Method for preparing copper foil production raw material electrolyte by industrially recycling waste batteries
By pretreating the used lithium-ion battery, dissolved in sulfuric acid and hydrogen peroxide solution and adding sodium chloride to adjust the pH, a high-purity electrolyte solution was prepared, which solved the problems of high cost and complex process in the production of electrolytic copper foil, and achieved high efficiency and environmental protection Copper foil electrolyte preparation is suitable for large-scale production.
Patent Information
- Application Number
- CN202410912095.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The existing electrolytic copper foil production process has high cost, complex process, serious pollution and it is difficult to effectively utilize waste copper powder, resulting in low production efficiency and environmental pollution.
After the waste lithium-ion battery is pretreated through continuous equipment, the copper powder is dissolved under stirring and heating using a mixed solution of sulfuric acid and hydrogen peroxide, and sodium chloride is added to adjust the pH, a high-purity electrolyte is prepared to reduce the impurity content and the difficulty of wastewater treatment. .
It realizes low-cost and high-efficiency copper foil electrolyte preparation, simplifies the process flow, reduces environmental pollution, and can effectively utilize waste copper powder, which is suitable for large-scale production.
Smart Images

Figure CN118880402A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recycling of waste lithium-ion batteries, and in particular to a method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production. Background Art
[0002] Research on the recycling of waste lithium-ion batteries mainly focuses on the recovery of valuable metals such as nickel, cobalt, lithium, and manganese, the recycling of positive electrode materials, and the high-value recovery of negative electrode graphite materials. Most of the recycling research does not involve waste copper foil in lithium batteries. Electrolytic copper foil, as the negative electrode current collector, is an important component of lithium-ion batteries. At present, the sulfate system is basically used in the industrial production of electrolytic copper foil. Copper sulfate and sulfuric acid are the basic components of the sulfate system electrolyte. After the copper foil in the waste battery is ground by a grinder, screened by a vibrating screen, and sorted by a sorter, the recycled copper powder has few impurities, high purity, regular particle morphology, and a large specific surface area, which is conducive to efficient sulfuric acid dissolution reaction.
[0003] Patent CN108570560A discloses a method for recovering copper from copper-containing waste. The ceramic and glass components in the copper waste easily cause some metals to be wrapped therein and cannot be recovered, affecting the quality of the electrolytic refining product. In addition, a large amount of non-metallic components are lost during the incineration process and cannot be effectively utilized, and the emitted gas will pollute the atmosphere, with high energy consumption. Patents CN102071312A and CN109504855A both disclose a method for producing copper foil from low-grade copper-containing materials. The copper content in these copper-containing materials is low, and they all need to be leached, extracted, etc. The production process is complicated, with many influencing factors, the process is discontinuous, and a large amount of toxic, harmful, and highly corrosive reagents are used. The waste liquid treatment cost is high and difficult to handle.
[0004] Since electrolytic copper foil has high requirements on the purity of copper sulfate, common copper sulfate is prepared from pure copper and pure sulfuric acid as raw materials. For example, patent CN116856019A records a method for preparing micron-level porous copper foil for lithium batteries and its application, which uses pure copper and pure sulfuric acid as raw materials. However, the copper sulfate electrolyte is prepared from pure copper and pure sulfuric acid, and the copper foil is made from pure copper, which has high costs for production enterprises, and the wastewater and waste liquid generated are difficult to treat, resulting in low production efficiency. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art, provide a method for industrially recycling waste batteries to prepare electrolyte as a raw material for copper foil production, and solve the problem of high cost of the existing electrolyte.
[0006] To achieve the above purpose, the technical solution adopted by this application is:
[0007] A method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production comprises the following steps:
[0008] 1) The charged waste batteries are pre-treated by continuous equipment such as shredding, crushing, demagnetization, pulverization and screening to quickly obtain copper powder;
[0009] 2) washing, filtering and drying the copper powder obtained in step 1) for later use;
[0010] 3) preparing a mixed solution of sulfuric acid and hydrogen peroxide, slowly adding the copper powder treated in step 2) thereto under stirring and heating until the copper powder is completely dissolved, and adding sodium chloride to the solution and stirring to obtain an electrolyte; and determining the purity of the electrolyte;
[0011] 4) When electroplating, adjust the pH with sodium hydroxide to obtain the electrolyte raw material required for electrolytic copper foil.
[0012] As a preferred technical solution, the charged waste batteries in 1) include various types of square, cylindrical and soft-pack lithium-ion batteries.
[0013] As a preferred technical solution, in the above 2), the cleaning agent used to clean the copper powder is at least one of dichloromethane, ethanol, N-methylpyrrolidone, dimethylacetamide, acetone, sulfuric acid and ultrapure water; the cleaning time is 20 to 30 minutes; the cleaning method is one or both of ultrasonic vibration and spray washing at room temperature.
[0014] As a preferred technical solution, when the cleaning agent is sulfuric acid, the concentration of the sulfuric acid is ≤10 mol / L.
[0015] As a preferred technical solution, the filtering method in 2) is one or both of bag filtering and mechanical filtration, wherein mechanical filtration includes quartz sand filtration, multi-media filtration and fiber ball filtration, and the filtration mesh number is ≤30.
[0016] As a preferred technical solution, the concentration of sulfuric acid in 3) is ≥15 mol / L; the concentration of hydrogen peroxide is ≥9 mol / L, heating and stirring are performed until the copper powder is completely dissolved, and the amount of hydrogen peroxide, sulfuric acid and copper powder is used in a mass ratio of 1:2-5:2-5.
[0017] As a preferred technical solution, after the copper powder is dissolved in 3), the concentration of the CuSO4 solution obtained is 10mmol / L~1mol / L; the concentration of H2SO4 is 0.5~2mol / L, and the heating is steam heating at a heating temperature of 50~60°C.
[0018] As a preferred technical solution, in said 3), sodium chloride is added to the dissolving solution in an amount of 1 mmol / L to 100 mmol / L; in said 4), sodium hydroxide is used to adjust the pH to 0.3 to 1.2.
[0019] As a preferred technical solution, in 4) during electroplating, an exhaust gas treatment device is set up, the absorbed gas is SO2, and the absorption method is one or more of activated carbon adsorption, UV photolysis, and spray tower; during electroplating, an exhaust gas collection device is added, and the collected gas is O2.
[0020] As a preferred technical solution, in said 3), the purity of the electrolyte is determined by an inductively coupled plasma atomic emission spectrometer, wherein the main impurity elements and their contents (ppm) are Co≤0.080, Mn≤0.020, Fe≤0.073, P≤0.077, and it does not contain toxic and harmful substances or elements such as As, Li, Hg, Cr, Cd, Pb, Br, PBB, PBDE, and the electrolyte purity is ≥99.8%.
[0021] The present invention has the following beneficial effects:
[0022] 1. The present invention utilizes waste batteries, and recovers copper powder with less impurities and regular morphology by tearing, crushing, demagnetizing, pulverizing and screening, and then removes impurities in the copper powder by washing, filtering and drying. The aluminum powder, black powder, over-crushed diaphragm and residual electrolyte in the copper powder can be removed during washing, and other solid impurities insoluble in sulfuric acid and hydrogen peroxide can be removed by selecting a reasonable filtering method, so as to prepare high-performance electrolytic copper foil electrolyte; the process has high dissolution efficiency, low impurity content, simple preparation steps, high production efficiency, and waste water can be recycled. It is an environmentally friendly, low-cost method that is easy to use for large-scale production.
[0023] 2. On the one hand, the present invention broadens the application field of copper material selection in the preparation of copper foil by electrolysis, and on the other hand, it realizes the efficient resource utilization of copper powder, a key component of waste battery crushing and sorting, which not only achieves the purpose of solid waste resource utilization, but also generates high economic benefits. It is a very promising new method with low cost, simple processing technology and no secondary pollution to the environment.
[0024] 3. The present invention adds sodium chloride to the electrolyte. The reducing effect of chloride ions is beneficial to stabilizing divalent copper ions in the electrolyte, thereby maintaining the stability and uniformity of the copper sulfate solution. For production enterprises, the obtained copper sulfate electrolyte is generally difficult to be immediately fed into the electroplating process in a short time. Therefore, adding a certain amount of chloride ions can avoid oxidation of divalent copper ions in copper sulfate and prolong the stabilization time. At the same time, the addition of chloride ions will not affect the electroplating of the copper sulfate solution by impurities, thereby avoiding affecting the purity. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The following drawings describe in detail the exemplary embodiments disclosed in this application. The same reference numerals represent similar structures in several views of the drawings. Those skilled in the art will understand that these embodiments are non-limiting, exemplary embodiments, and the drawings are only for the purpose of illustration and description, and are not intended to limit the scope of this application. Other embodiments may also accomplish the invention intent in this application.
[0026] Figure 1 This is a photo of the copper powder material recovered in Example 2 of the present invention;
[0027] Figure 2 This is a SEM image of the copper powder material recovered in Example 2 of the present invention;
[0028] Figure 3 This is the XRD diagram of the copper powder material recovered in Example 2 of the present invention. DETAILED DESCRIPTION
[0029] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0030] Embodiment 1:
[0031] A method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production comprises the following steps:
[0032] 1) The charged waste batteries are pre-treated by continuous equipment such as shredding, crushing, demagnetization, pulverization and screening to quickly obtain copper powder;
[0033] 2) washing, filtering and drying the copper powder obtained in step 1) for later use;
[0034] 3) preparing a mixed solution of sulfuric acid and hydrogen peroxide, slowly adding the copper powder treated in step 2) thereto under stirring and heating until the copper powder is completely dissolved, and adding sodium chloride to the solution and stirring to obtain an electrolyte; and determining the purity of the electrolyte;
[0035] 4) When electroplating, adjust the pH with sodium hydroxide to obtain the electrolyte raw material required for electrolytic copper foil;
[0036] The charged waste batteries in 1) include various types of square, cylindrical and soft-pack lithium-ion batteries;
[0037] In the above 2), the copper powder is cleaned with at least one of dichloromethane, ethanol, N-methylpyrrolidone, dimethylacetamide, acetone, sulfuric acid, and ultrapure water for 20 minutes, wherein the concentration of sulfuric acid is less than 10M, and the cleaning method is one or both of ultrasonic vibration and spray washing at room temperature;
[0038] The filtering method in step 2) is one or both of bag filtering and mechanical filtering, wherein mechanical filtering includes quartz sand filtering, multi-media filtering and fiber ball filtering, and the mesh number is ≤30;
[0039] In step 3), the concentration of sulfuric acid is ≥15M; the concentration of hydrogen peroxide is ≥9M, and heating and stirring are performed until the copper powder is completely dissolved;
[0040] In the step 3), after the copper powder is dissolved, the concentration of the CuSO4 solution is 10mM to 1M; the concentration of the H2SO4 is 0.5 to 2M, and the heating is steam heating;
[0041] In the step 3), the concentration of sodium chloride added is 1 mM to 100 mM; in the step 4), sodium hydroxide is used to adjust the pH to 0.3 to 1.2;
[0042] During electroplating, an exhaust gas treatment device is set up, and the gas absorbed is SO2. The absorption method is one or more of activated carbon adsorption, UV photolysis, and spray tower. During electroplating, an exhaust gas collection device is set up, and the collected gas is O 2;
[0043] In the step 3), the purity of the electrolyte is determined by an inductively coupled plasma atomic emission spectrometer, wherein the main impurity elements and their contents (ppm) are: Co≤0.080, Mn≤0.020, Fe≤0.073, P≤0.077, and it does not contain toxic and harmful substances or elements such as As, Li, Hg, Cr, Cd, Pb, Br, PBB, PBDE, etc., and the electrolyte purity is ≥99.8%.
[0044] Example 2
[0045] The charged waste batteries are shredded, crushed, demagnetized, pulverized and sieved by continuous equipment to quickly obtain copper powder; 10.00 kg of copper powder is ultrasonically cleaned in ethanol and ultrapure water for 20 minutes respectively, filtered with a 30-mesh bag and dried.
[0046] Slowly add 5.00 kg of 9.79 M hydrogen peroxide into 15.00 kg of 15 M sulfuric acid, and heat with steam and stir until the copper powder is completely dissolved.
[0047] 17.55kg of high-grade pure sodium chloride was added to make the concentration of sodium chloride in the solution 20mM, and the pH was adjusted to 1.0 with sodium hydroxide to obtain the electrolyte raw material required for electrolytic copper foil. The purity of the electrolyte was determined by ICP-AES, and the main impurity elements and their contents (ppm) were: Co: 0.010, Mn: 0.020, Fe: 0.003, P: 0.007, and it did not contain toxic and harmful substances or elements such as As, Li, Hg, Cr, Cd, Pb, Br, PBB, PBDE, etc. The electrolyte purity was 99.91%. The gas was SO2, and activated carbon adsorption, UV photolysis and spray tower tail gas absorption devices were installed.
[0048] Example 3
[0049] The charged waste batteries are pre-treated by continuous equipment such as shredding, crushing, demagnetization, pulverization and screening to quickly obtain copper powder; 5 kg of copper powder is spray-washed with N-methylpyrrolidone (NMP) for 20 minutes, filtered with quartz sand and dried.
[0050] Slowly add 5 kg of concentrated sulfuric acid (concentration 18.4 M) into 1 kg of 9.79 M hydrogen peroxide, and heat with steam and stir until the copper powder is completely dissolved.
[0051] 11.21kg of high-grade pure sodium chloride was added, and the pH was adjusted to 1.2 with sodium hydroxide to obtain the electrolyte raw material required for electrolytic copper foil. The gas is SO2, and activated carbon adsorption, UV photolysis and spray tower tail gas absorption devices are installed. The purity of the electrolyte was determined by ICP-AES, and the main impurity elements and their contents (ppm) were: Al: 0.015, Mn: 0.010, Fe: 0.043, P: 0.017, and it does not contain toxic and harmful substances or elements such as Co, As, Li, Hg, Cr, Cd, Pb, Br, PBB, PBDE, etc. The purity of the electrolyte is: 99.88%.
[0052] Example 4
[0053] The charged waste batteries are pre-treated by continuous equipment such as shredding, crushing, demagnetization, pulverization and screening to quickly obtain copper powder; 40 kg of copper powder is sprayed and washed with acetone and ethanol for 20 minutes respectively, filtered with fiber balls and dried.
[0054] Slowly add 10 kg of 9.79 M hydrogen peroxide into 20 kg of 15 M sulfuric acid, and heat with steam and stir until the copper powder is completely dissolved.
[0055] 17.72kg of high-grade pure sodium chloride was added, and the pH was adjusted to 0.5 with sodium hydroxide to obtain the electrolyte raw material required for electrolytic copper foil. The gas is SO2, and activated carbon adsorption, UV photolysis and spray tower tail gas absorption devices are installed. The purity of the electrolyte was determined by ICP-AES, and the main impurity elements and their contents (ppm) were: Mn: 0.020, Fe: 0.018, P: 0.003, and it did not contain toxic and harmful substances or elements such as Co, As, Li, Hg, Cr, Cd, Pb, Br, PBB, PBDE, etc. The electrolyte purity was 99.98%.
[0056] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production, characterized in that: The following steps are involved: 1) The charged waste batteries are pre-treated by continuous equipment such as shredding, crushing, demagnetization, pulverization and screening to quickly obtain copper powder; 2) washing, filtering and drying the copper powder obtained in step 1) for later use; 3) preparing a mixed solution of sulfuric acid and hydrogen peroxide, slowly adding the copper powder treated in step 2) thereto under stirring and heating until the copper powder is completely dissolved, and adding sodium chloride to the solution and stirring to obtain an electrolyte; and determining the purity of the electrolyte; 4) When electroplating, adjust the pH with sodium hydroxide to obtain the electrolyte raw material required for electrolytic copper foil.
2. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: The charged waste batteries in 1) include one or more of various types of square, cylindrical and soft-pack lithium-ion batteries.
3. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: In the above 2), the cleaning agent used to clean the copper powder is at least one of dichloromethane, ethanol, N-methylpyrrolidone, dimethylacetamide, acetone, sulfuric acid and ultrapure water; the cleaning time is 20 to 30 minutes; and the cleaning method is one or both of ultrasonic vibration and spray washing at room temperature.
4. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 3, characterized in that: When the cleaning agent is sulfuric acid, the concentration of the sulfuric acid is ≤10 mol / L.
5. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: The filtering method in 2) is one or both of bag filtering and mechanical filtering, wherein the mechanical filtering is one or more of quartz sand filtering, multi-media filtering or fiber ball filtering, and the filtering mesh number is ≤30.
6. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: The concentration of sulfuric acid in the above 3) is ≥15 mol / L; the concentration of hydrogen peroxide is ≥9 mol / L, and the mixture is heated and stirred until the copper powder is completely dissolved. The mass ratio of hydrogen peroxide, sulfuric acid and copper powder is 1:2-5:2-5.
7. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: After the copper powder in 3) is dissolved, the concentration of the CuSO4 solution obtained is 10mmol / L-1mol / L; the concentration of the H2SO4 is 0.5-2mol / L, and the heating is steam heating at a temperature of 50-60°C.
8. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: In the above 3), sodium chloride is added to the dissolving solution in an amount of 1 mmol / L to 100 mmol / L; and in the above 4), sodium hydroxide is used to adjust the pH to 0.3 to 1.
2.
9. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: 4) During electroplating, an exhaust gas treatment device is set up, and the gas absorbed is SO2, and the absorption method is one or more of activated carbon adsorption, UV photolysis, and spray tower; during electroplating, an exhaust gas collection device is set up, and the collected gas is O2.
10. The method for industrially recycling waste batteries to prepare raw material electrolyte for copper foil production as claimed in claim 1, characterized in that: In the above 3), the purity of the electrolyte is determined by inductively coupled plasma atomic emission spectrometer, wherein the main impurity elements and their contents are Co≤0.080ppm, Mn≤0.020ppm, Fe≤0.073ppm, P≤0.077ppm, and no toxic or harmful substances are contained, and the purity of the electrolyte is ≥99.8%.