Environment-friendly anti-counterfeit packaging material and manufacturing process thereof
By using polylactic acid and other materials to prepare substrates and coatings, environmentally friendly anti-counterfeiting packaging materials are formed, which solves the problem of difficult degradation of traditional anti-counterfeiting packaging materials, and achieves the improvement of the mechanical properties of the materials and environmentally friendly degradability.
Patent Information
- Application Number
- CN202411202026.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional anti-counterfeiting packaging materials are difficult to degrade, resulting in environmental pollution problems.
The substrate is prepared using polylactic acid, polyethylene glycol, plasticizer, antioxidant and modified silica and other materials, and coated with polylactic acid, polyethylene glycol, N,N'-methylene bis Coatings are prepared by materials such as acrylamide, carboxymethyl chitosan and nanotitanium dioxide, and environmentally friendly anti-counterfeiting packaging materials are formed through laser holographic molding, vacuum evaporation and heat treatment.
It improves the mechanical properties, dimensional stability and antibacterial properties of the material, and also has the advantages of degradability and recyclability, reducing the impact on the environment.
Smart Images

Figure BDA0005018072690000061 
Figure BDA0005018072690000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of anti-counterfeiting materials, and in particular relates to an environmentally friendly anti-counterfeiting packaging material and a manufacturing process thereof. Background Art
[0002] Anti-counterfeiting technology refers to measures taken to achieve the purpose of anti-counterfeiting. It can accurately identify the authenticity within a certain range and is not easy to be imitated or copied. Anti-counterfeiting is a preventive measure taken against activities that are imitated or copied for the purpose of deception without the permission of the owner. It is also a preventive technical measure taken to protect corporate brands, protect the market, and protect the legitimate rights and interests of consumers.
[0003] With the improvement of environmental awareness, the environmental protection of anti-counterfeiting packaging materials has become an important consideration, and the anti-counterfeiting packaging materials industry is moving towards a more environmentally friendly direction. At present, environmental protection and sustainability are important development directions for the anti-counterfeiting packaging industry. The impact on the environment can be reduced by adopting environmentally friendly materials, reducing packaging waste, optimizing packaging structure, etc. In order to reduce the burden on the environment, anti-counterfeiting packaging materials generally use biodegradable plastics, recycled paper, degradable bubble film, and recyclable packaging materials to improve environmental protection. These materials not only help reduce environmental pollution, but also solve the problem that traditional packaging materials are difficult to degrade to a certain extent. Summary of the invention
[0004] In order to solve the problem that traditional anti-counterfeiting packaging materials are difficult to degrade, the present invention provides an environmentally friendly anti-counterfeiting packaging material and a manufacturing process thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An environmentally friendly anti-counterfeiting packaging material comprises a substrate and a coating, wherein the coating is arranged on the top of the substrate, and the substrate comprises the following raw materials in parts by weight:
[0007] 70-90 parts of polylactic acid, 5-10 parts of polyethylene glycol, 0.1-1 parts of plasticizer, 0.5-2 parts of lubricant, 0.1-0.3 parts of antioxidant, and 5-13 parts of modified silica.
[0008] As a preferred embodiment of the present invention, the modified silicon dioxide comprises the following preparation steps:
[0009] Lactide is fully dissolved in dimethyl sulfoxide at 90-95° C., silicon dioxide and 4-dimethylaminopyridine are added, the temperature is raised to 135-140° C., and the mixture is reacted for 22-24 hours under a nitrogen atmosphere. The mixture is centrifugally filtered, washed, and dried to obtain modified silicon dioxide.
[0010] As a preferred embodiment of the present invention, the usage ratio of lactide, dimethyl sulfoxide, silicon dioxide and 4-dimethylaminopyridine is 8-10 g:50 mL:6-8 g:8.5 g.
[0011] As a preferred embodiment of the present invention, the plasticizer is one of glycerol citrate, acetyl tributyl citrate and triethyl citrate.
[0012] As a preferred embodiment of the present invention, the lubricant is at least one of paraffin wax, magnesium stearate and polyethylene wax.
[0013] As a preferred embodiment of the present invention, the antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.
[0014] As a preferred embodiment of the present invention, the coating comprises the following raw materials in parts by weight:
[0015] 80-90 parts of polylactic acid, 20-25 parts of polyethylene glycol, 0.5-1 part of N,N'-methylenebisacrylamide, 5-10 parts of carboxymethyl chitosan, and 10-20 parts of nano titanium dioxide.
[0016] As a preferred embodiment of the present invention, the polylactic acid includes at least one of poly-L-lactic acid, poly-D-lactic acid and poly-racemic polylactic acid.
[0017] The present invention also provides a process for producing an environmentally friendly anti-counterfeiting packaging material, comprising the following preparation steps:
[0018] S1. Weighing polylactic acid, polyethylene glycol, a plasticizer, a lubricant, an antioxidant and modified silicon dioxide in parts by weight, melt blending, extruding granulation, and blow molding to obtain a substrate;
[0019] Polylactic acid, polyethylene glycol, N,N'-methylenebisacrylamide, carboxymethyl chitosan and nano-titanium dioxide are uniformly mixed to obtain a coating;
[0020] S2. Apply the coating on the substrate, dry it, and then perform laser holographic molding, vacuum evaporation, and heat treatment on the coating to obtain an environmentally friendly anti-counterfeiting packaging material.
[0021] Beneficial effects of the present invention:
[0022] The present invention adopts polylactic acid, polyethylene glycol, plasticizer, lubricant, antioxidant and modified silica. Since polylactic acid itself is brittle, after being mixed with polyethylene glycol, plasticizer, lubricant, antioxidant and modified silica, the mechanical properties and dimensional stability of the substrate are greatly improved. The modified silica is prepared by grafting lactide with silica, so that the short chain of polylactic acid grows and extends on the surface of silica, thereby improving the compatibility and dispersibility between silica and the polylactic acid matrix. At this time, when the modified silica is used as a filler, the mechanical properties and thermal stability of the substrate are further enhanced. Furthermore, the coating of the present invention is prepared by mixing polylactic acid, polyethylene glycol, N,N'-methylenebisacrylamide, carboxymethyl chitosan and titanium dioxide. Doping nano titanium dioxide in the raw materials can improve the antibacterial performance of the composite coating. The nano titanium dioxide has a small particle size, a large specific surface area, and many active points, and can give full play to its antibacterial function. In addition, there is a strong hydrogen bonding interaction with the hydroxyl groups of carboxymethyl chitosan, which further enhances the antibacterial properties of the coating.
[0023] The anti-counterfeiting packaging material prepared in the present invention not only has an anti-counterfeiting function, but also conforms to the concept of green environmental protection, and has the advantages of being degradable and recyclable, so as to reduce the impact on the environment. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The carboxymethyl chitosan used in the present invention is prepared by the following steps:
[0026] 15 g of chitosan was alkalized and added to 150 mL of isopropanol, followed by 18 g of chloroacetic acid, and the reaction was continued for 2 h. The temperature was raised to 65° C. and the reaction was continued for another 2 h. The heating was stopped, and the pH was adjusted to neutral with 5% hydrochloric acid. The mixture was then washed repeatedly with methanol for 5 times and dried in an oven at 60° C. to obtain carboxymethyl chitosan.
[0027] Example 1
[0028] This embodiment provides an environmentally friendly anti-counterfeiting packaging material, including a substrate and a coating, wherein the coating is disposed on the substrate, and the substrate includes the following raw materials in parts by weight:
[0029] 70 parts of poly-L-lactic acid, 5 parts of polyethylene glycol, 0.1 parts of glyceryl citrate, 0.5 parts of paraffin, 0.1 parts of antioxidant, 5 parts of modified silicon dioxide;
[0030] The antioxidant is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 1:1.
[0031] The preparation steps of modified silicon dioxide are as follows:
[0032] 8 g of lactide was fully dissolved in 50 mL of dimethyl sulfoxide at 95° C., 6.5 g of silica and 8.5 g of 4-dimethylaminopyridine were added, the temperature was raised to 135° C., and the mixture was reacted for 24 h under a nitrogen atmosphere. The mixture was centrifuged 5 times with anhydrous ethanol, filtered, washed, and dried to obtain modified silica.
[0033] The coating comprises the following raw materials in parts by weight:
[0034] 80 parts of poly (L-lactic acid), 20 parts of polyethylene glycol, 0.5 parts of N,N'-methylenebisacrylamide, 5 parts of carboxymethyl chitosan, and 10 parts of nano titanium dioxide.
[0035] The production process is as follows:
[0036] S1. Weighing poly-L-lactic acid, polyethylene glycol, glyceryl citrate, paraffin, antioxidant and modified silicon dioxide in parts by weight, melt blending, extruding granulation, and blow molding to obtain a substrate;
[0037] The poly (L-lactic acid), polyethylene glycol, N,N'-methylenebisacrylamide, carboxymethyl chitosan and nano-titanium dioxide are uniformly mixed to obtain a coating;
[0038] S2. Apply the coating on the substrate, dry it, and then perform laser holographic molding, vacuum evaporation, and heat treatment on the coating to obtain an environmentally friendly anti-counterfeiting packaging material.
[0039] Example 2
[0040] The only difference from Example 1 is that:
[0041] The preparation steps of modified silica are as follows:
[0042] 10 g of lactide was fully dissolved in 50 mL of dimethyl sulfoxide at 95° C., 7.8 g of silica and 8.5 g of 4-dimethylaminopyridine were added, the temperature was raised to 135° C., and the mixture was reacted for 24 h under a nitrogen atmosphere. The mixture was centrifuged 5 times with anhydrous ethanol, filtered, washed, and dried to obtain modified silica.
[0043] Example 3
[0044] The only difference from Example 1 is that:
[0045] The substrate comprises the following raw materials in parts by weight:
[0046] 80 parts of poly-L-lactic acid, 6 parts of polyethylene glycol, 0.3 parts of acetyl tributyl citrate, 0.8 parts of paraffin, 0.1 parts of antioxidant, and 8 parts of modified silica.
[0047] Example 4
[0048] The only difference from Example 1 is that:
[0049] The substrate comprises the following raw materials in parts by weight:
[0050] 88 parts of poly-L-lactic acid, 6 parts of polyethylene glycol, 0.3 parts of acetyl tributyl citrate, 0.8 parts of paraffin, 0.1 parts of antioxidant, and 13 parts of modified silica.
[0051] Example 5
[0052] The only difference from Example 1 is that:
[0053] The coating comprises the following raw materials in parts by weight:
[0054] 85 parts of poly-L-lactic acid, 20 parts of polyethylene glycol, 0.8 parts of N,N'-methylenebisacrylamide, 6 parts of carboxymethyl chitosan, and 16 parts of nano titanium dioxide.
[0055] Comparative Example 1
[0056] The only difference from Example 1 is that:
[0057] The substrate comprises the following raw materials in parts by weight:
[0058] 70 parts of poly-L-lactic acid, 5 parts of polyethylene glycol, 0.1 parts of glyceryl citrate, 0.5 parts of paraffin, and 0.1 parts of antioxidant.
[0059] Comparative Example 2
[0060] The only difference from Example 1 is that:
[0061] Replace 5 parts of modified silica with 3 parts of modified silica.
[0062] Comparative Example 3
[0063] The only difference from Example 1 is that:
[0064] 5 parts of modified silica were replaced with 16 parts of modified silica.
[0065] Comparative Example 4
[0066] The only difference from Example 1 is that:
[0067] The coating comprises the following raw materials in parts by weight:
[0068] 80 parts of poly (L-lactic acid), 20 parts of polyethylene glycol, 0.5 parts of N,N'-methylenebisacrylamide, and 5 parts of carboxymethyl chitosan.
[0069] The environmentally friendly anti-counterfeiting packaging materials obtained in Examples 1 to 5 and Comparative Examples 1 to 4 were applied and tested for performance. The anti-counterfeiting packaging materials were prepared into square samples with a side length of 20 mm, and then the following tests were performed: (1) Tear strength test: The sample was placed on a universal testing machine and tested at a tensile speed of 5 mm / min; (2) Heat resistance test: Dimensional stability test: The sample was marked with lines, adjusted at room temperature of 25°C, the distance between the lines was measured, and the sample was placed on a support in an oven preheated at 180°C. The timer was started from the time when the oven temperature returned to the specified temperature. After 30 minutes, the sample was taken out and cooled to room temperature of 25°C. The distance between the lines was measured again. The change rate of the obtained data was the index of dimensional stability; (3) Antibacterial performance test: The test was performed in accordance with HG / T 3950-2007, and the antibacterial performance test was performed using Staphylococcus aureus and Escherichia coli. The above test results are shown in Table 1:
[0070] Table 1
[0071]
[0072]
[0073] It can be seen from Table 1 that the tear strength and dimensional stability of Examples 1-5 are better than those of Comparative Examples 1-3, and the antibacterial properties of Examples 1-5 are better than those of Comparative Example 4. It can be seen that the environmentally friendly anti-counterfeiting packaging material provided by the present invention has excellent mechanical properties, dimensional stability and antibacterial properties, and the raw materials are easily degradable and recyclable, thereby reducing the impact on the environment.
[0074] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0075] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An environmentally friendly anti-counterfeiting packaging material, comprising a substrate and a coating, wherein the coating is disposed on the substrate, characterized in that: The substrate comprises the following raw materials in parts by weight: 70-90 parts of polylactic acid, 5-10 parts of polyethylene glycol, 0.1-1 parts of plasticizer, 0.5-2 parts of lubricant, 0.1-0.3 parts of antioxidant, and 5-13 parts of modified silica.
2. The environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The modified silicon dioxide comprises the following preparation steps: Lactide is fully dissolved in dimethyl sulfoxide at 90-95° C., silicon dioxide and 4-dimethylaminopyridine are added, the temperature is raised to 135-140° C., and the mixture is reacted for 22-24 hours under a nitrogen atmosphere. The mixture is centrifugally filtered, washed, and dried to obtain modified silicon dioxide.
3. The environmentally friendly anti-counterfeiting packaging material according to claim 2, characterized in that: The usage ratio of lactide, dimethyl sulfoxide, silicon dioxide and 4-dimethylaminopyridine is 8-10 g:50 mL:6-8 g:8.5 g.
4. The environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The plasticizer is one of glycerol citrate, acetyl tributyl citrate and triethyl citrate.
5. The environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The lubricant is at least one of paraffin wax, magnesium stearate and polyethylene wax.
6. The environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The antioxidant is prepared by mixing antioxidant 1010 and antioxidant 168 in a mass ratio of 1:
1.
7. The environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The coating comprises the following raw materials in parts by weight: 80-90 parts of polylactic acid, 20-25 parts of polyethylene glycol, 0.5-1 part of N,N'-methylenebisacrylamide, 5-10 parts of carboxymethyl chitosan, and 10-20 parts of nano titanium dioxide.
8. The environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The polylactic acid includes at least one of poly-L-lactic acid, poly-D-lactic acid and poly-racemic polylactic acid.
9. The process for producing an environmentally friendly anti-counterfeiting packaging material according to claim 1, characterized in that: The method comprises the following preparation steps: S1. Weighing polylactic acid, polyethylene glycol, a plasticizer, a lubricant, an antioxidant and modified silicon dioxide in parts by weight, melt blending, extruding granulation, and blow molding to obtain a substrate; Polylactic acid, polyethylene glycol, N,N'-methylenebisacrylamide, carboxymethyl chitosan and nano-titanium dioxide are uniformly mixed to obtain a coating; S2. Apply the coating on the substrate, dry it, and then perform laser holographic molding, vacuum evaporation, and heat treatment on the coating to obtain an environmentally friendly anti-counterfeiting packaging material.
Citation Information