Quantitative analysis method for polysulfide in lithium-sulfur battery and application of quantitative analysis method

Directly measure the polysulfide concentration in the lithium sulfur battery electrolyte through an ultraviolet-visible spectrophotometer, combined with gradient dilution method and fitting curve, the accuracy and efficiency of polysulfide analysis in the prior art were solved, and the operation was simplified It also improves the cycle stability of the battery and the screening effect of adsorbent materials.

CN118883479APending Publication Date: 2024-11-01GUANGDONG UNIV OF TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411309237.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to accurately and quickly analyze the content of polysulfides in lithium-sulfur battery electrolytes, and the cumbersome operation can easily lead to experimental errors, affecting the cycle life of the battery and the efficiency of the Coulomb.

Method used

The polysulfide concentration in the electrolyte was directly measured by using an ultraviolet-visible spectrophotometer, and the polysulfide concentration was calculated by gradient dilution method and fitting standard curves, which simplified the operation and reduced air reaction interference. The content changes of Li2S6 dilution were used instead of polysulfide The adsorption properties of adsorbent materials are measured by the change of substance content.

Benefits of technology

Quantitative analysis of polysulfides with high accuracy and low energy consumption is achieved, the operation process is simplified, experimental errors are reduced, and the cycle stability performance of the battery and the screening efficiency of adsorbent materials are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a quantitative analysis method for polysulfide in a lithium-sulfur battery and application of the quantitative analysis method, and relates to the field of chemical detection analysis, and the quantitative analysis method comprises the following steps: adding a solvent into a diluted Li2S6 standard solution to obtain Li2S6 diluted standard solutions with different concentrations; respectively measuring the absorbance of the Li2S6 diluted standard solution by using an ultraviolet-visible spectrophotometer; carrying out linear fitting by taking the absorbance as a vertical coordinate and the concentration of the Li2S6 diluted standard solution as a horizontal coordinate to obtain a fitted standard curve equation; and diluting the electrolyte, measuring the absorbance of the diluted solution by using an ultraviolet-visible spectrophotometer, and obtaining the concentration of Li2S6 in the electrolyte to be measured by combining the fitting standard curve equation and the dilution ratio. The analysis method can be used for measuring the adsorption performance of the adsorption material on the polysulfide in the electrolyte, and has the advantages of low equipment requirement, convenience in measurement, simple process, low cost, good universality and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of chemical detection and analysis, and in particular to a quantitative analysis method for polysulfides in lithium-sulfur batteries and applications thereof. Background Art

[0002] Lithium-sulfur batteries use sulfur as the positive electrode reactant and lithium metal as the negative electrode. During discharge, the negative electrode reaction is that lithium loses electrons and becomes lithium ions, while the positive electrode reaction is that sulfur reacts with lithium ions and electrons to form sulfide. Lithium-sulfur batteries have a high theoretical specific capacity (1675 mAh g -1 ) and theoretical energy density (2600 Wh·kg -1 ), green and environmentally friendly, and low-cost, it is at the forefront of electrochemical energy storage devices and is the most promising next-generation energy system. However, during the charge and discharge process of lithium-sulfur batteries, the sulfur electrode will generate a series of high-order lithium polysulfides such as Li2S8, Li2S6, Li2S4, etc. during discharge. These lithium polysulfides are highly soluble in the electrolyte and, driven by the concentration difference, cross the diaphragm to reach the lithium negative electrode, reacting with the lithium negative electrode, reducing the active sulfur content in the electrolyte, and ultimately causing irreversible loss of effective substances in the battery and attenuation of battery life, thereby reducing the battery's cycle life and coulombic efficiency.

[0003] In order to fundamentally solve the problem of polysulfide crossing the diaphragm during battery charging and discharging and improve the battery's cycle stability, it is essential to study the working principles and complex operating mechanisms of lithium-sulfur batteries. The content of polysulfide in the electrolyte and how to accurately and quickly analyze the content of polysulfide in the electrolyte are also one of the problems that need to be overcome urgently.

[0004] Patent No. CN112034089A discloses a method for quantitatively analyzing sulfur and polysulfides in lithium-sulfur batteries. This analysis method uses ether solvents and non-polar organic solvents to immerse and dissolve the active material S8, the intermediate lithium polysulfide, and the final product Li2S2 / LiS2 in the lithium-sulfur battery components. This method achieves a stepwise dissolution and separation of soluble lithium polysulfide, insoluble S8, and the final product Li2S2 / LiS2. An oxidant and a vulcanization accelerator are then used to convert the dissolved lithium polysulfide into a Li2S precipitate. The total sulfur content of the polysulfide is then determined by weighing the Li2S precipitate. This invention proposes a direct measurement of polysulfide concentration in the lithium-sulfur battery electrolyte using a UV-visible spectrophotometer, eliminating the need for a conversion and precipitation step. Moreover, since lithium polysulfide reacts with air, the experimental process of patent number CN112034089A requires potentiometric titration, solvent evaporation and other operations in a high-purity argon glove box to eliminate air interference. The operation is relatively cumbersome and inconvenient to operate in the glove box, which can easily cause large experimental errors. In addition, this method cannot efficiently and quickly analyze the content of polysulfide in the electrolyte. Summary of the Invention

[0005] The present invention aims to provide a method for quantitative analysis of polysulfides in lithium-sulfur batteries, which uses an ultraviolet-visible spectrophotometer to measure the polysulfide concentration in the electrolyte, has high accuracy and is easy to operate.

[0006] Another object of the present invention is to provide an application of a method for quantitative analysis of polysulfides in lithium-sulfur batteries, in which the change in the content of Li2S6 dilution is used instead of the change in the polysulfide content to reflect the adsorption performance of the adsorption material on polysulfides in the electrolyte, thereby simplifying the detection method and avoiding the experimental error caused by the deliquescence of sulfides in the air.

[0007] The present invention solves the technical problem by adopting the following technical solutions.

[0008] In one aspect, an embodiment of the present invention provides a method for quantitatively analyzing polysulfides in a lithium-sulfur battery, comprising the following steps: S1: Add solvent to the Li2S6 standard solution of known concentration and dilute it into solutions of different concentrations according to the gradient to obtain Li2S6 diluted standard solutions of different concentrations; S2: Using a UV-visible spectrophotometer, measure the absorbance of the different concentrations of the Li2S6 diluted standard solutions prepared in step S1, wherein the scanning band is 350-600 nm and the cuvette optical path length is 10 nm; S3: Using the absorbance measured in step S2 as the ordinate and the concentration of the diluted Li2S6 standard solution in step S1 as the abscissa, perform linear fitting to obtain the fitted standard curve equation; S4: dilute the electrolyte to be tested with the solvent to a concentration within the range of step S1, measure the absorbance of the diluted solution using a UV-visible spectrophotometer, and obtain the concentration after dilution by combining the fitting standard curve equation of step S3. Then, calculate the Li2S6 concentration in the electrolyte to be tested by the dilution multiple.

[0009] In some embodiments of the present invention, in step S1, the solvent is a mixture of one or more of N,N-dimethylpyrrolidone, 1,3-dioxolane, ethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol dimethyl ether, and tetrahydrofuran. However, the solvent should not be limited to the aforementioned solvents. Any solvent that has solubility for polysulfides and lacks UV-visible light absorption at a specific wavelength is suitable, such as linear and cyclic ether solvents. When the solvent is a mixture of 1,3-dioxolane and ethylene glycol dimethyl ether, the volume ratio of the two is 1,3-dioxolane:ethylene glycol dimethyl ether = 1:1. For lithium-sulfur batteries, the solvent in their electrolyte is often a mixture of 1,3-dioxolane and ethylene glycol dimethyl ether. In the present invention, using this solvent to dilute the Li2S6 standard solution does not introduce other impurities, thus preventing the impact of other impurities on absorbance. Furthermore, the solvent is the same as that in actual electrolytes, making the test results more consistent with actual lithium-sulfur battery electrolytes.

[0010] In some embodiments of the present invention, in step S2, the absorbance at the characteristic absorption wavelength of Li2S6, 420 nm, is selected as the absorbance of the standard solution. In some embodiments of the present invention, in step S1, the step of gradient dilution is: taking 10 uL of 0.5 mol / L Li2S6 standard solution, adding 900 uL of the solvent, and shaking to obtain a primary dilution solution; Take 120uL, 160uL, 200uL, 240uL of the first dilution respectively, and then add 3880uL, 3840uL, 3800uL, 3760uL of the solvent respectively, shake well to obtain secondary dilutions of different concentrations, which are the Li2S6 diluted standard solutions. In the present invention, a low concentration dilution is selected as the test sample, and the linear correlation of the obtained fitting standard curve equation is good and the experimental error is small. The experiment found that when the concentration of the sample is high, the measured absorbance of the sulfide in the sample is low, and the linear correlation of the obtained fitting standard curve equation is poor, the error is large, and it cannot be used as a fitting equation.

[0011] In some embodiments of the present invention, in step S4, the supernatant is diluted using a two-fold dilution method, which facilitates subsequent calculation of the concentration of the original solution.

[0012] In some embodiments of the present invention, in step S3, the fitting standard curve is y=0.2356x-0.02646, and the correlation coefficient r 2 =0.99757.

[0013] On the other hand, an embodiment of the present invention provides an application of a quantitative analysis method for polysulfides in a lithium-sulfur battery, which is used to measure the adsorption performance of an adsorption material on polysulfides in an electrolyte, comprising the following steps: S11: Prepare a Li2S6 solution of known concentration and place it in a container to obtain a stock solution; under an inert atmosphere, add an adsorption material to the stock solution. After static adsorption for 12 hours, take the supernatant and dilute it twice to the concentration range of step S1; S12: Use a UV-visible spectrophotometer to measure the absorbance of the diluted supernatant in step S11, and combine it with the fitting standard curve equation in step S3 to obtain the concentration of the diluted supernatant. Combined with the two-fold dilution factor, after calculation, the concentration of the supernatant and the adsorption rate of the adsorption material are obtained respectively.

[0014] In some embodiments of the present invention, in step S12, the adsorption material is a mixture of one or more of a porous carbon material, an organic-metal framework material, and mesoporous silica. In the present invention, any material capable of adsorbing lithium polysulfide is applicable, such as carbon-based materials such as carbon fibers, graphene, and carbon nanotubes, and composite materials doped with heteroatoms or metal atoms; zeolites, metal-organic frameworks (MOFs), covalent organic frameworks (COFs), and other porous materials.

[0015] In some embodiments of the present invention, in step S11, the inert atmosphere is argon, and the water and oxygen content is less than 1 ppm. Preferably, all the steps in the present invention are completed in an inert atmosphere to reduce the deliquescence of polysulfides and thus reduce experimental errors.

[0016] Compared with the prior art, the embodiments of the present invention have at least the following advantages or beneficial effects: The detection method provided by the present invention has the advantages of low energy consumption and simple operation. The method has the advantages of low equipment requirements, convenient measurement, simple process, low cost, and good versatility. The method is used to test the adsorption of adsorption materials in the laboratory, which is simple to operate and highly reliable. Since lithium polysulfides such as Li2S8, Li2S6, and Li2S4 are present in actual electrolytes, when testing physical adsorbents, sulfides of different valence states will be adsorbed by the adsorbents. Then, Li2S6 is used instead of polysulfides, which can accurately reflect the changes in the sulfide content in the electrolyte before and after adsorption, and thus physical adsorption materials with good adsorption properties can be screened out. DETAILED DESCRIPTION

[0017] To make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are described clearly and completely below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer are used. Where the manufacturer of the reagents or instruments is not specified, all are conventional products that can be purchased commercially.

[0018] It should be noted that, in the absence of conflict, the embodiments and features of the embodiments of the present invention can be combined with each other. The present invention will be described in detail below with reference to specific embodiments.

[0019] The features and performance of the present invention are further described in detail below with reference to the embodiments.

[0020] Example 1 Follow the steps below to measure the Li2S6 content in the electrolyte: S1: Take 10uL of 0.5mol / L Li2S6 standard solution, add 900uL of solvent, shake well, and obtain the first dilution solution, whose concentration level is 5 mmol / L Li2S6 diluted solution; Take 120uL, 160uL, 200uL, and 240uL of the first dilution solution, respectively, and then add 3880uL, 3840uL, 3800uL, and 3760uL of the solvent, respectively. Shake thoroughly to obtain 0.15 mmol / L, 0.2 mmol / L, 0.25mmol / L, and 0.3 mmol / L Li2S6 secondary dilution solutions, respectively, which are the Li2S6 diluted standard solutions. The solvent is a mixture of 3-dioxolane and ethylene glycol dimethyl ether, wherein the volume ratio of the two is 1,3-dioxolane:ethylene glycol dimethyl ether = 1:1.

[0021] S2: Use a UV-visible spectrophotometer to measure the absorbance of the different concentrations of the Li2S6 diluted standard solutions prepared in step S1, wherein the scanning band is 350-600nm and the cuvette optical path is 10nm; take the Li2S6 characteristic absorption wavelength of 420nm to record the absorbance of the solution.

[0022] S3: With the absorbance measured in step S2 as the ordinate and the concentration of the diluted Li2S6 standard solution in step S1 as the abscissa, perform linear fitting to obtain the equation of the fitted standard curve; the fitted standard curve is y=0.2356x-0.02646, and the correlation coefficient r 2 =0.99757.

[0023] S4: Dilute the 2 mmol / L Li2S6 electrolyte to be tested with the solvent to a concentration within the concentration range of step S1, measure the absorbance of the diluted solution using a UV-visible spectrophotometer, and obtain the diluted concentration by combining the fitting standard curve equation of step S3. Then, calculate the Li2S6 concentration in the electrolyte to be tested by the dilution multiple.

[0024] In this embodiment, the Li2S6 standard solution was purchased from Suzhou Duoduo Chemical Technology Co., Ltd.; trade name: lithium-sulfur electrolyte (LS-243), batch number: E2172.50.010, concentration: 0.5M Li2S6DME:DOL = 1:1 Vol%; purity: industrial grade, its solute is Li2S6, and the solvent is DOL and DME (1,3-dioxolane and ethylene glycol dimethyl ether). The solvent used for dilution was purchased from Suzhou Duoduo Chemical Technology Co., Ltd.; trade name: lithium-sulfur electrolyte (LS-013), batch number: S20231109048, concentration: DME:DOL = 1:1 Vol%; purity: industrial grade, which contains only DME and DOL and does not contain Li2S6.

[0025] Example 2 Test the performance of Super P (porous carbon material) in adsorbing lithium polysulfide.

[0026] (1) Lithium polysulfide adsorption experiment: Mix 25 μL of 0.5 mol / L Li2S6 standard solution in 6225 μL of solvent (i.e., DOL and DME solution) and shake well to dilute the solution to a Li2S6 concentration of 2 mmol / L.

[0027] (2) In a glove box filled with argon and with a water and oxygen content of less than 1 ppm, 50 mg of porous carbon material sample was added to 6 ml of 2 mmol / L Li2S6 solution, shaken well, and allowed to stand for adsorption for 12 hours.

[0028] (3) The supernatant liquid in the above-mentioned step (2) was extracted and serially diluted by the two-fold dilution method. Specifically, 2 ml of the supernatant liquid to be tested was added with 2 ml of the above-mentioned solvent (DOL and DME solution) of equal volume to obtain a 1 / 2 dilution solution. Then 2 ml of the above-mentioned 1 / 2 dilution solution was taken and added with 2 ml of the above-mentioned solvent (DOL and DME solution) of equal volume to obtain a 1 / 4 dilution solution. The dilution was repeated to obtain a series of dilution solutions with concentrations gradually diluted to 1 / 2, 1 / 4, 1 / 8, 1 / 16, etc. of the original supernatant liquid, until the concentration reached the detectable concentration (0.15-0.3 mmol / L) in step S1 of Example 1.

[0029] (4) The absorbance of the diluted test solution is measured using a UV-visible spectrophotometer. The concentration of lithium polysulfide in the diluted supernatant is obtained by combining the standard curve y = 0.2356x - 0.02646. The concentration of lithium polysulfide in the original supernatant can then be calculated by combining the dilution factor. By comparing the concentrations of lithium polysulfide in the solution before and after adsorption, the amount of lithium polysulfide adsorbed by the porous carbon material in the electrolyte can be determined.

[0030] In this embodiment, the porous carbon material used was purchased from Taiyuan Lizhiyuancunfa Co., Ltd., model: SUPER P.LI, trade name: Carbon Black.

[0031] Example 3 Test the performance of Co-MOF (cobalt-containing organic-metal framework material) in adsorbing lithium polysulfide.

[0032] (1) Lithium polysulfide adsorption experiment: Mix 25 μL of 0.5 mol / L Li2S6 standard solution in 6225 μL of solvent (i.e., DOL and DME solution) and shake well to dilute the solution to a Li2S6 concentration of 2 mmol / L.

[0033] (2) In a glove box filled with argon and with a water and oxygen content of less than 1 ppm, 50 mg of Co-MOF material sample was added to 6 ml of 2 mmol / L Li2S6 solution, shaken well, and allowed to stand for adsorption for 12 hours.

[0034] (3) The supernatant liquid in the above-mentioned step (2) was extracted and serially diluted by the two-fold dilution method. Specifically, 2 ml of the supernatant liquid to be tested was added with 2 ml of the above-mentioned solvent (DOL and DME solution) of equal volume to obtain a 1 / 2 dilution solution. Then 2 ml of the above-mentioned 1 / 2 dilution solution was taken and added with 2 ml of the above-mentioned solvent (DOL and DME solution) of equal volume to obtain a 1 / 4 dilution solution. The dilution was repeated to obtain a series of dilution solutions with concentrations gradually diluted to 1 / 2, 1 / 4, 1 / 8, 1 / 16, etc. of the original supernatant liquid, until the concentration reached the detectable concentration (0.15-0.3 mmol / L) in step S1 of Example 1.

[0035] (4) The absorbance of the diluted test solution was measured using a UV-visible spectrophotometer. The concentration of lithium polysulfide in the diluted supernatant was calculated by combining the standard curve y = 0.2356x - 0.02646. The concentration of lithium polysulfide in the original supernatant was then calculated by combining the dilution factor. By comparing the concentrations of lithium polysulfide in the solution before and after adsorption, the amount of lithium polysulfide adsorbed by the MOF material in the electrolyte can be determined.

[0036] The Co-MOF adsorption material used in this example was synthesized in the laboratory by a hydrothermal method, mixing sodium hydroxide, 4,4'-bipyridine, and cobalt nitrate and heating them. 4,4'-bipyridine was purchased from Shanghai Aladdin Biochemical Technology Co., Ltd. under the brand name Aladdin and was of analytical standard anhydrous grade.

[0037] Example 4 Test the performance of HMS (porous silica material) in adsorbing lithium polysulfide.

[0038] (1) Lithium polysulfide adsorption experiment: Mix 25 μL of 0.5 mol / L Li2S6 standard solution in 6225 μL of solvent (i.e., DOL and DME solution) and shake well to dilute the solution to a Li2S6 concentration of 2 mmol / L.

[0039] (2) In a glove box filled with argon and with a water and oxygen content of less than 1 ppm, add 50 mg of HMS material sample to 6 ml of 2 mmol / L Li2S6 solution, shake well, and let it stand for adsorption for 12 hours.

[0040] (3) The supernatant liquid in the above-mentioned step (2) was extracted and serially diluted by the two-fold dilution method. Specifically, 2 ml of the supernatant liquid to be tested was added with 2 ml of the above-mentioned solvent (DOL and DME solution) of equal volume to obtain a 1 / 2 dilution solution. Then 2 ml of the above-mentioned 1 / 2 dilution solution was taken and added with 2 ml of the above-mentioned solvent (DOL and DME solution) of equal volume to obtain a 1 / 4 dilution solution. The dilution was repeated to obtain a series of dilution solutions with concentrations gradually diluted to 1 / 2, 1 / 4, 1 / 8, 1 / 16, etc. of the original supernatant liquid, until the concentration reached the detectable concentration (0.15-0.3 mmol / L) in step S1 of Example 1.

[0041] (4) The absorbance of the diluted test solution is measured using a UV-visible spectrophotometer. The concentration of lithium polysulfide in the diluted supernatant is obtained by combining the standard curve y = 0.2356x - 0.02646. The concentration of lithium polysulfide in the original supernatant can then be calculated by combining the dilution factor. By comparing the concentrations of lithium polysulfide in the solution before and after adsorption, the amount of lithium polysulfide adsorbed by the silica material in the electrolyte can be determined.

[0042] The porous silica adsorption material used in this embodiment was purchased from Guangzhou Rentai Technology Co., Ltd., manufactured by McLean, with the trade name of nano-silica, purity / concentration: 99% metals basis, 30 nm.

[0043] Experimental example The absorbance measured in Examples 2-4 was combined with the dilution factor of the supernatant to calculate the concentration of the supernatant. The results are shown in Table 1.

[0044] Table 1 Adsorption properties of adsorption materials of Examples 2-4

[0045] In Table 1, absorbance refers to the absorbance of the diluted supernatant measured using a UV-visible spectrophotometer. In Examples 3 and 4, where the supernatant was not diluted, this refers to the absorbance of the supernatant. Fitted concentration refers to the result obtained by fitting the measured absorbance to the standard curve with y = 0.2356x - 0.02646. Original concentration refers to the concentration of the supernatant before dilution, calculated based on the dilution factor. The "2 mmol / L Li2S6 unadsorbed solution" is the result measured in step S4 of Example 1.

[0046] As can be seen in Table 1, cobalt-containing MOF materials have the best adsorption effect on polysulfides, followed by silica HMS materials. Super P porous carbon materials, commonly used as battery conductive agents, have the worst adsorption effect on polysulfides, indicating that without additional strategies to limit the shuttling of lithium polysulfides, the electrochemical performance of lithium-sulfur batteries will quickly deteriorate.

[0047] The analytical method of the present invention can accurately measure the adsorption concentration of lithium polysulfide in the electrolyte, thereby accurately evaluating the adsorption capacity of different materials for lithium polysulfide. Furthermore, the analytical method uses a UV-visible spectrophotometer for measurement, and its test results are accurate and rapid.

[0048] The embodiments described above are some, but not all, of the embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention as claimed, but rather merely represents selected embodiments of the present invention. All other embodiments derived by persons of ordinary skill in the art based on the embodiments of the present invention without inventive effort are also within the scope of protection of the present invention.

Claims

1. A quantitative analysis method for polysulfide in lithium-sulfur battery, characterized in that: The following steps are included: S1: Add solvent to a Li2S6 standard solution of known concentration and dilute it into solutions of different concentrations according to a gradient to obtain Li2S6 diluted standard solutions of different concentrations; S2: using a UV-visible spectrophotometer to measure the absorbance of the different concentrations of the Li2S6 diluted standard solutions prepared in step S1, wherein the scanning band is 350-600nm and the cuvette optical path is 10nm; S3: With the absorbance measured in step S2 as the ordinate and the concentration of the diluted Li2S6 standard solution in step S1 as the abscissa, linear fitting is performed to obtain a fitting standard curve equation; S4: dilute the electrolyte to be tested with the solvent to a concentration range of step S1, measure the absorbance of the diluted solution using a UV-visible spectrophotometer, and obtain the concentration after dilution by combining the fitting standard curve equation of step S3, and then calculate the Li2S6 concentration in the electrolyte to be tested by the dilution multiple.

2. The quantitative analysis method of polysulfide in lithium-sulfur battery according to claim 1, characterized in that: In the step S1, the solvent is a mixture of one or more of N,N-dimethylpyrrolidone, 1,3-dioxolane, ethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol dimethyl ether and tetrahydrofuran.

3. The quantitative analysis method of polysulfide in lithium-sulfur battery according to claim 1, characterized in that: In step S2, the absorbance at the characteristic absorption wavelength of Li2S6, 420 nm, is selected as the absorbance of the standard solution.

4. The quantitative analysis method of polysulfide in lithium-sulfur battery according to claim 1, characterized in that: In step S1, the step of gradient dilution is: take 10uL of 0.5mol / L Li2S6 standard solution, add 900uL of the solvent, shake well, and obtain a primary dilution solution; Take 120uL, 160uL, 200uL, and 240uL of the primary dilution solution respectively, and then add 3880uL, 3840uL, 3800uL, and 3760uL of the solvent respectively, shake well to obtain secondary dilution solutions of different concentrations, which are the Li2S6 dilution standard solutions.

5. The quantitative analysis method of polysulfide in lithium-sulfur battery according to claim 1, characterized in that: In the step S4, the electrolyte to be tested is diluted by a two-fold dilution method.

6. The quantitative analysis method of polysulfide in lithium-sulfur battery according to claim 1, characterized in that: In step S3, the fitting standard curve is y=0.2356x-0.02646, and the correlation coefficient r 2 =0.99757.

7. An application of the method for quantitative analysis of polysulfide in a lithium-sulfur battery as claimed in any one of claims 1 to 6, wherein the method is used to measure the adsorption performance of an adsorbent material on polysulfide in an electrolyte, comprising the following steps: S11: Prepare a Li2S6 solution of known concentration and place it in a container to obtain a raw solution; under an inert atmosphere, add an adsorption material to the raw solution, and after static adsorption for 12 hours, take the supernatant and dilute it twice to the concentration range of step S1; S12: Use a UV-visible spectrophotometer to measure the absorbance of the diluted supernatant in step S11, and combine it with the fitting standard curve equation of step S3 to obtain the concentration of the diluted supernatant. Combined with the dilution multiple and the original solution concentration, the concentration of the supernatant and the adsorption rate of the adsorption material are calculated.

8. Application of the method for quantitative analysis of polysulfides in lithium-sulfur batteries according to claim 7, characterized in that: In the step S11, the adsorption material is a mixture of one or more of porous carbon materials, organic-metal framework materials, covalent organic framework materials, mesoporous silica, carbon fibers, graphene, and carbon nanotubes.

9. Application of the quantitative analysis method for polysulfide in lithium-sulfur battery according to claim 7, characterized in that: In the step S11, the inert atmosphere is argon gas, and the water oxygen content is less than 1 ppm.

Citation Information

Patent Citations

  • Quantitative analysis method for sulfur and polysulfide in lithium-sulfur battery

    CN112034089A