Non-oriented electrical steel and preparation method thereof
By reasonably adding copper and nickel elements to non-oriented electrical steel and controlling the oxygen inflow of hot-rolled heating furnace, a copper-rich nickel precipitation phase is formed, which solves the problem of heavy leather defects of non-oriented electrical steel and improves the strength of the material and surface quality reduces alloy cost and ensures the safety and economicality of high-speed motors.
Patent Information
- Application Number
- CN202411200447.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-01
AI Technical Summary
Existing non-oriented electrical steels are prone to heavy skin defects in the process of increasing strength, resulting in increased safety hazards of the motor and increased alloy cost, making it difficult to find a balance between the two.
By reasonably designing the chemical composition of non-oriented electrical steel, adding copper elements and nickel elements in composite, and controlling the ratio of nickel-copper elements and the oxygen inlet in the hot-rolled heating furnace to the oxygen required for the complete combustion of combustible gases, forming copper-rich The nickel precipitation phase reduces the oxidation of surface grain grain boundaries and inhibits the occurrence of heavy skin defects.
It effectively reduces the incidence of heavy leather defects on the surface of non-oriented electrical steel, improves the strength and quality of the material, and controls the alloy cost, ensuring the safety and economicality of high-speed motors.
Smart Images

Figure CN118880179A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of electrical steel, and in particular to a non-oriented electrical steel and a preparation method thereof. Background Art
[0002] With the development of high-speed motors, the drive motors, as the core components of high-speed motors, have begun to develop towards high speed, high power density and miniaturization, which puts forward higher requirements on the performance of non-oriented electrical steel as the core material of the drive motor. At present, high-speed motors are mainly permanent magnet synchronous motors. Due to the narrow magnetic bridge of the rotor core of the permanent magnet synchronous motor, stress concentration will inevitably occur at the magnetic bridge when the rotor rotates at high speed. Fatigue fracture is prone to occur after long-term service, causing safety hazards. Therefore, high-strength non-oriented electrical steel materials are needed to prepare the rotor core laminations. Dislocation strengthening, precipitation strengthening and solid solution strengthening are usually used to improve the yield strength of the material, but the above methods will lead to a significant deterioration of the magnetic properties, resulting in a reduction in the overall efficiency of the motor.
[0003] At present, most of the high-strength non-oriented electrical steel is prepared by adding copper to achieve copper-rich phase precipitation strengthening. The size of the copper-rich precipitate phase is generally controlled at 5-50nm, which is smaller than the magnetic domain width, and has little effect on the magnetic properties. At the same time, the copper-rich phase and the matrix are coherent or semi-coherent, which can effectively hinder dislocation slip and significantly improve the material strength. However, the addition of copper will cause hot brittleness defects, which are reflected in the finished electrical steel as heavy skin defects.
[0004] The large addition of nickel can effectively avoid the occurrence of heavy skin defects, but at the same time the alloy cost will also increase significantly. Therefore, it is necessary to seek a balance between the alloy cost and the incidence of heavy skin defects from the perspective of suppressing the occurrence of heavy skin defects. Summary of the invention
[0005] The present application provides a non-oriented electrical steel and a preparation method thereof to solve the following technical problem: how to control the heavy skin defect of the non-oriented electrical steel.
[0006] In a first aspect, the present application provides a non-oriented electrical steel, wherein the chemical composition of the non-oriented electrical steel comprises, by mass fraction, Si: 2.50% to 5.00%, Al: 0.30% to 1.50%, Mn: 0.2% to 1.2%, Cu: 0.6% to 2.3%, Ni: 0.3% to 3.0%, C≤0.0040%, S≤0.0020%, N≤0.002%, V≤0.005%, Ti≤0.005%, and P≤0.002%.
[0007] Optionally, the chemical composition of the non-oriented electrical steel includes, by mass fraction: Si: 2.50% to 5.00%, Al: 0.30% to 1.50%, Mn: 0.2% to 1.2%, Cu: 0.6% to 2.3%, and Ni: 0.3% to 3.0%.
[0008] Optionally, the chemical composition of the non-oriented electrical steel further includes: any one of Sn and Sb.
[0009] Optionally, the mass fraction of Sn is 0.001% to 0.10%, and the mass fraction of Sb is 0.001% to 0.10%.
[0010] In a second aspect, the present application provides a method for preparing the non-oriented electrical steel described in the first aspect, the method comprising:
[0011] Obtaining the non-oriented electrical steel slab;
[0012] The slab is sequentially heated, rough rolled, finish rolled and coiled to obtain a hot rolled coil;
[0013] The hot-rolled coil is subjected to normalizing treatment, pickling and cold rolling in sequence to obtain a cold-rolled coil;
[0014] The cold-rolled coil is continuously annealed, and then an insulating layer is coated on at least a portion of the surface of the cold-rolled coil to obtain a continuously undone coil;
[0015] The continuous uncoil is subjected to aging annealing to obtain non-oriented electrical steel.
[0016] Optionally, the heating temperature is 1000° C. to 1200° C., the heating includes a first soaking section, and the duration of the first soaking section is 20 min to 100 min.
[0017] Optionally, the key process indicator K of the heating satisfies the following relationship:
[0018] K=2Q / P 4 ≥1.30;
[0019] In the formula, Q=[Ni] / [Cu], [Ni] represents the mass fraction of Ni element in the non-oriented electrical steel, and [Cu] represents the mass fraction of Cu element in the non-oriented electrical steel; P represents the ratio of the oxygen intake amount in the heating furnace to the oxygen amount required for complete combustion of the combustible gas.
[0020] Optionally, the start temperature of the finish rolling is 850° C. to 1050° C., the end temperature of the finish rolling is 820° C. to 920° C., and the thickness of the hot-rolled coil is 2.0 mm to 3.0 mm.
[0021] Optionally, the temperature of the normalizing treatment is 850°C to 1000°C, and the holding time of the normalizing treatment is 0.5min to 4min.
[0022] Optionally, the continuous annealing includes a second soaking zone, the temperature of the second soaking zone is 800° C. to 1050° C., and the duration of the second soaking zone is 0.3 min to 2 min.
[0023] Optionally, the temperature of the aging annealing is 400° C. to 600° C., and the soaking time of the aging annealing is 0.5 min to 30 min.
[0024] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0025] The present application provides a non-oriented electrical steel, wherein the chemical composition of the non-oriented electrical steel includes, by mass fraction, Si: 2.50% to 5.00%, Al: 0.30% to 1.50%, Mn: 0.2% to 1.2%, Cu: 0.6% to 2.3%, and Ni: 0.3% to 3.0%. By rationally designing the chemical composition of the non-oriented electrical steel, adding copper and nickel elements in combination, and limiting the amount of nickel added and the ratio of nickel to copper elements, the nickel and copper elements form a copper-rich nickel precipitation phase on the surface, and the copper content in the precipitation phase is greatly reduced. At the same time, by controlling the ratio of the oxygen intake in the hot rolling heating furnace to the oxygen required for complete combustion of the combustible gas, the solid solution of oxygen in the copper-rich phase at the grain boundary of the surface grain is reduced to inhibit the grain boundary oxidation of the slab surface, so that the probability of heavy skin occurrence is greatly reduced, and a high-strength non-oriented electrical steel with excellent surface quality is obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0027] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0028] Figure 1 A schematic flow chart of a method for preparing non-oriented electrical steel provided in an embodiment of the present application.
[0029] Figure 2 Surface state diagram of the embodiments and comparative examples of the non-oriented electrical steel provided in this application. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0031] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range; for example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which applies regardless of the range; in addition, whenever a numerical range is indicated in this document, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0032] In this document, the terms including "including" and "including" mean "including but not limited to". Relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. "And / or" describes the association relationship of associated objects, indicating that there can be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone; where A and B can be singular or plural. "At least one" means one or more, and "plurality" means two or more; "at least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items; for example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be single or multiple. Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0033] In a first aspect, the present application provides a non-oriented electrical steel, wherein the chemical composition of the non-oriented electrical steel comprises, by mass fraction, Si: 2.50% to 5.00%, Al: 0.30% to 1.50%, Mn: 0.2% to 1.2%, Cu: 0.6% to 2.3%, Ni: 0.3% to 3.0%, C≤0.0040%, S≤0.0020%, N≤0.002%, V≤0.005%, Ti≤0.005%, and P≤0.002%.
[0034] In some embodiments, the chemical composition of the non-oriented electrical steel includes, by mass fraction: Si: 2.50%-5.00%, Al: 0.30%-1.50%, Mn: 0.2%-1.2%, Cu: 0.6%-2.3%, Ni: 0.3%-3.0%.
[0035] The positive effect of controlling the Si content to 2.50% to 5.00% is that the main function of Si is to increase the resistivity. Adding Si can significantly reduce the core loss and reduce the magnetostriction of electrical steel. However, if the Si content is excessive, the plasticity of the strip steel will be greatly reduced, resulting in poor rollability. Therefore, the Si content is controlled to 2.50% to 5.00%, preferably 3.0% to 4.5%.
[0036] The positive effects of controlling the Al content to 0.30% to 1.50% are as follows: Al can be dissolved in ferrite to increase resistivity and reduce iron loss, and can also deoxidize and fix nitrogen, but it is easy to cause oxidation in the surface layer of the finished plate; Al can increase the yield strength, but high Al content is prone to blockage of the tundish outlet, making smelting and casting difficult, so the Al content is controlled to 0.30% to 1.50%, preferably 0.3% to 1.0%.
[0037] The positive effects of controlling the Mn content to 0.2% to 1.2% are as follows: Mn plays a role of solid solution strengthening in steel, improving the resistivity of electrical steel and reducing iron loss; Mn easily forms MnS inclusions with S to prevent hot brittleness caused by FeS, and MnS coarsening is beneficial to grain growth. At the same time, adding Mn is beneficial to punching and cutting properties. Therefore, the Mn content is controlled to 0.2% to 1.2%, preferably 0.2% to 0.8%.
[0038] The positive effect of controlling the Cu content to 0.6% to 2.3% is that the solid solubility of Cu element in ferrite is low at room temperature, and it can be precipitated in the form of copper-rich precipitation phase through aging treatment. The strength of the material can be greatly improved when the copper-rich phase is precipitated coherently or semi-coherently, which is the main strengthening method in this patent. At the same time, when the Cu content is less than 0.6%, the strengthening effect of the copper-rich phase precipitation is not obvious; when the copper content is greater than 2.3%, the incidence of hot cracking defects during high-temperature processing is greatly increased, so the Cu content is controlled to be 0.6% to 2.3%, preferably 0.6% to 2.3%.
[0039] The positive effect of controlling the Ni content to 0.3% to 3.0% is that the Ni element is a ferromagnetic element, which can improve the resistivity of electrical steel and reduce iron loss, and has no obvious deterioration effect on the processing performance of the material. At the same time, since the addition of the Cu element easily leads to hot brittle defects, the addition of the Ni element can change the composition and precipitation position of the copper-rich phase during high-temperature processing, and effectively reduce the occurrence rate of hot brittle defects. In order to reduce the occurrence rate of hot brittle defects, the amount of Ni element added needs to be controlled at more than 0.3%. At the same time, the price of nickel element is relatively high, and a large amount of addition will significantly increase the alloy cost. Therefore, the Ni element content should be reduced as much as possible while ensuring the surface quality of the material. Therefore, it is necessary to control the Ni element addition amount to be less than 2.3%, so the Ni content is controlled to be 0.3% to 3.0%, preferably 0.4% to 2.0%.
[0040] The positive effect of controlling the C content to ≤0.0040%: In electrical steel, C is the main element that produces magnetic aging. When the residual C content in the steel is high, the coercive force and hysteresis loss increase, and magnetic aging also occurs. Therefore, the C content is controlled to ≤0.0040%.
[0041] Positive effect of controlling the S content to ≤0.0020%: In non-oriented electrical steel, S element is the main precipitation phase forming element, mainly existing in the form of MnS and CuS. Such sulfides hinder grain growth and worsen iron loss. Therefore, the S content is controlled to ≤0.0020%.
[0042] Positive effect of controlling the N content to ≤0.002%: N, like C, will deteriorate the magnetic properties, so the N content is controlled to ≤0.002%.
[0043] Positive effects of controlling the V content to ≤ 0.005%: V is a harmful element in the non-oriented electrical steel of the present invention. V is a strong carbonitride-forming element and is very likely to form fine precipitates to deteriorate the magnetic properties. Therefore, the V content is controlled to ≤ 0.005%.
[0044] Positive effects of controlling the Ti content to ≤0.005%: Ti, as a strong carbonitride-forming element, is very likely to form fine precipitates in non-oriented electrical steel and deteriorate the magnetic properties. It is effective in improving strength, but it also has a significant effect on deteriorating iron loss. Usually, Ti is a harmful element in electrical steel like V, so the Ti content is controlled to ≤0.005%.
[0045] The positive effect of controlling the P content to ≤0.002% is that P is a strong grain boundary segregation element. Increased P content will cause embrittlement of electrical steel and lead to poor processing performance. Therefore, the P content is controlled to ≤0.002%.
[0046] In some embodiments, the chemical composition of the non-oriented electrical steel further includes: any one of Sn and Sb.
[0047] In some embodiments, the mass fraction of Sn is 0.001% to 0.10%, and the mass fraction of Sb is 0.001% to 0.10%.
[0048] The positive effect of controlling the content of Sn and Sb to 0.001% to 0.10% is that the addition of the segregation elements Sn and Sb generally plays the role of interface and surface segregation, improves the texture type during the recrystallization process, and thus improves the magnetic induction. The present invention sets the content of Sn and Sb to 0.001% to 0.10%, preferably 0.01% to 0.08%.
[0049] Figure 1 A schematic flow chart of a method for preparing non-oriented electrical steel provided in an embodiment of the present application.
[0050] See also Figure 1 In a second aspect, the present application provides a method for preparing non-oriented electrical steel, the method comprising:
[0051] S1. obtaining a slab of the non-oriented electrical steel;
[0052] S2, sequentially heating, rough rolling, finish rolling and coiling the slab to obtain a hot rolled coil;
[0053] In some embodiments, the heating temperature is 1000° C. to 1200° C., the heating includes a first soaking section, the duration of the first soaking section is 20 min to 100 min, and a reducing atmosphere is used in the heating furnace.
[0054] The positive effect of controlling the heating temperature to 1000℃~1200℃: If the heating temperature is too high than 1200℃, AlN will be re-solidified, and re-dispersed and precipitated in the subsequent process, which will deteriorate the magnetic properties; if the heating temperature is lower than 1000℃, the deformation resistance of the material will be large during the subsequent hot rolling process, and the hot rolling mill load will be large. Therefore, the heating temperature is controlled to be 1000℃~1200℃.
[0055] The positive effect of controlling the time of the first soaking section to 20min~100min: If the soaking time is less than 20min, the core temperature of the slab cannot reach the set temperature. If the soaking time is too long, it will waste heating resources and thicken the iron oxide scale. Therefore, the time of the first soaking section is controlled to 20min~100min.
[0056] The positive effect of using a reducing atmosphere in the heating furnace: Using a reducing atmosphere in the heating furnace can effectively avoid grain boundary oxidation, reduce the incidence of hot brittleness and heavy skin defects, and ensure surface quality.
[0057] In some embodiments, the key process indicator K of the heating satisfies the following relationship:
[0058] K=2Q / P 4 ≥1.30;
[0059] Wherein, Q=[Ni] / [Cu], [Ni] represents the mass fraction of Ni element in the non-oriented electrical steel, and [Cu] represents the mass fraction of Cu element in the non-oriented electrical steel; P represents the hot rolling heating atmosphere parameter, and the hot rolling heating atmosphere parameter is defined as the ratio of the oxygen intake amount in the heating furnace to the oxygen amount required for complete combustion of the combustible gas.
[0060] The principle and positive effect of the relationship K are as follows: the formula limits the Ni element, Cu element and hot rolling heating atmosphere in the material. Through the coordination between the three elements, the incidence of hot brittleness and heavy skin defects can be effectively reduced, ensuring the surface quality of hot rolling.
[0061] In some embodiments, the start temperature of the finish rolling is 850° C. to 1050° C., the end temperature of the finish rolling is 820° C. to 920° C., and the thickness of the hot-rolled coil is 2.0 mm to 3.0 mm.
[0062] The positive effect of controlling the start rolling temperature of finishing rolling to 850℃~1050℃: if the heating temperature is higher than 1050℃, it will lead to energy waste and poor plate shape stability; if the heating temperature is lower than 850℃, the deformation resistance of the material will be large during the subsequent finishing rolling process and the load of the hot rolling mill will be large. Therefore, the start rolling temperature of finishing rolling is controlled to 850℃~1050℃.
[0063] The positive effects of controlling the end temperature of finishing rolling to 820℃~920℃: if the end temperature of finishing rolling is too high, it will lead to energy waste and thicken the surface oxide scale; if the end temperature of finishing rolling is too low, it will increase the load of the finishing mill and affect the shape of the hot-rolled plate.
[0064] The positive effects of controlling the thickness of the hot-rolled coil to 2.0mm to 3.0mm: If the thickness of the hot-rolled coil is greater than 3.0mm, the processing volume of the subsequent cold-rolling process will increase, reducing the efficiency of the cold-rolling process. At the same time, due to the increase in deformation in the cold-rolling process, the magnetic properties of the final product will deteriorate; if the thickness of the hot-rolled coil is less than 2.0mm, the plate shape control capability of the hot-rolling mill is too high, and the hot-rolling stability is reduced.
[0065] S3, sequentially performing normalizing treatment, pickling and cold rolling on the hot-rolled coil to obtain a cold-rolled coil;
[0066] In some embodiments, the temperature of the normalizing treatment is 850° C. to 1000° C., and the holding time of the normalizing treatment is 0.5 min to 4 min.
[0067] The positive effects of controlling the temperature of normalizing treatment to 850℃~1000℃: Normalizing treatment can improve the uniformity of the organization and improve the magnetic properties of the finished product. When the normalizing temperature is higher than 1000℃, for high-grade non-oriented electrical steel, the cold rolling machinability of the steel coil deteriorates, and edge cracks or even strip breaks are prone to occur during the cold rolling of the steel coil. When the normalizing temperature is lower than 850℃, the effect of normalizing treatment becomes weaker, the hot-rolled deformed organization cannot complete recrystallization, the organization uniformity deteriorates, and it is not conducive to the improvement of texture components and the magnetic properties deteriorate.
[0068] The positive effects of controlling the holding time of normalizing treatment to 0.5min to 4min are as follows: the shorter the normalizing time, the weaker the normalizing effect, the inability of the hot-rolled deformed structure to complete recrystallization, the worsening of the structure uniformity, and the deterioration of the texture component improvement and magnetic properties; too long normalizing time causes waste of resources and deteriorates the cold rolling machinability.
[0069] In some embodiments, the cold rolling may be a single cold rolling or a double cold rolling; the cold rolling may be performed in a multi-stand continuous rolling mill or on a twenty-high rolling mill.
[0070] S4, continuously annealing the cold-rolled coil, and then coating an insulating layer on at least a portion of the surface of the cold-rolled coil to obtain a continuously undone coil;
[0071] In some embodiments, the continuous annealing includes a second soaking section, the temperature of the second soaking section is 800° C. to 1050° C., and the duration of the second soaking section is 0.3 min to 2 min.
[0072] The positive effect of controlling the temperature of the second soaking section to 800℃~1050℃: If the annealing temperature is too high, the finished product grains will be coarse and the high-frequency iron loss will increase significantly, which is not conducive to the application of the material in high-speed motors. If the annealing temperature is too low, the grains cannot complete recrystallization, the material structure may have deformed structure, and the magnetic properties will be greatly deteriorated.
[0073] The positive effects of controlling the time of the second soaking stage to 0.3min to 2min: If the soaking time is too long, the finished product grains will be coarse and the high-frequency iron loss will increase significantly, which is not conducive to the application of the material in high-speed motors; if the soaking time is too long, the grains cannot complete recrystallization, the material structure may have deformed structure, and the magnetic properties will be greatly deteriorated.
[0074] S5, performing aging annealing on the continuous uncoiling to obtain non-oriented electrical steel.
[0075] In some embodiments, the temperature of the aging annealing is 400° C. to 600° C., and the soaking time of the aging annealing is 0.5 min to 30 min.
[0076] The positive effects of controlling the aging annealing temperature to 400℃~600℃: if the aging annealing temperature is too high, the copper-rich precipitates are in an over-aged state, the size of the precipitates increases, the ability to hinder dislocation movement becomes weaker, and the role of the precipitates in improving the material strength becomes weaker; if the aging annealing temperature is too low, the precipitates cannot be effectively precipitated, the copper-rich precipitates cannot play the role of hindering dislocation movement, and the material strength is reduced.
[0077] The positive effects of controlling the soaking time of aging annealing to 0.5min to 30min: if the soaking time of aging annealing is too long, the copper-rich precipitates are in an over-aged state, the size of the precipitates increases, the ability to hinder dislocation movement becomes weaker, and the role of the precipitates in improving the material strength becomes weaker; if the soaking time of aging annealing is too short, the precipitates cannot be effectively precipitated, the copper-rich precipitates cannot play the role of hindering dislocation movement, and the material strength is reduced.
[0078] In some embodiments, aging annealing may be performed in a bell-type furnace or a continuous annealing furnace.
[0079] The present application is further described below in conjunction with specific examples. The experimental methods in the following examples that do not specify specific conditions are usually measured according to industry standards; if there are no corresponding industry standards, they are carried out according to common international standards, conventional conditions, or conditions recommended by the manufacturer.
[0080] The molten steel is smelted in a converter to obtain the chemical composition of non-oriented electrical steel, as shown in Table 1.
[0081] Based on the chemical composition of the non-oriented electrical steel in the embodiment and the comparative example, this embodiment also provides a method for preparing the non-oriented electrical steel, comprising the following steps:
[0082] Obtaining the non-oriented electrical steel slab;
[0083] The slab is sequentially heated, rough rolled, finish rolled and coiled to obtain a hot rolled coil;
[0084] The hot-rolled coil is subjected to normalizing treatment, pickling and cold rolling in sequence to obtain a cold-rolled coil;
[0085] The cold-rolled coil is continuously annealed, and then an insulating layer is coated on at least a portion of the surface of the cold-rolled coil to obtain a continuously undone coil;
[0086] The continuous uncoil is subjected to aging annealing to obtain non-oriented electrical steel.
[0087] The non-oriented electrical steels obtained in the examples and comparative examples were subjected to surface quality inspection, and the inspection results are shown in Table 1.
[0088] Table 1 Chemical composition (wt%) and surface quality inspection results of non-oriented electrical steel
[0089]
[0090] It can be seen from Table 1 that the chemical composition and key process indicator K of the embodiment are both within the required range of the present invention, the number of surface heavy skin defects meets the requirements, and the average number of heavy skin defects per 1000 m of the steel coil is less than 0.2 times.
[0091] In Comparative Examples 2, 7-9, due to the low nickel-copper ratio parameter Q, even if the hot rolling heating atmosphere parameter P is adjusted to 0.90, the surface of the finished steel coil will still have obvious heavy skin defects; as the nickel-copper ratio parameter Q increases, the requirements for the hot rolling heating atmosphere parameter P become looser. In Examples 2, 5-7, when the nickel-copper ratio parameter Q reaches 0.96, adjusting the heating furnace parameter P within the range of 0.90-1.10 will not cause obvious heavy skin defects. The hot rolling heating furnace also has strict regulations on the content of combustible gas in the post-combustion gas. When the ratio of the oxygen intake to the amount of oxygen required for the complete combustion of the combustible gas is too low, it will cause the gas emission standard to fail to meet the standard. In order to effectively suppress the surface heavy skin defects, minimize the addition of nickel elements, and reduce the alloy cost, it is recommended that the nickel-copper ratio parameter Q be controlled in the range of 0.56-0.70, and the hot rolling heating atmosphere parameter P be controlled in the range of 0.90-0.95, which can meet the gas emission standards while ensuring that the number of heavy skin defects on the surface of the finished electrical steel is lower than the standard.
[0092] Attached Figure 2 Detailed description:
[0093] Figure 2 The surface state diagram of the embodiments and comparative examples of the non-oriented electrical steel provided in this application; Figure 2 As shown, the left side is a surface state diagram of the embodiment, and the right side is a surface state diagram of the comparative example. Figure 2 It can be seen that the non-oriented electrical steel provided in the examples of the present application has excellent surface quality.
[0094] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0095] (1) The non-oriented electrical steel provided in the embodiments of the present application has excellent surface quality, and the number of heavy skin defects within 1000 m is less than 0.2.
[0096] (2) The amount of nickel added to the non-oriented electrical steel provided in the embodiments of the present application is minimized while the heavy skin defects are effectively controlled, and the cost is controlled.
[0097] The above is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. It will be apparent to those skilled in the art that various modifications to these embodiments are possible, and the general principles defined in the present application can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to these embodiments shown in the present application, but will conform to the widest scope consistent with the principles and novel features applied for by the present application.
Claims
1. A non-oriented electrical steel, It is characterized in that The chemical composition of the non-oriented electrical steel is as follows: Including: Si: 2.50% ~ 5.00%, Al: 0.30% ~ 1.50%, Mn: 0.2% ~ 1.2%, Cu: 0.6% ~ 2.3%, Ni:
0. 3%~3.0%, C≤0.0040%, S≤0.0020%, N≤0.002%, V≤0.005%, Ti≤0.005%, P≤0.002%.
2. The non-oriented electrical steel according to claim 1, It is characterized in that Calculated by mass fraction, the chemical composition of the non-oriented electrical steel includes: Si: 3.0% to 4.5%, Al: 0.3% to 1.0%, Mn: 0.2% to 0.8%, Cu: 0.6% to 2.3%, and Ni: 0.4% to 2.0%.
3. The non-oriented electrical steel according to claim 1 or 2, Features The chemical composition of the non-oriented electrical steel also includes: any one of Sn and Sb.
4. The non-oriented electrical steel according to claim 3, It is characterized in that The mass fraction of Sn is 0.001% to 0.10%, and the mass fraction of Sb is 0.001% to 0.10%.
5. A method for preparing non-oriented electrical steel according to any one of claims 1 to 4, It is characterized in that The method comprises: Obtaining the non-oriented electrical steel slab; The slab is sequentially heated, rough rolled, finish rolled and coiled to obtain a hot rolled coil; The hot-rolled coil is subjected to normalizing treatment, pickling and cold rolling in sequence to obtain a cold-rolled coil; The cold-rolled coil is continuously annealed, and then an insulating layer is coated on at least a portion of the surface of the cold-rolled coil to obtain a continuously unrolled coil; The continuous uncoil is subjected to aging annealing to obtain non-oriented electrical steel.
6. The method according to claim 5, It is characterized in that The heating temperature is 1000° C. to 1200° C., the heating includes a first soaking section, and the duration of the first soaking section is 20 min to 100 min.
7. The method according to claim 5, It is characterized in that The key process indicator K of the heating satisfies the following relationship: K=2Q / P 4 ≥1.30; In the formula, Q=[Ni] / [Cu], [Ni] represents the mass fraction of Ni element in the non-oriented electrical steel, and [Cu] represents the mass fraction of Cu element in the non-oriented electrical steel; P represents the ratio of the oxygen intake amount in the heating furnace to the oxygen amount required for complete combustion of the combustible gas.
8. The method according to claim 5, It is characterized in that The start temperature of the finishing rolling is 850° C. to 1050° C., the end temperature of the finishing rolling is 820° C. to 920° C., and the thickness of the hot-rolled coil is 2.0 mm to 3.0 mm.
9. The method according to claim 5, It is characterized in that The temperature of the normalizing treatment is 850° C. to 1000° C., and the holding time of the normalizing treatment is 0.5 min to 4 min.
10. The method according to claim 5, It is characterized in that The continuous annealing includes a second soaking section, the temperature of the second soaking section is 800° C. to 1050° C., and the duration of the second soaking section is 0.3 min to 2 min; and / or, The temperature of the aging annealing is 400° C. to 600° C., and the soaking time of the aging annealing is 0.5 min to 30 min.
Citation Information
Cited By
A process method for solving the peeling defect of the rolling surface of a new energy non-oriented silicon steel hot-rolled plate