-. In some embodiments, one, more or all Rf contains -S(O)2F. In some embodiments, one, more or all Rf contains -(O=)P(O-)2.
[0355] In the present application, the term "radical" refers to a group having two or more atoms.
[0356] By introducing other heteroatoms other than fluorine atoms into Rf, such as one or more heteroatoms of iodine, nitrogen, oxygen, sulfur, silicon, boron, phosphorus, etc., special properties can be given to the polymer layer. For example, phosphorus has a certain flame retardant effect. For another example, iodine can also play a certain role in regulating the deposition of lithium ions. For another example, fluorosulfonyl (-S(=O)2F) has a certain effect on improving the ionic conductivity of the polymer layer and promoting the uniform deposition of lithium ions.
[0357] In some embodiments, in the structure of the polymer Poly, any Rf is independently a linear structure or a branched structure.
[0358] The linear Rf is beneficial to improving the elasticity of the polymer material, while the side chain Rf is beneficial to improving the swelling capacity of the electrolyte membrane, thereby improving the ionic conductivity.
[0359] In some embodiments, in the structure of the polymer Poly, any Rf is independently a saturated structure or an unsaturated structure.
[0360] When the fluorine-substituted aliphatic chain has a saturated structure, it can give the polymer Poly molecular chain a higher mobility, which is beneficial for improving the elasticity regulation of the polymer layer. In addition, by introducing unsaturated bonds in Rf, the polymer layer can be cross-linked to enhance the elastic modulus of the polymer protective layer.
[0361] In some embodiments, in the structure of the polymer Poly, the structure of any Rf is independently represented by formula (III-1), formula (III-2) or formula (III-3):
[0362]
[0363] in,
[0364] In formula (III-1), m3 is an integer selected from 2 to 10; R 31 , R 32 and R 3 Each occurrence is independently H or F; the structure represented by formula (III-1) contains at least 4 F atoms;
[0365] In formula (III-2), m 4a and m 4b Each independently represents an integer selected from 1 to 9; R 41a , R 42a , R 4a , R 41b , R 42b and R 4b Each occurrence is independently H or F; the structure represented by formula (III-2) contains at least 4 F atoms;
[0366] In formula (III-3), m5 is an integer selected from 2 to 10; R 51 and R 52 Each occurrence is independently H or F; the structure represented by formula (III-3) contains at least 4 F atoms.
[0367] In formula (III-1), m3 is an integer selected from 2 to 10. m3 can also be any of the following values or an interval consisting of any two of the following values: 2, 3, 4, 5, 6, 7, 8, 9 and 10; m3 can also be selected from any of the following ranges: 3 to 10, 3 to 8, etc.
[0368] In formula (III-1), R 31 , R 32 and R 3 Each occurrence is independently H or F, and the structure shown in formula (III-1) contains at least 4 F atoms. The number of fluorine atoms in the structure shown in formula (III-1) can also be further any suitable value defined above, which can refer to but is not limited to the number of fluorine atoms in Rf, the fluorine substitution rate in Rf, the mass proportion of fluorine element in the polymer Poly, the number of main chain carbon atoms contained in Rf, the number of carbon atoms in Rf, etc.
[0369] The structure of formula III-1 is a linear saturated fluorinated aliphatic chain. On the one hand, it can give the polymer layer better elasticity, reduce or avoid the rupture of the polymer layer under large volume deformation. On the other hand, it can effectively promote the uniform deposition of lithium ions through the fluorine element, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium metal negative electrode side.
[0370] In formula (III-2), m 4a and m 4b Each independently represents an integer selected from 1 to 9, and may also independently represent any of the following values or independently represent an interval consisting of any two of the following values: 1, 2, 3, 4, 5, 6, 7, 8 and 9. 4a and m 4b They can also be independently selected from any of the following ranges: 2 to 8, 3 to 8, 3 to 6, etc.
[0371] In formula (III-2), R 41a , R 42a , R 4a , R 41b , R 42b and R 4b Each occurrence is independently H or F, and the structure shown in formula (III-2) contains at least 4 F atoms. The number of fluorine atoms in the structure shown in formula (III-2) can also be any suitable value defined above, which can refer to but is not limited to the number of fluorine atoms in Rf, the fluorine substitution rate in Rf, the mass proportion of fluorine element in polymer Poly, the number of main chain carbon atoms contained in Rf, the number of carbon atoms in Rf, etc.
[0372] The structure of formula III-2 can introduce phosphorus elements. In addition, the phosphate group therein has a flame retardant effect, which is beneficial to improving the safety performance of the battery cell.
[0373] In formula (III-3), m5 is an integer selected from 2 to 10, and can also be any of the following values or an interval consisting of any two of the following values: 2, 3, 4, 5, 6, 7, 8, 9 and 10. m5 can also be selected from any of the following ranges: 3 to 10, 3 to 8, etc.
[0374] In formula (III-3), R 51 and R 52 Each occurrence is independently H or F; the structure shown in formula (III-3) contains at least 4 F atoms. The number of fluorine atoms in the structure shown in formula (III-3) can also be any suitable value defined above, which can refer to but is not limited to the number of fluorine atoms in Rf, the fluorine substitution rate in Rf, the mass proportion of fluorine element in polymer Poly, the number of main chain carbon atoms contained in Rf, the number of carbon atoms in Rf, etc.
[0375] The structure of formula III-3 can introduce a fluorosulfonyl group, which has a certain positive effect on improving the ionic conductivity of the polymer layer.
[0376] In some embodiments, the polymer Poly satisfies one or more of the following characteristics:
[0377] m3 is an integer selected from 3 to 10; alternatively, m3 is an integer selected from 3 to 8;
[0378] m 4a and m 4b are each independently an integer selected from 2 to 9; optionally, m 4a and m 4b are each independently an integer selected from 2 to 8; further optionally, m 4a and m 4b are each independently an integer selected from 3 to 8; further optionally, m 4a and m 4b Each independently is an integer selected from 3 to 6
[0379] m5 is an integer selected from 3 to 10; optionally, m5 is an integer selected from 3 to 8.
[0380] In some embodiments, in the structure of the polymer Poly, the structure of Rf is as shown in formula (III-1); or, the structure of Rf is as shown in formula (III-2); or, the structure of Rf is as shown in formula (III-3).
[0381] In some embodiments, in the structure of the polymer Poly, each time formula (III-1) appears, the number of H atoms therein is 0, 1, 2, 3 or 4; each time formula (III-2) appears, the number of H atoms therein is 0, 1, 2, 3, 4, 5 or 6; each time formula (III-3) appears, the number of H atoms therein is 0, 1, 2, 3 or 4.
[0382] In some embodiments, the number of H atoms in formula (III-1) is 0.
[0383] In some embodiments, the number of H atoms in formula (III-2) is 0.
[0384] In some embodiments, the number of H atoms in formula (III-3) is 0.
[0385] By controlling the number of H atoms, the number of sites available for fluorine substitution can be controlled.
[0386] In some embodiments, in the structure of the polymer Poly, any Rf is independently any of the following structures:
[0387]
[0388] R 10 is a branched structure Rf. 01 , Rf 02 , Rf 03 , Rf 04 , Rf 05 , Rf 06 , Rf 07 , Rf 08 and Rf 09 In some embodiments, in the structure of the polymer Poly, any one Rf is independently any of the following structures: Rf 01 , Rf 02 , Rf 03 , Rf 05 , Rf 07 , Rf 08 , Rf 09 and Rf 10 .
[0389] In some embodiments, the number average molecular weight of the polymer Poly is selected from 10 kDa to 200 kDa; optionally, the number average molecular weight of the polymer Poly is selected from 40 kDa to 100 kDa; optionally, the number average molecular weight of the polymer Poly is selected from 50 kDa to 80 kDa.
[0390] The number average molecular weight of the polymer Poly can also be any of the following molecular weights or an interval consisting of any two of the following molecular weights: 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 22, 25, 26, 28, 30, 35, 40, 44, 45, 46, 48, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, etc. (all in kDa).
[0391] By adjusting the degree of polymerization or molecular weight of the polymer Poly, the molecular chain length of the polymer Poly can be adjusted, which can not only achieve effective coating of lithium metal, but also maintain stable chemical connection, and can also affect the density and uniformity of the polymer layer.
[0392] In some embodiments, the lithium-containing metal comprises lithium or a lithium alloy. The lithium alloy contains lithium and may also contain, but is not limited to, one or more elements selected from the group consisting of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel, and titanium.
[0393] Lithium metal has the highest specific capacity (3860 mAh / g) and the lowest electrochemical potential (-3.04 V, relative to standard hydrogen electrode) among all negative electrode materials for lithium-based batteries. It is an optimal negative electrode material for lithium metal batteries and helps to achieve high energy density.
[0394] In some embodiments, the amount of lithium metal in the lithium-containing metal relative to the polymer Poly is greater than or equal to the catalyst amount, calculated by molar ratio.
[0395] In the lithium metal negative electrode material provided in the present application, the lithium-containing metal only needs to provide a catalytic amount to successfully catalyze the in-situ polymerization reaction of cyano olefin carboxylic acid derivative monomers (such as cyanoacrylic acid derivative monomers) on the surface of the lithium-containing metal. The lithium metal only needs to be in contact with the polymer Poly in a catalytic amount to catalyze the in-situ polymerization reaction of cyano olefin carboxylic acid derivative monomers (such as cyanoacrylic acid derivative monomers) on the surface of the lithium metal.
[0396] In a second aspect, the present application provides a negative electrode plate, which includes a lithium-containing layer and a polymer layer stacked, and the negative electrode plate includes the lithium metal negative electrode material described in the first aspect of the present application;
[0397] The lithium-containing layer includes the lithium-containing metal in the lithium metal negative electrode material, and the polymer layer includes the polymer Poly in the lithium metal negative electrode material.
[0398] In this application, "active material" and "active substance" have the same meaning and can be used interchangeably; "positive electrode active substance" and "positive electrode active material" have the same meaning and can be used interchangeably; "negative electrode active substance" and "negative electrode active material" have the same meaning and can be used interchangeably.
[0399] In the present application, the "negative electrode sheet substrate" can provide a negative electrode active material for a lithium metal battery. The negative electrode sheet substrate in the negative electrode sheet at least includes a lithium-containing layer in contact with the polymer layer, that is, the lithium-containing layer is located at the outermost layer of the negative electrode sheet substrate. In other words, the outermost layer of at least one side of the negative electrode sheet substrate is a lithium-containing layer. In one embodiment, the negative electrode sheet substrate consists of a lithium-containing layer. The polymer layer is chemically connected to at least a portion of the lithium in the lithium-containing layer. Further, "chemical connection" here refers to covalent connection. The thickness of the negative electrode sheet substrate can be the thickness of the lithium negative electrode in a conventional lithium metal battery. The "lithium negative electrode" here refers to the thickness of the negative electrode active material layer provided by lithium metal or lithium alloy. A non-limiting example of the thickness of the lithium-containing layer is 5 μm to 40 μm. The thickness of the lithium-containing layer can also be selected from the interval consisting of any one or two of the following thicknesses: 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 40 μm, etc.
[0400] In the present application, the term "lithium-containing layer" refers to a structural layer containing metallic lithium. The lithium-containing layer can be substantially composed of lithium (Li) metal, or a lithium alloy, or a composition comprising lithium metal and a lithium alloy (e.g., a composition substantially composed of lithium metal and a lithium alloy). The lithium in the lithium-containing layer can play multiple roles. On the one hand, it can catalyze the in-situ polymerization reaction of cyano-olefin carboxylic acid derivative monomers, on the other hand, it can form a stable covalent connection with the cyano group carried by the polymer Poly, and on the other hand, it can also serve as a lithium source for the negative electrode active material. The thickness of the lithium-containing layer can be any suitable thickness, as long as it is sufficient to provide an amount of catalyst that can support the in-situ polymerization reaction of cyano-olefin carboxylic acid derivative monomers, such as the thickness of the lithium negative electrode in a conventional lithium metal battery. When the thickness of the lithium-containing layer is relatively thin, a second negative electrode active material layer can also be provided on the side of the lithium-containing layer away from the polymer layer. At this time, the negative electrode sheet substrate includes the lithium-containing layer and the second negative electrode active material layer. The composition and content of the lithium-containing layer and the second negative electrode active material layer can be the same or different.
[0401] In the present application, the lithium-containing layer “substantially consists of lithium metal” means that the weight proportion of metallic lithium is very high. The proportion described by “substantially” here is, for example, greater than or equal to 80%, greater than or equal to 85%, greater than or equal to 90%, greater than or equal to 95%, greater than or equal to 96%, greater than or equal to 97%, greater than or equal to 98%, greater than or equal to 99%, equal to 100%, etc.
[0402] The negative electrode plate includes a lithium metal negative electrode material distributed in a lithium-containing layer and a polymer layer. On at least one side of the negative electrode plate, the lithium-containing layer is stably connected to a dense and uniform polymer layer by chemical bonding. The polymer layer has certain elasticity, flexibility and swelling properties, which can make the polymer layer and the lithium-containing layer, and the polymer layer and the isolation membrane fit firmly, tightly and durably. It can better adapt to the larger volume expansion of the negative electrode side during charging, and can play the role of a protective layer at the negative electrode of the lithium metal secondary battery for a long time. The polymer layer can effectively inhibit the contact reaction between the electrolyte and lithium metal, reduce the consumption of the electrolyte and lithium metal, and extend the cycle life. It can also utilize the fluorinated aliphatic chain Rf in the lithium metal negative electrode material to promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium metal negative electrode side. In addition, the elasticity, flexibility and swelling comprehensive performance of the polymer layer not only promote the close fit between the polymer layer and the lithium-containing layer, but also help to exert good ionic conductivity, reduce interface polarization, and reduce interface impedance, so that the lithium metal secondary battery can achieve higher energy density, power density, charge and discharge cycle stability and higher safety performance in the presence of the polymer layer.
[0403] In some embodiments, the lithium-containing layer is substantially composed of the lithium-containing metal. In some embodiments, the material of the lithium-containing layer is lithium. In other embodiments, the material of the lithium-containing layer is a lithium alloy.
[0404] In the present application, the lithium-containing layer “substantially consists of lithium-containing metal” means that the weight proportion of lithium-containing metal is very high. The proportion described by “substantially” here is, for example, greater than or equal to 80%, greater than or equal to 85%, greater than or equal to 90%, greater than or equal to 95%, greater than or equal to 96%, greater than or equal to 97%, greater than or equal to 98%, greater than or equal to 99%, equal to 100%, etc.
[0405] In some embodiments, the polymer layer further contains a first electrolyte, and the first electrolyte contains a lithium salt (referred to as a first electrolyte lithium salt) and a solvent (referred to as a first electrolyte solvent).
[0406] In some embodiments, the lithium salt is selected from one or more of lithium hexafluorophosphate (LiPF6), tetrafluoroboric acid (LiBF4), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiDFOB), lithium perchlorate (LiClO4) and lithium bis(oxalate)borate (LiBOB).
[0407] In some embodiments, the first electrolyte solvent is selected from one or more of ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), diphenyl carbonate (DPhC), dibutyl carbonate (DBC), butylene carbonate (BC), ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), dioxolane (DOL), methyl nonafluoro-n-butyl ether (MFE), 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (HFE-458), octafluoropentyl-tetrafluoroethyl ether (F-EAE), 1,2-bis(cyanoethoxy)ethane (DENE), diphenyl ether (DPE) and 18-crown-6.
[0408] In some embodiments, the negative electrode plate satisfies one or more of the following characteristics:
[0409] The lithium salt includes one or more of lithium hexafluorophosphate, tetrafluoroboric acid, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate and lithium bis(oxalate)borate;
[0410] The first electrolyte solvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, diphenyl carbonate, dibutyl carbonate, butylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, dioxolane, methyl nonafluoro-n-butyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, octafluoropentyl-tetrafluoroethyl ether, 1,2-bis(cyanoethoxy)ethane, diphenyl ether and 18-crown-6.
[0411] In some embodiments, the concentration of the lithium salt in the first electrolyte is selected from 0.2mol / L to 8mol / L; optionally, the concentration of the lithium salt in the first electrolyte is selected from 0.5mol / L to 5mol / L; further optionally, the concentration of the lithium salt in the first electrolyte is selected from 0.5mol / L to 2mol / L. The concentration of the lithium salt in the first electrolyte can also be any of the following concentrations or an interval consisting of any two of the following concentrations: 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, etc. (all units are mol / L).
[0412] The polymer layer of the lithium metal negative electrode material contains an electrolyte (which can be recorded as the first electrolyte). The concentration of lithium salt in the first electrolyte can affect the deposition morphology of lithium ions. The concentration of lithium salt can change the Li +The solvation effect affects the composition of the solid electrolyte interface film (SEI film) and the deposition morphology of lithium ions. By controlling the lithium salt in the electrolyte at a more appropriate concentration, it is more conducive to promoting dense and uniform deposition of lithium ions and reducing the volume expansion of the negative electrode side. In addition, by controlling the lithium salt in the electrolyte at a more appropriate concentration, the polymer layer can also have more suitable mechanical properties, such as flexibility and elasticity, and can also achieve better lithium ion conductivity during charging and discharging. When the lithium salt concentration is too high, the mechanical properties of the polymer layer may deviate from the optimal range. When the lithium salt concentration is too low, the lithium ion conductivity during charging and discharging may deviate from the larger range.
[0413] In some embodiments, the mass proportion of the first electrolyte in the polymer layer is 20% to 80%; optionally, the mass proportion of the first electrolyte in the polymer layer is 30% to 60%; further optionally, the mass proportion of the first electrolyte in the polymer layer is 40% to 60%; further optionally, the mass proportion of the first electrolyte in the polymer layer is 40% to 55%. The mass proportion of the first electrolyte in the polymer layer can also be any of the following percentages or an interval consisting of any two of the following percentages: 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 80%, etc. Non-limiting examples of the interval consisting of any two percentages are 30% to 80%, 40% to 80%, 30% to 60%, 40% to 60%, 30% to 55%, 40% to 55%, etc.
[0414] In some embodiments, the mass ratio of the polymer Poly to the first electrolyte is 4:1 to 0.25:1; optionally, the mass ratio of the polymer Poly to the first electrolyte is 3:1 to 0.5:1; further optionally, the mass ratio of the polymer Poly to the first electrolyte is 2.5:1 to 1:1; further optionally, the mass ratio of the polymer Poly to the first electrolyte is 7:3 to 2:1. The mass ratio of the polymer Poly to the first electrolyte can also be 4:1, 3.5:1, 3:1, 2.5:1, 7:3, 2:1, 1.5:1, 1:1, 0.9:1, 0.8:1, 0.7:1, 0.6:1, 0.5:1, 0.4:1, 0.3:1, 1:3, 1:3.5, 0.25:1, etc. It can also be selected from the interval consisting of any two of the above ratios.
[0415] By controlling the mass proportion of the first electrolyte in the polymer layer or controlling the mass ratio of the polymer Poly and the first electrolyte in the polymer layer within a more suitable range, the electrolyte can be adjusted to have a more suitable mass proportion in the polymer layer. The mass proportion of the electrolyte in the polymer layer can affect the elastic modulus and ionic conductivity of the protective layer. In the first electrolyte, the presence of a certain amount of lithium salt (recorded as the first electrolyte lithium salt) and solvent (recorded as the first electrolyte solvent) can plasticize the polymer layer and improve the elasticity of the polymer layer. In addition, in the process of forming a polymer layer by in-situ polymerization, the lithium salt and solvent in the first electrolyte can be incorporated into the polymer layer, so that the polymer layer has a sponge-like loose porous structure on a microscopic scale, and the pores are filled with electrolyte, which can provide a path for the subsequent transmission of lithium ions.
[0416] In some embodiments, based on the first electrolyte, the swelling rate of the polymer layer can be any of the following percentages or an interval selected from any two of the following percentages: 8%, 10%, 11%, 12%, 14%, 15%, 16%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, etc. Based on the first electrolyte, non-limiting examples of the swelling rate of the polymer layer are also such as 15% to 65%, 18% to 65%, 30% to 65%, 15% to 55%, 18% to 55%, 30% to 55%, 15% to 40%, 18% to 40%, 30% to 40%, etc.
[0417] In the present application, the "swelling rate of the polymer layer" generally refers to the test value at 20°C to 30°C unless otherwise specified. In some embodiments, the swelling rate of the polymer layer refers to the swelling rate at 25°C. Please refer to the test method of "Structure and Performance Test" in the Examples section below.
[0418] In some embodiments, based on the first electrolyte, the swelling rate of the polymer layer at 25°C is 8% to 65%; further optionally, the swelling rate of the polymer layer at 25°C is 15% to 55%; further optionally, the swelling rate of the polymer layer at 25°C is 18% to 44%; further optionally, the swelling rate of the polymer layer at 25°C is 30% to 40%.
[0419] In some embodiments, based on the first electrolyte, the ionic conductivity of the swollen polymer layer can be any of the following values or an interval selected from any two of the following values: 5mS / cm, 4.5mS / cm, 4mS / cm, 3.5mS / cm, 3mS / cm, 2.6mS / cm, 2.5mS / cm, 2mS / cm, 1.5mS / cm, 1mS / cm, 0.95mS / cm, 0.9mS / cm, 0.8mS / cm, 0.7mS / cm, 0.6mS / cm, 0.5mS / cm, 0.4mS / cm, 0.3mS / cm, 0.2mS / cm, 0 .1mS / cm, 0.09mS / cm, 0.08mS / cm, 0.07mS / cm, 0.06mS / cm, 0.05mS / cm, 0.04mS / cm, 0.03mS / cm, 0.02mS / cm, 0.01mS / cm, 0.005mS / cm, 0.001mS / cm, etc., and can also be selected from any of the following ranges: 0.001mS / cm to 5mS / cm, 0.1mS / cm to 5mS / cm, 0.5mS / cm to 5mS / cm, 0.9mS / cm to 4.8mS / cm, 0.95mS / cm to 2.6mS / cm.
[0420] In this application, 1mS / cm means 1×10 -3 S / cm.
[0421] In the present application, "ionic conductivity of the swollen polymer layer" generally refers to the test value at 20°C to 30°C unless otherwise specified. In some embodiments, the ionic conductivity of the swollen polymer layer refers to the ionic conductivity at 25°C. Please refer to the test method of "Structure and Performance Test" in the Examples section below.
[0422] In some embodiments, based on the first electrolyte, the ionic conductivity of the swollen polymer layer at 25°C is selected from 0.001mS / cm to 5mS / cm; optionally, the ionic conductivity of the swollen polymer layer at 25°C is selected from 0.1mS / cm to 5mS / cm; alternatively, the ionic conductivity of the swollen polymer layer at 25°C is selected from 0.5mS / cm to 5mS / cm; alternatively, the ionic conductivity of the swollen polymer layer at 25°C is selected from 0.9mS / cm to 4.8mS / cm; alternatively, the ionic conductivity of the swollen polymer layer at 25°C is selected from 0.95mS / cm to 2.6mS / cm.
[0423] In some embodiments, the thickness of the polymer layer is 5 nm to 10 μm; optionally, the thickness of the polymer layer is 0.02 μm to 8 μm; further optionally, the thickness of the polymer layer is 0.05 μm to 8 μm; further optionally, the thickness of the polymer layer is 0.05 μm to 5 μm; further optionally, the thickness of the polymer layer is 0.1 μm to 5 μm. The thickness of the polymer layer can also be any of the following thicknesses or a range consisting of any two of the following thicknesses: 5nm, 5.5nm, 6nm, 6.5nm, 7nm, 7.5nm, 8nm, 8.5nm, 9nm, 9.5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 200nm, 250nm, 300nm, 400nm, 500nm, 600nm, 700nm, 800nm, 900nm, 1μm, 1.5μm, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 6μm, 7μm, 8μm, 9μm, 9.5μm, 10μm, etc.
[0424] The thickness of the polymer layer on the surface of the lithium-containing metal can be controlled at a thin nanoscale, which is more conducive to the assembled battery cell showing a smaller interface impedance.
[0425] In some embodiments, the elastic modulus of the polymer layer can be any of the following values or an interval selected from any two of the following values: 0.1 MPa, 0.2 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, 14 MPa, 15 MPa, 16 MPa, 18 MPa, 20 MPa, 25 MPa, 29 MPa, 30 MPa, 35 MPa, 40 MPa, 41 MPa, 45 MPa, 46 MPa, 50 MPa, 60 MPa, 65 MPa, etc. Non-limiting examples of the elastic modulus of the polymer layer are: 0.1 MPa to 65 MPa, 0.5 MPa to 65 MPa, 1 MPa to 65 MPa, 10 MPa to 65 MPa, 15 MPa to 65 MPa, 18 MPa to 65 MPa, 20 MPa to 65 MPa, 29 MPa to 65 MPa, 0.1 MPa to 50 MPa, 0.5 MPa to 50 MPa, 1 MPa to 50 MPa, 10 MPa to 50 MPa, 15 MPa to 50 MPa, 18 MPa to 50 MPa, 20 MPa to 50 MPa, 29 MPa to 65 MPa, Pa~50MPa, 0.1MPa~46MPa, 0.5MPa~46MPa, 1MPa~46MPa, 10MPa~46MPa, 15MPa~46MPa, 18MPa~46MPa, 20MPa~46MPa, 29MPa~46 MPa, 0.1MPa~41MPa, 0.5MPa~41MPa, 1MPa~41MPa, 10MPa~41MPa, 15MPa~41MPa, 18MPa~41MPa, 20MPa~41MPa, 29MPa~41MPa, etc.
[0426] In the present application, the "elastic modulus of the polymer layer" generally refers to the test value at 20°C to 30°C unless otherwise specified. In some embodiments, the elastic modulus of the polymer layer refers to the elastic modulus at 25°C. Please refer to the test method of "Structure and Performance Test" in the Examples section below.
[0427] In some embodiments, the elastic modulus of the polymer layer at 25°C is 0.1MPa to 65MPa; optionally, the elastic modulus of the polymer layer at 25°C is 0.5MPa to 50MPa; further optionally, the elastic modulus of the polymer layer at 25°C is 10MPa to 46MPa; further optionally, the elastic modulus of the polymer layer at 25°C is 18MPa to 41MPa; further optionally, the elastic modulus of the polymer layer at 25°C is 29MPa to 41MPa.
[0428] In some embodiments, the elastic deformation range of the polymer layer can be selected from any one of the following percentages or any two percentage intervals: 55%, 60%, 65%, 70%, 80%, 90%, 100%, 150%, 200%, 220%, 240%, 250%, 260%, 265%, 270%, 280%, 300%, 350%, etc. Non-limiting examples of the elastic deformation range of the polymer layer are also such as: 55% to 350%, 55% to 300%, 55% to 280%, 150% to 350%, 150% to 300%, 150% to 280%, 160% to 350%, 160% to 300%, 160% to 280%, 168% to 350%, 168% to 300%, 168% to 280%, etc.
[0429] In the present application, the "elastic deformation range of the polymer layer" generally refers to the test value under the condition of 20°C to 30°C unless otherwise specified. In some embodiments, the elastic deformation range of the polymer layer refers to the elastic deformation range at 25°C. Please refer to the test method of "Structure and Performance Test" in the Examples section below.
[0430] In some embodiments, the elastic deformation range of the polymer layer at 25°C is 55% to 350%; optionally, the elastic deformation range of the polymer layer at 25°C is 150% to 350%; further optionally, the elastic deformation range of the polymer layer at 25°C is 150% to 300%; further optionally, the elastic deformation range of the polymer layer at 25°C is 168% to 280%.
[0431] By controlling parameters such as the elastic modulus and elastic deformation range of the polymer layer within a more appropriate range, it is beneficial to make the polymer layer have more appropriate elasticity, better promote close contact between the polymer layer and the lithium-containing metal layer, reduce interface impedance, and help achieve better energy density and power density.
[0432] In some embodiments, the volume expansion rate of the negative electrode plate is less than 130%, and further, it can be selected from 5% to 130%. The volume expansion rate of the negative electrode plate can also be any of the following percentages or an interval consisting of any two of the following percentages: 6%, 7%, 8%, 9%, 10%, 11%, 12%, 14%, 15%, 16%, 18%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 92%, 95%, 100%, 102%, etc. In some embodiments, the volume expansion rate of the negative electrode plate is 5% to 128%. In some embodiments, the volume expansion rate of the negative electrode plate is 5% to 102%.
[0433] In this application, the "volume expansion rate of the pole piece", unless otherwise specified, generally refers to the test value under the condition of 20°C to 30°C. In some embodiments, the volume expansion rate of the pole piece refers to the volume expansion rate at 25°C. Please refer to the test method of "Structure and Performance Test" in the Examples section below.
[0434] In some embodiments, the negative electrode sheet substrate further includes a negative electrode current collector; the negative electrode current collector is located on a side of the lithium-containing layer away from the polymer layer.
[0435] In some embodiments, the negative electrode current collector is located between the negative electrode current collector and the lithium-containing layer and is provided with or without a second negative electrode active material layer. Furthermore, the components of the second negative electrode active material layer and the lithium-containing layer may be the same or different.
[0436] In some embodiments, the negative electrode sheet includes a negative electrode current collector, and the second negative electrode active material layer is disposed between the negative electrode current collector and the lithium-containing layer.
[0437] In some embodiments, only the outermost layer on one side of the negative electrode substrate is provided with a lithium-containing layer (see Figure 1 , Figure 2 and Figure 3 ).
[0438] In some embodiments, the outermost layers on both sides of the negative electrode substrate are provided with lithium-containing layers (see Figure 4 and Figure 5 ). The lithium-containing layers on both sides may contain the same or different amounts of lithium. The lithium content in the lithium-containing layer may refer to the above definition. The lithium content in the second negative electrode active material layer may be selected from the lithium content in the negative electrode active material layer of a conventional lithium metal battery. Non-limiting examples of the second negative electrode active material layer include lithium metal, lithium alloy, or a combination of the two. Regarding the combination of the two, for example, different regions of the negative electrode active material layer may have different compositional compositions.
[0439] In the present application, the "second negative electrode active material layer" can be any suitable negative electrode active material layer among the active material layers of reported lithium metal batteries. The second negative electrode active material layer can be substantially composed of lithium (Li) metal, or a lithium alloy, or a combination substantially composed of lithium metal and a lithium alloy.
[0440] In some embodiments, the outermost layers on both sides of the negative electrode substrate are provided with lithium-containing layers, and the surfaces of the lithium-containing layers on both sides are provided with polymer layers (see Figure 4 and Figure 5 ); The chemical composition and content of the polymer layers on both sides can be the same or different.
[0441] In some embodiments, the negative electrode sheet includes Figure 1 The structure shown includes a stacked lithium-containing layer 130 and a polymer layer 200. The lithium-containing layer contains lithium, lithium alloy or a combination of the two, and the lithium-containing layer here serves as a negative electrode active material layer; the polymer layer contains a polymer Poly, which is covalently bonded to the lithium in the lithium-containing layer (for example, through the reaction between the cyanide group in the Poly and the lithium), forming a stable chemical connection, so that the polymer layer is firmly connected to the surface of the lithium-containing layer. The polymer Poly can be selected from the polymer Poly described in any embodiment of the first aspect. The definition of the first electrolyte is as described above.
[0442] In some embodiments, the negative electrode sheet includes Figure 2 The structure shown includes a stacked negative electrode sheet substrate 100 and a polymer layer 200; the negative electrode sheet substrate 100 includes a stacked negative electrode current collector 110 and a lithium-containing layer 130, and the polymer layer 200 is located on the surface of the lithium-containing layer 130 away from the negative electrode current collector 110. Further, the polymer layer includes a polymer Poly and a first electrolyte. The lithium-containing layer contains lithium, a lithium alloy, or a combination of the two, and the polymer layer contains a polymer Poly, which is covalently bonded to the lithium in the lithium-containing layer to form a stable chemical connection, so that the polymer layer is firmly connected to the surface of the negative electrode sheet substrate.
[0443] In some embodiments, the negative electrode sheet includes Figure 3 The structure shown includes a negative electrode sheet substrate 100 and a polymer layer 200 which are stacked and distributed; the negative electrode sheet substrate 100 includes a negative electrode current collector 110, a second negative electrode active material layer 120 and a lithium-containing layer 130 which are stacked and distributed in sequence, and the polymer layer is located on the surface of the lithium-containing layer 130 away from the negative electrode current collector 110.
[0444] In some embodiments, the negative electrode sheet includes Figure 4 The structure shown includes a negative electrode sheet substrate 100 and two polymer layers 200 respectively disposed on the surfaces of both sides of the negative electrode sheet substrate 110; the negative electrode sheet substrate includes a negative electrode current collector 110, and two lithium-containing layers 130 respectively disposed on the surfaces of both sides of the negative electrode current collector 110, and the lithium-containing layers 130 on both sides of the negative electrode sheet are directly connected to the corresponding polymer layers 200 (chemical connection is achieved through covalent action). The chemical composition and content of the polymer layers 130 on both sides can be the same or different. The chemical composition and content of the lithium-containing layers 130 on both sides can be the same or different.
[0445] In some embodiments, the negative electrode sheet includes Figure 5The structure shown includes a negative electrode sheet substrate 100 and two polymer layers 200 respectively arranged on the two side surfaces of the negative electrode sheet substrate 110; the negative electrode sheet substrate includes a negative electrode current collector 110, two second negative electrode active material layers 120 respectively arranged on the two side surfaces of the negative electrode current collector 110, and two lithium-containing layers 130 respectively arranged on the two second negative electrode active material layers 120 away from the negative electrode current collector 110. The lithium-containing layers 130 on both sides of the negative electrode sheet are directly connected to the corresponding polymer layers 200 (chemical connection is achieved through covalent action). The chemical composition and content of the polymer layers 130 on both sides can be the same or different. The chemical composition and content of the second negative electrode active material layers 120 on both sides can be the same or different. The chemical composition and content of the lithium-containing layers 130 on both sides can be the same or different.
[0446] In some embodiments, the negative electrode plate generally includes a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector. The negative electrode film layer includes the aforementioned lithium-containing layer, and also includes a polymer layer formed on at least one side of the surface of the lithium-containing layer away from the inside of the negative electrode film layer, that is, the polymer layer is located on the surface of the lithium-containing layer away from the negative electrode current collector, and the polymer layer is located at the outermost layer of the negative electrode plate, and further, the polymer layer and the lithium-containing layer are chemically connected through covalent action.
[0447] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0448] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material on a polymer material substrate. Non-limiting examples of metal materials may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. Non-limiting examples of polymer material substrates may include one or more substrates of materials such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0449] In some embodiments, the negative electrode active material in the negative electrode active material layer may adopt the negative electrode active material for lithium metal batteries known in the art. As an example, the negative electrode active material suitable for the present application may include one or more of lithium metal and lithium alloy. In addition to lithium, the lithium alloy may also contain one or more of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel, titanium, etc. The lithium-containing layer in the present application can be used as the first negative electrode active material layer, and a second negative electrode active material layer may be provided between the lithium-containing layer and the negative electrode current collector. The composition and content of the second negative electrode active material layer may be the same as or different from the composition and content in the lithium-containing layer.
[0450] In some embodiments, the negative electrode film layer may further include a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0451] In some embodiments, the negative electrode film layer may further include a conductive agent, which may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0452] In some embodiments, the negative electrode active material layer may further optionally include other auxiliary agents, such as a thickener, etc. Non-limiting examples of the thickener may include sodium carboxymethylcellulose (CMC-Na), and the like.
[0453] In a third aspect, the present application provides a secondary battery (also referred to as a lithium metal secondary battery), which includes a positive electrode sheet, a separator, and the negative electrode sheet described in the second aspect of the present application, wherein the separator is disposed between the positive electrode sheet and the negative electrode sheet, and the polymer layer is disposed on a side of the negative electrode sheet close to the separator. Since the negative electrode sheet includes a lithium-containing layer, the secondary battery in the third aspect is also referred to as a lithium metal secondary battery.
[0454] The negative electrode plate in the lithium metal secondary battery includes a lithium metal negative electrode material distributed in a lithium-containing layer and a polymer layer. On at least one side of the negative electrode plate, the lithium-containing layer is stably connected to a dense and uniform polymer layer by chemical bonding. The polymer layer has certain elasticity, flexibility and swelling properties, which can make the polymer layer and the lithium-containing layer, and the polymer layer and the isolation membrane fit firmly, tightly and durably. It can better adapt to the larger volume expansion of the negative electrode side during charging, and can play the role of a protective layer at the negative electrode of the lithium metal secondary battery for a long time. The polymer layer can effectively inhibit the contact reaction between the electrolyte and lithium metal, reduce the consumption of electrolyte and lithium metal, and extend the cycle life. It can also use the fluorinated aliphatic chain Rf in the lithium metal negative electrode material to promote the uniform deposition of lithium ions, inhibit the formation of lithium dendrites, and alleviate the volume expansion of the lithium metal negative electrode side. In addition, the elasticity, flexibility and swelling comprehensive performance of the polymer layer not only promote the close fit between the polymer layer and the lithium-containing layer, but also help to exert good ionic conductivity, reduce interface polarization, and reduce interface impedance, so that the lithium metal secondary battery can achieve higher energy density, power density, charge and discharge cycle stability and higher safety performance in the presence of the polymer layer. .
[0455] In addition, by inhibiting the contact reaction between the electrolyte and lithium metal and reducing the consumption of the electrolyte and lithium metal, the coulombic efficiency of the battery can also be improved.
[0456] In some embodiments, the lithium metal secondary battery further includes a second electrolyte, and the components of the second electrolyte and the first electrolyte in the polymer layer may be the same or different.
[0457] Typically, a secondary battery includes a positive electrode sheet, a negative electrode sheet, a cell electrolyte and a separator. During the battery charge and discharge process, active ions are embedded and removed back and forth between the positive electrode sheet and the negative electrode sheet. The cell electrolyte plays a role in conducting active ions between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing active ions to pass through. The active ions in the secondary battery provided in the present application may be lithium ions, but may not be limited thereto.
[0458] Positive electrode
[0459] In the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, the positive electrode film layer includes a positive electrode active material layer, and further, the positive electrode active material layer includes a positive electrode active substance.
[0460] As a non-limiting example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0461] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material on a polymer material substrate. In the negative electrode current collector, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the negative electrode current collector, non-limiting examples of the polymer material substrate include one or more substrates of materials such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.
[0462] In some embodiments of the present application, the secondary battery is a lithium-ion secondary battery. A lithium-ion secondary battery utilizes the embedding and de-embedding of lithium ions in electrodes and the transmission in electrolytes to achieve the charging and discharging process. Generally speaking, the active ions in a lithium-ion secondary battery are lithium ions, but this is not limited to this.
[0463] The positive electrode active material may adopt the positive electrode active material for the battery known in the art. As a non-limiting example, the positive electrode active material may include one or more of the following materials or substances: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials or substances, and other traditional materials or substances that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, non-limiting examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and their modified compounds. Non-limiting examples of lithium cobalt oxide include LiCoO2; non-limiting examples of lithium nickel oxide include LiNiO2; non-limiting examples of lithium manganese oxide include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxide include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc. Non-limiting examples of lithium nickel cobalt aluminum oxides include LiNi 0.85 Co 0.15 Al 0.05 O2. Non-limiting examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon. Non-limiting examples of lithium iron phosphate include LiFePO4 (also referred to as LFP); non-limiting examples of lithium manganese phosphate include LiMnPO4.
[0464] In some embodiments, the positive electrode active material may include but is not limited to one or more of the following materials or substances: lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, sodium oxide and potassium oxide, and materials consisting of any of the foregoing substances and doping elements; further, the doping elements in any one of the positive electrode active materials independently include one or more of transition metal elements and non-transition metal elements.
[0465] In some embodiments, the positive electrode active material layer may also optionally include a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0466] In some embodiments, the positive electrode active material layer may further include a conductive agent. As a non-limiting example, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0467] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive active material, the conductive agent, the binder and any other components, are dispersed in a solvent to form a positive electrode slurry; the positive electrode slurry is coated on at least one side of the positive electrode collector, and after drying, compaction (compacting can be performed by cold pressing), etc., the positive electrode sheet can be obtained. The type of solvent can be selected from but not limited to any one of the aforementioned embodiments, such as N-methylpyrrolidone (NMP). The surface of the positive electrode collector coated with the positive electrode slurry can be on a single surface of the positive electrode collector or on both surfaces of the positive electrode collector. The solid content of the positive electrode slurry can be 40wt% to 80wt%. The compacted density of the positive electrode sheet can be 3.0 to 3.6g / cm 3 , can be selected as 3.3~3.5g / cm 3 .
[0468] Cell electrolyte
[0469] The cell electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of cell electrolyte, which can be selected according to needs. For example, the cell electrolyte can be liquid, gel or all-solid.
[0470] In some embodiments, the battery cell electrolyte uses a second electrolyte solution, which includes an electrolyte salt and a solvent (which may be referred to as a second electrolyte solution solvent).
[0471] In some embodiments, the components of the core electrolyte (eg, the second electrolyte) and the first electrolyte in the polymer layer may be the same or different.
[0472] When the cell electrolyte (such as the second electrolyte) in the secondary battery has the same composition as the first electrolyte in the polymer layer, the consistency of lithium ion transmission in the cell can be maintained, reducing interference from multiple factors such as electrolyte solvation and interface side reactions.
[0473] When the composition of the core electrolyte in the secondary battery is different from that of the first electrolyte in the polymer layer, the formation of a stable SEI can be induced in a direction on the lithium-containing layer side, thereby regulating the deposition morphology of lithium ions.
[0474] In some embodiments, the electrolyte salt in the second electrolyte may include one or more of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0475] In some embodiments, the solvent in the second electrolyte may include one or more of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0476] In some embodiments, the battery electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0477] In some embodiments, the additives in the battery electrolyte may include one or more of vinylene carbonate (VC), vinyl ethylene carbonate (VEC), fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), trifluoromethylethylene carbonate (TFPC), methylene methanedisulfonate (MMDS), 1-propylene-1,3-sultone (PST), vinyl sulfite (ES), propylene sulfite (PS), vinyl sulfate (DTD), succinonitrile (SN), adiponitrile (AND), sulfonate cyclic quaternary ammonium salt, tris(trimethylsilyl) phosphate (TMSP), tris(trimethylsilyl) borate (TMSB) and anisole.
[0478] Isolation film
[0479] In this application, unless otherwise specified, "separation membrane" and "diaphragm" have the same meaning and can be used interchangeably.
[0480] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0481] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0482] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0483] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the cell electrolyte.
[0484] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and further, non-limiting examples of plastic may include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0485] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 6 The secondary battery 5 is a square structure as an example.
[0486] In some embodiments, reference Figure 7 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can choose according to specific actual needs. The secondary battery provided in the present application can be circulated under certain charging current density conditions.
[0487] In some embodiments, the charging current density of the secondary battery can be selected from any one of the following values or an interval consisting of any two values: 0.1 mA / cm 2 , 0.2mA / cm 2 , 0.3mA / cm 2 , 0.4mA / cm 2 , 0.5mA / cm 2 , 0.6mA / cm 2 , 0.7mA / cm 2 , .8mA / cm 2 , 0.9mA / cm 2 , 1mA / cm 2 , 1.5mA / cm 2 , 2mA / cm 2 , 2.5mA / cm 2 , 3mA / cm 2 , 3.5mA / cm 2 , 4mA / cm 2 , 4.5mA / cm 2, 5mA / cm 2 , 5.5mA / cm 2 , 6mA / cm 2 , 7mA / cm 2 , 8mA / cm 2 , 9mA / cm 2 , 10mA / cm 2 , 11mA / cm 2 , 12mA / cm 2 wait.
[0488] In some embodiments, the applicable charging current density can also be selected from any of the following ranges: 0.1 mA / cm 2 ~3.5mA / cm 2 , 1mA / cm 2 ~3.5mA / cm 2 , 0.1mA / cm 2 ~12mA / cm 2 , 1mA / cm 2 ~12mA / cm 2 , 0.1mA / cm 2 ~4mA / cm 2 , 1mA / cm 2 ~4mA / cm 2 wait.
[0489] The secondary battery provided in the present application can be cycled under the aforementioned charging current density conditions.
[0490] In some embodiments, the capacity retention rate of the secondary battery after a certain number of cycles (such as 50 cycles) is very high. In some embodiments, the capacity retention rate of the secondary battery after 50 cycles is higher than 80%.
[0491] In this application, the "capacity retention rate after 50 cycles" of a secondary battery, unless otherwise specified, generally refers to a test value at 20°C to 30°C. In some embodiments, the capacity retention rate of a secondary battery after 50 cycles refers to the volume expansion rate at 25°C. Please refer to the test method of "Structure and Performance Test" in the Examples section below.
[0492] The present application may also provide a battery module, which includes the secondary battery described in the fourth aspect of the present application.
[0493] The present application may also provide a battery pack, which includes the battery module described above. In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0494] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0495] In a fourth aspect, the present application provides an electrical device, which includes the lithium metal secondary battery described in the third aspect of the present application.
[0496] The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include mobile devices, electric vehicles, electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto. Among them, the mobile device may be, for example, a mobile phone, a laptop computer, etc.; the electric vehicle may be, for example, a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc., but are not limited thereto.
[0497] As the electrical device, a secondary battery can be selected according to its usage requirements.
[0498] Figure 8 The power consumption device 6 is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. In order to meet the power consumption device's requirements for high power and high energy density of secondary batteries, a battery pack or a battery module can be used.
[0499] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0500] In a fifth aspect, the present application provides an application of a monomer composition in preparing a negative electrode sheet or a lithium metal secondary battery, wherein the monomer composition comprises a first monomer represented by formula (M1) and a second monomer represented by formula (M2):
[0501]
[0502] wherein X1, X2, Y1, Y2, A1, A2, Rf and Rd are respectively as defined in the first aspect of the present application; z is as defined in the first aspect of the present application; at least one of Y1 and Y2 is cyano;
[0503] The negative electrode plate includes a lithium-containing layer, and the lithium-containing layer contains lithium metal;
[0504] The first monomer and the second monomer are used to form a polymer layer bonded to the lithium metal in the negative electrode plate.
[0505] In the present application, the first monomer may also be referred to as monomer compound M1, and the second monomer may also be referred to as monomer compound M2.
[0506] The first monomer and the second monomer in the monomer composition are both cyanoacrylic acid derivatives, the cyano group therein can contact with the lithium in the outermost layer of the negative electrode plate matrix to form a chemical connection, and the carbon-carbon double bonds therein can undergo in-situ polymerization reaction under lithium catalysis, thereby preparing the lithium metal negative electrode material of the first aspect of the present application. At this time, a firmly connected, dense and uniform polymer layer can be formed on the surface of the lithium-containing layer of the negative electrode. The polymer layer has certain elasticity, flexibility and swelling properties, and can play the role of a protective layer for a long time.
[0507] In some embodiments, Y1 and Y2 are both cyano.
[0508] In some embodiments, the application comprises the following steps: the first monomer and the second monomer are brought into contact with lithium metal in the lithium-containing layer to form the polymer layer through an in-situ polymerization reaction.
[0509] In some embodiments, the negative electrode plate is as defined in the second aspect of the present application, and the lithium metal secondary battery is as defined in the third aspect of the present application.
[0510] In a sixth aspect, the present application provides a method for preparing a negative electrode sheet, which comprises the following steps:
[0511] Providing a negative electrode substrate, wherein the outermost layer of at least one side of the negative electrode substrate is a lithium-containing layer, and the lithium-containing layer contains lithium metal; and also providing a reaction mixture containing a monomer composition and a first electrolyte;
[0512] The reaction mixture is coated on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, so that the monomer composition contacts at least a catalytic amount of lithium metal, and the monomer composition undergoes an in-situ polymerization reaction to form a polymer Poly bonded to the lithium metal in the lithium-containing layer;
[0513] Wherein, the monomer composition is as defined in the fifth aspect of the present application;
[0514] The first electrolyte is as defined in the second aspect of the present application.
[0515] In the presence of the first electrolyte, the cyano group in the monomer composition can contact the lithium in the outermost layer of the negative electrode sheet substrate to form a chemical connection (further, a covalent connection), and the carbon-carbon double bond therein can undergo an in-situ polymerization reaction under lithium catalysis to form the aforementioned polymer Poly, thereby preparing the lithium metal negative electrode material of the first aspect of the present application. At this time, a firmly connected, dense and uniform polymer layer can be formed on the surface of the lithium-containing layer of the negative electrode. The polymer layer has certain elasticity, flexibility and swelling properties, and can play a protective layer role for a long time. Compared with the polymer coating of the physical coating method in the conventional technology, the polymer layer formed in the present application is not only stably bonded to the surface of the lithium-containing layer through chemical connection, but also can reduce, avoid or effectively delay the polymer layer from falling off from the surface of the lithium-containing layer during the charge and discharge process. In addition, the polymer layer of the present application is dense and uniform, and the thickness of the polymer layer can be controlled at the nanoscale by in-situ polymerization, so that the assembled battery cell can exhibit a smaller interface impedance.
[0516] In some embodiments, a lithium sheet or a lithium alloy sheet may be used as the negative electrode sheet substrate. In which case, except for unavoidable impurities, the lithium sheet may be substantially composed of lithium alone. In which case, except for unavoidable impurities, the lithium alloy sheet may be substantially composed of lithium alloy.
[0517] In some embodiments, a lithium layer or a lithium alloy layer may be formed on the negative electrode current collector to prepare a negative electrode sheet substrate, wherein the lithium layer is substantially composed of lithium alone except for unavoidable impurities, and the lithium alloy layer is substantially composed of lithium alloy except for unavoidable impurities.
[0518] In the method for preparing the negative electrode sheet, the monomer composition provided in the present application contacts at least a catalytic amount of lithium metal in the lithium-containing layer, on the one hand, providing a chemical connection site for the polymer layer, and on the other hand, effectively catalyzing the in-situ polymerization reaction of the polymerizable monomer (such as a cyano olefin carboxylic acid derivative monomer, and further, a cyano acrylic acid derivative monomer).
[0519] The mass ratio of the polymer Poly in the generated polymer layer to the first electrolyte can be regulated by adjusting the mass ratio of the monomer composition and the first electrolyte. Numerically, it can be estimated and converted according to the mass ratio of the monomer composition raw material to the first electrolyte raw material being equal to the mass ratio of the polymer Poly in the polymer layer to the first electrolyte. In the method for preparing the negative electrode sheet, the mass ratio of the polymer Poly raw material to the first electrolyte raw material can refer to any suitable ratio in the previous or later text of this application, including but not limited to the definition in the second aspect.
[0520] In some embodiments, in the step of coating the reaction mixture on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, the coating method may include at least one of a coating method, a spraying method, a spin coating method, and a vapor deposition method. The coating thickness may be controlled according to the desired thickness of the polymer layer.
[0521] In some embodiments, the reaction temperature of the in-situ polymerization is selected from 30°C to 100°C; alternatively, the reaction temperature of the in-situ polymerization is selected from 30°C to 60°C; alternatively, the reaction temperature of the in-situ polymerization is selected from 40°C to 80°C. The reaction temperature of the in-situ polymerization can also be any of the following temperatures or a range consisting of any two of the following temperatures: 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, etc.
[0522] In some embodiments, the reaction time of the in-situ polymerization is selected from 0.1h to 24h; alternatively, the reaction time of the in-situ polymerization is selected from 0.1h to 12h; further optionally, the reaction time of the in-situ polymerization is selected from 0.1h to 6h. The reaction time of the in-situ polymerization can be any of the following time lengths or an interval consisting of any two of the following time lengths: 0.1h, 0.2h, 0.3h, 0.4h, 0.5h, 0.6h, 0.8h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h, 10h, 11h, 12h, 14h, 15h, 16h, 18h, 20h, 21h, 22h, 24h, etc.
[0523] In some embodiments, the polymer layer formed by the in-situ polymerization reaction is as defined in the second aspect of the present application.
[0524] In some embodiments, the polymer layer described in the second aspect of the present application is formed on the surface of the negative electrode plate substrate.
[0525] In some embodiments, the negative electrode plate substrate is a pure lithium sheet or a lithium alloy. The definition of lithium alloy applicable to the present application can be found in the above text. In some of the embodiments, the mass proportion of the lithium element in the lithium alloy is ≥50%. The mass proportion of the lithium element in the lithium alloy can also be independently any of the following percentages, or independently greater than or equal to any of the following percentages and less than 100%, or independently selected from the interval consisting of any two of the following percentages: 50%, 55%, 60%, 65%, 70%, 75%, 80%, 90%, 95%, 96%, 97%, 98%, 99%.
[0526] When the negative electrode plate substrate is a pure lithium plate or a lithium alloy, the negative electrode plate of the battery may further introduce a negative electrode current collector to facilitate the assembly of the pole lug, or a pure lithium plate covered with a polymer layer may be used as the negative electrode plate.
[0527] In some embodiments, the negative electrode plate is as defined in the second aspect of the present application.
[0528] In a seventh aspect, the present application provides a method for preparing the lithium metal secondary battery described in the third aspect of the present application, the method comprising the following steps: injecting a cell electrolyte into a battery housing containing the aforementioned positive electrode sheet, negative electrode sheet and separator. The separator is disposed between the positive electrode sheet and the negative electrode sheet, and the polymer layer in the negative electrode sheet is disposed on the side of the negative electrode sheet close to the separator.
[0529] Some embodiments of the present application are described below.
[0530] The parameter characterizations mentioned above, including but not limited to elastic modulus, elastic deformation range, polymer swelling rate, ionic conductivity, flexibility test, negative electrode sheet expansion rate, battery cycle performance, etc., can be achieved by adopting or referring to the test methods below, including but not limited to the "Structure and Performance Test" section.
[0531] The embodiments described below are exemplary, are only used to explain the present application, and cannot be construed as limiting the present application. In the embodiments, if the technology or conditions are not indicated, they are carried out according to the description above, or according to the technology or conditions described in the document in this area or according to the product specification. The reagents used or the instruments that do not indicate the manufacturer are conventional products that can be obtained commercially, or can be synthesized in a conventional manner by commercially available products.
[0532] In the following embodiments, room temperature refers to 20°C to 30°C, and further, may be 25°C.
[0533] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed.
[0534] In the following embodiments, unless otherwise specified, the monomer-electrolyte mixture is coated by a coating method. When the polymer layer thickness is expressed as an approximate number, the deviation may be expressed to be no more than ±10%, for example, 0.1±0.01 μm, 1±0.05 μm.
[0535] Preparation of Monomer Compound M1 (First Monomer) and Monomer Compound M2 (Second Monomer)
[0536] The monomer compounds used in the following examples can be obtained from the market (such as 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate, CH2=C(-CN)-C(=O)-OH), or prepared by the following method. For the preparation of intermediates and synthetic products, those skilled in the art can test according to (but not limited to) Fourier transform infrared spectroscopy (FT-IR), 1 It is achievable for those skilled in the art to perform structural characterization by methods such as H NMR testing, gel permeation chromatography (GPC), and X-ray photoelectron spectroscopy (XPS) to confirm whether the structure of the synthesized product conforms to the structural design.
[0537] 1. When X1 or X2 is H
[0538] When X1 in the monomer compound M1 is H, it corresponds to the compound M11 in the following formula, with a structure of CH2=C(-CN)-C(=O)-A1-Rf, which is a cyanoacrylic acid derivative and can be prepared by a condensation reaction between a compound C10 (2-cyanoacrylic acid) and a compound C21 (Rf-A1H), and the reaction generates a linker C(=O)-A1, wherein, when A1 is O, an ester bond (C(=O)-O) is generated by a condensation reaction between a carboxyl group and a hydroxyl group, and when A1 is NH, an amide bond (C(=O)-NH) is generated by a condensation reaction between a carboxyl group and -NH2.
[0539] When X2 in the monomer compound M2 is H, the corresponding compound M21 in the following formula has the structure CH2=C(-CN)-C(=O)-A2-(CH2CH2O) z -pRd can be obtained by reacting compound C10 (2-cyanoacrylic acid) with compound C22 (H-A2-(CH2CH2O) z -pRd) to form a linker C(=O)-A2, wherein when A2 is O, an ester bond (C(=O)-O) is generated by a condensation reaction between a carboxyl group and a hydroxyl group, and when A2 is NH, an amide bond (C(=O)-NH) is generated by a condensation reaction between a carboxyl group and -NH2.
[0540] Wherein, z is a positive integer; when z≥2, the monomer compound M2 is an ether derivative of cyanoacrylic acid. "Ether derivative" refers to a compound containing an ether bond (-O-).
[0541] Wherein, pRd is Rd or a protected form of Rd as defined above. When compound C10 and compound C22 react, if Rd does not undergo an irreversible side reaction, the reaction can be carried out without Rd being protected, that is, pRd is Rd; for example, when Rd is an alkyl group. When compound C10 and compound C22 react, if Rd may undergo an irreversible side reaction, the reaction can be carried out with Rd being protected, that is, pRd is a protected form of Rd. "Irreversible side reaction" means that after an irreversible side reaction occurs, it is difficult to reconvert to the Rd group according to the usual organic chemical synthesis method. In contrast, if, when C10 and compound C22 react, the new group Rd' formed by the transformation of Rd can be reconverted to Rd by using common chemical modification and de-modification methods such as protection, deprotection, complexation, decomplexation, salification, desalination, ionization, deionization, etc., it can be considered that a reversible change occurs and does not fall into the category of "irreversible side reaction".
[0542] The reaction conditions for preparing monomers M11 and M21 can be combined with the raw material structure and refer to the existing methods in the field of organic chemistry, which can be easily realized by those skilled in the art.
[0543]
[0544] 2. When X1 or X2 is not H
[0545] When X1 or X2 is not H, X1 or X2 modified cyanoacrylic acid X1-CH=C(-CN)-C(=O)-OH (denoted as compound C11) or X2-CH=C(-CN)-C(=O)-OH (denoted as compound C12) can be prepared first, and then reacted with the corresponding compound C21 or compound C22 with reference to the preparation method when X1 or X2 is H to prepare the corresponding monomer compound M12 or M22.
[0546] The structural formula of M12 is X1-CH=C(-CN)-C(=O)-A1-Rf, wherein the definitions of X1, A1 and Rf are consistent with those described above.
[0547] The structural formula of M22 is X2-CH=C(-CN)-C(=O)-A2-(CH2CH2O) z -pRd, wherein z, X2, A2 and pRd are defined as above.
[0548]
[0549] Taking compound C11 and X1 as -N(CH3)2 as an example, reference can be made to the synthesis method of the literature "Bredereck, Hellmut, et al. Chemische Berichte, 1964, 97(12), 3397-3406", using acetal compound C31 and cyanoacrylate compound C4 (such as ethyl 2-cyanoacrylate) to prepare X1-modified cyanoacrylate derivatives (compound C51, such as 1-X1-2-ethyl cyanoacrylate), which are hydrolyzed to form X1-modified cyanoacrylic acid (compound C11).
[0550] Taking compound C12 and X2 as -N(CH3)2 as an example, reference can be made to the method in the literature "Bredereck, Hellmut, et al. Chemische Berichte, 1964, 97(12), 3397-3406", using acetal compound C32 and cyanoacrylate compound C4 (such as ethyl 2-cyanoacrylate) to prepare X2-modified cyanoacrylate derivatives (compound C52, such as 1-X2-2-cyanoethyl acrylate), which are hydrolyzed to form X2-modified cyanoacrylic acid (compound C12).
[0551]
[0552] According to nuclear magnetic resonance spectroscopy ( 1 Whether the target compound is formed can be determined based on at least one of the results of H NMR and gas chromatography-mass spectrometry (GC-MS), but not limited thereto. Whether the polymer Poly is formed can be determined based on at least one of the results of molecular weight and viscosity tests.
[0553] Example 1.
[0554] The monomer compound M1 is 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate, the monomer compound M2 is pentaethylene glycol monomethyl ether cyanoacrylate, the first electrolyte lithium salt is lithium bis(fluorosulfonyl)imide, the first electrolyte solvent is ethylene glycol dimethyl ether, and the negative electrode plate substrate is a pure lithium plate.
[0555] (1) Preparation of polymer layer reaction mixture
[0556] At 25°C, 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate, pentaethylene glycol monomethyl ether cyanoacrylate, lithium bis(fluorosulfonyl)imide (LiFSI) and ethylene glycol dimethyl ether (DME) were stirred evenly at room temperature to obtain a monomer-electrolyte mixture. The amount of raw materials used is shown in Table 1-3. The electrolyte here is recorded as the first electrolyte. The concentration of LiFSI in the first electrolyte is 1.0 mol / L.
[0557] (2) Preparation of negative electrode sheet
[0558] The obtained monomer-electrolyte mixture was coated on one side of the lithium sheet and allowed to react at 30°C for 3 hours to obtain a lithium sheet with a transparent and dense polymer layer on one side. The operating parameters can be seen in Table 1-3. The sheet was cut into a Φ16mm diameter disc as the negative electrode sheet.
[0559] (3) Preparation of positive electrode sheet:
[0560] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1 O2, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 98:1:1, and solvent N-methylpyrrolidone (NMP) was added and stirred until the system was uniform to obtain a positive electrode slurry; the positive electrode slurry was evenly coated on one side of the positive electrode current collector aluminum foil, dried at room temperature, transferred to an oven for further drying, and then cut into discs with a diameter of Φ14mm as positive electrode sheets, and the positive electrode surface capacity was 3mAh / cm 2 .
[0561] (4) Preparation of electrolyte:
[0562] Lithium bis(fluorosulfonyl)imide (LiFSI) was slowly added into ethylene glycol dimethyl ether (DME) to prepare an electrolyte with a LiFSI concentration of 1 mol / L.
[0563] (5) Isolation film: Polypropylene film is used.
[0564] (6) Preparation of lithium metal secondary batteries:
[0565] Place the above-mentioned positive electrode sheet, isolation membrane, and negative electrode sheet in order, so that the isolation membrane is located between the positive electrode sheet and the negative electrode sheet to play an isolating role, inject the electrolyte prepared in (4) above, and assemble into a button battery.
[0566] Example 2-23 adopts a method basically the same as Example 1, except that step (1) is different, and the parameter differences can be seen in Tables 1-3.
[0567] Comparative Examples 1-9 adopt a method substantially the same as Example 1, except that step (1) and / or step (2) are different, as shown in the parameter differences in Tables 1-3.
[0568] In Examples 2-23 and Comparative Examples 1-9, the types and molar ratio m / n of the monomer compound M1 and the monomer compound M2 in the monomer composition, the fluorine substitution rate in Rf in the monomer compound M1, the type, concentration and dosage of the lithium salt in the first electrolyte (corresponding to the first electrolyte lithium salt), the type and dosage of the solvent in the first electrolyte (corresponding to the first electrolyte solvent), the dosage of the monomer compound M1 and the monomer compound M2, the temperature and time of the in-situ polymerization reaction, the thickness of the polymer layer, the molecular weight, PDI and glass transition temperature (Tg) of the polymer Poly, the mass proportion of the fluorine element in the polymer Poly, and the mass proportion of the first electrolyte in the polymer layer can be referred to Table 1-3. The dosage of the first electrolyte lithium salt and the first electrolyte solvent can be converted according to the total mass of the two and the lithium salt concentration in the first electrolyte. The amount of monomer compound M1 and monomer compound M2 can be converted based on the total mass of the two and m / n, assuming that the molar ratio of monomer compound M1 to monomer compound M2 is numerically equal to the ratio of the degree of polymerization of the two repeating units in the polymer Poly. The mass ratio of the polymer Poly in the polymer layer to the first electrolyte can be estimated based on the parameter conversion of Table 1-3, assuming that the mass ratio of the polymer Poly in the polymer layer to the first electrolyte is numerically equal to the ratio of the total mass of the monomer composition raw material to the total mass of the first electrolyte raw material.
[0569] Compared with Example 1, in Examples 2-6, at least the monomer compound M1 and the monomer compound M2 in the monomer composition were adjusted.
[0570] Compared with Example 1, at least the m / n value is adjusted in Examples 7-10.
[0571] Compared with Example 1, Examples 11-14 at least adjust the content of the first electrolyte in the monomer-electrolyte mixture.
[0572] Compared with Example 1, Examples 15-18 at least adjusted the lithium salt concentration of the first electrolyte in the monomer-electrolyte mixture.
[0573] Compared with Example 1, at least the thickness of the polymer layer is adjusted in Examples 19-22.
[0574] Compared with Example 1, Example 23 changes the negative electrode plate substrate from a pure lithium plate to a lithium-magnesium alloy, and the mass ratio of lithium to magnesium is 1:1.
[0575] Comparative Example 1: The preparation method is basically the same as that of Example 1, except that the negative electrode sheet is different. This comparative example uses a pure lithium sheet as the negative electrode sheet, that is, there is no polymer layer. The other preparation parameters are the same as those of Example 1.
[0576] Comparative Example 2. Physical application of polymer coating.
[0577] The preparation method is substantially the same as that in Example 1, except that the connection method between the polymer layer and the lithium-containing layer is different.
[0578] In this comparative example, the polymer solution is sprayed onto the surface of the pure lithium sheet and dried to obtain a polymer coating with a thickness of about 0.1 microns, as shown in Table 1-3. A tetrahydrofuran (THF) solution containing 6 g of the polymer and 4.3 g of the first electrolyte (the first electrolyte lithium salt and the first electrolyte solvent, the concentration of the first electrolyte lithium salt in the first electrolyte is 1.0 mol / L) are mixed to prepare a polymer solution, wherein the polymer is a copolymer of 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate and pentaethylene glycol monomethyl ether cyanoacrylate, and the weight average molecular weight is 70 kDa (i.e., 70,000 Daltons). The polymer used in this example adopts the monomer composition in Example 1. The two monomer raw materials were polymerized in the same amount ratio as in Example 1, and the molecular weight of the product was controlled by adjusting the reaction temperature and time. The obtained polymer was prepared into a polymer solution, and then sprayed in this example.
[0579] Comparative Example 3.
[0580] The preparation method is basically the same as that of Comparative Example 2, except that the coating amount of the polymer solution is different, and the thickness of the polymer layer formed is different. The thickness of the polymer layer in this example is about 1 micron. Please refer to Tables 1-3. The polymer is a copolymer of 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate and pentaethylene glycol monomethyl ether cyanoacrylate, with a weight average molecular weight of 68 kDa (i.e. 68,000 Daltons). The polymer used in this example adopts the monomer composition in Example 1. The two monomer raw materials were polymerized in the same amount ratio as in Example 1, and the molecular weight of the product was controlled by adjusting the reaction temperature and time. The obtained polymer was prepared into a polymer solution, and then sprayed in this example.
[0581] Comparative Example 4.
[0582] The preparation method is basically the same as that of Example 1, except that no cyano group is provided in the monomer compound M1 and the monomer compound M2. The remaining preparation parameters are the same as those in Example 1.
[0583] Comparative Example 5.
[0584] The preparation method is basically the same as that in Example 1, except that a single monomer compound M1 is used. The monomer compound containing EO block was omitted. The remaining preparation parameters were the same as those in Example 1.
[0585] Comparative Example 6.
[0586] The preparation method is basically the same as that in Example 1, except that a single monomer compound M2 is used. The monomer compound containing the fluorinated aliphatic chain Rf was omitted. The remaining preparation parameters were the same as those in Example 1.
[0587] Comparative Example 7.
[0588] The preparation method is basically the same as that in Example 1, except that a single monomer is used. The monomer does not include the monomer compound M1 containing Rf, nor the monomer compound M2 containing EO block. The remaining preparation parameters are the same as those in Example 1.
[0589] Comparative Example 8.
[0590] The preparation method is basically the same as that of Example 1, except that the Rf and EO blocks are provided in the same monomer compound and the single monomer is used. The remaining preparation parameters are the same as those in Example 1.
[0591] Comparative Example 9.
[0592] The preparation method is basically the same as that in Example 1, except that the monomer compound M2 is replaced by The EO block is thereby replaced by a polyoxypropylene PPO segment, and the remaining parameters refer to Example 1.
[0593] Table 1.
[0594]
[0595]
[0596] In Table 1, in each embodiment and related comparative example, the raw material molar ratio of the monomer compound M1 to the monomer compound M2 is numerically equal to the polymerization degree ratio m / n of the two repeating units in the target polymer Poly.
[0597] Table 2.
[0598]
[0599]
[0600]
[0601] In each example, the mass ratio of the polymer Poly in the polymer layer to the first electrolyte can be estimated by conversion using the following formula: m10 / m20, that is, the sum of the masses of the monomer compound M1 and the monomer compound M2 in Table 2 (m10) divided by the sum of the mass of the lithium salt and the mass of the solvent in the first electrolyte (m20); wherein, the respective amounts of the monomer compound M1 and the monomer compound M2 can be obtained by conversion according to m / n, assuming that the molar ratio of the monomer compound M1 to the monomer compound M2 is numerically equal to the ratio of the degree of polymerization of the two repeating units in the polymer Poly.
[0602] In each example, the mass proportion of the first electrolyte in the polymer layer can be estimated by the following formula: m20 / (m20+m10)×100%, see Table 3.
[0603] Table 3.
[0604]
[0605]
[0606] Test sample preparation
[0607] 1. Preparation of polymer layer membrane
[0608] The monomer compound M1 is 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate. The monomer compound M2 is pentaethylene glycol monomethyl ether cyanoacrylate. The lithium salt and the solvent in the first electrolyte are lithium bis(fluorosulfonyl)imide (LiFSI) and ethylene glycol dimethyl ether (DME), respectively.
[0609] (1) At 25° C., 2,2,3,3,4,4,5,5-octafluoropentane-2-cyanoacrylate and pentaethylene glycol monomethyl ether cyanoacrylate were mixed in a molar ratio of 2:1 (equal to m / n), lithium bis(fluorosulfonyl)imide (LiFSI) and ethylene glycol dimethyl ether (DME) were mixed in a lithium salt concentration of 1.0 mol / L, and the monomer compound M1, the monomer compound M2, and the lithium salt and the solvent of the first electrolyte were stirred at room temperature to obtain a uniform solution.
[0610] (2) Add 0.1 g of lithium powder to the uniform solution obtained in step (1), quickly stir and then apply on a glass plate, and let it stand for reaction at 30° C. for 3 h to obtain a transparent polymer layer film with a thickness of 15 μm. Refer to the in-situ polymerization conditions of Example 1.
[0611] Structure and performance testing
[0612] 1. Characterization of polymer components in the polymer layer
[0613] The lithium sheet containing the polymer layer is immersed in isopropanol, the lithium sheet will be corroded and consumed, and the generated lithium isopropoxide can be dissolved in isopropanol, while the polymer is insoluble in isopropanol and precipitates. After centrifugal drying, a solid sample of the polymer can be obtained.
[0614] 1.1. Fourier transform infrared spectroscopy (FT-IR) test: ATR mode, 4cm -1 Resolution, scan 32 times, wave number range 4000cm -1 ~400cm -1 .
[0615] 1.2. 1 H NMR test: 1 The H resonance frequency was 400 MHz, the solvent was deuterated dimethyl sulfoxide (DMSO-d6), and tetramethylsilane (TMS) was used as the internal standard.
[0616] 1.3. Molecular weight test: The polymer sample is dissolved in NMP and the molecular weight is tested by gel permeation chromatography (GPC) to obtain the weight average molecular weight, number average molecular weight and molecular weight polydispersity index (PDI).
[0617] 1.4. Polymer layer thickness test: The polymer layer thickness is measured using a laser thickness gauge.
[0618] 2. Fluorine content
[0619] The content of fluorine in the polymer layer can be detected by X-ray photoelectron spectroscopy (XPS).
[0620] 3. Swelling parameters
[0621] The swelling parameters of the polymer layer were tested using the following method:
[0622] The test temperature is 25°C. The lithium metal sheet containing the polymer layer is cut into 30mm×30mm square samples, three parallel samples in each group, and the mass of each sample is weighed W1. Then, the sample is immersed in 1mol / L LiFSI DME electrolyte for 2h for swelling. After swelling, the sample is gently wiped with filter paper to remove the residual electrolyte on the surface, and then the mass of the swollen sample is weighed W2. The swelling rate of the polymer layer is the percentage of the mass increase of the swollen sample to the original sample mass = (W2-W1) / W1×100%.
[0623] 4. Ionic conductivity
[0624] The test temperature is 25°C. The polymer layer membrane is punched into a disc with a diameter of Φ16 mm; the polymer layer membrane disc is soaked in the electrolyte for 1 hour, taken out, and the electrolyte on the membrane surface is wiped with filter paper; the ionic conductivity σ of the polymer layer membrane after swelling the electrolyte is calculated using the formula σ=d / RA, where d is the membrane thickness, measured with a micrometer, A is the area of the membrane, and R is the impedance of the membrane. The impedance of the symmetrical battery is tested using an electrochemical workstation, and the test frequency is 10 -6 ~10 -1 Hz, the voltage amplitude is 5mV; the intersection of the Nyquist graph obtained by the test and the horizontal axis is the impedance R of the polymer layer.
[0625] 5. Elastic modulus and elastic deformation
[0626] Elastic modulus: The test temperature is 25°C. The polymer layer film is cut into strips with a length L0 of 150 mm and a width of 20 mm. The elastic modulus of the polymer layer film is measured by a universal testing machine with a stretching distance of 100 mm and a stretching speed of 50 mm / min. The maximum tensile force of the polymer layer film is the elastic modulus.
[0627] Elastic deformation: The test temperature is 25° C. When a polymer film with an initial length of L0 is stretched, the length when the film breaks is L, and the elastic deformation of the polymer layer film can be calculated as (L-L0) / L0×100%.
[0628] 6. Test of bonding performance of polymer layer (peeling degree)
[0629] The thickness of the polymer layer on the surface of lithium metal is controlled to be about 5μm by controlling the reaction time. A range of 50×100 mm is used as a peeling test sample. A sharp blade (with a sharp angle of 15° to 30°) is used to draw 10×10 1mm×1mm small grids on the surface of the protective layer sample. Each line should be deep enough to reach the bottom layer of the protective layer. Use a brush to clean the debris in the test area. Use an adhesive force of 350g / cm 2 ~400g / cm 2 Use adhesive tape (3M 600 tape or equivalent) to firmly stick the small grid to be tested, and use an eraser to rub the tape vigorously to increase the contact area and strength between the tape and the tested area; grab one end of the tape with your hand, and quickly tear off the tape in the vertical direction (90°), and perform the same test twice at the same position; finally, use a magnifying glass to observe the situation of the grid area. If there is no peeling or it occurs in the protective layer interval, it is qualified, but the peeling is between the metal and polymer layers, and the area is greater than 65%, it is 0B grade; the area is 35%-65%, it is 1B grade; the area is 15%-35%, it is 2B grade; the area is 5%-15%, it is 3B grade; the area is less than or equal to 5%, it is 4B grade; the cut edge is completely smooth, and there is no peeling at the grid edge, it is 5B grade.
[0630] 7. Flexibility of polymer materials
[0631] The glass transition temperature Tg of the polymer material is characterized by a differential scanning calorimeter (DSC). The smaller the Tg, the better the molecular weight flexibility. The DSC test temperature range is 35-800°C, the heating rate is 5°C / min, and the atmosphere is argon.
[0632] 8. Negative electrode performance test
[0633] Negative electrode volume expansion rate: The test temperature is 25°C. The thickness of the fresh lithium sheet is d1. After the battery is cycled for 50 cycles to a fully discharged state, the battery is disassembled and the thickness of the lithium sheet is measured under an optical microscope to be d2. The expansion rate of the negative electrode sheet is (d2-d1) / d1×100%.
[0634] 9. Battery performance test
[0635] (1) Cycle performance test: The test temperature is 25°C. The lithium metal battery is first charged to 4.25V at a constant current density, and then discharged to 3.0V to obtain the first-week discharge capacity (Cd1). This charge and discharge cycle is repeated for 50 cycles. The discharge capacity of the lithium metal battery after n cycles is recorded as Cdn. Capacity retention rate = discharge capacity after n cycles (Cdn) / first-week discharge capacity (Cd1) × 100%. The charging current density can be referred to Table 4.
[0636] (2) Observation of the surface of the lithium negative electrode: After the battery was fully discharged at the 50th cycle, the uniformity of lithium deposition / dissolution and the flatness of the lithium negative electrode surface were observed under an optical microscope.
[0637] Test Results
[0638] The molecular weight, PDI and Tg of the polymer Ploy in the polymer layer, the mass proportion of fluorine element in the polymer Poly, the mass proportion of the first electrolyte in the polymer layer, the thickness of the polymer layer, the swelling rate of the polymer layer, the ionic conductivity, the elastic modulus and the elastic deformation, as well as the test analysis results of the capacity retention rate, lithium dendrites, negative electrode plate volume expansion rate and peeling degree test of the lithium metal secondary battery prepared using the negative electrode plate containing the polymer layer of the present application after 50 cycles can be seen in Table 2-4.
[0639] Table 4.
[0640]
[0641]
[0642] According to the experimental test results, by adjusting the fluorine content of the protective layer film, the proportion of EO repeating units, the length of EO repeating units, the lithium salt concentration in the first electrolyte, the content of the first electrolyte in the polymer layer and the thickness of the polymer layer, the polymer layer can obtain good ionic conductivity and good mechanical strength, which is beneficial for the application of the protective layer in lithium metal batteries that are charged and discharged at a high current density.
[0643] Embodiments 1 to 23 use the negative electrode sheets provided by the present application, which include a lithium-containing layer and a polymer layer, and a chemical bond is formed between the two. The polymer layer formed in embodiments 1 to 23 has an appropriate swelling rate, elastic modulus, elastic deformation and ionic conductivity, and can be used in lithium metal batteries that perform charge and discharge cycles at a high current density. The lithium metal secondary batteries prepared in embodiments 1 to 23 have improved cycle performance relative to comparative example 1 without a polymer layer, and the lithium dendrite phenomenon is suppressed. Among them, relative to comparative example 1, the volume expansion of the negative electrode sheets of embodiments 1-9, 11-12, 15-16, 19-20, and 23 is significantly suppressed, and the lithium metal secondary batteries have significantly improved cycle performance, the cycle capacity retention rate is significantly improved, and there are only a small amount or no lithium dendrites, and the lithium dendrites are significantly suppressed. It should be noted that the lithium dendrite phenomenon in embodiments 10, 13-14, 17-18, and 21-22 is also statistically improved to a certain extent.
[0644] Comparative Examples 2 and 3 both use physical coating to coat the polymer layer on the lithium sheet, and the thickness of the polymer layer is about 0.1 micron and 1 micron, respectively. The results show that compared with Example 1 (polymer layer thickness of about 0.1 micron), the bonding firmness of the polymer layer in Comparative Examples 2 and 3 is significantly reduced, and the volume expansion of the negative electrode sheet increases sharply, the cycle capacity retention rate decreases significantly, the cycle performance deteriorates significantly, and serious lithium dendrites occur. It can be seen that the embodiments of the present application can achieve a firm fit on the lithium-containing layer under the condition of a thinner polymer layer thickness, and significantly improve the cycle performance of the battery and greatly improve the cycle capacity retention rate. Comparative Example 3 increases the thickness of the physically coated polymer layer to 1 micron. Although the volume expansion of the negative electrode sheet is alleviated relative to Comparative Example 1, however, it leads to a significant decrease in the ionic conductivity of Comparative Example 3.
[0645] Compared with the polymerized monomers M1 and M2 in Example 1, the polymerized monomers in Comparative Example 4 do not contain cyano groups, resulting in the polymer layer formed by in-situ polymerization being only physically attached to the lithium-containing layer without forming chemical bonds, and the bonding strength being significantly deteriorated. It also leads to a sharp increase in the volume expansion of the negative electrode plate, a significant deterioration in the cycle performance, and the occurrence of serious lithium dendrites.
[0646] Compared with the polymerized monomers M1 and M2 in Example 1, the polymerized monomer in Comparative Example 5 does not contain an EO block, that is, the polymerized monomer M2 is omitted, which affects the regulation of the flexibility and elasticity of the polymer layer, resulting in an increase in the volume expansion of the negative electrode plate, a decrease in the cycle capacity retention rate, and a deterioration in the cycle performance.
[0647] Compared with the polymerized monomers M1 and M2 in Example 1, the polymerized monomers in Comparative Example 6 do not contain a fluorinated aliphatic chain Rf chain, that is, the polymerized monomer M1 is omitted, which affects the regulation of the lithium ion deposition morphology. As a result, serious lithium dendrite phenomenon occurs, the volume expansion of the negative electrode plate increases dramatically, the cycle capacity retention rate decreases significantly, and the cycle performance deteriorates significantly.
[0648] Compared with the polymerized monomers M1 and M2 in Example 1, the polymerized monomers in Comparative Example 7 have neither fluorinated fatty chains nor EO blocks, which affects the regulation of lithium ion deposition morphology and the flexibility and elasticity of the polymer layer, resulting in a sharp increase in the volume expansion of the negative electrode plate, a significant decrease in the cycle capacity retention rate, a significant deterioration in the cycle performance, and a serious lithium dendrite phenomenon. In addition, the ionic conductivity of the polymer layer in Comparative Example 7 also decreases.
[0649] Compared with the polymerized monomers M1 and M2 in Example 1, in Comparative Example 8, the Rf chain and the EO block are placed in the same monomer molecule, which results in the volume expansion of the negative electrode plate increasing by nearly 1 times, the cycle capacity retention rate also decreasing to a certain extent, and the cycle performance being deteriorated to a certain extent. This may be due to the increase in the steric hindrance of the Rf chain and the EO block in the side chain contacting the lithium-containing layer, which affects the bonding with the lithium-containing layer.
[0650] Compared with Example 1, the EO block in Comparative Example 9 has an increased side group, reduced flexibility, and changed the coordination relationship with the first side chain (including Rf). As a result, a small amount of lithium dendrites appeared, the volume expansion of the negative electrode sheet was significantly increased, and the cycle capacity retention rate decreased to a certain extent. In addition, the ionic conductivity of the polymer layer in Comparative Example 9 also decreased to a certain extent.
[0651] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0652] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples. Within the scope of the technical solution of the present application, the embodiments that have the same structure as the technical idea and play the same effect are all included in the technical scope of the present application. The above-mentioned embodiments only express several embodiments of the present application, and the description is relatively detailed, but it cannot be understood as a limitation on the scope of the patent. In addition, without departing from the scope of the subject matter of the present application, various deformations that can be thought of by those skilled in the art are applied to the embodiments, and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several deformations and improvements can be made, which all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the attached claims, and the description and drawings can be used to explain the content of the claims.
Claims
1. A lithium metal negative electrode material, characterized in that: The invention comprises a lithium-containing metal and a polymer Poly bonded to the lithium metal in the lithium-containing metal, wherein the polymer Poly has a linear carbon chain and a first side chain and a second side chain grafted to the side group of the linear carbon chain, wherein the first side chain contains a fluorinated aliphatic chain Rf, and the second side chain contains an EO block, wherein the structure of the EO block is *-(CH2CH2O) z -, z is a positive integer, and * represents a connection site pointing to the linear carbon chain.
2. The lithium metal negative electrode material according to claim 1, characterized in that In the structure of the polymer Poly, the number of the first side chains is m, and the number of the second side chains is n; wherein m and n are each independently an integer greater than or equal to 8; Optionally, m and n are each independently an integer selected from 8-600.
3. The lithium metal negative electrode material according to claim 2, characterized in that The polymer Poly satisfies one or more of the following characteristics: The ratio of m to n satisfies 0.5≤m / n≤8, optionally, 1≤m / n≤5, further optionally, 1≤m / n≤3; m is an integer selected from 50 to 250, optionally, m is an integer selected from 50 to 200; n is an integer selected from 25 to 200, and optionally, n is an integer selected from 40 to 150.
4. The lithium metal negative electrode material according to any one of claims 1 to 3, characterized in that z is an integer selected from 2 to 10; Optionally, z is an integer selected from 3-7.
5. The lithium metal negative electrode material according to any one of claims 1 to 4, characterized in that The polymer Poly comprises repeating units of the structure shown in formula (U1) and repeating units of the structure shown in formula (U2): in, X1 and X2 are each independently H or an electron withdrawing group; Y1 and Y2 are each independently a cyano group or a linking group formed by a cyano group bonded to the lithium metal in the lithium-containing metal; A1 and A2 are each independently O, S or NR 11 ; Among them, R 11 H or C 1-3 alkyl; Rd is a hydrocarbon group or a hydrocarbon group substituted by Q1, Q1 is selected from the following substituents: cyano, -C(=O)NH2, -OC(=O)NHR 6 and -S(=O)2F,R 6 H or C 1-6 alkyl; Optionally, at least one of Y1 and Y2 is a linking group formed by a cyano group bonded to the lithium metal in the lithium-containing metal.
6. The lithium metal negative electrode material according to claim 5, characterized in that In the structure of the polymer Poly, X1 and X2 each appear and are independently H or cyano, nitro or -NR 21 R 22 ; Among them, R 21 and R 22 Each independently is H or C 1-3 alkyl; Optionally, R 21 and R 22 are each independently H or methyl; Further optionally, R 21 and R 22 All are methyl.
7. The lithium metal negative electrode material according to claim 5 or 6, characterized in that: In the structure of the polymer Poly, each occurrence of A1 and A2 is independently O, S or NH; Optionally, each occurrence of A1 and A2 is independently O or NH.
8. The lithium metal negative electrode material according to any one of claims 5 to 7, characterized in that Rd is C 1-4 Hydrocarbon; Optionally, Rd is C 1-4 alkyl; Further optionally, Rd is C 1-3 alkyl; In a further alternative, Rd is methyl.
9. The lithium metal negative electrode material according to any one of claims 5 to 8, characterized in that In the structure of the polymer Poly, m repeating units represented by formula (U1) and n repeating units represented by formula (U2) are included; m and n are as defined in claim 2 or 3; Optionally, m repeating units represented by formula (U1) and n repeating units represented by formula (U2) are arranged linearly; Further optionally, the polymer Poly has a general structure as shown in formula (P1):
10. The lithium metal negative electrode material according to any one of claims 1 to 9, characterized in that The polymer Poly satisfies one or more of the following characteristics: The fluorine substitution rate in any Rf is independently ≥ 50%; The number of fluorine atoms in any Rf is independently ≥ 4; The mass percentage of fluorine element in the polymer Poly is 15% to 44%.
11. The lithium metal negative electrode material according to claim 10, characterized in that The polymer Poly satisfies one or more of the following characteristics: The fluorine substitution rate in any Rf is independently ≥55%; The number of fluorine atoms in any Rf is independently ≥ 5, and optionally, the number of fluorine atoms in any Rf is independently 5 to 15; The mass proportion of fluorine element in the polymer Poly is 15% to 41%, and optionally 20% to 41%.
12. The lithium metal negative electrode material according to any one of claims 1 to 11, characterized in that The polymer Poly satisfies one or more of the following characteristics: Each Rf independently contains 2 to 10 main chain carbon atoms; The number of carbon atoms in any one Rf is independently an integer selected from 2 to 10.
13. The lithium metal negative electrode material according to claim 12, characterized in that: The polymer Poly satisfies one or more of the following characteristics: Any Rf independently contains 2 to 8 main chain carbon atoms, optionally, any Rf independently contains 3 to 8 main chain carbon atoms; The number of carbon atoms in any Rf is independently an integer selected from 2 to 8. Alternatively, the number of carbon atoms in any Rf is independently an integer selected from 3 to 8.
14. The lithium metal negative electrode material according to any one of claims 1 to 13, characterized in that In the structure of the polymer Poly, one, more or all Rf independently contain one or more heteroatoms selected from the group consisting of iodine, nitrogen, oxygen, sulfur, silicon, boron and phosphorus; Optionally, the number of heteroatoms in any one, more or all Rf is independently 1 or more; Further optionally, the number of the heteroatoms in any one, multiple or all Rf is selected from 1 or 2-6.
15. The lithium metal negative electrode material according to claim 14, characterized in that In the structure of the polymer Poly, one, more or all Rf satisfy one or more of the following characteristics: The number of oxygen atoms in one, more than one or all Rf is 1, 2, 3, 4 or 5; The number of nitrogen atoms in one, more than one or all Rf is 1, 2 or 3; The number of sulfur atoms in one, more than one or all Rf is 1, 2 or 3; The number of phosphorus atoms in one, more than one or all Rf is 1 or 2; The number of iodine atoms in one, more or all Rf is 1, 2, 3, 4, 5 or 6; The number of silicon atoms in one, more than one or all of Rf is 1 or 2; and The number of boron atoms in one, more than one or all of Rf is 1 or 2.
16. The lithium metal negative electrode material according to any one of claims 14 to 15, characterized in that In the structure of the polymer Poly, one, more or all of the Rf contain one or more selected from iodine, -NR 12 -, -O-, -S-, -S(O)2-, >Si<, >B- and >P(=O)-, wherein R 12 H or C 1-3 alkyl; Optionally, R 12 is H or methyl; Further optionally, R 12 For H.
17. The lithium metal negative electrode material according to any one of claims 14 to 16, characterized in that In the structure of the polymer Poly, one, more or all Rf contain one or more atoms or atomic groups selected from the group consisting of -O-, -S(O)2- and -(O=)P(O-)2; Optionally, one, more or all of Rf contain one or more -O-; Optionally, one, more or all of Rf contain -S(O)2F; Optionally, one, more than one or all of Rf contain -(O=)P(O-)2.
18. The lithium metal negative electrode material according to any one of claims 1 to 17, characterized in that In the structure of the polymer Poly, any Rf is independently a linear structure or a branched structure.
19. The lithium metal negative electrode material according to any one of claims 1 to 18, characterized in that In the structure of the polymer Poly, any one Rf is independently a saturated structure or an unsaturated structure.
20. The lithium metal negative electrode material according to any one of claims 1 to 19, characterized in that In the structure of the polymer Poly, the structure of any Rf is independently represented by formula (III-1), formula (III-2) or formula (III-3): in, In formula (III-1), m3 is an integer selected from 2 to 10; R 31 , R 32 and R 3 Each occurrence is independently H or F; the structure represented by formula (III-1) contains at least 4 F atoms; In formula (III-2), m 4a and m 4b Each independently represents an integer selected from 1 to 9; R 41a , R 42a , R 4a , R 41b , R 42b and R 4b Each occurrence is independently H or F; the structure represented by formula (III-2) contains at least 4 F atoms; In formula (III-3), m5 is an integer selected from 2 to 10; R 51 and R 52 Each occurrence is independently H or F; the structure represented by formula (III-3) contains at least 4 F atoms.
21. The lithium metal negative electrode material according to claim 20, characterized in that The polymer Poly satisfies one or more of the following characteristics: m3 is an integer selected from 3 to 10; alternatively, m3 is an integer selected from 3 to 8; m 4a and m 4b Each is independently an integer selected from 2 to 9; optionally, m 4a and m 4b are each independently an integer selected from 2 to 8; further optionally, m 4a and m 4b are each independently an integer selected from 3 to 8; further optionally, m 4a and m 4b Each independently is an integer selected from 3 to 6 m5 is an integer selected from 3 to 10; optionally, m5 is an integer selected from 3 to 8.
22. The lithium metal negative electrode material according to claim 20 or 21, characterized in that: In the structure of the polymer Poly, the structure of Rf is as shown in formula (III-1); or, the structure of Rf is as shown in formula (III-2); or, the structure of Rf is as shown in formula (III-3).
23. The lithium metal negative electrode material according to any one of claims 20 to 22, characterized in that In the structure of the polymer Poly, each time formula (III-1) appears, the number of H atoms therein is 0, 1, 2, 3 or 4; each time formula (III-2) appears, the number of H atoms therein is 0, 1, 2, 3, 4, 5 or 6; each time formula (III-3) appears, the number of H atoms therein is 0, 1, 2, 3 or 4; Optionally, the number of H atoms in formula (III-1) is 0; Optionally, the number of H atoms in formula (III-2) is 0; Optionally, the number of H atoms in formula (III-3) is 0.
24. The lithium metal negative electrode material according to any one of claims 1 to 23, characterized in that In the structure of the polymer Poly, any Rf is independently any of the following structures:
25. The lithium metal negative electrode material according to any one of claims 1 to 24, characterized in that The number average molecular weight of the polymer Poly is selected from 10kDa to 200kDa; Optionally, the number average molecular weight of the polymer Poly is selected from 40 kDa to 100 kDa; Further optionally, the number average molecular weight of the polymer Poly is selected from 50 kDa to 80 kDa.
26. The lithium metal negative electrode material according to any one of claims 1 to 25, characterized in that The lithium-containing metal comprises lithium alone or a lithium alloy; Optionally, the lithium alloy contains lithium element and also contains one or more elements selected from the group consisting of silver, magnesium, aluminum, gold, zinc, tin, copper, nickel and titanium.
27. The lithium metal negative electrode material according to any one of claims 1 to 26, characterized in that The amount of lithium metal in the lithium-containing metal relative to the polymer Poly is greater than or equal to the catalyst amount, calculated by molar ratio.
28. A negative electrode plate, characterized in that: It comprises a lithium-containing layer and a polymer layer stacked together, and the negative electrode sheet comprises the lithium metal negative electrode material according to any one of claims 1 to 27; The lithium-containing layer includes the lithium-containing metal in the lithium metal negative electrode material, and the polymer layer includes the polymer Poly in the lithium metal negative electrode material.
29. The negative electrode sheet according to claim 28, characterized in that: The lithium-containing layer consists essentially of the lithium-containing metal; Optionally, the material of the lithium-containing layer is lithium element; Alternatively, the material of the lithium-containing layer is a lithium alloy.
30. The negative electrode sheet according to claim 28 or 29, characterized in that: The polymer layer further contains a first electrolyte, which contains a lithium salt and a first electrolyte solvent.
31. The negative electrode sheet according to any one of claims 28 to 30, characterized in that: Meet one or more of the following characteristics; The lithium salt includes one or more of lithium hexafluorophosphate, tetrafluoroboric acid, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium difluorooxalatoborate, lithium perchlorate and lithium bis(oxalate)borate; The first electrolyte solvent includes one or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dipropyl carbonate, diphenyl carbonate, dibutyl carbonate, butylene carbonate, ethylene glycol dimethyl ether, tetrahydrofuran, dioxolane, methyl nonafluoro-n-butyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, octafluoropentyl-tetrafluoroethyl ether, 1,2-bis(cyanoethoxy)ethane, diphenyl ether and 18-crown-6.
32. The negative electrode sheet according to any one of claims 30 to 31, characterized in that: The concentration of the lithium salt in the first electrolyte is selected from 0.2 mol / L to 8 mol / L; Optionally, the concentration of the lithium salt in the first electrolyte is selected from 0.5 mol / L to 5 mol / L; Further optionally, the concentration of the lithium salt in the first electrolyte is selected from 0.5 mol / L to 2 mol / L.
33. The negative electrode sheet according to any one of claims 30 to 32, characterized in that: The mass proportion of the first electrolyte in the polymer layer is 20% to 80%; Optionally, the mass proportion of the first electrolyte in the polymer layer is 30% to 60%; Further optionally, the mass proportion of the first electrolyte in the polymer layer is 40% to 60%; Further optionally, the mass percentage of the first electrolyte in the polymer layer is 40% to 55%.
34. The negative electrode sheet according to any one of claims 30 to 33, characterized in that: The mass ratio of the polymer Poly to the first electrolyte is 4:1 to 0.25:1; Optionally, the mass ratio of the polymer Poly to the first electrolyte is 3:1 to 0.5:1; Further optionally, the mass ratio of the polymer Poly to the first electrolyte is 2.5:1 to 1:1; Further optionally, the mass ratio of the polymer Poly to the first electrolyte is 7:3 to 2:
1.
35. The negative electrode sheet according to any one of claims 30 to 34, characterized in that: Based on the first electrolyte, the swelling rate of the polymer layer at 25° C. is 8% to 65%; Further optionally, the swelling rate of the polymer layer at 25° C. is 15% to 55%; Further optionally, the swelling rate of the polymer layer at 25° C. is 18% to 44%; Further optionally, the swelling ratio of the polymer layer at 25° C. is 30% to 40%.
36. The negative electrode sheet according to any one of claims 30 to 35, characterized in that: Based on the first electrolyte, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.001 mS / cm to 5 mS / cm; Optionally, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.1 mS / cm to 5 mS / cm; Alternatively, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.5 mS / cm to 5 mS / cm; Alternatively, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.9 mS / cm to 4.8 mS / cm; Alternatively, the ionic conductivity of the swollen polymer layer at 25° C. is selected from 0.95 mS / cm to 2.6 mS / cm.
37. The negative electrode sheet according to any one of claims 28 to 36, characterized in that: The thickness of the polymer layer is 5 nm to 10 μm; Optionally, the thickness of the polymer layer is 0.02 μm to 8 μm; Further optionally, the thickness of the polymer layer is 0.05 μm to 8 μm; Further optionally, the thickness of the polymer layer is 0.05 μm to 5 μm; Further optionally, the thickness of the polymer layer is 0.1 μm to 5 μm.
38. The negative electrode sheet according to any one of claims 28 to 37, characterized in that: The elastic modulus of the polymer layer at 25° C. is 0.1 MPa to 65 MPa; Optionally, the elastic modulus of the polymer layer at 25° C. is 0.5 MPa to 50 MPa; Further optionally, the elastic modulus of the polymer layer at 25° C. is 10 MPa to 46 MPa; Further optionally, the elastic modulus of the polymer layer at 25° C. is 18 MPa to 41 MPa; Further optionally, the elastic modulus of the polymer layer at 25° C. is 29 MPa to 41 MPa.
39. The negative electrode sheet according to any one of claims 28 to 38, characterized in that: The elastic deformation range of the polymer layer at 25°C is 55% to 350%; Optionally, the elastic deformation range of the polymer layer at 25° C. is 150% to 350%; Further optionally, the elastic deformation range of the polymer layer at 25° C. is 150% to 300%; Further optionally, the elastic deformation range of the polymer layer at 25° C. is 168% to 280%.
40. A lithium metal secondary battery, characterized in that: It comprises a positive electrode sheet, a separator and the negative electrode sheet as claimed in any one of claims 28 to 39, wherein the separator is arranged between the positive electrode sheet and the negative electrode sheet, and the polymer layer is arranged on the side of the negative electrode sheet close to the separator.
41. The lithium metal secondary battery according to claim 40, characterized in that The lithium metal secondary battery further includes a second electrolyte, and the components of the second electrolyte and the first electrolyte in the polymer layer may be the same or different.
42. An electrical device, characterized in that: It includes the lithium metal secondary battery according to claim 40 or 41.
43. Use of a monomer composition in preparing a negative electrode sheet or a lithium metal secondary battery, characterized in that: The monomer composition includes a first monomer represented by formula (M1) and a second monomer represented by formula (M2): wherein X1, X2, Y1, Y2, A1, A2, Rf and Rd are defined as any one of claims 5 to 25; z is defined as described in claim 1 or 4; at least one of Y1 and Y2 is cyano; The negative electrode plate includes a lithium-containing layer, and the lithium-containing layer contains lithium metal; The first monomer and the second monomer are used to form a polymer layer bonded to the lithium metal in the negative electrode plate.
44. The use according to claim 43, characterized in that The method comprises the following steps: the first monomer and the second monomer are contacted with lithium metal in the lithium-containing layer together, and the polymer layer is formed through an in-situ polymerization reaction.
45. The use according to claim 43 or 44, characterized in that The negative electrode plate is as defined in any one of claims 27 to 40, and the lithium metal secondary battery is as defined in claim 40 or 41.
46. A method for preparing a negative electrode sheet, characterized in that: The steps include: Providing a negative electrode substrate, wherein the outermost layer of at least one side of the negative electrode substrate is a lithium-containing layer, and the lithium-containing layer contains lithium metal; and also providing a reaction mixture containing a monomer composition and a first electrolyte; The reaction mixture is coated on the surface of the lithium-containing layer on at least one side of the negative electrode substrate, so that the monomer composition contacts at least a catalytic amount of lithium metal, and the monomer composition undergoes an in-situ polymerization reaction to form a polymer Poly bonded to the lithium metal in the lithium-containing layer; wherein the monomer composition is as defined in claim 43; The first electrolyte is as defined in any one of claims 30 to 34.
47. The preparation method according to claim 46, characterized in that The reaction temperature of the in-situ polymerization is selected from 30°C to 100°C; Optionally, the reaction temperature of the in-situ polymerization is selected from 30°C to 60°C; Alternatively, the reaction temperature of the in-situ polymerization is selected from 40°C to 80°C.
48. The preparation method according to any one of claims 46 to 47, characterized in that The reaction time of the in-situ polymerization is selected from 0.1h to 24h; Optionally, the reaction time of the in-situ polymerization is selected from 0.1h to 12h; Further optionally, the reaction time of the in-situ polymerization is selected from 0.1h to 6h.
49. The preparation method according to any one of claims 46 to 48, characterized in that The polymer layer according to any one of claims 27 to 40 is formed on the surface of the negative electrode plate substrate.
50. The preparation method according to any one of claims 46 to 49, wherein The negative electrode plate substrate is a pure lithium plate or a lithium alloy; Optionally, the mass proportion of the lithium element in the lithium alloy is ≥50%.
51. The preparation method according to any one of claims 46 to 50, wherein The negative electrode plate is as defined in any one of claims 27 to 40.
Citation Information
Patent Citations
A method for protecting the negative electrode of a metal secondary battery by a polymer and an application thereof
CN109103517A
Lithium metal battery
CN111326736A
Electrode protective layer polymer and secondary battery to which same is applied
CN111587503A
Polymer protective film, metal lithium negative electrode, lithium battery and vehicle
CN115528242A
Polymer electrolyte, method of preparing the polymer electrolyte, and lithium metal battery including the same
US20170373347A1
Cited By
Electrolyte, preparation method thereof and lithium ion battery
CN121642146A
Electrolyte and method for its preparation, and lithium-ion battery
CN121642146B