Application of solid additive in organic solar cell and cell preparation method

By introducing 1,4-diphenoxybenzene as a solid additive in organic solar cells, the aggregation characteristics of non-fullerene receptors are regulated, and the problems of additive toxicity and single structure in the prior art are solved, which significantly improves the battery Photoelectric conversion efficiency and stability, suitable for a variety of polymer solar cell systems.

CN118890906APending Publication Date: 2024-11-01HANGZHOU INST FOR ADVANCED STUDY UCAS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410912688.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The volatile solid additives used in existing organic solar cells mostly contain halogen, are toxic, have a single structure, and are not clear in working mechanism of non-planar structures, making it difficult to effectively regulate battery performance.

Method used

Using 1,4-diphenoxybenzene as a solid additive for organic solar cells, the additive is introduced into the active layer to regulate the aggregation and accumulation characteristics of the non-fullerene receptors and improve the loading. Flowton physical process, enhancing exciton dissociation and charge transport.

Benefits of technology

It significantly improves the photoelectric conversion efficiency of the battery, improves the short-circuit current density and filling factor, and has good universality, and is suitable for different polymer solar cell systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118890906A_ABST
    Figure CN118890906A_ABST
Patent Text Reader

Abstract

According to the application of the solid additive in the organic solar cell and the preparation method of the cell, the solid additive is 1, 4-diphenoxy benzene and serves as an additive of the organic solar cell adopting a non-fullerene receptor; according to the preparation method of the organic solar cell, the organic solar cell is a positive device, the structure of the device sequentially comprises an ITO electrode, an anode interface layer, an active layer, a cathode interface layer and a metal electrode from bottom to top, non-fullerene serves as an acceptor material of the active layer, meanwhile, 1, 4-diphenoxy benzene serves as a solid additive, and the metal electrode serves as a cathode interface layer of the active layer. PEDOT: PSS is used as an anode interface layer, PDIN is used as a cathode interface layer, and silver is used as a metal electrode. According to the application of the solid additive in the organic solar cell and the preparation method of the organic solar cell, the short-circuit current density and the filling factor of a cell device are greatly improved, and then high photoelectric conversion efficiency is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic solar cells, and specifically relates to an application of a solid additive in an organic solar cell and a method for preparing the cell. Background Art

[0002] Organic solar cells (OSCs) are thin-film cells with organic materials as light-absorbing layers. They have the unique advantages of low cost, light weight, translucency and flexibility, and are expected to be widely used in the construction of integrated, flexible wearable devices. With the development of new structural donor and acceptor materials, interface engineering and device structure optimization, the photoelectric conversion efficiency (PCE) of a single cell has exceeded 19%, and the PCE of a stacked cell has exceeded 20%.

[0003] The morphology of the active layer can effectively affect the carrier transport process inside the battery, thereby directly determining the photoelectric performance of the battery. Therefore, researchers have developed a variety of morphology control strategies, such as molecular structure optimization, thermal annealing, solvent annealing, layer-by-layer deposition and additive strategies. Among the many methods, additives are an effective and simple morphology control strategy. Unlike traditional high-boiling point liquid additives, volatile solid additives can form strong interactions with donor and acceptor molecules due to their unique molecular characteristics, which can greatly improve the efficiency and stability of the device. However, the volatile solid additives reported so far mostly contain halogens (toxic); and have good planarity, while non-planar volatile solid additives may provide a larger space for molecules, which is conducive to the self-assembly of active layer molecules. For example: Although the research group of Professor Tan Zhan'ao of Beijing University of Chemical Technology reported that the three-dimensional solid additive 4-fluoro-N, N-diphenylaniline (FPA) can adjust the morphology of the active layer and improve battery performance, the additive contains halogens, and halogen-containing organic matter is toxic.

[0004] Therefore, how to solve the problems of single additive structure, high halogen content and toxic planar structure, and unclear working mechanism of additives, and provide a new type of green non-halogen, non-planar structure additive is a technical problem that needs to be solved urgently by technical personnel in this field. Summary of the invention

[0005] The first object of the present invention is to provide an application of a solid additive in an organic solar cell in view of the problems in the prior art.

[0006] To this end, the above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0007] An application of a solid additive in an organic solar cell, characterized in that the solid additive is 1,4-diphenoxybenzene, which is used as an additive for an organic solar cell using a non-fullerene acceptor.

[0008] A second object of the present invention is to provide a method for preparing an organic solar cell in view of the problems in the prior art.

[0009] To this end, the above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0010] The method for preparing an organic solar cell is characterized in that: the organic solar cell is an upright device, and the device structure is ITO electrode / anode interface layer / active layer / cathode interface layer / metal electrode from bottom to top, wherein the active layer uses non-fullerene as an acceptor material, 1,4-diphenoxybenzene as a solid additive, PEDOT:PSS as an anode interface layer, PDIN as a cathode interface layer, and silver as a metal electrode.

[0011] While adopting the above technical solutions, the present invention may also adopt or combine the following technical solutions:

[0012] As a preferred technical solution of the present invention: the active layer uses polymer PM6 as a donor and non-fullerene Y6 as an acceptor. In the active layer, the donor PM6 and the acceptor Y6 are dissolved in the solvent chloroform at a mass ratio of 1:1.2, and the concentration is 17.8 mg mL -1 .

[0013] As a preferred technical solution of the present invention: 1,4-diphenoxybenzene is dissolved in chloroform at a concentration of 2.5-7.5 mg mL -1 , preferably 5 mg mL -1 .

[0014] As a preferred technical solution of the present invention: comprising the following steps:

[0015] S1, cleaning of ITO glass: placing the ITO glass substrate in deionized water, cleaning it with detergent, then placing it in an ultrasonic cleaner, and ultrasonically cleaning it with deionized water, acetone, and isopropanol for 20 minutes in sequence, then drying the cleaned ITO glass with nitrogen, placing it in a plasma cleaner, and cleaning the surface with oxygen plasma for 3 minutes to remove residual organic matter on the surface, and then taking it out for use;

[0016] S2, preparation of PEDOT:PSS hole transport layer: filter PEDOT:PSS for later use, use a pipette to take 50 μL of PEDOT:PSS solution and drop it on the cleaned ITO glass surface, so that the PEDOT:PSS solution covers the entire ITO glass, then spin-coat at 4000 rpm for 30 seconds, and finally place it on a constant temperature hot stage at 130°C for annealing for 20 minutes in an atmospheric environment to form a thin film;

[0017] S3, active layer preparation process: The donor PM6 and the acceptor Y6 were dissolved in the solvent chloroform at a mass ratio of 1:1.2, with a concentration of 17.8 mg mL-1 ; At the same time, the system adjusts the concentration of solid additives to 2.5-7.5mg mL -1 ; Take 10 μL of the solution in the glove box, drop it on the surface of the PEDOT:PSS film, and make it completely covered, then spin-coat it at a speed of 3000 rpm for 30 seconds, and after spin-coating, place it on a hot plate at 80°C for constant temperature annealing for 10 minutes to form an organic active layer film;

[0018] S4, preparation of cathode interface layer PDIN: use a pipette to take 30 μL of PDIN methanol solution and drop it on the surface of the active layer film to make it completely covered, and then spin-coat it at a speed of 5000 rpm for 30 seconds;

[0019] S5, silver electrode evaporation: put the prepared sample into the chamber of the thermal evaporation coating machine and wait until the vacuum degree reaches 2×10 -4 Pa, the silver electrode was evaporated and the film deposition rate was The thickness is controlled at 100 nm.

[0020] As a preferred technical solution of the present invention: in step S3, 1,4-diphenoxybenzene is removed by annealing during heat treatment at 80°C or above.

[0021] As a preferred technical solution of the present invention: a polymer solar cell PM6:IT-4F system is prepared, with PM6 as the donor and non-fullerene IT-4F as the acceptor, the mass ratio of donor PM6 to acceptor IT-4F is 1:1.2, and the total concentration is 17.8 mg mL -1, , solid additives at 5 mg mL -1 The concentration was dissolved in chloroform.

[0022] As a preferred technical solution of the present invention: a polymer solar cell D18-Cl:N3 system is prepared, with D18-Cl as the donor and non-fullerene N3, the mass ratio of donor D18-Cl and acceptor N3 is 1:1.4, and the solution concentration is 16 mg mL -1 Dissolve in chloroform, solid additive at 5 mg mL -1 The concentration was dissolved in chloroform.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The invention discloses an application of a solid additive in an organic solar cell and a method for preparing the cell, and provides a green non-halogen, non-planar volatile solid additive, which is introduced into a polymer solar cell. The morphology of the cell active layer is effectively regulated by the introduced novel non-halogen, non-planar volatile solid additive. The 1,4-diphenoxybenzene can significantly improve the aggregation and stacking characteristics of non-fullerene receptors. After adding 1,4-diphenoxybenzene, the arrangement of non-fullerene receptor molecules in the active layer is more compact and orderly, thereby improving the internal carrier physical process, enhancing the exciton dissociation, Improved charge transfer and reduced charge recombination, thereby greatly improving the short-circuit current density and fill factor of the battery device, and then obtaining a higher photoelectric conversion efficiency; in the present invention, by systematically optimizing the additive concentration, annealing temperature and annealing time, the battery efficiency of the PM6:Y6 system was ultimately increased from 15.54% to 16.97%, and can be applied to other polymer solar cell systems D18-Cl:N3 and PM6:IT-4F. The results show that the photoelectric conversion efficiency of such polymer solar cells is greatly improved, that is, the solid additive has good universality. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The device structure used in the present invention and the molecular structure formula of the donor PM6, the acceptor Y6 and the additive 1,4-diphenoxybenzene;

[0026] Figure 2 The structural formulas of the polymer donor D18-Cl, the non-fullerene acceptor IT-4F and N3 used in the present invention;

[0027] Figure 3 (a) JV curve and (b) EQE curve of PM6:Y6 battery device before and after the solid additive treatment is introduced in the present invention;

[0028] Figure 4 JV curves of (a) PM6:IT-4F and (b) D18-Cl:N3 battery devices before and after the solid additive treatment is introduced in the present invention;

[0029] Figure 5 The molecular structure of the additive (1,4-diphenoxybenzene) optimized for density functional theory (DFT) calculations;

[0030] Figure 6 This is the TGA diagram of the additive 1,4-diphenoxybenzene of the present invention;

[0031] Figure 7 The pictures are before and after thermal annealing of the thin film spin-coated with the additive solution of the present invention on a silicon wafer;

[0032] Figure 8Fourier transform infrared spectra of the solid additive of the present invention, PM6:Y6, PM6:Y6 (additive) untreated and PM6:Y6 (additive) annealed films;

[0033] Fig. 9 (a) Height map of PM6 and Y6 pure films observed by atomic force microscopy (AFM) before and after the introduction of the solid additive of the present invention; and (b) height map and phase diagram of PM6:Y6 blended film. DETAILED DESCRIPTION

[0034] The present invention will be described in further detail with reference to the accompanying drawings and specific embodiments.

[0035] Example 1

[0036] Experimental materials: donor PM6, acceptor Y6, solid additive (1,4-diphenoxybenzene), ITO conductive glass, PEDOT:PSS, PDIN, chloroform, methanol, Ag particles, etc.

[0037] Experimental method: donor PM6 and non-fullerene acceptor Y6 were mixed at a mass ratio of 1:1.2 and a total concentration of 17.8 mg mL -1 1,4-Diphenoxybenzene was dissolved in chloroform at different concentrations (0, 2.5, 5, 7.5 and 10 mg mL -1 ) was dissolved in chloroform; a battery device was prepared according to the above device preparation process. Then the battery device was placed in standard sunlight AM 1.5G (100mWcm -2 ) conditions, and tested its JV curve, and tested the external quantum efficiency EQE of the prepared device, and studied the influence of different concentrations of additives on the photovoltaic performance of the battery device.

[0038] Experimental results: As shown in Table 1, the concentration of 1,4-diphenoxybenzene increased from 0 to 10 mg mL -1 The photoelectric conversion efficiency of the battery shows a trend of first increasing and then decreasing; the JV curves of various battery devices are as follows Figure 3 (a) shows that the short-circuit current density of the control battery device without additive is 25.32 mA cm -2 , the open circuit voltage is 0.886 V, the fill factor is 69.8%, and the photoelectric conversion efficiency is only 15.54%; when the additive concentration is 5 mg mL -1 When the photoelectric conversion efficiency of the battery is as high as 16.97%, the corresponding short-circuit current density is 26.84 mA cm -2 , the open circuit voltage is 0.838V, and the fill factor is 75.4%. The EQE curves of the battery device before and after the introduction of the additive are shown in Figure 3(b) shows that the corresponding integrated current densities of EQE are 24.26 and 25.86 mA cm -2 , which is consistent with the results measured by the JV curve of the battery device, with an error of less than 5%.

[0039] Table 1 Photoelectric performance parameters of battery devices corresponding to different concentrations of additives

[0040]

[0041] Embodiment 2:

[0042] Experimental materials: polymer donor PM6, non-fullerene acceptor IT-4F, polymer donor D18-Cl, non-fullerene acceptor N3, solid additive (1,4-diphenoxybenzene), ITO conductive glass, PEDOT:PSS, PDIN, chloroform, methanol, Ag particles, etc.

[0043] Experimental method: Pre-mix the solid additive at 5 mg mL -1 In the PM6:IT-4F system, the mass ratio of donor PM6 to acceptor IT-4F was 1:1.2, and the total concentration was 17.8 mg mL -1 Dissolved in chloroform. In the D18-Cl:N3 system, the mass ratio of donor D18-Cl and acceptor N3 is 1:1.4, and the solution concentration is 16 mg mL -1 Dissolve in chloroform. Then prepare the battery device according to the above device preparation process. Then place the battery device under standard sunlight AM 1.5G (100mW cm -2 ) conditions to test its JV curve and study the influence of additives on the photovoltaic performance of battery devices in different systems.

[0044] Experimental results: As shown in Table 2, in the PM6:IT-4F system, when no additives were introduced, the photoelectric conversion efficiency of the battery was 11.44%, and the corresponding short-circuit current density was 18.80 mA cm -2 , the open circuit voltage is 0.920V, and the fill factor is 69.1%. After the introduction of the additive, the battery efficiency is significantly improved to 12.68%, and the corresponding short-circuit current density is 19.06mAcm -2 , the open circuit voltage is 0.864V, the fill factor is 77.0%, and the JV curve is as follows Figure 4 (a) In the D18-Cl:N3 battery system, before the introduction of additives, the battery photoelectric conversion efficiency can reach 17.23%, and the short-circuit current density is 26.66 mA cm -2, the open circuit voltage is 0.875V, and the fill factor is 73.8%. After the additive is introduced, the cell photoelectric conversion efficiency can reach 18.15%, and its short-circuit current density is 27.52mA cm -2 , the open circuit voltage is 0.859V, the fill factor is 76.8%, and the JV curve is as follows Figure 4 (b) In summary, 1,4-diphenoxybenzene solid additive has good universality and can effectively improve the photovoltaic performance of polymer solar cells in D18-Cl:N3 and PM6:IT-4F systems.

[0045] Table 2 Photovoltaic performance parameters of D18-Cl:N3 and PM6:IT-4F battery systems before and after solid additive treatment

[0046]

[0047] Embodiment 3:

[0048] Experimental materials: donor PM6, acceptor Y6, solid additive (1,4-diphenoxybenzene), silicon wafer, glass and chloroform, etc.

[0049] Experimental method: First, we optimized the molecular structure of the additives by density functional theory (DFT) calculations, e.g. Figure 5 As shown, it presents a "Z" shape, that is, a non-planar structure. At the same time, the additive was placed in a nitrogen atmosphere, and a thermogravimetric analyzer (TGA) was used to test the change in the mass of the additive 1,4-diphenoxybenzene with temperature. The temperature range was: 25℃-300℃; the heating rate was: 10℃min -1 ; Then, the solid additive was dissolved in chloroform to prepare a concentration of 5 mg mL -1 The solution was then spin-coated on a silicon wafer. The removability of the solid additive was analyzed by observing the changes before and after the silicon wafer was annealed on a hot plate at 80°C for 10 minutes. The active layer solution was prepared according to the battery preparation conditions (the donor PM6 and the acceptor Y6 were mixed in a mass ratio of 1:1.2 and the solution concentration was 17.8 mg mL -1 Dissolve in chloroform. Add 5 mg mL -1 The concentration of the additive was dissolved in chloroform) and the additive solution, and then the thin film samples were prepared by spin coating. The Fourier infrared spectra of the sample films (additive films, active layer without additives, active layer without treatment after additives were introduced, and active layer after additives were thermally annealed) were tested by Nicolet 6700 infrared spectrometer and Continum infrared microscope to further verify the volatility of the additives.

[0050] Experimental results: Figure 6As shown in Figure 2, when the temperature is raised to 80°C and stabilized for 2 hours, the mass of the additive 1,4-diphenoxybenzene gradually decreases, indicating that the additive can be removed by heat treatment at 80°C or above. Figure 7 As shown in the figure, by comparing the pictures of the corresponding silicon wafer before and after thermal annealing after the introduction of the additive, it is found that the surface of the silicon wafer is smooth and clean after annealing, which indicates that the additive has been completely volatilized during the thermal annealing process, which further proves that the solid additive can be removed after thermal annealing. Figure 8 As shown in the Fourier infrared spectrum of the prepared film sample, it is found that the sample with the additive annealing treatment has a higher wavelength at 1500cm-1 than the sample with the additive but no annealing. -1 The peak at is significantly weakened, which corresponds to the characteristic peak of the benzene ring structure of the additive. This result further shows that the additive has been completely volatilized during the thermal annealing process of the blend film.

[0051] Example 4

[0052] Experimental materials: donor PM6, acceptor Y6, solid additive (1,4-diphenoxybenzene), ITO conductive glass, PEDOT:PSS and chloroform, etc.

[0053] Experimental method: Pre-mix the solid additive at 5 mg mL -1 The pure membrane was dissolved in chloroform with a concentration of 8 mg mL -1 , Y6 concentration was 10 mg mL -1 Dissolved in chloroform; the mixed film used a donor PM6 and an acceptor Y6 mass ratio of 1:1.2, and the total concentration was 17.8 mg mL -1 Dissolve in chloroform. Prepare the PEDOT:PSS hole transport layer and active layer in sequence according to the above process. Use atomic force microscopy AFM (tapping mode) to observe the height map of PM6 and Y6 pure films before and after the introduction of additives; as well as the height map and phase map of PM6:Y6 blended film, so as to analyze the effect of additives on its surface morphology. Experimental results: Fig. 9 As shown in the figure, after the introduction of additives, the surface root mean square roughness of PM6 pure film increased from 1.33nm to 1.68nm, and the surface root mean square roughness of Y6 pure film increased from 0.81nm to 2.83nm, indicating that the introduction of additives improved the crystallinity of PM6 and Y6 molecules, and the effect of additives on Y6 was more obvious; the surface root mean square roughness of the blended film slightly increased from 0.97nm to 1.22nm, and the crystallinity and ordered structure of the active layer were significantly improved. The phase diagram of the blended film shows that the surface fiber distribution is more obvious after the introduction of additives, forming a better fiber interpenetrating network structure, which is conducive to charge transfer and inhibits charge recombination.

[0054] The above-mentioned specific implementation methods are used to explain the present invention and are only preferred embodiments of the present invention, rather than limiting the present invention. Any modifications, equivalent substitutions, improvements, etc. made to the present invention within the spirit of the present invention and the protection scope of the claims shall fall within the protection scope of the present invention.

Claims

1. Application of a solid additive in an organic solar cell, characterized in that: The solid additive is 1,4-diphenoxybenzene, which is used as an additive for an organic solar cell using a non-fullerene acceptor.

2. The method for preparing an organic solar cell according to claim 1, wherein: The organic solar cell is an upright device, and the device structure is ITO electrode / anode interface layer / active layer / cathode interface layer / metal electrode from bottom to top, wherein the active layer uses non-fullerene as the acceptor material, 1,4-diphenoxybenzene as the solid additive, PEDOT:PSS as the anode interface layer, PDIN as the cathode interface layer, and silver as the metal electrode.

3. The method for preparing an organic solar cell according to claim 2, wherein: The active layer uses polymer PM6 as donor and non-fullerene Y6 as acceptor. The donor PM6 and acceptor Y6 are dissolved in chloroform solvent at a mass ratio of 1:1.2, with a concentration of 17.8 mg mL -1 .

4. The method for preparing an organic solar cell according to claim 2, wherein: The concentration of 1,4-diphenoxybenzene dissolved in chloroform is 2.5-7.5 mg mL -1 , preferably 5 mg mL -1 .

5. The method for preparing an organic solar cell according to claim 3, wherein: The specific steps include: S1, cleaning of ITO glass: placing the ITO glass substrate in deionized water, cleaning it with detergent, and then placing it in an ultrasonic cleaner, and ultrasonically cleaning it with deionized water, acetone, and isopropanol for 20 minutes in sequence, then drying the cleaned ITO glass with nitrogen, placing it in a plasma cleaner, and cleaning the surface with oxygen plasma for 3 minutes to remove residual organic matter on the surface, and then taking it out for use; S2, preparation of PEDOT:PSS hole transport layer: filter PEDOT:PSS for later use, use a pipette to take 50 μL of PEDOT:PSS solution and drop it on the cleaned ITO glass surface, so that the PEDOT:PSS solution covers the entire ITO glass, then spin-coat at 4000 rpm for 30 seconds, and finally place it on a constant temperature hot stage at 130°C for annealing for 20 minutes in an atmospheric environment to form a PEDOT:PSS film; S3, active layer preparation process: The donor PM6 and the acceptor Y6 were dissolved in the solvent chloroform at a mass ratio of 1:1.2, with a concentration of 17.8 mg mL -1 ; At the same time, the system adjusts the concentration of solid additives to 2.5-7.5mg mL -1 ; Take 10 μL of the solution and drop it on the surface of the PEDOT:PSS film to completely cover it, then spin coat it at 3000 rpm for 30 seconds. After spin coating, place it on a hot plate at 80°C for constant temperature annealing for 10 minutes to form an organic active layer film; S4, preparation of cathode interface layer PDIN: use a pipette to take 30 μL of PDIN methanol solution and drop it on the surface of the active layer film to make it completely covered, and then spin-coat it at a speed of 5000 rpm for 30 seconds; S5, silver electrode evaporation: put the prepared sample into the chamber of the thermal evaporation coating machine and wait until the vacuum degree reaches 2×10 -4 Pa, the silver electrode was evaporated and the film deposition rate was The thickness is controlled at 100 nm.

6. The method for preparing an organic solar cell according to claim 5, characterized in that: The 1,4-diphenoxybenzene is removed by annealing during a heat treatment at 80° C. or above.

7. The method for preparing an organic solar cell according to claim 2, wherein: The PM6:IT-4F system of polymer solar cells was prepared, with PM6 as the donor and non-fullerene IT-4F as the acceptor. The mass ratio of PM6 donor and IT-4F acceptor was 1:1.2, and the total concentration was 17.8 mg mL -1, , solid additives at 5 mg mL -1 The concentration was dissolved in chloroform.

8. The method for preparing an organic solar cell according to claim 2, wherein: The polymer solar cell D18-Cl:N3 system was prepared with D18-Cl as the donor and non-fullerene N3. The mass ratio of donor D18-Cl and acceptor N3 was 1:1.4, and the solution concentration was 16 mg mL -1 Dissolve in chloroform, solid additive at 5 mg mL -1 The concentration was dissolved in chloroform.

Citation Information

Cited By

  • Organic metal complex as well as preparation method and application thereof

    CN119462772A

  • Mesogenic element-containing low-melting-temperature solid additive as well as preparation method and application thereof

    CN119504497A