Non-fused ring acceptor material based on benzotriazole asymmetric structure as well as preparation method and application of non-fused ring acceptor material

By introducing asymmetric non-covalent fused ring acceptor materials with benzotriazole units with strong electron withdrawal ability in organic solar cells, the structure of asymmetric fullerene small molecule receptors in the prior art is solved and Cost issues broaden the spectrum absorption range and improve the efficiency and performance of solar cells.

CN119019416APending Publication Date: 2024-11-26UNIV OF CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411124822.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing asymmetric fullerene small molecule receptors have problems such as limited structural modification, weak absorption of visible light zones, high production costs and unstable morphology in organic solar cells, which limit their application efficiency and are non-covalent fused ring materials. The absorption spectrum is still different from that of the condensed ring, limiting the improvement of photocurrent and energy conversion efficiency.

Method used

Using a non-floxed ring acceptor material based on asymmetric structure of benzotriazole, the spectral absorption range of the material is broadened by introducing benzotriazole unit cores with strong electron absorption capacity, and simplifying the spectral absorption range of the material through direct carbon hydrocarbon activation method. Synthesis step, construct a non-covalent fused ring material with A-D1-A'-D2-A structure.

Benefits of technology

It improves the short-circuit current density of the material and the performance of solar cell devices, simplifies the synthesis steps, reduces costs, and provides good solubility and film formation, significantly redshift absorption spectrum, and improves the utilization efficiency of sunlight.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019416A_ABST
    Figure CN119019416A_ABST
Patent Text Reader

Abstract

The invention relates to a non-fused ring acceptor material based on a benzotriazole asymmetric structure and a preparation method and application of the non-fused ring acceptor material based on the benzotriazole asymmetric structure, a series of novel asymmetric-structure small molecule acceptor materials are constructed by introducing a benzotriazole unit with high electron withdrawing capacity, and the material has a remarkable red-shift absorption spectrum and can be applied to the field of electron absorption. Compared with an asymmetric fused ring material, the material provided by the invention is relatively simple in synthesis steps, has good solubility and film-forming property, has relatively high energy conversion efficiency in the aspect of organic solar cell devices, and can be applied to the field of organic solar cell devices. Reference is provided for receptor development of organic solar cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic solar energy, and in particular to a non-condensed ring receptor material based on an asymmetric structure of benzotriazole, and a preparation method and application thereof. Background Art

[0002] Compared with traditional silicon-based solar cells, organic solar cells have attracted extensive attention from researchers due to their advantages such as mechanical flexibility, light weight, solution processability and translucency. At present, organic solar cells are usually manufactured using bulk heterostructures, in which the blend layer is mainly divided into two components: polymer donors and small molecule acceptors. The small molecule acceptors can be divided into symmetric acceptors and asymmetric acceptors according to their molecular symmetry. Due to the widespread use of phenyl-C 61 -Methyl butyrate (PC 61 BM) and phenyl-C 71 -Methyl butyrate (PC 71 Asymmetric fullerene small molecule receptors have appeared in various organic solar cells in the past few decades. However, due to the shortcomings of asymmetric fullerene small molecule receptors such as limited structural modification, weak absorption in the visible light region, high production cost and unstable morphology, their application is greatly limited, and their efficiency is less than 11%. On the contrary, non-fullerene small molecule receptors have great potential for the development of asymmetric non-fullerene small molecule receptors because of their easy modification of structure and good absorption in the visible light and even near-infrared region.

[0003] At present, the representative materials of asymmetric fused ring receptors are IT-3F and BTP-S9, and after being matched with PM6, high PCEs of 13.83% and 17.61% are obtained respectively (J. Mater. Chem. A 2018, 6, 23644; Adv. Energy Mater. 2024, 14, 2303785), but the synthesis steps of such asymmetric materials are cumbersome, resulting in high synthesis costs of such materials. Therefore, it is urgent to simplify the synthesis route to reduce the cost of materials. For this reason, a "conformational lock" strategy can be introduced to construct non-covalent fused rings to avoid complex fused ring synthesis steps. Such molecules are locked by non-covalent interaction forces within the molecule to obtain a relatively planar conjugated skeleton. At present, Tang Weihua et al. have reported a class of non-condensed ring molecules DBT-4F and DBT-HD with asymmetric structures, and obtained high efficiencies of 12.14% and 13.57% respectively after being matched with the polymer donor PBDB-T (Chemical Engineering Journal 412 (2021) 128770; Chemical Engineering Journal 427 (2022) 131828). This result shows that the design of non-covalent condensed ring materials with asymmetric structures is of great significance in the field of organic solar cells. However, since the absorption spectrum of this type of material is still quite different from that of condensed rings, the further improvement of photocurrent and energy conversion efficiency is limited.

[0004] Asymmetric non-covalent fused ring molecules currently mostly adopt the A-D1-A'-D2-A structure, where the electron-accepting unit core in the middle and the electron-withdrawing unit at the end are connected by an electron-donating unit, which is conducive to charge transfer within the molecule, thereby broadening the absorption spectrum range. Therefore, based on its structural characteristics, it is urgent to provide a benzotriazole unit core with strong electron-accepting ability to broaden its spectral absorption range in order to obtain a better short-circuit current density. Therefore, it is of great research significance to construct a type of asymmetric non-covalent fused ring with a benzotriazole core to improve the device performance of solar cells. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a non-condensed ring acceptor material based on the asymmetric structure of benzotriazole and a preparation method and application thereof, which can broaden the absorption spectrum range of the current asymmetric non-covalent condensed ring acceptor material to obtain a better short-circuit current density for application in organic solar cells.

[0006] The present invention solves the technical problem by adopting the following technical solutions:

[0007] A non-condensed ring receptor material based on the asymmetric structure of benzotriazole, the structural formula is:

[0008]

[0009] In Formula I, R1, R2, R3, and R4 are each independently selected from C1 to C 50 A straight chain or branched alkyl group;

[0010] X1 and X3 are each independently selected from any one of oxygen atom, sulfur atom or selenium atom substitution, and X2 is any one of oxygen atom, sulfur atom, selenium atom or nitrogen atom substitution;

[0011] A is an electron-withdrawing unit.

[0012] Furthermore, R1, R2, R3, and R4 optionally contain an ether bond, an ester bond, a perfluoroalkyl group, a substituted or unsubstituted phenyl group, or a substituted or unsubstituted heteroaryl group;

[0013] The alkyl and alkoxy groups contain straight or branched chains with 1 to 16 carbon atoms.

[0014] Furthermore, when X2 is substituted with a nitrogen atom, it also includes a straight chain or branched chain having 2 to 12 carbon atoms.

[0015] Moreover, A is selected from any one of the structural formulas shown in the following formula II-1 to formula II-6:

[0016]

[0017] In Formula II-1 to Formula II-4, X4 is at least one of H, F, Cl, Br, I, alkyl, ester or alkylthio, and X5 is at least one of F, Cl, Br, I, alkyl, ester or alkylthio;

[0018] The alkyl group and the alkylthio group contain a straight chain or a branched chain with 1 to 6 carbon atoms.

[0019] Moreover, the non-condensed ring receptor material based on the asymmetric structure of benzotriazole is any one of the following compounds A1-A12:

[0020]

[0021]

[0022] A method for preparing a non-condensed ring receptor material based on an asymmetric structure of benzotriazole comprises the following steps:

[0023] S1. Under a protective atmosphere, a mixture of the compound of formula III-1, the compound of formula III-3, potassium carbonate, pivalic acid and anhydrous toluene is placed in a reactor, and then Pd2(dba)3 and P(o-CH3OPh)3 are added. The reaction temperature is 60-140°C. After reacting for 5-12 hours, the mixture is cooled to room temperature, and the reaction solution is concentrated to 2-5 mL. The mixture is purified by a silica gel column, and the collected product is concentrated by rotary evaporation to obtain a compound of formula (a);

[0024]

[0025] S2. Under a protective atmosphere, the compound of formula (a), the compound of formula III-2, potassium carbonate, pivalic acid and anhydrous toluene are placed in a reactor, and Pd2(dba)3 and P(o-CH3OPh)3 are added. The reaction temperature is 60-140°C. After reacting for 5-12 hours, the mixture is cooled to room temperature, and the reaction solution is concentrated to 2-5 mL. The mixture is purified by a silica gel column, and the collected product is concentrated by rotary evaporation to obtain a compound of formula (b);

[0026]

[0027] S3, placing the compound of formula (b), the electron-withdrawing unit A and a mixture of chloroform into a reactor, and then dropping an acidic or alkaline liquid to carry out a Knoevenagel condensation reaction, the reaction temperature is 60-80°C, the reaction time is 12-36h, after the reaction is completed, the reaction temperature is lowered to room temperature, the reaction solution is concentrated to 2-5mL, purified by a silica gel column, and then the collected product is concentrated and precipitated in methanol, and filtered to obtain a compound of formula I;

[0028]

[0029] The acidic liquid is trimethylchlorosilane, and the alkaline liquid is either piperidine or pyridine.

[0030] Moreover, when A in the formula I is a structure of formula II-4, the preparation method comprises the following steps:

[0031] S1. In a nitrogen atmosphere, reactant 1, reactant 2, cesium carbonate and pivalic acid are subjected to coupling reaction in anhydrous toluene under the action of Pd2(dba)3 and P(o-CH3OPh)3, the reaction temperature is 60-140°C, the reaction is cooled to room temperature after 5-12 hours, the reaction solution is concentrated to 2-5 mL, purified by silica gel column, and the collected product is concentrated by rotary evaporation to obtain intermediate P1; wherein the reactant 1 is selected from the compound represented by formula III-1, and the reactant 2 is selected from the compound represented by formula III-3;

[0032] S2. In a nitrogen atmosphere, in the presence of Pd2(dba)3 and P(o-CH3OPh)3, the intermediate P1, reactant 3, cesium carbonate and pivalic acid are subjected to coupling reaction in anhydrous toluene at a reaction temperature of 60 to 140°C. After reacting for 5 to 12 hours, the reaction solution is cooled to room temperature, and the reaction solution is concentrated to 2 to 5 mL. The product is purified by a silica gel column, and the collected product is concentrated by rotary evaporation to obtain the intermediate P2; wherein the reactant 3 is selected from the compound represented by formula III-2;

[0033] S3, injecting the intermediate P2 and reactant 4 or reactant 5 into chloroform, and then dropping an acidic or alkaline liquid to carry out Knoevenagel condensation reaction, the reaction temperature is 60-80°C, the reaction time is 12-36h, after the reaction is completed, the reaction temperature is lowered to room temperature, the reaction solution is concentrated to 2-5mL, purified by silica gel column, and then the collected product is concentrated and precipitated in methanol, and filtered to obtain a compound of formula I wherein A is formula II-4; wherein the reactant 4 is selected from the compound shown in formula III-4, and the reactant 5 is selected from the compound shown in formula III-5;

[0034] In step S1, the eluent is petroleum ether and dichloromethane in a volume ratio of 1:1 to 1:3, and the molar ratio of reactant 1: reactant 2: Pd2(dba)3: P(o-CH3OPh)3: cesium carbonate: pivalic acid is 1:1:0.1:0.2:3:0.4;

[0035] In step S2, the eluent is petroleum ether and dichloromethane in a volume ratio of 1:1 to 1:3, and the molar ratio of the intermediate P1: reactant 3: Pd2(dba)3: P(o-CH3OPh)3: cesium carbonate: pivalic acid is 1:1.3:0.15:0.3:10:1;

[0036] In step S3, the eluent is petroleum ether and dichloromethane in a volume ratio of 3:1 to 1:1, the molar ratio of the intermediate P2: the reactant 4 or the reactant 5 is 1:3.5, the acidic liquid is trimethylchlorosilane, and the alkaline liquid is any one of piperidine or pyridine;

[0037] The structural formulas of reactant 1, reactant 2, reactant 3, reactant 4 and reactant 5 are as follows:

[0038]

[0039] In formula III-1, R1 and R2 are each independently selected from C1 to C 50 A straight or branched alkyl group, which optionally contains an ether bond, an ester bond, a perfluoroalkyl group, a substituted or unsubstituted phenyl group, or a substituted or unsubstituted heteroaryl group;

[0040] X3 is any one of oxygen atom, sulfur atom or selenium atom substitution;

[0041] X6 is a halogen atom selected from any one of Cl, Br or I;

[0042] In formula III-2 and formula III-3, X1 is any one of oxygen atom, sulfur atom or selenium atom substitution, and X2 is any one of oxygen atom, sulfur atom, selenium atom or nitrogen atom substitution;

[0043] R3 and R4 are each independently selected from C1 to C 50 A straight or branched alkyl group, which optionally contains an ether bond, an ester bond, a perfluoroalkyl group, a substituted or unsubstituted phenyl group, or a substituted or unsubstituted heteroaryl group;

[0044] In Formula III-4 and Formula III-5, X4 is at least one of H, F, Cl, Br, I, alkyl, ester or alkylthio.

[0045] Moreover, the temperature of the coupling reaction is preferably 110 to 120° C., and the reaction time is preferably 10 to 12 h.

[0046] Moreover, the reaction temperature of the Knoevenagel condensation reaction is preferably 65° C., and the reaction time can be 12 to 36 hours, preferably 18 hours.

[0047] An application of the non-condensed ring acceptor material based on the asymmetric structure of benzotriazole in polymer organic solar cells.

[0048] A polymer organic solar cell, comprising a conductive ITO glass electrode, a hole transport layer, an active layer, an electron transport layer and a metal electrode coated in sequence from bottom to top;

[0049] The conductive ITO glass electrode comprises a glass substrate and a conductive ITO film, and a layer of conductive ITO film is plated on the upper surface of the glass substrate;

[0050] The active layer is a blended film of a polymer donor material and a benzotriazole core non-condensed ring acceptor material, and the mass ratio of the donor material to the acceptor material is 0.5 to 2:1;

[0051] Wherein, the polymer donor material is any one of the following materials:

[0052]

[0053] A method for preparing a polymer organic solar cell comprises the following steps:

[0054] The polymer donor material and the non-condensed ring acceptor material based on benzotriazole core are mixed in a mass ratio of 0.5 to 2:1, and a solvent is added to fully dissolve them to prepare a slurry with a concentration of 10 mg / mL to 30 mg / mL, and the slurry is coated on a conductive ITO glass electrode to prepare a thin film, and finally an organic solar cell is prepared;

[0055] Wherein, the solvent is at least one of chloroform, chlorobenzene and o-dichlorobenzene.

[0056] The advantages and positive effects of the present invention are:

[0057] 1. The present invention introduces a benzotriazole unit with strong electron-withdrawing ability to synthesize a type of asymmetric receptor material with an A-D1-A'-D2-A structure, which enhances the charge transfer within the molecule and broadens the solar spectrum absorption range of the material, which is conducive to obtaining a higher short-circuit current density, thereby improving the performance of solar cell devices. In addition, when synthesizing such asymmetric non-covalent fused ring materials, the direct carbon-hydrogen activation method is used for coupling, which saves more synthesis steps than the traditional Stille coupling, and when used with low-cost donor materials, the prepared solar cells also show good performance.

[0058] 2. The asymmetric non-covalent fused ring receptor material of the present invention has good solubility, film-forming property and relatively wide spectral absorption, and is a class of receptor materials with great potential in the preparation of high-performance devices and flexible organic solar cells.

[0059] 3. The present invention constructs a series of novel asymmetric small molecule receptor materials by introducing benzotriazole units with strong electron-withdrawing ability. The material has a significantly red-shifted absorption spectrum, which improves the utilization of sunlight, thereby obtaining a larger short-circuit current density. Compared with asymmetric fused ring materials, the material synthesis steps provided by the present invention are relatively simple, and the obtained material has good solubility and film-forming properties. At the same time, in terms of organic solar cell devices, it has a higher energy conversion efficiency, which provides a reference for the development of receptors for organic solar cells.

[0060] 4. The design of the asymmetric receptor material involved in the present invention is highly flexible. By connecting different units, the material properties can be precisely controlled, while the color of the solar cell can be diversified to meet the aesthetic requirements of architectural design.

[0061] 5. The asymmetric receptor material of the present invention can be easily prepared on a large scale through roll-to-roll printing, spraying and other processes, and is suitable for fields such as building integrated photovoltaics (BIPV). BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1The UV-visible absorption spectra of the receptor material A9 prepared in the present invention in chloroform solution and in the thin film state.

[0063] Figure 2 This is a cyclic voltammetric characteristic curve of the acceptor material A9 prepared in the present invention in a thin film state.

[0064] Figure 3 The nuclear magnetic resonance hydrogen spectrum of the receptor material A9 prepared by the present invention is 1 H-NMR.

[0065] Figure 4 The carbon NMR spectrum of the receptor material A9 prepared by the present invention is 1 C-NMR.

[0066] Figure 5 This is a current density and voltage (JV) characteristic curve of a device prepared with PTVT-T:A9 as the active layer.

[0067] Figure 6 This is the external quantum efficiency (EQE) graph obtained by testing a device prepared with PTVT-T:A9 as the active layer.

[0068] Figure 7 This is a structural diagram of the organic solar cell device prepared in the present invention.

[0069] Reference numerals

[0070] 1-metal electrode, 2-electron transport layer, 3-active layer, 4-hole transport layer, 5-glass substrate, 6-conductive ITO film. DETAILED DESCRIPTION

[0071] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0072] The technical solution of the present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments, but the description of the embodiments is only a part of the embodiments of the present invention, most of which are not limited to this. The methods are conventional methods unless otherwise specified, and the materials can be obtained from public commercial channels unless otherwise specified.

[0073] Example 1

[0074] This embodiment provides a method for preparing a non-condensed ring receptor material based on an asymmetric structure of benzotriazole, and the specific steps are as follows:

[0075]

[0076] S1. Add 1 mmol of compound 1 (Science China Chemistry 2021, 64, 228-231), 1 mmol of compound 2 (Org. Electron. 2012, 13, 570-578), 3 mmol of cesium carbonate, 0.4 mmol of pivalic acid, 0.1 mmol of Pd2(dba)3 and 0.2 mmol of P(o-CH3OPh)3 to a 50 mL Schlenk reaction tube, and add 15.0 mL of anhydrous toluene as the reaction solvent. After evacuation three times under a nitrogen atmosphere, the temperature was raised to 110°C and reacted for 5 hours to obtain a crude product, which was separated and extracted and dried over anhydrous sodium sulfate; finally, it was separated and purified by column chromatography, the eluent was petroleum ether: dichloromethane = 1:2 (volume ratio), and after purification, rotary evaporation was performed to finally obtain compound 3, which was a light yellow oil with a yield of 34%.

[0077] 1 HNMR (500MHz, CDCl3, δ): 10.12 (s, 1H), 8.28 (s, 1H), 4.72 (d, 1H), 3.96 (d, 2H), 3.05–3.02 (t, 2H), 2.23–2.20(m, 1H), 2.04–2.01(m, 1H), 1.79–1.73(m, 2H), 1.58–1.25(m, 31H), 1.02–0.86(m, 15H); 13 CNMR (126MHz, CDCl3, δ): 182.63, 152.13, 151.14, 142.94, 139.44, 137.65, 133.46, 116.28, 78.75, 59.46, 40.51, 40.42, 31. 94, 31.58, 30.73, 30.45, 29.77, 29.50, 29.30, 29.16, 28.69, 28.64, 24.11, 23.76, 23.16, 23.01, 22.72, 14.14, 11.07, 10.69.

[0078] S2. Add 0.3 mmol of compound 3, 0.36 mmol of compound 4 (ACS Appl, Mater. Interfaces 2020, 12, 16531-16540), 3 mmol of cesium carbonate, 0.4 mmol of pivalic acid, 0.045 mmol of Pd2(dba)3 and 0.09 mmol of P(o-CH3OPh)3 to a 50 mL Schlenk reaction tube, and add 15.0 mL of anhydrous toluene as the reaction solvent. After evacuation three times under a nitrogen atmosphere, the temperature was raised to 110 ° C and reacted for 10 hours to obtain a crude product, which was separated and extracted and dried over anhydrous sodium sulfate; finally, it was separated and purified by column chromatography, the eluent was petroleum ether: dichloromethane = 1:2 (volume ratio), and after purification, rotary evaporation was performed to finally obtain compound 5, which was an orange-yellow oil with a yield of 73.3%.

[0079] 1 H NMR (500MHz, CDCl3, δ): 10.12(s,1H),9.85(s,1H),8.57–8.48(t,1H),8.27–8.24(t,1H),7.60(t,1H),4.73–4.71(m,2H ),4.01–3.96(m,4H),3.05–3.02(t,2H),2.22–2.00(m,7H),1.78–1.76(m,2H),1.58–1.25(m,46H),1.02–0.61(m,61H); 13C NMR(126MHz, CDCl3, δ):182.49,161.71,161.64,158.25,152.16,151.35, 149.24,148.39,143.38,139.59,139.29,139.22,139.14,139.07,139.00 ,138.42,137.30,133.03,130.75,125.68,125.64,117.88,117.85,117.8 1,114.68,114.66,78.73,78.58,59.36,59.28,59.19,54.04,43.35,43.2 8,43.21,40.55,40.42,40.38,35.39,31.95,31.61,30.81,30.78,30.50,30.48,30.41,29.78,29.32,29.18,29.06,29.01,28.96,28.78,28.69,28 .68,28.53,27.60,27.42,24.13,23.77,23.26,23.24,23.19,23.05,22.82,22.77,22.74,14.24,14.17,14.12,14.01,11.21,11.14,11.09,10.75.

[0080] S3. In a 100 mL reaction bottle, compound 5 (0.1 mmol) and commercially purchased compound 6 (0.4 mmol) were dissolved in 25.0 mL of chloroform, and 2.0 mL of trimethylsilyl chloride was added dropwise, and then the temperature was raised to 60°C for reaction for 20 h. After the reaction was completed, the mixture was returned to room temperature, 10.0 mL of methanol was poured in and filtered to obtain a crude product, which was separated and purified by column chromatography, with the eluent being petroleum ether: dichloromethane = 1:1 (volume ratio). After purification, it was rotary evaporated to finally obtain a dark brown solid A9 with a yield of 68.0%.

[0081] 1 H NMR(500MHz, CDCl3,δ):9.20–9.04(dd,4H),8.76–8.61(dd,2H),8.28(d,2H),7.87–7.72(m,5H),4.80–4.78(m,2H),4.13–4.09(m ,4H),3.13–3.10(t,2H),2.41(s,1H),2.26(s,2H),2.13–2.02(m,4H),1.81–1.72(m,4H),1.50–1.29(m,48H),1.09–0.63(m,58H); 13C NMR(126MHz, CDCl3, δ):187.99,187.05,165.95,165.91,165.85,161.30,161.03,160.59,160.40,160.05,153.25, 153.20,153.11,153.03,152.89,152.52,151.19,151.05,150.99,150.97,150.92,150.18,143.91,143.84,140.28, 139.88,139.68,139.30,139.24,139.18,138.74,138.66,135.86,135.59,135.44,134.60,133.80,133.65,133.39,133.34,132.64,132.58,132.52,132.46,126.44,126.39,126.34,125.60,125.37,123.26,123.03,122.98,121.46, 118.73,118.68,116.60,116.47,116.11,116.04,115.99,115.81,115.67,115.62,79.52,79.21,67.49,65.98,59.48,59.41,59.33,53.91,43.52,43.43,43.25,40.61,40.55,40.06,40.04,35.63,35.56,34.48,34.07,32.02,32.00, 30.86,30.83,30.58,30.27,29.81,29.63,29.47,29.36,29.18,28.86,28.46,27.59,27.35,24.15,23.94,23.41,23.29,23.05,22.89,22.84,22.78,19.82,14.53,14.29,14.23,14.18,14.06,11.31,11.17,10.77,10.73; High resolution mass spectrometry, calculated: C 101 H 115 F4N7O4S3,1663.25; Exp. value:1662.371.

[0082] Example 2

[0083] The absorption data of the asymmetric non-covalent fused ring receptor material A9 synthesized in Example 1 in chloroform solution and film were measured by UV-visible absorption spectrometer. The absorption spectra of the material solution and film are as follows: Figure 1 And as shown in Table 1.

[0084] It can be seen that the maximum absorption peak of A9 in solution is 752nm, and the maximum absorption peak in the film is 810nm, which indicates that the material has an obvious red shift. At the same time, the absorption spectrum is also broadened, and the optical band gap is 1.39eV. This result shows that the optical absorption of the asymmetric acceptor material A9 is comparable to that of the Y6 series condensed ring materials.

[0085] Table 1: Optical absorption data of asymmetric non-covalent fused ring receptor A9:

[0086]

[0087] Example 3

[0088] The electronic energy level data of the asymmetric non-covalent fused ring receptor A9 synthesized in Example 1 were measured by electrochemical cyclic voltammetry. The cyclic voltammetry curve of the material is shown in FIG. Figure 2 shown.

[0089] The asymmetric non-covalent fused ring receptor A9 synthesized in Example 1 was dissolved in dichloromethane solvent, and then the solution was dripped onto the working electrode and dried; a 0.1 mol / L acetonitrile solution of tetrabutylammonium hexafluorophosphate was used as the electrolyte; a platinum wire was used as the counter electrode; and Ag / AgCl was used as the reference electrode to measure the oxidation and reduction curves of the receptor A9.

[0090] According to the measured oxidation and reduction potentials, the HOMO and LUMO energy levels of the acceptor A9 were calculated to be -5.59 eV and -3.88 eV, respectively. The results show that A9 has a suitable energy level and can well match the energy levels of common polymer donor materials.

[0091] Example 4

[0092] Preparation and performance testing of organic solar cell devices:

[0093] The acceptor material A9 synthesized in Example 1 was matched with the polymer donor PTVT-T to prepare an organic solar cell device with a device structure of ITO / PEDOT:PSS / D:A / PDIN / Ag. The indium tin oxide (ITO) glass-coated substrate was ultrasonically cleaned with detergent, deionized water and ethanol. The cleaned ITO substrate was blown dry with high-purity nitrogen and then treated with oxygen plasma for 1 minute. Subsequently, the PEDOT:PSS solution was spin-coated on the ITO glass substrate at a speed of 5000 rpm per minute and then annealed at 150°C in air for 15 minutes. After annealing, the ITO substrate coated with PEDOT:PSS was transferred to a glove box filled with high-purity nitrogen. PTVT-T and A9 were dissolved in chloroform at a mass ratio of 1:1.2 to prepare a mixed solution of 17 mg / mL. After heating and stirring at 45°C for 3 hours, the mixed solution was spin-coated on the PEDOT:PSS film. Afterwards, PDIN solution (2 mg / mL, dissolved in methanol, containing 0.25 vol% acetic acid) was spin-coated on top of the active layer at a speed of 5000 rpm. -4 100 nm of silver (Ag) was deposited by thermal evaporation under a vacuum degree of 1.5 Pa.

[0094] like Figure 5 As shown in Figure 2, the open circuit voltage of the organic solar cell prepared by blending the acceptor A9 and the simple structure polymer donor PTVT-T is 0.847 V and the short circuit current is 25.09 mA / cm 2 , the filling factor is 72.13%, and the final energy conversion efficiency is as high as 15.33%. This result shows that asymmetric acceptors and low-cost donors can also achieve a higher efficiency, providing a reference for the future development of high-performance and low-cost materials.

[0095] The above embodiments are only used to illustrate the technical solution of the present application, but should not be construed as limiting the scope of the present application. Any technician familiar with the profession should recognize that although the embodiments describe the present invention in detail, modifications and equivalent substitutions can be made within the scope defined by the technical solution of the present invention.

[0096] Although the embodiments of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments.

Claims

1. A non-condensed ring receptor material based on the asymmetric structure of benzotriazole, Features: The structural formula is: In Formula I, R 1 , R 2 , R 3 , R 4 Each independently selected from C 1 ~C 50 A straight chain or branched alkyl group; X 1 and X 3 Each independently selected from any one of oxygen atom, sulfur atom or selenium atom substitution, X 2 is substituted by any of oxygen, sulfur, selenium or nitrogen atoms; A is an electron-withdrawing unit.

2. The non-condensed ring receptor material based on the asymmetric structure of benzotriazole according to claim 1, Features: R 1 , R 2 , R 3 , R 4 Optionally containing ether bonds, ester bonds, perfluoroalkyl groups, substituted or unsubstituted phenyl groups, substituted or unsubstituted heteroaryl groups; The alkyl and alkoxy groups contain straight or branched chains with 1 to 16 carbon atoms.

3. The non-condensed ring receptor material based on the asymmetric structure of benzotriazole according to claim 2, Features: X 2 When the substitution is with a nitrogen atom, it also includes a straight chain or branched chain having 2 to 12 carbon atoms.

4. The non-condensed ring receptor material based on the asymmetric structure of benzotriazole according to claim 3, Features: A is selected from any one of the following structural formulas II-1 to II-6: In Formula II-1 to Formula II-4, X 4 is at least one of H, F, Cl, Br, I, alkyl, ester or alkylthio, X 5 is at least one of F, Cl, Br, I, an alkyl group, an ester group or an alkylthio group; The alkyl group and the alkylthio group contain a straight chain or a branched chain with 1 to 6 carbon atoms.

5. The non-condensed ring receptor material based on the asymmetric structure of benzotriazole according to claim 4, Features: Any one of the following compounds A1-A12:

6. A method for preparing the non-condensed ring receptor material based on the asymmetric structure of benzotriazole according to claim 5, Features: The steps include: S1. Under a protective atmosphere, a mixture of the compound of formula III-1, the compound of formula III-3, potassium carbonate, pivalic acid and anhydrous toluene is placed in a reactor, and then Pd 2 (dba) 3 and P(o-CH 3 OPh) 3 The reaction temperature is 60-140°C, and the reaction is cooled to room temperature after 5-12 hours. The reaction solution is concentrated to 2-5 mL, purified by silica gel column, and the collected product is concentrated by rotary evaporation to obtain a compound of general formula (a); S2. Under a protective atmosphere, a mixture of the compound of formula (a), the compound of formula III-2, potassium carbonate, pivalic acid and anhydrous toluene is placed in a reactor, and Pd 2 (dba) 3 and P(o-CH 3 OPh) 3 The reaction temperature is 60-140°C, and the reaction is cooled to room temperature after 5-12 hours. The reaction solution is concentrated to 2-5 mL, purified by silica gel column, and the collected product is concentrated by rotary evaporation to obtain a compound of general formula (b); S3, placing the compound of formula (b), the electron-withdrawing unit A and a mixture of chloroform into a reactor, and then dropping an acidic or alkaline liquid to carry out a Knoevenagel condensation reaction, the reaction temperature is 60-80°C, the reaction time is 12-36h, after the reaction is completed, the reaction temperature is lowered to room temperature, the reaction solution is concentrated to 2-5mL, purified by a silica gel column, and then the collected product is concentrated and precipitated in methanol, and filtered to obtain a compound of formula I; The acidic liquid is trimethylchlorosilane, and the alkaline liquid is either piperidine or pyridine.

7. The method for preparing the non-condensed ring receptor material based on the asymmetric structure of benzotriazole according to claim 6, Features: When A in the formula I is a structure of formula II-4, the preparation method comprises the following steps: S1. In a nitrogen atmosphere, 2 (dba) 3 and P(o-CH 3 OPh) 3 Under the action of, reactant 1, reactant 2, cesium carbonate and pivalic acid are subjected to coupling reaction in anhydrous toluene, the reaction temperature is 60-140°C, the reaction is cooled to room temperature after 5-12 hours, the reaction solution is concentrated to 2-5 mL, purified by silica gel column, and the collected product is concentrated by rotary evaporation to obtain intermediate P1; wherein, the reactant 1 is selected from the compound represented by formula III-1, and the reactant 2 is selected from the compound represented by formula III-3; S2. In a nitrogen atmosphere, 2 (dba) 3 and P(o-CH 3 OPh) 3 Under the action of, the intermediate P1, reactant 3, cesium carbonate and pivalic acid are subjected to coupling reaction in anhydrous toluene at a reaction temperature of 60 to 140°C. After reacting for 5 to 12 hours, the reaction solution is cooled to room temperature, and the reaction solution is concentrated to 2 to 5 mL. The product is purified by a silica gel column, and the collected product is concentrated by rotary evaporation to obtain the intermediate P2; wherein the reactant 3 is selected from the compound represented by formula III-2; S3, injecting the intermediate P2 and reactant 4 or reactant 5 into chloroform, and then dropping an acidic or alkaline liquid to carry out Knoevenagel condensation reaction, the reaction temperature is 60-80°C, the reaction time is 12-36h, after the reaction is completed, the reaction temperature is lowered to room temperature, the reaction solution is concentrated to 2-5mL, purified by silica gel column, and then the collected product is concentrated and precipitated in methanol, and filtered to obtain a compound of formula I wherein A is formula II-4; wherein the reactant 4 is selected from the compound shown in formula III-4, and the reactant 5 is selected from the compound shown in formula III-5; In step S1, the eluent is petroleum ether and dichloromethane in a volume ratio of 1:1 to 1:3, and the reactant 1: reactant 2: Pd 2 (dba) 3 :P(o-CH 3 OPh) 3 : The molar ratio of cesium carbonate: pivalic acid is 1:1:0.1:0.2:3:0.4; In step S2, the eluent is petroleum ether and dichloromethane in a volume ratio of 1:1 to 1:3, and the intermediate P1: reactant 3: Pd 2 (dba) 3 :P(o-CH 3 OPh) 3 : The molar ratio of cesium carbonate: pivalic acid is 1:1.3:0.15:0.3:10:1; In step S3, the eluent is petroleum ether and dichloromethane in a volume ratio of 3:1 to 1:1, the molar ratio of the intermediate P2: the reactant 4 or the reactant 5 is 1:3.5, the acidic liquid is trimethylchlorosilane, and the alkaline liquid is any one of piperidine or pyridine; The structural formulas of reactant 1, reactant 2, reactant 3, reactant 4 and reactant 5 are as follows: In Formula III-1, R 1 , R 2 Each independently selected from C 1 ~C 50 A straight or branched alkyl group, which optionally contains an ether bond, an ester bond, a perfluoroalkyl group, a substituted or unsubstituted phenyl group, or a substituted or unsubstituted heteroaryl group; X 3 is substituted by any of oxygen, sulfur or selenium atoms; X 6 is a halogen atom selected from any one of Cl, Br or I; In Formula III-2 and Formula III-3, X 1 is any one of oxygen, sulfur or selenium atoms, X 2 is substituted by any of oxygen, sulfur, selenium or nitrogen atoms; R 3 , R 4 Each independently selected from C 1 ~C 50 A straight or branched alkyl group, which optionally contains an ether bond, an ester bond, a perfluoroalkyl group, a substituted or unsubstituted phenyl group, or a substituted or unsubstituted heteroaryl group; In Formula III-4 and Formula III-5, X 4 is at least one of H, F, Cl, Br, I, an alkyl group, an ester group or an alkylthio group.

8. Use of the non-condensed ring acceptor material based on the asymmetric structure of benzotriazole according to claim 5 in polymer organic solar cells.

9. A polymer organic solar cell, Features: It comprises a conductive ITO glass electrode, a hole transport layer (4), an active layer (3), an electron transport layer (2) and a metal electrode (1) which are coated in sequence from bottom to top; The conductive ITO glass electrode comprises a glass substrate (5) and a conductive ITO film (6), wherein a layer of the conductive ITO film (6) is plated on the upper surface of the glass substrate (5); The active layer is a blended film of a polymer donor material and a benzotriazole core non-condensed ring acceptor material, and the mass ratio of the donor material to the acceptor material is 0.5 to 2:1; Wherein, the polymer donor material is any one of the following materials:

10. A method for preparing the polymer organic solar cell according to claim 9, Features: The steps include: The polymer donor material and the non-condensed ring acceptor material based on benzotriazole core are mixed in a mass ratio of 0.5 to 2:1, and a solvent is added to fully dissolve them to prepare a slurry with a concentration of 10 mg / mL to 30 mg / mL, and the slurry is coated on a conductive ITO glass electrode to prepare a thin film, and finally an organic solar cell is prepared; Wherein, the solvent is at least one of chloroform, chlorobenzene and o-dichlorobenzene.

Citation Information

Cited By

  • Short-wave infrared receptor small molecule based on quinone fused benzotriazole as well as preparation method and application of short-wave infrared receptor small molecule

    CN117946139A