Method for preparing methylamine-free perovskite thin film through blade coating vacuum and perovskite solar cell
By adding 2-imidazolidinone to the perovskite precursor solution and using a scraping vacuum preparation method, the instability of methylamine cations in the perovskite solar cell film was solved, and a high-quality perovskite layer film was prepared. , improves the performance and stability of solar cells and supports large-scale commercial production.
Patent Information
- Application Number
- CN202410918892.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The methylamine cations in existing perovskite solar cell thin films have thermal instability and humidity instability, which affect the long-term stability of the device and hinder the commercialization process of perovskite solar cells.
The non-volatile solid ligand 2-imidazolidinone was added to the perovskite precursor solution, and the 2-imidazolidinone was sublimated during annealing. A poreless, high-quality perovskite layer film was prepared by scraping and vacuum preparation. .
A perovskite film with large grain size and dense grain size is obtained, which improves the performance and stability of solar cells, supports large-scale commercial production, and is used in air environments, with higher universality and commercial value.
Smart Images

Figure CN118890939A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cells, and in particular to a method for preparing a methylamine-free perovskite film by vacuum scraping and a perovskite solar cell. Background Art
[0002] Since organic-inorganic metal halide perovskite solar cells were first reported in 2009, they have achieved a certified power conversion efficiency of 26.7% per cell in more than a decade due to their high photoelectric conversion efficiency (theoretical efficiency of 33% for a single cell), adjustable band gap, simple preparation method and low production cost. The conversion efficiency of perovskite and crystalline silicon stacking has achieved a breakthrough of 33.46%.
[0003] However, currently, high-efficiency perovskite solar cells are usually prepared in a nitrogen glove box by spin coating, but the effective area of the cell is usually less than 1cm 2 , therefore, it is not suitable for commercial large-scale and large-area production.
[0004] At present, the preparation of perovskite solar cells based on scraping has high repeatability, which provides feasibility for improving the stability of solar cells and large-area preparation, and is conducive to the commercial development of perovskite solar cells.
[0005] At present, most studies usually choose to add methyl ammonium chloride (MACl) to perovskite to improve the quality of perovskite films and increase the conversion efficiency of perovskite solar cells.
[0006] For example, the Chinese patent CN111009615B of the prior art discloses a method for preparing a high-quality perovskite layer by a methylammonium chloride doping evaporation method, comprising the following steps: A. cleaning to obtain a clean substrate, B. using a thermal evaporator to co-evaporate lead iodide and methylammonium chloride powder onto the substrate to obtain a sample, C. soaking the sample obtained in step B in an isopropanol solvent, D. taking out the sample and placing it on a heating table to heat and evaporate to dryness, E. using a thermal evaporator to evaporate methylammonium iodide onto the sample to obtain a perovskite layer; or dripping a methylammonium iodide solution onto the sample by spin coating and heating to obtain a perovskite layer.
[0007] However, the inventors found that the methylamine cations in the above-mentioned perovskite film are thermally unstable and humidity unstable, which will accelerate the degradation of the perovskite film under actual working conditions, have an adverse effect on the long-term stability of the device, and seriously hinder the commercialization process of perovskite solar cells. Summary of the invention
[0008] In view of the problems existing in the background technology, the purpose of the present invention is to provide a method for preparing a methylamine-free perovskite film by vacuum scraping and a method for preparing a perovskite solar cell.
[0009] The present invention adds a non-volatile solid ligand additive 2-imidazolidone to a perovskite precursor solution to increase the nucleation barrier and delay crystallization, and during the annealing process, the additive disappears in the form of sublimation, thereby preparing a hole-free, high-quality perovskite layer film, and the film is applied to the manufacture of solar cells.
[0010] To achieve the above object, the technical solution of the present invention is as follows:
[0011] A method for preparing a methylamine-free perovskite film by vacuum scraping, comprising the following steps:
[0012] Step 1, preparing a perovskite precursor solution, and adding 2-imidazolidinone to the precursor solution;
[0013] Step 2: In the process of preparing a perovskite solar cell, the perovskite precursor solution prepared in step 1 is dripped between the scraper and the substrate surface, and the perovskite precursor solution is evenly scraped onto the substrate surface by the scraper;
[0014] Step 3, quickly transferring the substrate obtained in step 2 into a vacuum chamber and evacuating the chamber;
[0015] Step 4: annealing the substrate obtained in step 3 to obtain a methylamine-free perovskite film.
[0016] Furthermore, in step 1: the solvent in the perovskite precursor solution is NN-dimethylformamide.
[0017] Furthermore, in the step 2: the scraper evenly scrapes the perovskite precursor solution onto the surface of the substrate at a speed of 5 mm / s.
[0018] Furthermore, in step 3: the vacuum chamber is evacuated to 10 Pa and maintained for 10 seconds.
[0019] Furthermore, in step 4: the annealing temperature is 70-150° C., and the time is 10-60 min.
[0020] The present invention also provides a method for preparing a perovskite solar cell based on the above-mentioned method for preparing a methylamine-free perovskite film by vacuum scraping.
[0021] The specific steps include the following:
[0022] Step (1), preparing a hole transport layer on a conductive substrate;
[0023] Step (2), preparing a methylamine-free perovskite film on the surface of the hole transport layer based on a method for preparing a methylamine-free perovskite film by vacuum coating;
[0024] Step (3), preparing an electron transport layer on the surface of the methylamine-free perovskite film;
[0025] Step (4), preparing a perovskite solar cell by evaporating a back electrode.
[0026] Furthermore, in the step (1), the conductive substrate is selected from FTO glass or ITO glass.
[0027] Furthermore, in step (4), the electrode is a gold electrode or a silver electrode.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The present invention proposes a method for preparing a high-quality methylamine-free perovskite film by vacuum coating, namely, adding a solid additive 2-imidazolidone to a perovskite precursor solution, and delaying crystallization by increasing the nucleation barrier. During annealing, the 2-imidazolidone will slowly evaporate. The finally obtained perovskite film has the advantages of large grain size, density and no holes, thus providing a basis for the preparation of efficient perovskite batteries.
[0030] (2) The perovskite film prepared based on the scalable scraping vacuum technology can be seamlessly connected with the slit coating technology used in actual production, providing process support for the commercial production of perovskite solar cells.
[0031] (3) The preparation method provided by the present invention can be applied in an air environment and has greater commercial application value. In addition, the prepared methylamine-free perovskite film is uniform and of high quality. The solar cell obtained in this way has excellent parameters in all aspects and is more universal than the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 It is a schematic diagram of the preparation process of the methylamine-free perovskite film proposed in the present invention;
[0033] Figure 2 is the surface morphology of the perovskite film prepared in Example 1;
[0034] Figure 3 is a surface morphology image of the perovskite film prepared in Comparative Example 1;
[0035] Figure 4 is a surface morphology image of the perovskite film prepared in Comparative Example 2;
[0036] Figure 5 is a surface morphology image of the perovskite film prepared in Comparative Example 3;
[0037] Figure 6 is a surface morphology image of the perovskite film prepared in Comparative Example 4;
[0038] Figure 7 is a surface morphology image of the perovskite film prepared in Comparative Example 5;
[0039] Figure 8 is a cross-sectional morphology comparison diagram of the perovskite film prepared in Example 1 and Comparative Example 1;
[0040] Fig. 9 It is a comparison of the JV curves and photovoltaic parameter data of the perovskite solar cells prepared in Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0041] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0042] The present invention provides a method for preparing a methylamine-free perovskite film by vacuum coating, which can be found in Figure 1 The preparation process of the methylamine-free perovskite film shown in the figure is as follows: the first step is to use a scraper to scrape the perovskite precursor solution onto the substrate; the second step is to place the substrate in a vacuum chamber and remove the solvent by vacuuming; the third step is to perform high-temperature annealing on the film after the vacuum treatment.
[0043] In detail, the following steps are included:
[0044] Step 1, preparing a perovskite precursor solution, and adding 2-imidazolidinone to the precursor solution;
[0045] Step 2: In the process of preparing a perovskite solar cell, the perovskite precursor solution prepared in step 1 is dripped between the scraper and the substrate surface, and the perovskite precursor solution is evenly scraped onto the substrate surface by the scraper;
[0046] Step 3, quickly transferring the substrate obtained in step 2 into a vacuum chamber and evacuating the chamber;
[0047] Step 4: annealing the substrate obtained in step 3 to obtain a methylamine-free perovskite film.
[0048] Embodiment 1:
[0049] A method for preparing a perovskite solar cell, wherein 2-imidazolidone is added to a perovskite precursor solution, specifically comprising the following steps:
[0050] Step 1: Prepare the substrate
[0051] An ITO glass with a size of 2.5 cm×2.5 cm was selected as the substrate, and the ITO glass was placed in a cleaning rack, and was cleaned with a glass cleaning agent, ultrapure water and anhydrous ethanol in sequence, and finally dried with nitrogen gas for later use.
[0052] Step 2: Prepare the hole transport layer solution
[0053] DMAcPA powder was mixed with ethanol for dilution (to a concentration of 1 mg / mL) and shaken for 20 min to mix them evenly.
[0054] Step 3: Prepare Al2O3 solution
[0055] The Al2O3 stock solution and isopropanol were mixed at a volume ratio of 1:50 and shaken for 20 minutes to mix them evenly.
[0056] Step 4: Prepare PEABr-DMF solution and PEABr-IPA solution
[0057] PEABr powder was mixed with N,N-dimethylformamide (DMF) (prepared at a concentration of 1 mg / mL) and shaken for 20 minutes to obtain a PEABr-DMF solution after mixing evenly.
[0058] PEABr powder was mixed with isopropyl alcohol (IPA) (prepared at a concentration of 1 mg / mL) and shaken for 20 min to obtain a PEABr-IPA solution after mixing evenly.
[0059] Step 5: Prepare the perovskite precursor solution
[0060] According to the molar ratio of lead iodide to iodoformamidine of 1:1, 0.6915 g of lead iodide and 0.2579 g of iodoformamidine were weighed respectively, and then 0.0775 g of a 60% molar ratio of 2-imidazolidinone solid additive was weighed, and they were dissolved together in 1 mL of DMF and shaken for 20 minutes until completely dissolved to obtain a perovskite precursor solution. The concentration of the perovskite precursor solution was 1.5 M.
[0061] Step 6: The ITO glass substrate prepared in step 1 is subjected to UV-ozone treatment for 15 minutes.
[0062] Step 7: Take 80 μL of the DMAcPA solution in step 2 and drop it on the ITO glass surface treated with UV ozone in step 6, and use a coater to spin coat it into a film at 5000 rpm for 30 seconds, and then place it on a hot plate at 100°C for annealing for 10 minutes.
[0063] Step 8: Take 80 μL of the Al2O3 solution in step 3 and add it dropwise onto the ITO glass surface cooled to room temperature in step 7. At this time, the coating speed of the coating machine is 5000 rpm for 30 seconds, and then it is placed on a hot plate at 100°C for annealing for 10 minutes.
[0064] Step 9: Take 80 μL of the PEABr-DMF solution in step 4 and add it dropwise onto the ITO glass surface cooled to room temperature in step 8. At this time, the coating machine speed is 5000 rpm for 30 seconds, and then it is placed on a hot plate at 100°C for annealing for 5 minutes.
[0065] Step 10: Take 20 μL of the perovskite precursor solution in step 5 and drop it between the ITO glass surface cooled to room temperature in step 9 and the scraper. The scraper evenly scrapes the solution on the substrate surface at a speed of 5 mm / s, and then quickly transfers it to the vacuum chamber, evacuates to 10 Pa and maintains for 10 seconds. After the end, annealing is performed at 120°C for 20 minutes to obtain a perovskite film.
[0066] Step 11: Take 80 μL of the PEABr-IPA solution in step 4 and add it dropwise to the ITO glass surface cooled to room temperature in step 10. At this time, the coating speed of the coating machine is 5000 rpm for 30 seconds, and then it is placed on a hot plate at 100°C for annealing for 10 minutes.
[0067] Step 12: Using vacuum evaporation technology, continue to evaporate 30nm of C on the surface of the ITO glass in step 11. 60 .
[0068] Step 13: Using an atomic layer deposition device, continue to deposit 20 nm of SnO2 on the ITO glass surface of step 12.
[0069] Step 14: Using vacuum evaporation technology, continue to evaporate 100nm of metal Ag electrode on the surface of the ITO glass in step 13, and finally prepare a perovskite solar cell.
[0070] Comparative Example 1:
[0071] A method for preparing a perovskite solar cell, wherein no 2-imidazolidinone is added to the perovskite precursor solution, specifically comprising the following steps:
[0072] Step 1: Prepare the substrate
[0073] An ITO glass with a size of 2.5 cm×2.5 cm was selected as the substrate, and the ITO glass was placed in a cleaning rack, and was cleaned with a glass cleaning agent, ultrapure water and anhydrous ethanol in sequence, and finally dried with nitrogen gas for later use.
[0074] Step 2: Prepare the hole transport layer solution
[0075] DMAcPA powder was mixed with ethanol for dilution (to a concentration of 1 mg / mL) and shaken for 20 min to mix them evenly.
[0076] Step 3: Prepare Al2O3 solution
[0077] The Al2O3 stock solution and isopropanol were mixed at a volume ratio of 1:50 and shaken for 20 minutes to mix them evenly.
[0078] Step 4: Prepare PEABr-DMF solution and PEABr-IPA solution
[0079] PEABr powder was mixed with N,N-dimethylformamide (DMF) (prepared at a concentration of 1 mg / mL) and shaken for 20 minutes to obtain a PEABr-DMF solution after mixing evenly.
[0080] PEABr powder was mixed with isopropyl alcohol (IPA) (prepared at a concentration of 1 mg / mL) and shaken for 20 min to obtain a PEABr-IPA solution after mixing evenly.
[0081] Step 5: Prepare the perovskite precursor solution
[0082] According to the molar ratio of lead iodide to iodoformamidine of 1:1, 0.6915 g of lead iodide and 0.2579 g of iodoformamidine were weighed respectively, dissolved together in 1 mL of DMF, and shaken for 20 minutes until completely dissolved to prepare a perovskite precursor solution. The concentration of the perovskite precursor solution was 1.5 M.
[0083] Step 6: The ITO glass substrate prepared in step 1 is subjected to UV-ozone treatment for 15 minutes.
[0084] Step 7: Take 80 μL of the DMAcPA solution in step 2 and drop it on the ITO glass surface treated with UV ozone in step 6, and use a coater to spin coat it into a film at 5000 rpm for 30 seconds, and then place it on a hot plate at 100°C for annealing for 10 minutes.
[0085] Step 8: Take 80 μL of the Al2O3 solution in step 3 and add it dropwise onto the ITO glass surface cooled to room temperature in step 7. At this time, the coating speed of the coating machine is 5000 rpm for 30 seconds, and then it is placed on a hot plate at 100°C for annealing for 10 minutes.
[0086] Step 9: Take 80 μL of the PEABr-DMF solution in step 4 and add it dropwise onto the ITO glass surface cooled to room temperature in step 8. At this time, the coating machine speed is 5000 rpm for 30 seconds, and then it is placed on a hot plate at 100°C for annealing for 5 minutes.
[0087] Step 10: Take 20 μL of the perovskite precursor solution in step 5 and drop it between the ITO glass surface cooled to room temperature in step 9 and the scraper. The scraper evenly scrapes the solution on the substrate surface at a speed of 5 mm / s, and then quickly transfers it to the vacuum chamber, evacuates to 10 Pa and maintains for 10 seconds. After the end, annealing is performed at 120°C for 20 minutes to obtain a perovskite film.
[0088] Step 11: Take 80 μL of the PEABr-IPA solution in step 4 and add it dropwise to the ITO glass surface cooled to room temperature in step 10. At this time, the coating speed of the coating machine is 5000 rpm for 30 seconds, and then it is placed on a hot plate at 100°C for annealing for 10 minutes.
[0089] Step 12: Using vacuum evaporation technology, continue to evaporate 30nm of C on the surface of the ITO glass in step 11. 60 .
[0090] Step 13: Using an atomic layer deposition device, continue to deposit 20 nm of SnO2 on the ITO glass surface of step 12.
[0091] Step 14: Using vacuum evaporation technology, continue to evaporate 100nm of metal Ag electrode on the surface of the ITO glass in step 13, and finally prepare a perovskite solar cell.
[0092] The following are comparative examples 2 to 5. Since the perovskite films finally obtained therefrom have poor performance, no corresponding perovskite solar cell preparation tests were subsequently performed for these comparative examples.
[0093] Comparative Example 2: Dimethyl sulfoxide was added to the perovskite precursor solution, and a FAPbI3 film was prepared by a blade coating vacuum method, which specifically includes the following steps:
[0094] Step 1: Use an ITO glass of 2.5 cm×2.5 cm size as a substrate, put the ITO glass into a cleaning rack, and clean it with glass cleaning agent, ultrapure water and anhydrous ethanol in turn, and finally use nitrogen to blow dry the ITO glass for standby use.
[0095] Step 2: According to the molar ratio of lead iodide to iodoformamidine of 1:1, weigh 0.6915g of lead iodide and 0.2579g of iodoformamidine, and then weigh 60% of dimethyl sulfoxide, dissolve them together in 1mL of DMF, and shake for 20min until completely dissolved to prepare a perovskite precursor solution with a concentration of 1.5M.
[0096] Step 3: Take 20 μL of the perovskite precursor solution in step 2 and drop it between the ITO glass surface cooled to room temperature in step 1 and the scraper. The scraper evenly scrapes the solution on the surface of the substrate at a speed of 5 mm / s, and then quickly transfers it to the vacuum chamber, evacuates to 10 Pa and maintains for 10 seconds. After the end, annealing is performed at 120°C for 20 minutes to obtain a perovskite film.
[0097] Comparative Example 3: N-methylpyrrolidone was added to the perovskite precursor solution, and a FAPbI3 film was prepared by a blade coating vacuum method, which specifically includes the following steps:
[0098] Step 1: Use an ITO glass of 2.5 cm×2.5 cm size as a substrate, put the ITO glass into a cleaning rack, and clean it with glass cleaning agent, ultrapure water and anhydrous ethanol in turn, and finally use nitrogen to blow dry the ITO glass for standby use.
[0099] Step 2: According to the molar ratio of lead iodide to iodoformamidine of 1:1, weigh 0.6915g of lead iodide and 0.2579g of iodoformamidine, and then weigh 60% of N-methylpyrrolidone, dissolve them together in 1mL of DMF, and shake for 20min until completely dissolved to obtain a perovskite precursor solution with a concentration of 1.5M.
[0100] Step 3: Take 20 μL of the perovskite precursor solution in step 2 and drop it between the ITO glass surface cooled to room temperature in step 1 and the scraper. The scraper evenly scrapes the solution on the surface of the substrate at a speed of 5 mm / s, and then quickly transfers it to the vacuum chamber, evacuates to 10 Pa and maintains for 10 seconds. After the end, annealing is performed at 120°C for 20 minutes to obtain a perovskite film.
[0101] Comparative Example 4: 1-methyl-2-imidazolidinone was added to the perovskite precursor solution, and a FAPbI3 film was prepared by a blade coating vacuum method, which specifically includes the following steps:
[0102] Step 1: Use an ITO glass of 2.5 cm×2.5 cm size as a substrate, put the ITO glass into a cleaning rack, and clean it with glass cleaning agent, ultrapure water and anhydrous ethanol in turn, and finally use nitrogen to blow dry the ITO glass for standby use.
[0103] Step 2: According to the molar ratio of lead iodide to iodoformamidine of 1:1, weigh 0.6915g of lead iodide and 0.2579g of iodoformamidine, and then weigh 60% of 1-methyl-2-imidazolidinone, dissolve them together in 1mL of DMF, and shake for 20min until completely dissolved to obtain a perovskite precursor solution with a concentration of 1.5M.
[0104] Step 3: Take 20 μL of the perovskite precursor solution in step 2 and drop it between the ITO glass surface cooled to room temperature in step 1 and the scraper. The scraper evenly scrapes the solution on the surface of the substrate at a speed of 5 mm / s, and then quickly transfers it to the vacuum chamber, evacuates to 10 Pa and maintains for 10 seconds. After the end, annealing is performed at 120°C for 20 minutes to obtain a perovskite film.
[0105] Comparative Example 5: 1,3-dimethyl-2-imidazolidinone was added to the perovskite precursor solution, and a FAPbI3 film was prepared by a blade coating vacuum method, which specifically includes the following steps:
[0106] Step 1: Use an ITO glass of 2.5 cm×2.5 cm size as a substrate, put the ITO glass into a cleaning rack, and clean it with glass cleaning agent, ultrapure water and anhydrous ethanol in turn, and finally use nitrogen to blow dry the ITO glass for standby use.
[0107] Step 2: According to the molar ratio of lead iodide to iodoformamidine of 1:1, weigh 0.6915g of lead iodide and 0.2579g of iodoformamidine, and then weigh 60% of 1,3-dimethyl-2-imidazolidinone, dissolve them together in 1mL of DMF, and shake for 20min until completely dissolved to obtain a perovskite precursor solution with a concentration of 1.5M.
[0108] Step 3: Take 20 μL of the perovskite precursor solution in step 2 and drop it between the ITO glass surface cooled to room temperature in step 1 and the scraper. The scraper evenly scrapes the solution on the surface of the substrate at a speed of 5 mm / s, and then quickly transfers it to the vacuum chamber, evacuates to 10 Pa and maintains for 10 seconds. After the end, annealing is performed at 120°C for 20 minutes to obtain a perovskite film.
[0109] The following is a comparative analysis of the performance tests of the perovskite films and devices of Example 1 and Comparative Example 1; and an analysis of the performance of the perovskite films of Comparative Examples 2 to 5.
[0110] The surface and cross-sectional morphologies of the above-mentioned FAPbI3 light-absorbing layer films were observed using a scanning electron microscope (SEM). The JV test instrument was used to characterize the above-mentioned 0.093 cm 2Photovoltaic properties of FAPbI3 perovskite solar cells.
[0111] 1. Among them, Figure 2 The surface morphology of the perovskite film prepared in Example 1 is shown. Figure 3 Shown is the surface morphology of the perovskite film prepared in Comparative Example 1.
[0112] By comparison Figure 2 and Figure 3 It can be seen that, compared with Example 1 in which 2-imidazolidone is not added to the perovskite precursor solution, the grain size of the perovskite film in Example 1 is larger and denser, without pores, and the surface morphology is relatively better.
[0113] 2. Among them, Figure 4 , Figure 5 , Figure 6 , Figure 7 The surface morphologies of the perovskite films prepared in Comparative Example 2, Comparative Example 3, Comparative Example 4, and Comparative Example 5 are shown respectively.
[0114] from Figures 4 to 7 It can be seen from the above film morphology diagram that the additives added to the perovskite precursor solution, such as dimethyl sulfoxide, N-methylpyrrolidone, 1-dimethyl-2-imidazolidinone or 1,3-dimethyl-2-imidazolidinone, can produce perovskites with smaller grains and poorer surface morphology.
[0115] 3. Among them, Figure 8 A comparison of the cross-sectional morphologies of the perovskite films prepared in Example 1 and Comparative Example 1.
[0116] It can be seen that in Example 1 in which 2-imidazolidone is added to the perovskite precursor solution, compared with Comparative Example 1 in which 2-imidazolidone is not added to the perovskite precursor solution, the perovskite in Example 1 grows perpendicular to the substrate direction and there are no holes on its lower interface.
[0117] Four, Fig. 9 The JV curves and photovoltaic parameter data of the perovskite solar cells prepared in Example 1 of the present invention and Comparative Example 1 are compared.
[0118] It can be seen that in Example 1, in which 2-imidazolidinone is added to the perovskite precursor solution, the open circuit voltage (Voc) is 1120 mV and the short circuit current (Jsc) is 24.85 mA / cm 2, the fill factor (FF) is 83.29%, and the final device energy conversion efficiency (PCE) is 23.14%; while in comparative example 1, in which 2-imidazolidinone is not added to the perovskite precursor solution, the open circuit voltage (Voc) is 0.82mV and the short circuit current (Jsc) is 17.12mA / cm 2 , the fill factor (FF) is 58.18%, and the final device power conversion efficiency (PCE) is 8.24%.
[0119] Therefore, the battery performance of Example 1 in which 2-imidazolidone is added to the perovskite precursor solution is better than the battery performance of Comparative Example 1 in which 2-imidazolidone is not added to the perovskite precursor solution.
[0120] Conclusion: The present invention proposes a process for preparing high-quality methylamine-free perovskite film by scraping vacuum, which abandons the traditional spin coating preparation method and uses the scraping vacuum assisted method to add a solid additive 2-imidazolidinone to the perovskite precursor solution to increase the nucleation barrier and delay crystallization. During the high-temperature annealing process, 2-imidazolidinone disappears in the form of sublimation. The perovskite film prepared based on this reduces the defects on the surface and bulk of the film, and prepares a hole-free, high-quality perovskite layer film, which is beneficial to the transmission of carriers, thereby improving the performance of the device. Finally, an efficient 0.093cm 2 The solar cell device has a simple and easy preparation method, a non-toxic preparation process, is more environmentally friendly, and has greater commercial potential and production universality.
[0121] The above are only some embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.
Claims
1. A method for preparing methylamine-free perovskite thin film by vacuum blade coating, characterized in that: The following steps are involved: Step 1, preparing a perovskite precursor solution, and adding 2-imidazolidinone to the precursor solution; Step 2: In the process of preparing a perovskite solar cell, the perovskite precursor solution prepared in step 1 is dripped between the scraper and the substrate surface, and the perovskite precursor solution is evenly scraped onto the substrate surface by the scraper; Step 3, quickly transferring the substrate obtained in step 2 into a vacuum chamber and evacuating the chamber; Step 4: annealing the substrate obtained in step 3 to obtain a methylamine-free perovskite film.
2. The method for preparing methylamine-free perovskite thin film by vacuum coating according to claim 1, characterized in that: In the step 1: the solvent in the perovskite precursor solution is NN-dimethylformamide.
3. The method for preparing methylamine-free perovskite thin film by vacuum coating according to claim 1, characterized in that: In the step 2: the scraper evenly scrapes the perovskite precursor solution onto the surface of the substrate at a speed of 5 mm / s.
4. The method for preparing methylamine-free perovskite thin film by vacuum coating according to claim 1, characterized in that: In the step 3: the vacuum chamber is evacuated to 10 Pa and maintained for 10 seconds.
5. The method for preparing methylamine-free perovskite thin film by vacuum blade coating according to claim 1, characterized in that: In step 4: the annealing temperature is 70-150° C., and the time is 10-60 min.
6. A method for preparing a perovskite solar cell, characterized in that: The invention comprises the method for preparing methylamine-free perovskite film by vacuum coating as described in any one of claims 1 to 5.
7. The method for preparing a perovskite solar cell according to claim 6, characterized in that: The following steps are involved: Step (1), preparing a hole transport layer on a conductive substrate; Step (2), preparing a methylamine-free perovskite film on the surface of the hole transport layer based on a method for preparing a methylamine-free perovskite film by vacuum coating; Step (3), preparing an electron transport layer on the surface of the methylamine-free perovskite film; Step (4), preparing a perovskite solar cell by evaporating a back electrode.
8. The method for preparing a perovskite solar cell according to claim 7, characterized in that: In the step (1): the conductive substrate is selected from FTO glass or ITO glass.
9. The method for preparing a perovskite solar cell according to claim 7, characterized in that: In the step (4): the electrode is a gold electrode or a silver electrode.