Preparation method and application of antimony and arsenic polluted soil oxidation stabilization repair material
The synthesis of zero-valent iron ZVI-sodium metasilicate SMA composite material through co-precipitation method has solved the problem of the inability to oxidize trivalent antimony and arsenic in soils in the existing technology, and achieved long-term and stable restoration of antimony and arsenic contaminated soils, with simple process , environmentally friendly, efficient, stable and economical advantages.
Patent Information
- Application Number
- CN202410915145.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art cannot oxidize trivalent antimony and arsenic in soil at the same time, reducing their toxicity, resulting in difficulty in effectively stabilizing and repairing antimony and arsenic pollution generated during antimony mining and smelting.
The zero-valent iron ZVI-sodium metasilicate SMA composite material was synthesized by co-precipitation method, and the core-shell structure of zero-valent iron particles and the adsorption and networking of iron oxides were used to oxidize trivalent antimony and trivalent arsenic to a lower toxicity by oxidizing trivalent antimony and trivalent arsenic to a lower toxicity using the core-shell structure of zero-valent iron particles and iron oxide adsorption and complexation of iron oxides. pentavalent antimony and pentavalent arsenic achieve long-term and stable repair.
It realizes the toxicity of antimony and arsenic in solidified and stable soil, and has the advantages of simple process, environmental protection, high efficiency, stability and cost-effectiveness, significantly reduces the leaching and effective content of antimony and arsenic in the soil, and improves soil restoration. efficiency.
Smart Images

Figure CN118879330A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of soil remediation, in particular to a preparation method and application of an antimony-arsenic contaminated soil oxidation stabilization remediation material. Background Art
[0002] China is the largest country in terms of antimony (Sb) reserves and production, accounting for about 84% of the world's total antimony output. With the mining and smelting of antimony, tin and other non-ferrous metal minerals, the wastewater discharge, the stacking and leaching of waste rock and tailings have caused a large amount of antimony to accumulate in the surrounding soil. The mineralization process of antimony is accompanied by the generation of arsenic (As), so the antimony mining and smelting process will normally cause the combined pollution of antimony and arsenic.
[0003] Antimony (Sb) and arsenic (As) are both Group V elements with similar physical and chemical properties. Their migration and transformation are closely related to the redox state, and the toxicity of trivalent (III) antimony and arsenic is greater than that of pentavalent (V) antimony and arsenic. Arsenic is a highly toxic and highly carcinogenic metalloid, belonging to the first class of carcinogens, while antimony has certain cumulative toxicity and carcinogenicity and has been listed as a priority pollutant by various countries.
[0004] Since the mining and storage of antimony cannot avoid the serious pollution of the soil by highly toxic antimony and arsenic, the existing technology usually adopts sulfate-reducing bacteria (SRB) remediation treatment technology and carbon-based remediation materials. However, although they solidify and stabilize the release of antimony and arsenic in the soil, they cannot oxidize trivalent antimony and arsenic at the same time to reduce their toxicity.
[0005] Zero-valent iron (ZVI) among iron-based materials has been widely studied and applied in the oxidation and removal of pollutants in the environmental field, including chlorinated organic matter, nitrates, heavy metals in contaminated soil, etc., due to its advantages such as being green and non-toxic, abundant reserves, low cost and easy to produce.
[0006] Sodium metasilicate (SMA) is a salt of silicic acid and an inorganic salt product. It is a non-toxic, odorless, pollution-free white powder or crystalline particles that can prevent the redeposition of dirt, has strong detergency and large buffering capacity, can neutralize acidic dirt, has a deflocculation effect on inorganic matter, and has an anti-corrosion effect on metals.
[0007] Therefore, it is necessary to design a preparation method and application of an oxidation stabilization remediation material for antimony-arsenic contaminated soil. For shallow antimony-arsenic pollution in typical antimony mining areas, a zero-valent iron ZVI-sodium metasilicate SMA composite material is synthesized by co-precipitation. While solidifying and stabilizing the antimony and arsenic in the soil, trivalent antimony and trivalent arsenic are oxidized into less toxic pentavalent antimony and pentavalent arsenic, and long-term stable remediation can be achieved. Summary of the invention
[0008] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing an antimony-arsenic contaminated soil oxidation stabilization remediation material and its application. Aiming at shallow antimony-arsenic pollution in typical antimony mining areas, a zero-valent iron ZVI-sodium metasilicate SMA composite material is synthesized by co-precipitation method. While solidifying and stabilizing the antimony and arsenic in the soil, trivalent antimony and trivalent arsenic are oxidized into pentavalent antimony and pentavalent arsenic with lower toxicity, and long-term stable remediation can be achieved.
[0009] In order to achieve the above object, the present invention provides a method for preparing an antimony-arsenic contaminated soil oxidation stabilization repair material, comprising the following steps:
[0010] S1, dissolving zero-hydrate sodium metasilicate SMA in deionized water, and stirring thoroughly to make it fully dissolved;
[0011] S2, weigh the corresponding proportion of zero-valent iron ZVI and put it into a small beaker, add the corresponding proportion of zero-water sodium metasilicate SMA solution, and stir it evenly on a stirrer;
[0012] S3, placing the mixture of zero-valent iron ZVI and zero-hydrate sodium metasilicate SMA in a vacuum freeze dryer for freeze drying;
[0013] S4, placing the dried mixture in a ball mill, controlling a certain rotation speed, and dry-milling for a certain period of time to prepare ZVI-SMA composite materials with different ratios;
[0014] The specific ratio in S2 is: the ratio of zero-hydrate sodium metasilicate SMA to zero-valent iron ZVI is 1:3 to 1:80.
[0015] The invention discloses an application of an oxidation stabilization and remediation material for antimony-arsenic contaminated soil, which is used for oxidation stabilization and remediation of antimony-arsenic contaminated soil.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention adopts a coprecipitation method to synthesize a ZVI-SMA composite material. The core-shell structure of zero-valent iron particles in the composite material is a key component that reacts with heavy metal ions. The iron oxide formed on the surface of the zero-valent iron is conducive to the adsorption, complexation and coprecipitation of antimony and arsenic, and can form stable Fe-Sb-O bonds and Fe-Sb-As bonds. Therefore, while solidifying and stabilizing antimony and arsenic in the soil, trivalent antimony and trivalent arsenic can be oxidized into pentavalent antimony and pentavalent arsenic with lower toxicity, and long-term stable restoration can be achieved. The application method has the advantages of simple process, environmental protection, high efficiency, stability, high economic cost performance, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The curves of soil Sb leaching and effective content under different ratios and addition amounts of the present invention are shown in FIG. Figure 1 .
[0019] Figure 2 The curves of soil Sb leaching and effective content under different ratios and addition amounts of the present invention are shown in FIG. Figure 2 .
[0020] Figure 3 The curves of soil Sb leaching and effective content under different ratios and addition amounts of the present invention are shown in FIG. Figure 3 .
[0021] Figure 4 The curves of soil Sb leaching and effective content under different ratios and addition amounts of the present invention are shown in FIG. Figure 4 .
[0022] Figure 5 Schematic diagram of the effect of ferrosilicon material on the change of valence state of Sb and As in the soil of a contaminated site according to an embodiment of the present invention.
[0023] Figure 6 Schematic diagram of the leaching toxicity of Sb and As in the soil of a contaminated site by ferrosilicon material according to an embodiment of the present invention.
[0024] Figure 7 Schematic diagram of the effect of ferrosilicon material on the effective state of Sb and As in the soil of a contaminated site according to an embodiment of the present invention.
[0025] Figure 8 Schematic diagram of the effect of ferrosilicon material on the bioavailability of As in contaminated site soil according to an embodiment of the present invention.
[0026] Fig. 9 This is a SEM schematic diagram of the characterization of the ferrosilicon composite material before reaction in an embodiment of the present invention.
[0027] Fig.10 This is a schematic EDS diagram for characterizing the ferrosilicon composite material before reaction in an embodiment of the present invention.
[0028] Fig.11 This is a schematic diagram of XRD characterization of the ferrosilicon composite material before reaction in an embodiment of the present invention.
[0029] Fig.12 This is a schematic diagram of FTIR characterization of the ferrosilicon composite material before reaction in an embodiment of the present invention.
[0030] Fig.13 This is a schematic diagram of XRD characterization of the ferrosilicon composite material after reaction in an embodiment of the present invention.
[0031] Fig.14 This is a schematic XPS diagram for characterizing the ferrosilicon composite material after reaction according to an embodiment of the present invention. DETAILED DESCRIPTION
[0032] The present invention will now be further described with reference to the accompanying drawings.
[0033] See also Figures 1 to 14 The present invention provides a method for preparing an antimony-arsenic contaminated soil oxidation stabilization repair material, which is characterized by comprising the following steps:
[0034] S1, dissolving zero-hydrate sodium metasilicate SMA in deionized water, and stirring thoroughly to make it fully dissolved;
[0035] S2, weigh the corresponding proportion of zero-valent iron ZVI and put it into a small beaker, add the corresponding proportion of zero-water sodium metasilicate SMA solution, and stir it evenly on a stirrer;
[0036] S3, placing the mixture of zero-valent iron ZVI and zero-hydrate sodium metasilicate SMA in a vacuum freeze dryer for freeze drying;
[0037] S4, placing the dried mixture in a ball mill, controlling a certain rotation speed, and dry-milling for a certain period of time to prepare ZVI-SMA composite materials with different ratios;
[0038] The specific ratio in S2 is: the ratio of zero-hydrate sodium metasilicate SMA to zero-valent iron ZVI is 1:3 to 1:80.
[0039] The invention discloses an oxidation stabilization and remediation material for antimony-arsenic contaminated soil, which is used for oxidation stabilization and remediation of antimony-arsenic contaminated soil.
[0040] The present invention uses a laboratory simulation method to carry out an actual soil sample experiment using ferrosilicon composite materials to repair the following:
[0041] 1. Embodiment 1:
[0042] Weigh 2.00g of contaminated soil into a 50ml centrifuge tube, add a certain amount of ZVI-SMA composite material with a certain ratio, and add 10ml deionized water; shake at a constant temperature of 25 and 210r / min for 6h, collect the supernatant by centrifugation after the reaction, pass the sample solution through a 0.45μm needle filter membrane, and determine the antimony and arsenic concentration in the solution.
[0043] Example 1 Experimental results:
[0044] like Figure 1 to Figure 4As shown in the figure, the ZVI-SMA composite material with a ratio of 1:3 has a significant immobilization effect and is not easy to release at a 3% addition amount. After 60 days of remediation, the Sb leaching content is reduced by 76%, and the effective content is reduced by 90%. After adding 30g / kg of composite material, the remediation and removal rate of 1000mg / kg antimony in the soil is the most significant. After adding 10g / kg of composite material, the soil pH is significantly increased, mainly due to the oxidation of FeO and the release of OH- of the material. The increase in soil pH promotes the dissociation of antimonate, and reacts with Fe-OH on the composite material through coprecipitation and surface complexation. After 30 days of cultivation, the soil pH gradually stabilizes. Relatively speaking, the soil soluble ion concentration (EC) is relatively stable and does not change much.
[0045] 2. Embodiment 2:
[0046] Under normal temperature and pressure conditions, 5% zero-valent iron powder and 2mM zero-hydrated sodium metasilicate solution were added to the soil of the test site. The pH value of the zero-hydrated sodium metasilicate solution was adjusted with hydrochloric acid to a pH value of 2, and the zero-hydrated sodium metasilicate solution with adjusted pH was added, and the moisture content of the soil at the site was controlled between 30% and 35%, and the soil at the site was repaired in situ.
[0047] Example 2 Experimental results:
[0048] like Figure 5 As shown in the figure, the average contents of trivalent antimony and pentavalent antimony in the soil before stabilization were 263.83 mg / kg and 1881.50 mg / kg, respectively, and decreased to 102.18 mg / kg and 584.91 mg / kg after stabilization. The average contents of trivalent arsenic and pentavalent arsenic in the soil before stabilization were 0.66 mg / kg and 133.83 mg / kg, respectively, and decreased to 1.39 mg / kg and 42.93 mg / kg after stabilization.
[0049] like Figure 6 As shown, the leaching toxicity of heavy metals antimony and arsenic in the soil changed significantly. The leaching toxicity of antimony in the soil was 4.56±1.85 mg / kg before adding the stabilizer. After 7 days of repair, the leaching toxicity of antimony was reduced to 0.93±0.56 mg / kg. The leaching toxicity of antimony in each treatment was significantly reduced after 1 day of repair. After 3 days, the leaching toxicity increased and then stabilized. The stabilization efficiency of soil antimony leaching toxicity was 67.71% to 70.42%.
[0050] The arsenic leaching toxicity content in the soil before adding the stabilizer was 0.06±0.02mg / kg. After adding 5% zero-valent iron and 2mmol / L silicate solution for 7 days, the arsenic leaching toxicity content was reduced to 0.02±0.005mg / kg. The arsenic leaching toxicity content of each treatment decreased significantly after 1 day of repair and then tended to stabilize. The stabilization efficiency of soil arsenic leaching toxicity content was 46.38% to 64.29%.
[0051] like Figure 7 As shown, the effective antimony content in the soil before adding the stabilizer was 21.95±10.48 mg / kg, and after 7 days of restoration, the effective content decreased to 2.63±1.17 mg / kg. The effective antimony content of each treatment in the soil decreased significantly after 1 day of restoration, fluctuated in a small range for 3 to 5 days, and then stabilized as the cultivation progressed. The effective antimony content in the soil decreased by 28.19% to 72.56%.
[0052] The content of available arsenic in the soil before adding stabilizer was 0.23±0.29mg / kg. After 7 days of restoration, the content of available arsenic decreased to 0.06±0.02mg / kg. The content of available arsenic in each treatment of soil decreased significantly after 1 day of restoration and then tended to be stable. The content of available arsenic in soil decreased by 10.69% to 69.79%.
[0053] like Figure 8 As shown in the figure, the bioavailable state of antimony in the stomach phase and the bioavailable state in the intestine phase were 922.55±168.24mg / kg and 858.03±182.48mg / kg, respectively. After 7 days of restoration, the bioavailable state of antimony in the stomach phase and the bioavailable state in the intestine phase decreased to 466.13±106.39mg / kg and 386.29±79.21mg / kg, respectively. The average contents of bioavailable state of arsenic in the stomach phase and the bioavailable state in the intestine phase were 29.19±10.52mg / kg and 28.66±11.28mg / kg, respectively. After 1d of restoration, the bioavailable state in the stomach phase increased and then stabilized. After 7 days of restoration, the average contents of bioavailable state of arsenic in the stomach phase and the bioavailable state in the intestine phase decreased to 5.37±3.18mg / kg and 4.37±2.28mg / kg, respectively.
[0054] like Figures 9 to 12 As shown, after the composite material of the present invention is prepared, XRD results show that the main component of the sample is zero-valent iron, FTIR shows that the sample has Si-O-Fe bonds at 475cm-1, SEM finds that the ZVI after ball milling is a flaky solid, the increase of Si will cause more SiO2 balls to be embedded in the interior and surface of ZVI, and EDS results show that SiO2 is successfully loaded onto the surface of ZVI.
[0055] like Figure 13-14As shown, after the material of the present invention reacts with antimony and arsenic contaminated soil, the XRD spectrum shows that new characteristic peaks of Fe-Sb-O and Fe-Sb-As appear, and the characteristic peak intensity of zero-valent iron decreases significantly, indicating that Sb and As react with the ferrosilicon composite material. From the XPS results, it is observed that Sb3d and As3d orbitals appear in the full spectrum after adsorption, and the Fe2p orbital moves.
[0056] The above are only preferred embodiments of the present invention, which are only used to help understand the method and core idea of the present application. The protection scope of the present invention is not limited to the above embodiments. All technical solutions under the idea of the present invention belong to the protection scope of the present invention. It should be pointed out that for ordinary technicians in this technical field, some improvements and modifications without departing from the principle of the present invention should also be regarded as the protection scope of the present invention.
[0057] In the description of the present invention, it should be noted that the terms "upper", "lower", "inside", "outside", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.
[0058] The invention solves the problem that the prior art uses sulfate-reducing bacteria (SRB) bacteria remediation treatment technology and carbon-based remediation materials, but although the release of antimony and arsenic in the stabilized soil can be solidified, trivalent antimony and arsenic cannot be oxidized at the same time to reduce their toxicity. The zero-valent iron (ZVI)-sodium metasilicate (SMA) composite material is synthesized by a coprecipitation method. While solidifying the antimony and arsenic in the stabilized soil, trivalent antimony and trivalent arsenic are oxidized into pentavalent antimony and pentavalent arsenic with lower toxicity, and long-term stable remediation can be achieved. The invention has the advantages of simple application process, environmental protection, high efficiency, stability, high economic cost performance, and the like.
Claims
1. A method for preparing an oxidation-stabilized remediation material for antimony-arsenic contaminated soil, characterized in that: The following steps are involved: S1, dissolving zero-hydrate sodium metasilicate SMA in deionized water, and stirring thoroughly to make it fully dissolved; S2, weigh the corresponding proportion of zero-valent iron ZVI and put it in a small beaker, add the corresponding proportion of zero-water sodium metasilicate SMA solution, stir well on the stirrer; S3, placing the mixture of zero-valent iron ZVI and zero-hydrate sodium metasilicate SMA in a vacuum freeze dryer for freeze drying; S4, placing the dried mixture in a ball mill, controlling a certain rotation speed, and dry-milling for a certain period of time to prepare ZVI-SMA composite materials with different ratios; The specific ratio in S2 is: the ratio of the zero-hydrate sodium metasilicate SMA to the zero-valent iron ZVI is 1:3 to 1:
80.