Preparation method of sodium oxalate phosphate
Sodium oxalate phosphate is prepared by the reaction of sodium oxalate and phosphoric acid, which solves the problem of water sensitivity and unstable performance of sodium hexafluorophosphate to water and achieves high-purity and low-impact electrolyte preparation, and improves the performance and safety of sodium ion batteries. , has industrialization potential.
Patent Information
- Application Number
- CN202411351277.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing sodium-ion battery electrolytes such as sodium hexafluorophosphate are highly sensitive to water, have safety risks, and the high-temperature performance is unstable. The high cost of lithium difluorophosphate increases the difficulty of industrialization.
The reaction of sodium oxalate and phosphoric acid under heating and stirring conditions was adopted to obtain a mixture of sodium oxalate phosphate and sodium hydroxide by decompression, and then filtered and dried in acetonitrile in vacuo to simplify the purification process and achieve efficient preparation of sodium oxalate phosphate.
The obtained sodium oxalic acid phosphate has high purity and low impurity content, significantly reduces the moisture and acidity of the electrolyte, improves the high-temperature cycle stability and rate performance of sodium ion batteries, and has broad industrial prospects.
Smart Images

Figure CN118878583A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a method for preparing sodium oxalate phosphate. Background Art
[0002] Sodium-ion battery is a secondary battery that mainly relies on the movement of sodium ions between the positive and negative electrodes to work. It has a similar working principle to lithium-ion batteries, and both are called "rocking chair" batteries.
[0003] The main components of sodium-ion batteries are positive electrode, negative electrode, separator, electrolyte and current collector. The electrolyte is a carrier for transmitting ions, which is composed of electrolyte, solvent and additives. The electrolyte of sodium-ion batteries is very similar to that of lithium-ion batteries, with sodium salts replacing lithium salts, such as sodium perchlorate, and its cost is lower than that of lithium salts.
[0004] Electrolyte is a bridge for material transfer between positive and negative electrodes. It is used to transfer ions to form a closed circuit. It is an important guarantee for maintaining electrochemical reactions. It not only directly affects the battery's rate, cycle life, self-discharge and other performance, but is also one of the core factors that determine battery stability and safety. Sodium salts are similar to lithium batteries and are divided into inorganic sodium salts and organic sodium salts. The former includes sodium hexafluorophosphate, sodium perchlorate, etc., and the latter mainly includes sodium salts of fluorosulfonic acid and sodium salts of fluorosulfonyl imide. Generally speaking, organic sodium salts are more stable, while inorganic sodium salts are cheaper. At present, the most commonly used sodium salt is sodium hexafluorophosphate, which has the best conductivity, but is highly sensitive to water and is easy to form HF with water in the air, which poses a safety hazard. Moreover, sodium hexafluorophosphate is easy to decompose at high temperature, resulting in unstable high temperature performance of the battery. Compared with the commercial sodium ion electrolyte salt sodium hexafluorophosphate, sodium oxalate phosphate has good stability, less environmental pollution of decomposition products, high decomposition potential, and can significantly reduce the moisture and acidity of the electrolyte. It has become a sodium salt that may replace sodium hexafluorophosphate and be commercially used in sodium ion batteries.
[0005] At present, there are not many reports on sodium oxalate phosphate, but there are some reports on lithium oxalate phosphate. The Chinese patent document with publication number CN106299473B discloses a method for preparing lithium oxalate phosphate using lithium difluorophosphate and lithium oxalate, but the reactant lithium difluorophosphate is expensive and difficult to obtain, which not only increases the cost but also increases the difficulty of industrialization. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing sodium oxalate phosphate, which has a simple process route and is environmentally friendly, and the product can reduce the moisture and acidity of the electrolyte and has high yield and high purity.
[0007] The preparation method of sodium oxalate phosphate of the present invention comprises the following steps: (1) adding phosphoric acid dropwise to a sodium oxalate aqueous solution under heating and stirring conditions, and distilling under reduced pressure after the reaction is completed to obtain a mixture of sodium oxalophosphate and sodium hydroxide; The reaction equation is as follows:
[0008] (2) A mixture of sodium oxalate phosphate and sodium hydroxide is dissolved in acetonitrile, filtered, the filtrate is distilled under reduced pressure, and the obtained solid is vacuum dried to obtain sodium oxalate phosphate.
[0009] Preferably, in step (1), the ratio of sodium oxalate to phosphoric acid is 1 mol:0.8-1.2 mol; the heating and stirring temperature is 60-90°C, and the reaction time is 14-24h; the temperature of the reduced pressure distillation is 70-90°C, and the time is 12-20h.
[0010] More preferably, in step (1), the heating and stirring temperature is 70-80° C., and the reaction time is 16-22 h.
[0011] Preferably, in step (2), the ratio of the mixture of sodium oxalate phosphate and sodium hydroxide to acetonitrile is 1 g:5-15 ml, the temperature of the reduced pressure distillation is 40-60° C., and the time is 16-24 h; the temperature of the vacuum drying is 50-70° C., and the time of the vacuum drying is 18-24 h.
[0012] The beneficial effects of the present invention are: The present invention can synthesize sodium oxalate phosphate in one step, and the reaction solvent is water, the reaction is simple and environmentally friendly; the purification step only requires filtration and vacuum distillation, which is convenient to operate and has a high yield (>94%). The obtained sodium oxalate phosphate has high purity (>99.9%) and low impurity content (free acid <20ppm, water <20ppm, chloride ion <5ppm, sulfate ion <5ppm). And the obtained sodium oxalate phosphate has better performance than the commonly used sodium hexafluorophosphate as a sodium battery electrolyte solute (high temperature cycle stability and rate performance are significantly better than sodium hexafluorophosphate), especially in terms of being able to control the moisture and acidity of the electrolyte. Adding the sodium oxalate phosphate battery of the present invention, the capacity retention rate after 300 cycles at 50°C is 81.3%-87.2%, and the 5C discharge battery capacity is 166.9mAh / g-176.8mAh / g, which has broad industrial prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is the P-NMR spectrum of the sodium oxalate phosphate of Example 1 of the present invention. DETAILED DESCRIPTION
[0014] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and embodiments. However, those skilled in the art will understand that the embodiments described below are part of the embodiments of the present invention, rather than all of the embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Example 1
[0015] Dissolve 1 mol of sodium oxalate in water to prepare a 1 mol / L sodium oxalate aqueous solution; then add 1 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 75°C for 19 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 70°C under reduced pressure for 12 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0016] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 100 ml of acetonitrile, filtered, and the filtrate was distilled at 50°C under reduced pressure for 16 h, and vacuum dried at 60°C for 21 h to obtain sodium oxalate phosphate crystals. The yield was 96%.
[0017] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is well-known common additives. And compared with sodium hexafluorophosphate available on the market. Example 1 adds sodium oxalate phosphate battery and the capacity retention rate after 300 cycles at 50°C is 83.5%, while that of Comparative Example 1 and Comparative Example 5 is only 79.5% and 71.4%; Example 1 adds sodium oxalate phosphate battery 5C discharge battery capacity is 169.5mAh / g, while that of Comparative Example 1 and Comparative Example 5 is only 162.1mAh / g and 151.4mAh / g. Example 2
[0018] Dissolve 1 mol of sodium oxalate in water to prepare a 1.2 mol / L sodium oxalate aqueous solution; then add 0.8 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 60°C for 14 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 90°C under reduced pressure for 20 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0019] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 50 ml of acetonitrile, filtered, and the filtrate was distilled under reduced pressure at 40°C for 24 h, and vacuum dried at 50°C for 18 h to obtain sodium oxalate phosphate crystals. The yield was 95%.
[0020] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is a well-known common additive. And compared with sodium hexafluorophosphate available on the market. Example 2 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 81.3%, while the comparative example 2, comparative example 5 sodium hexafluorophosphate only 78.4%, 71.4%; Example 2 adds sodium oxalate phosphate battery 5C discharge battery capacity is 166.9mAh / g, while the comparative example 2, comparative example 5 sodium hexafluorophosphate only 161.4mAh / g, 151.4mAh / g. Example 3
[0021] Dissolve 1 mol of sodium oxalate in water to prepare a 1.1 mol / L sodium oxalate aqueous solution; then add 1.2 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 90°C for 24 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 80°C under reduced pressure for 16 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0022] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 150 ml of acetonitrile, filtered, and the filtrate was distilled at 60°C under reduced pressure for 20 h, and vacuum dried at 70°C for 24 h to obtain sodium oxalate phosphate crystals. The yield was 96%.
[0023] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is a well-known common additive. And compared with sodium hexafluorophosphate available on the market. Example 3 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 82.5%, while the comparison example 3, comparison example 5 sodium hexafluorophosphate only 78.7%, 71.4%; Example 3 adds sodium oxalate phosphate battery 5C discharge battery capacity is 168.7mAh / g, while the comparison example 3, comparison example 5 sodium hexafluorophosphate only 163.2mAh / g, 151.4mAh / g. Example 4
[0024] Dissolve 1 mol of sodium oxalate in water to prepare a 0.9 mol / L sodium oxalate aqueous solution; then add 1.1 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 70°C for 16 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 75°C under reduced pressure for 14 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0025] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 120 ml of acetonitrile, filtered, and the filtrate was distilled at 45°C under reduced pressure for 18 h, and vacuum dried at 50°C for 20 h to obtain sodium oxalate phosphate crystals. The yield was 98%.
[0026] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is a well-known common additive. And compared with sodium hexafluorophosphate available on the market. Example 4 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 87.2%, while the comparison example 4, comparison example 5 sodium hexafluorophosphate is only 78.2%, 71.4%; add sodium oxalate phosphate battery 5C discharge battery capacity is 176.8mAh / g, while the comparison example 4, comparison example 5 sodium hexafluorophosphate is only 161.5mAh / g, 151.4mAh / g. Example 5
[0027] Dissolve 1 mol of sodium oxalate in water to prepare a 1.2 mol / L sodium oxalate aqueous solution; then add 0.9 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 80°C for 22 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 85°C under reduced pressure for 18 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0028] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 90 ml of acetonitrile, filtered, and the filtrate was distilled at 55°C under reduced pressure for 22 hours, and vacuum dried at 70°C for 22 hours to obtain sodium oxalate phosphate crystals. The yield was 98%.
[0029] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is well-known common additives. And compared with sodium hexafluorophosphate available on the market. Example 5 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 86.7%, while the comparative sodium hexafluorophosphate is only 71.4%; the sodium oxalate phosphate battery 5C discharge battery capacity is 175.2mAh / g, while the comparative sodium hexafluorophosphate is only 151.4mAh / g. Example 6
[0030] Dissolve 1 mol of sodium oxalate in water to prepare a 1.1 mol / L sodium oxalate aqueous solution; then add 1.1 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 75°C for 23 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 80°C under reduced pressure for 17 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0031] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 130 ml of acetonitrile, filtered, and the filtrate was distilled at 60°C under reduced pressure for 23 h, and vacuum dried at 65°C for 24 h to obtain sodium oxalate phosphate crystals. The yield was 97%.
[0032] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is well-known common additives. And compared with commercially available sodium hexafluorophosphate. Example 6 added sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 85.1%, while the comparative sodium hexafluorophosphate is only 71.4%; added sodium oxalate phosphate battery 5C discharge battery capacity is 173.3mAh / g, while the comparative sodium hexafluorophosphate is only 151.4mAh / g. Comparative Example 1
[0033] Dissolve 1 mol of sodium oxalate in water to prepare a 1 mol / L sodium oxalate aqueous solution; then add 1 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 50°C for 12 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 70°C under reduced pressure for 12 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0034] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 100 ml of acetonitrile, filtered, and the filtrate was distilled at 50°C under reduced pressure for 16 h, and vacuum dried at 60°C for 21 h to obtain sodium oxalate phosphate crystals. The yield was 96%.
[0035] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is well-known common additives. And compared with sodium hexafluorophosphate available on the market. Example 1 adds sodium oxalate phosphate battery and the capacity retention rate after 300 cycles at 50°C is 83.5%, while that of Comparative Example 1 and Comparative Example 5 is only 79.5% and 71.4%; Example 1 adds sodium oxalate phosphate battery 5C discharge battery capacity is 169.5mAh / g, while that of Comparative Example 1 and Comparative Example 5 is only 162.1mAh / g and 151.4mAh / g. Comparative Example 2
[0036] Dissolve 1 mol of sodium oxalate in water to prepare a 1.2 mol / L sodium oxalate aqueous solution; then add 0.8 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 40°C for 10 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 90°C under reduced pressure for 20 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0037] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 50 ml of acetonitrile, filtered, and the filtrate was distilled under reduced pressure at 40°C for 24 h, and vacuum dried at 50°C for 18 h to obtain sodium oxalate phosphate crystals. The yield was 95%.
[0038] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is a well-known common additive. And compared with sodium hexafluorophosphate available on the market. Example 2 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 81.3%, while the comparative example 2, comparative example 5 sodium hexafluorophosphate only 78.4%, 71.4%; Example 2 adds sodium oxalate phosphate battery 5C discharge battery capacity is 166.9mAh / g, while the comparative example 2, comparative example 5 sodium hexafluorophosphate only 161.4mAh / g, 151.4mAh / g. Comparative Example 3
[0039] Dissolve 1 mol of sodium oxalate in water to prepare a 1.1 mol / L sodium oxalate aqueous solution; then add 1.2 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 100°C for 26 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 80°C under reduced pressure for 16 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0040] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 150 ml of acetonitrile, filtered, and the filtrate was distilled at 60°C under reduced pressure for 20 h, and vacuum dried at 70°C for 24 h to obtain sodium oxalate phosphate crystals. The yield was 96%.
[0041] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is a well-known common additive. And compared with sodium hexafluorophosphate available on the market. Example 3 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 82.5%, while the comparison example 3, comparison example 5 sodium hexafluorophosphate only 78.7%, 71.4%; Example 3 adds sodium oxalate phosphate battery 5C discharge battery capacity is 168.7mAh / g, while the comparison example 3, comparison example 5 sodium hexafluorophosphate only 163.2mAh / g, 151.4mAh / g. Comparative Example 4
[0042] Dissolve 1 mol of sodium oxalate in water to prepare a 0.9 mol / L sodium oxalate aqueous solution; then add 1.1 mol of phosphoric acid dropwise to the sodium oxalate aqueous solution under heating and stirring conditions, and react at 110°C for 28 hours. After the reaction, the solution is filtered, and the filtrate is distilled at 75°C under reduced pressure for 14 hours to obtain a mixture of sodium oxalophosphate and sodium hydroxide.
[0043] A mixture of 10 g of sodium oxalate phosphate and sodium hydroxide was dissolved in 120 ml of acetonitrile, filtered, and the filtrate was distilled at 45°C under reduced pressure for 18 h, and vacuum dried at 50°C for 20 h to obtain sodium oxalate phosphate crystals. The yield was 98%.
[0044] Sodium oxalate phosphate was heated at 3.3 V Na 0.83 Li 0.25 Mn 0.75The O2 / hard carbon soft pack battery system was tested for high temperature cycle stability and rate performance. Among them, the sodium electrolyte solvent is 30wt% DMC + 25wt% DEC, the electrolyte is sodium oxalate phosphate, the content is 30wt%-40wt%, and the rest is a well-known common additive. And compared with sodium hexafluorophosphate available on the market. Example 4 adds sodium oxalate phosphate battery 50 ° C cycle 300 times capacity retention rate is 87.2%, while the comparison example 4, comparison example 5 sodium hexafluorophosphate is only 78.2%, 71.4%; add sodium oxalate phosphate battery 5C discharge battery capacity is 176.8mAh / g, while the comparison example 4, comparison example 5 sodium hexafluorophosphate is only 161.5mAh / g, 151.4mAh / g. Comparative Example 5
[0045] The sodium hexafluorophosphate in this comparative example was purchased from the market, the manufacturer is McLean, the purity is 99.9%, and the brand is 21324-39-0. 0.83 Li 0.25 Mn 0.75 The O2 / hard carbon soft pack battery system was tested for high temperature and rate performance. The sodium electrolyte solvent was 30wt% DMC + 25wt% DEC, the electrolyte was sodium hexafluorophosphate, the content was 30wt%-40wt%, and the rest was commonly used additives.
[0046]
[0047] It can be seen from Table 1 that the obtained sodium oxalate phosphate has high purity (>99.9%) and low impurity content (free acid <20ppm, water <20ppm, chloride ion <5ppm, sulfate ion <5ppm). The sodium oxalate phosphate in each embodiment can control the free acid and water content within 20ppm, which plays a positive role in reducing the acidity and water content of the electrolyte. The impurity content of the comparative example (the synthesis reaction temperature and time are different from those of the embodiment) is higher than that of the embodiment. It shows that the reaction temperature and time of the present invention are more effective.
[0048] The purity of sodium oxalate phosphate was tested by the nuclear magnetic resonance internal standard method. The internal standard was triphenyl phosphate and the solvent was deuterated methanol. A small amount of sodium oxalate phosphate and triphenyl phosphate were dissolved in deuterated methanol to prepare the test solution. Then the test was performed to obtain 31 P NMR spectrum, and the purity of sodium oxalate phosphate was obtained by internal standard method calculation formula.
[0049]
[0050] As can be seen from Table 2, the high temperature and rate performance of the sodium oxalate phosphate obtained in each embodiment is significantly higher than that of the comparative example. In Example 4, the capacity retention rate of the battery with sodium oxalate phosphate added at 50°C for 300 cycles reached 87.2%, while that of the comparative example sodium hexafluorophosphate was only 71.4%; the capacity of the battery with sodium oxalate phosphate added at 5C discharge reached 176.8mAh / g in Example 4, while that of the comparative example sodium hexafluorophosphate was only 151.4mAh / g. Moreover, the battery performance of the embodiment with sodium oxalate phosphate added is better than that of comparative examples 1-4 (the synthesis reaction temperature and time are different from those of the embodiment). This shows that the reaction temperature and time effects of the present invention are better. It also shows that the sodium oxalate phosphate of the present invention has better performance as a sodium electrolyte than sodium hexafluorophosphate.
[0051] Figure 1 This is the P-NMR spectrum of the sodium oxalate phosphate of Example 1 of the present invention. The absorption peaks at 10.3 ppm and 18.8 ppm belong to the sodium oxalate phosphate.
Claims
1. A method for preparing sodium oxalate phosphate, characterized in that: The following steps are involved: (1) adding phosphoric acid dropwise to a sodium oxalate aqueous solution under heating and stirring conditions, and distilling under reduced pressure after the reaction is completed to obtain a mixture of sodium oxalophosphate and sodium hydroxide; (2) The obtained mixture of sodium oxalate phosphate and sodium hydroxide is dissolved in acetonitrile, filtered, the filtrate is distilled under reduced pressure, and the obtained solid is vacuum dried to obtain sodium oxalate phosphate.
2. The method for preparing sodium oxalate phosphate according to claim 1, characterized in that: In the step (1), the ratio of sodium oxalate to phosphoric acid is 1 mol:0.8-1.2 mol, the heating and stirring temperature is 60-90°C, the time is 14-24 hours, and the reduced pressure distillation temperature is 70-90°C, and the time is 12-20 hours.
3. The method for preparing sodium oxalate phosphate according to claim 2, characterized in that: The heating and stirring temperature is 70-80°C and the time is 16-22h.
4. The method for preparing sodium oxalate phosphate according to claim 1, characterized in that: In the step (2), the ratio of the mixture of sodium oxalate phosphate and sodium hydroxide to acetonitrile is 1 g:5-15 ml, the temperature of the reduced pressure distillation is 40-60° C., and the time is 16-24 h; the temperature of the vacuum drying is 50-70° C., and the time is 18-24 h.
Citation Information
Patent Citations
Oxalic acid lithium phosphate and preparation method therefor
CN106299473A
Method for preparing trioxalate phosphate
CN110229189A
Preparation method of oxalate phosphate, oxalate phosphate derivative and preparation method thereof, and electrolyte salt
CN114075104A
Preparation process of oxalate phosphate
CN117624244A
Synthetic method of lithium bis(oxalato) borate
KR101358682B1