Preparation process of insert waterproof adhesive tape for cavity structure
The insert waterproof adhesive prepared by using acid-resistant modifiers and microcapsule coating technology at the battery pole columns, the aging and complexity of the battery pole sealing structure is solved, and more efficient waterproof performance and longer use are achieved. life.
Patent Information
- Application Number
- CN202410971404.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-11-01
AI Technical Summary
The existing battery pole sealing structure is prone to aging and cracking during use, resulting in seal failure. The double-layer adhesive sealing method is complex and difficult to accurately control, affecting waterproof performance.
The insert waterproof adhesive preparation process for cavity structure is adopted. By pretreating the polyurethane resin with an acid-resistant modifier, adding inorganic fillers and surfactants, and microcapsules are coated with acid-resistant materials. Combine the additives for grinding and defoaming, forming an efficient waterproof adhesive.
It improves the waterproof performance and service life of the waterproof adhesive, can quickly release acidic reactants in an acidic environment to block pores, prevent electrolyte leakage, and extend the stability and acid resistance of the sealing structure.
Smart Images

Figure CN118879261A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a field related to an insert waterproof adhesive for a cavity structure, specifically to the field of waterproof adhesive for sealing a battery pole inside a battery, and in particular to a preparation process of an insert waterproof adhesive for a cavity structure. Background Art
[0002] With the rapid development of science and technology, the popularity of electronic products and electric equipment has increased year by year. As the core energy component of these devices, the performance stability and safety of batteries are particularly important. In the design and production of batteries, waterproofing and sealing technology is one of the key links. Especially inside the battery, the battery pole is the main transmission channel for battery current, and its waterproof sealing performance is directly related to the overall performance and service life of the battery. Therefore, the insert waterproof gluing technology for cavity structure came into being and became an indispensable part of the battery industry. The insert waterproof gluing technology for cavity structure is a technology specially used for waterproof sealing inside the battery. As the key component inside the battery, the waterproof sealing performance of the battery pole is crucial. Due to the large number of gaps and voids at the pole, these gaps and voids are easily affected by the external environment during the use of the battery, resulting in leakage of electrolyte inside the battery.
[0003] However, the pole sealing structure commonly used in the prior art mainly adopts a double-layer glue sealing method. Although this sealing structure improves the waterproof performance of the pole to a certain extent, it still has many shortcomings in practical applications. First, the double-layer glue sealing structure is relatively complicated in the sealing process, and the thickness and uniformity of the glue layer need to be precisely controlled, otherwise it is easy to lead to poor sealing effect. Secondly, after long-term use, due to the influence of factors such as internal temperature changes and mechanical vibrations of the battery, the double-layer glue sealing structure is prone to aging, cracking and other problems, resulting in sealing failure. Summary of the invention
[0004] The present invention overcomes the shortcomings of the prior art and provides a process for preparing an insert waterproof adhesive for a cavity structure.
[0005] To achieve the above object, the technical solution adopted by the present invention is: a process for preparing a waterproof adhesive insert for a cavity structure, comprising the following steps:
[0006] S1: pretreating the polyurethane resin with an acid-resistant modifier to improve the acid resistance of the polyurethane resin;
[0007] S2: Mix the inorganic filler and the surfactant by stirring, add them to the product in S1, and continue stirring to obtain a mixture;
[0008] S3: encapsulating the acidic reactant and the acid-resistant material into microcapsules; adding the acidic reactant and the auxiliary agent to the mixture obtained in S2 and continuing to stir;
[0009] S4: Grind the product of S3, filter it, and perform vacuum degassing to obtain a gel-like waterproof adhesive.
[0010] In a preferred embodiment of the present invention, in S1, the acid-resistant modifier is selected from one of epoxy curing agent, silane coupling agent and polyvinyl alcohol modifier, and the added amount of the acid-resistant modifier accounts for 1%-5% of the amount of the polyurethane resin.
[0011] In a preferred embodiment of the present invention, in S1, the polyurethane resin is pretreated with an acid-resistant modifier as follows:
[0012] The acid-resistant modifier is mixed and stirred with the polyurethane resin in proportion, so that the acid resistance of the acid-resistant modifier is grafted onto the polyurethane resin, and a protective layer is formed on the outside of the polyurethane resin to achieve the acid-resistant effect.
[0013] In a preferred embodiment of the present invention, the specific parameters of the mixing and stirring are a stirring speed of 1400-1800 r / min, a first stage temperature of 108-112° C., a time of 1-2 h, and a second stage temperature of 65-85° C., a time of 3-4 h.
[0014] In a preferred embodiment of the present invention, in S2, the inorganic filler includes one or more of silicon dioxide, aluminum oxide and titanium dioxide, the inorganic filler accounts for 10%-40% of the polyurethane resin, and the surfactant accounts for 0.5%-5% of the inorganic filler.
[0015] In a preferred embodiment of the present invention, in S2, the stirring and mixing parameters are 1500-3000 r / min, the time is 10-30 min, and the continuous stirring parameters are 1000-1500 r / min, and the time is 10-20 min.
[0016] In a preferred embodiment of the present invention, in S3, the auxiliary agent includes one or more of a thickener, a leveling agent and an anti-aging agent, and the stirring parameter is continued to be 1000-1500 r / min for 20-30 min.
[0017] In a preferred embodiment of the present invention, in S3, the specific operation of microencapsulating the acidic reactant and the acid-resistant material is as follows:
[0018] S31: purifying the acidic reactant as a core material, and selecting a material that is compatible with the core material and can form a stable coating layer as a wall material;
[0019] S32: dispersing the core material in the colloidal solution of the wall material by a coacervation phase separation method, so that the wall material forms a coating layer on the surface of the core material.
[0020] In a preferred embodiment of the present invention, the acidic reactant is one of silica gel, mullite silicate and aluminum silicate, the acid-resistant material is one of sodium bicarbonate, silicate ceramics and polytetrafluoroethylene; the condensed phase separation method parameters are a temperature of 35-50°C and a pH value of 4.0-4.5.
[0021] In a preferred embodiment of the present invention, in S4, the grinding and refining parameters are grinding with a three-roll mill, a rotation speed of 200-500r / min, a time of 30-60min, filtration of 180-220 mesh, and vacuum degassing parameters of vacuum degree 1-10Pa, and time of 30-60min.
[0022] The present invention solves the defects existing in the background technology and has the following beneficial effects:
[0023] (1) The present invention provides a process for preparing an insert waterproof adhesive tape for a cavity structure, wherein an acidic reactant and an acid-resistant material are used in combination so that the acid-resistant material is coated on the outside of the acidic reactant, thereby ensuring the stability and long-term effectiveness of the acidic reactant, so that it can fully function when needed, and the coating structure allows the acidic reactant to be released when it contacts an acidic substance or an acidic electrolyte. Compared with the prior art, when the waterproof adhesive tape is applied to the pole of a wet acidic battery, the acidic reactant in the coating is rapidly released and reacts with the acidic electrolyte after contacting the electrolyte, thereby causing the acidic reactant to rapidly expand and block the pores around the pole, thereby preventing electrolyte leakage. Compared with uncoated acidic reactants, microencapsulated acidic reactants can achieve expansion and blockage more quickly and effectively, thereby improving the waterproof performance of the waterproof adhesive tape.
[0024] (2) The present invention provides a process for preparing an insert waterproof adhesive for a cavity structure. By using an acid-resistant modifier and an anti-aging agent in coordination with each other, the acid-resistant modifier reacts with hydrogen ions in the acid solution by introducing specific chemical groups or structures to form a stable compound or protective layer, thereby effectively preventing the acid solution from damaging the waterproof adhesive. At the same time, the anti-aging agent can capture and stabilize free radicals in the material, interrupt the chain reaction that causes aging, and maintain the physical and chemical stability of the waterproof adhesive. Compared with the prior art, by adding the acid-resistant modifier and the anti-aging agent at the same time, not only the acid resistance is improved, but also the service life is extended. In comparison, the comprehensive performance of the waterproof adhesive in a moist acidic environment is more excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.
[0026] Figure 1 is a flow chart of a preferred embodiment of the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein. Therefore, the protection scope of the present invention is not limited to the specific embodiments disclosed below.
[0029] As shown in the figure, a process for preparing a waterproof adhesive insert for a cavity structure includes the following steps:
[0030] S1: pretreating the polyurethane resin with an acid-resistant modifier to improve the acid resistance of the polyurethane resin;
[0031] In a preferred embodiment of the present invention, in S1, the acid-resistant modifier is selected from one of epoxy curing agent, silane coupling agent and polyvinyl alcohol modifier, and the added amount of the acid-resistant modifier accounts for 1%-5% of the amount of the polyurethane resin.
[0032] In a preferred embodiment of the present invention, in S1, the polyurethane resin is pretreated with an acid-resistant modifier as follows:
[0033] The acid-resistant modifier is mixed and stirred with the polyurethane resin in proportion, so that the acid resistance of the acid-resistant modifier is grafted onto the polyurethane resin, and a protective layer is formed on the outside of the polyurethane resin to achieve the acid-resistant effect.
[0034] In a preferred embodiment of the present invention, the specific parameters of the mixing and stirring are a stirring speed of 1400-1800 r / min, a first stage temperature of 108-112° C., a time of 1-2 h, and a second stage temperature of 65-85° C., a time of 3-4 h.
[0035] It should be noted that the use of an acid-resistant modifier to pretreat the polyurethane resin is specifically as follows: the acid-resistant modifier is mixed and stirred with the polyurethane resin in proportion. During the mixing and stirring process, the entire reaction process is divided into two stages: the first stage prepolymer synthesis stage and the second stage chain extension reaction stage. By controlling the reaction temperature and time of the two stages, the substances can efficiently complete the reaction. The epoxy curing agent reacts with the polyurethane resin to change the chemical structure of the polyurethane resin and introduce more stable chemical bonds and functional groups. This change in chemical structure can enhance the molecular chain stability of the polyurethane resin and make it less susceptible to corrosion in an acidic environment. That is, the epoxy groups contained in the epoxy curing agent react with the hydroxyl and amino groups in the polyurethane resin. During the reaction, the epoxy groups open the ring and form new chemical bonds, namely ether bonds and ester bonds, with the groups in the polyurethane resin. These newly formed chemical bonds are usually more stable than the original chemical bonds of the polyurethane resin, thereby improving the chemical stability of the entire material. Due to the introduction of new chemical bonds, the chemical structure of the polyurethane resin is changed, and its acid resistance is therefore enhanced.
[0036] Moreover, during the reaction process, the reaction between the epoxy curing agent and the polyurethane resin will form a tighter network structure, that is, increase the cross-linking density. High cross-linking density means more connection points between the molecular chains, which makes the entire material tougher and more resistant to external environmental erosion (such as acidic substances). That is, as the reaction of the epoxy curing agent and the polyurethane resin proceeds, more connection points, i.e., cross-linking points, will be formed between the molecular chains of the polyurethane resin. The increase in cross-linking density makes the connection between the molecular chains tighter, forming a tighter network structure. This structure gives the material higher strength, toughness and chemical resistance. High cross-linking density makes the material more resistant to external environmental erosion, i.e., acidic substances, because it is more difficult for acidic substances to penetrate into the material.
[0037] At the same time, after the epoxy curing agent reacts with the polyurethane resin, a denser protective layer is formed on the polyurethane resin. This protective layer can prevent external acidic substances from penetrating into the material, thereby protecting the internal polyurethane resin from being corroded. That is, due to the increase in cross-linking density and the change in chemical structure, the material formed after the epoxy curing agent reacts with the polyurethane resin has a denser surface and internal structure. This dense structure can prevent external acidic substances from penetrating into the material, thereby protecting the internal polyurethane resin from being corroded. In addition, the newly formed chemical bonds and functional groups also have a stronger resistance to acidic substances, further enhancing the acid resistance of the material.
[0038] S2: Mix the inorganic filler and the surfactant by stirring, add them to the product in S1, and continue stirring to obtain a mixture;
[0039] In a preferred embodiment of the present invention, in S2, the inorganic filler includes one or more of silicon dioxide, aluminum oxide and titanium dioxide, the inorganic filler accounts for 10%-40% of the polyurethane resin, and the surfactant accounts for 0.5%-5% of the inorganic filler.
[0040] In a preferred embodiment of the present invention, in S2, the stirring and mixing parameters are 1500-3000 r / min, the time is 10-30 min, and the continuous stirring parameters are 1000-1500 r / min, and the time is 10-20 min.
[0041] It should be noted that in the process of stirring and mixing the inorganic filler and the surfactant, a ball mill is used for stirring to grind the surface of the filler, so that the surface of the filler particles becomes rougher and its surface activity is increased. In this way, the specific surface area of the filler is increased, and more active sites are generated on its surface. These active sites can form stronger physical adsorption with the resin molecules, that is, chemical bonding of van der Waals force or covalent bond, thereby significantly improving the bonding strength between the filler and the resin. And the surfactant molecule has the characteristics of one end being hydrophilic (polar end) and one end being hydrophobic (non-polar end). In the process of combining the filler with the resin, this amphiphilic property plays a key role. When the surfactant is added to the mixture of the filler and the resin, its polar end will combine with the surface of the filler, while the non-polar end will face the resin. Due to the principle of similar compatibility, it has good compatibility with the resin molecules. Through this arrangement, the originally hydrophilic filler surface is transformed into an oleophilic (or resin-philic) surface, thereby greatly improving the compatibility and bonding between the filler and the resin. In this way, the filler is activated. Due to the change in its surface properties, the activated filler is easier to disperse evenly in the resin, which helps to avoid filler agglomeration and precipitation. At the same time, the uniform dispersion ensures a larger contact area between the filler particles and the resin, thereby providing more bonding opportunities and stronger bonding force. The surfactant actually forms a "bridge" between the filler and the resin. This "bridge" not only improves the compatibility between the two, but also enhances the interaction between them. Due to the presence of the surfactant, the adhesion strength between the filler and the resin is significantly improved. This enhanced adhesion strength is further converted into better mechanical properties of the composite material, such as tensile strength, compressive strength and impact toughness.
[0042] S3: encapsulating the acidic reactant and the acid-resistant material into microcapsules; adding the acidic reactant and the auxiliary agent to the mixture obtained in S2 and continuing to stir;
[0043] In a preferred embodiment of the present invention, in S3, the auxiliary agent includes one or more of a thickener, a leveling agent and an anti-aging agent, and the stirring parameter is continued to be 1000-1500 r / min for 20-30 min.
[0044] In a preferred embodiment of the present invention, in S3, the specific operation of microencapsulating the acidic reactant and the acid-resistant material is as follows:
[0045] S31: purifying the acidic reactant as a core material, and selecting a material that is compatible with the core material and can form a stable coating layer as a wall material;
[0046] S32: dispersing the core material in the colloidal solution of the wall material by a coacervation phase separation method, so that the wall material forms a coating layer on the surface of the core material.
[0047] In a preferred embodiment of the present invention, the acidic reactant is one of silica gel, mullite silicate and aluminum silicate, the acid-resistant material is one of sodium bicarbonate, silicate ceramics and polytetrafluoroethylene; the condensed phase separation method parameters are a temperature of 35-50°C and a pH value of 4.0-4.5.
[0048] It should be noted that the specific operation of microencapsulation of the acidic reactant and the acid-resistant material is: mixing the acidic reactant, i.e. sodium bicarbonate, with the coating material, and using a microencapsulation device to completely coat the acidic reactant inside the acid-resistant material to form a microcapsule. The specific coating method used is the condensed phase separation method, and the specific operation is:
[0049] A1: First, add the core material into a reaction medium containing a surfactant that is immiscible with the core material. Through mechanical stirring, a stable emulsified dispersion system is formed. In this system, the core material is evenly dispersed into fine particles or droplets, wherein the medium is specifically toluene, the stirring parameters are 800-1000r / min, and the time is 20-30min.
[0050] A2: Dissolve the polymer monomer of the wall material into the ethanol solution to form a uniform wall material solution.
[0051] A3: Mix the product in A1 with the wall material solution in A2 and change the pH to pH 4.0-4.5, so that the wall material is separated from the continuous solution to form a discontinuous new phase rich in wall material. Due to the thermodynamic instability of the particles in the wall material-rich phase, these particles will gather on the surface of the core material dispersed phase. This is a dynamic process, and the wall material particles will continue to gather on the surface of the core material until a complete coating layer is formed.
[0052] A4: As the wall material particles continue to gather on the surface of the core material, they will be deposited on the surface of the core material to form a continuous coating layer. In order to enhance the stability and mechanical strength of the coating layer, curing treatment is required. This can be done by heating to 35-50℃. The cured coating layer will become stronger and more durable, thus completing the coating operation.
[0053] It should also be noted that the use of an acid-resistant material, i.e., silica gel, as a coating layer can protect the internal acidic reactant from interference from the external environment, while ensuring that the acidic reactant can be dissolved and released in time when in contact with the electrolyte. The release rate of the acidic reactant can be controlled by adjusting the wall thickness and preparation process of the microcapsule. When the microcapsule comes into contact with the electrolyte, the electrolyte will gradually penetrate the coating layer and dissolve the internal acidic reactant, thereby achieving a gradual release and reaction effect.
[0054] S4: Grind the product of S3, filter it, and perform vacuum degassing to obtain a gel-like waterproof adhesive.
[0055] In a preferred embodiment of the present invention, in S4, the grinding and refining parameters are grinding with a three-roll mill, a rotation speed of 200-500r / min, a time of 30-60min, filtration of 180-220 mesh, and vacuum degassing parameters of vacuum degree 1-10Pa, and time of 30-60min.
[0056] It should be noted that grinding and refining is the process of refining materials using a three-roll mill. In the end, physical methods are used to further reduce the particle size of the material to improve its uniformity and fineness. By using the shear force between the three relatively rotating rollers in the three-roll mill, the material is repeatedly ground to gradually reduce its particle size, thereby achieving a refining effect. During the grinding process, the material is constantly tumbling and extruding between the rollers, making the particle size distribution more uniform and avoiding local agglomeration.
[0057] Vacuum degassing is a process in which the material is placed in a vacuum environment and the air pressure is reduced to gradually release the bubbles in the material. In a vacuum environment, the bubbles in the material gradually expand and escape due to the reduction of external air pressure, thereby achieving effective removal of bubbles. The removal of bubbles improves the purity of the material and avoids the adverse effects of bubbles on product performance and quality. The degassing material is more stable and is not prone to quality problems such as cracking and deformation due to the presence of bubbles.
[0058] Grinding and vacuum degassing are two steps, which respectively reduce the particle size of the material and remove bubbles through physical methods and vacuum technology, thereby improving the uniformity, fineness and purity of the product. These two steps play a key role in the preparation of the finished product and provide a guarantee for the high quality of the product.
[0059] Embodiment 1:
[0060] 100 parts of polyurethane resin were pretreated with epoxy curing agent to improve the acid resistance of polyurethane resin. The amount of epoxy curing agent added accounted for 3% of the amount of polyurethane resin. The specific operation was to mix the epoxy curing agent with the polyurethane resin in proportion so that the acid resistance of the epoxy curing agent was grafted onto the polyurethane resin and a protective layer was formed on the outside of the polyurethane resin to achieve the acid resistance effect. The mixing and stirring parameters were 1600r / min, the temperature of the first stage was 110℃, the time was 1.5h, and the temperature of the second stage was 75℃, the time was 3.5h.
[0061] 30 parts of inorganic filler and surfactant are stirred and mixed, added to the product in S1, and stirred continuously to obtain a mixture, wherein the inorganic filler is 20 parts of silica and 10 parts of alumina, the inorganic filler accounts for 30% of the polyurethane resin, and the surfactant accounts for 3% of the inorganic filler. The stirring and mixing parameters are 2000 r / min and the time is 25 min. The continuous stirring parameters are 1300 r / min and the time is 15 min.
[0062] 5 parts of acidic reactant and 20 parts of acid-resistant material are microencapsulated; and the auxiliary agents are added to the mixture obtained in S2 at the same time and continued to stir, wherein the auxiliary agents are 2 parts of thickener, 1 part of leveling agent and 3 parts of anti-aging agent, and the stirring parameters are continued at 1300r / min for 25min. The specific operation of microencapsulating the acidic reactant and the acid-resistant material is as follows: the acidic reactant is purified as the core material, and the material that is compatible with the core material and can form a stable coating layer is selected as the wall material; the core material is dispersed in the colloidal solution of the wall material by the condensed phase separation method, so that the wall material forms a coating layer on the surface of the core material, the acidic reactant is silica gel, and the acid-resistant material is sodium bicarbonate; the parameters of the condensed phase separation method are a temperature of 40°C and a pH value of 4.3.
[0063] Finally, the S3 product is ground, filtered, and vacuum degassed to obtain a gel-like waterproof adhesive. The grinding and refining parameters are grinding with a three-roll mill, a rotation speed of 400r / min, a time of 45min, filtration of 200 mesh, and vacuum degassing parameters of vacuum degree 7Pa, time 45min, to obtain a water-repellent adhesive.
[0064] Experiment 1:
[0065] Based on the preparation process of the waterproof adhesive prepared in Example 1, the dosage of the acidic reactant and the acid-resistant material was changed respectively to prepare several control groups, and the waterproof adhesive prepared by the preparation process of Example 1 was used as a preferred embodiment, and the waterproof adhesive prepared by the preferred embodiment was used as an experimental group to detect the anti-leakage property of the waterproof adhesive in a wet acidic environment. The specific experiment was as follows: a transparent cavity was constructed, a through hole was opened at the top of the cavity, a battery pole was placed at the through hole, and the temperature inside the cavity was controlled to be 40°C, the electrolyte was 0.5L, the humidity was 60%, and the acidic pH value was 1.2. The cavity was placed on a uniformly shaking platform to simulate the shaking of the battery in normal use, and the connection between the pole and the cavity was sealed inside the cavity, and the humidity outside the through hole was detected. After 48 hours, the humidity change outside the through hole and the corrosion of the part above the pole seal were detected, as shown in Table 1:
[0066] Table 1
[0067]
[0068] According to several control groups in Table 1, it can be seen that the preferred parameter of the acidic reactant is 5 parts, and the corresponding preferred parameter of the acid-resistant material is 20 parts. It can be seen that as the acidic reactant and the acid-resistant material both tend to the preferred parameters at the same time, the detected humidity change gradually decreases and the corrosion situation also gradually decreases. It can be seen that when the platform shakes, the acidic electrolyte is splashed on the acid-resistant material, and the acid-resistant material provides a certain protection for the pole. With the increase of electrolyte and the occurrence of capillary phenomenon, the acidic electrolyte penetrates into the acid-resistant material and reacts with the acidic reactant. The acidic reactant expands when it encounters acid and blocks the gap at the pole to reduce the occurrence of capillary phenomenon.
[0069] The above is based on the ideal embodiment of the present invention. Through the above description, relevant personnel can make various changes and modifications without departing from the technical concept of the present invention. The technical scope of the present invention is not limited to the content in the specification, and the technical scope must be determined according to the scope of the claims.
Claims
1. A process for preparing a waterproof adhesive insert for a cavity structure, characterized in that: The following steps are involved: S1: Pretreatment of polyurethane resin using an acid-resistant modifier; S2: Mix the inorganic filler and the surfactant by stirring, add them to the product in S1, and continue stirring to obtain a mixture; S3: encapsulating the acidic reactant and the acid-resistant material into microcapsules; adding the acidic reactant and the auxiliary agent to the mixture obtained in S2 and continuing to stir; S4: Grind the product of S3, filter it, and perform vacuum degassing to obtain a gel-like waterproof adhesive.
2. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In the above S1, the acid-resistant modifier is selected from one of epoxy curing agent, silane coupling agent and polyvinyl alcohol modifier, and the added amount of the acid-resistant modifier accounts for 1%-5% of the amount of the polyurethane resin.
3. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In S1, the polyurethane resin is pretreated with an acid-resistant modifier as follows: The acid-resistant modifier is mixed and stirred with the polyurethane resin in proportion, so that the acid resistance of the acid-resistant modifier is grafted onto the polyurethane resin and a protective layer is formed on the outside of the polyurethane resin.
4. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 3, characterized in that: The specific parameters of the mixing and stirring are a stirring speed of 1400-1800 r / min, a temperature of 108-112° C. for 1-2 h in the first stage, and a temperature of 65-85° C. for 3-4 h in the second stage.
5. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In the above S2, the inorganic filler includes one or more of silicon dioxide, aluminum oxide and titanium dioxide, the inorganic filler accounts for 10%-40% of the polyurethane resin, and the surfactant accounts for 0.5%-5% of the inorganic filler.
6. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In the S2, the stirring and mixing parameters are 1500-3000 r / min, the time is 10-30 min, and the continuous stirring parameters are 1000-1500 r / min, and the time is 10-20 min.
7. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In S3, the auxiliary agent includes one or more of a thickener, a leveling agent and an anti-aging agent, and the stirring parameter is continued to be 1000-1500 r / min for 20-30 min.
8. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In S3, the specific operation of microencapsulating the acidic reactant and the acid-resistant material is as follows: S31: purifying the acidic reactant as a core material, and selecting a material that is compatible with the core material and can form a stable coating layer as a wall material; S32: dispersing the core material in the colloidal solution of the wall material by a coacervation phase separation method, so that the wall material forms a coating layer on the surface of the core material.
9. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: The acidic reactant is one of silica gel, mullite silicate and aluminum silicate, and the acid-resistant material is one of sodium bicarbonate, silicate ceramics and polytetrafluoroethylene; the parameters of the condensed phase separation method are a temperature of 35-50°C, a pH value of 4.0-4.5, and a ratio of the acidic reactant to the acid-resistant material of 1:
4.
10. The process for preparing a waterproof adhesive insert for a cavity structure according to claim 1, characterized in that: In S4, the grinding and refining parameters are grinding with a three-roll mill, a rotation speed of 200-500 r / min, a time of 30-60 min, filtration of 180-220 mesh, and vacuum degassing parameters of vacuum degree 1-10 Pa, and time of 30-60 min.