Lens part and laminated film
By adopting a combined structure of a reflective polarizing member, a semi-reflective mirror and a lens part in the VR goggles, the problems of large weight and insufficient visual resolution in the prior art are solved, and lightweight and visual resolution are improved, reducing the Light loss and ghosting phenomena.
Patent Information
- Application Number
- CN202380025208.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-28
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-01
AI Technical Summary
The lens portion of the existing VR goggles has problems such as large weight and insufficient visual resolution, especially in the reflection problem, which is difficult to effectively solve.
The combined structure of reflective polarization member, semi-reflective mirror, lens part and protective member is adopted. Through optical path design and material selection, the polarization and reflection control of light is realized, the reflectivity and diffusion of light is reduced, and the visual resolution is improved.
The lightweight and visual resolution of VR goggles have been achieved, reducing light loss and ghosting phenomena, and significantly improving the display effect.
Smart Images

Figure CN118891564A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a lens portion and a laminated film. Background Art
[0002] Image display devices represented by liquid crystal display devices and electroluminescent (EL) display devices (e.g., organic EL display devices) are rapidly becoming popular. In image display devices, optical components such as polarizing components and phase difference components are generally used to realize image display and improve image display performance (e.g., see Patent Document 1).
[0003] In recent years, new uses for image display devices have been developed. For example, goggles with displays (VR goggles) for realizing Virtual Reality (VR) have begun to be commercialized. There are studies to use VR goggles in various situations, so it is expected to be lightweight and have improved visibility. Lightweighting can be achieved, for example, by thinning the lenses used for VR goggles. On the other hand, it is also expected to develop optical components suitable for display systems using thin lenses. For example, in order to improve visibility, it is expected to have optical components that can solve the reflection problem that occurs in VR goggles.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: (Japanese) Patent Publication No. 2021-103286 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] In view of the above, a main object of the present invention is to provide a lens portion that can achieve weight reduction and improved visibility of VR goggles.
[0009] Technical solutions for solving technical problems
[0010] 1. A lens unit according to an embodiment of the present invention is used in a display system for displaying an image to a user, and comprises: a reflective polarizing member for reflecting light emitted forward from a display surface of a display element for displaying an image and passing through the polarizing member and a first λ / 4 member; a first lens unit arranged on an optical path between the display element and the reflective polarizing member; a half mirror arranged between the display element and the first lens unit, the half mirror transmitting light emitted from the display element and reflecting light reflected by the reflective polarizing member toward the reflective polarizing member; and a second A lens portion, which is arranged in front of the reflective polarizing component; a second λ / 4 component, which is arranged on the optical path between the half-mirror and the reflective polarizing component; and a first protective component and a second protective component, which are arranged on the optical path between the half-mirror and the reflective polarizing component; the first protective component and the second protective component are arranged in a manner of facing each other with a space therebetween; and the maximum value of the 30° normal reflectance spectrum of the first protective component and the second protective component in the wavelength range of 420nm to 680nm is less than 1.4%.
[0011] 2. In the lens unit according to item 1 above, each of the first protective member and the second protective member may have a normal reflectivity of 30° at a wavelength of 450 nm of 0.5% or less.
[0012] 3. In the lens portion according to 1 or 2 above, each of the first protective member and the second protective member may have a normal reflectivity of 30° at a wavelength of 600 nm of 0.5% or less.
[0013] 4. In the lens unit according to any one of 1 to 3 above, each of the first protection member and the second protection member may have a surface smoothness of 0.5 arcmin or less.
[0014] 5. In the lens unit according to any one of 1 to 4 above, the second λ / 4 member may satisfy Re(450)<Re(550).
[0015] 6. The lens unit according to any one of 1 to 5 above may include: a first laminated portion including the second λ / 4 member and the first protective member; and a second laminated portion including the reflective polarizing member and the second protective member.
[0016] 7. In the lens section according to 6 above, the second laminated section may include an absorptive polarizing member disposed between the reflective polarizing member and the second lens section.
[0017] 8. In the lens unit according to 6 or 7 above, the second laminated portion may include a third λ / 4 member disposed between the reflective polarizing member and the second lens unit.
[0018] 9. In the lens unit according to the above 8, the third λ / 4 member may satisfy Re(450)<Re(550).
[0019] 10. The laminated film of an embodiment of the present invention is used in a display method having the following steps: a step of allowing light of a display image emitted via a polarizing member and a first λ / 4 member to pass through a half-mirror and a first lens portion; a step of allowing light passing through the half-mirror and the first lens portion to pass through a second λ / 4 member; a step of allowing light passing through the second λ / 4 member to be reflected toward the half-mirror by a reflective polarizing member; a step of allowing light reflected by the reflective polarizing member and the half-mirror to pass through the second λ / 4 member and transmit through the reflective polarizing member; and a step of allowing light transmitting through the reflective polarizing member to pass through a second lens portion; the laminated film is arranged on an optical path between the half-mirror and the reflective polarizing member and is connected to a space formed between the first lens portion and the second lens portion; and the maximum value of a normal reflectance spectrum of 30° of the laminated film in a wavelength range of 420nm to 680nm is less than 1.4%.
[0020] Effects of the Invention
[0021] According to the lens portion of the embodiment of the present invention, it is possible to reduce the weight of VR goggles and improve visibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram showing a schematic configuration of a display system according to an embodiment of the present invention.
[0023] Figure 2 Yes means Figure 1 A schematic cross-sectional view showing an example of details of a lens unit of the display system.
[0024] Figure 3 This is a schematic cross-sectional view showing a schematic structure of a laminated film according to one embodiment of the present invention.
[0025] Figure 4 This is a schematic perspective view showing an example of a multilayer structure included in a reflective polarizing film.
[0026] Figure 5 This is a graph showing the 30° normal reflectance spectra of the laminated films of Example 1, Comparative Example 1, and Comparative Example 2.
[0027] Figure 6 In the drawings, (a), (b), and (c) are photographs showing the results of appearance evaluation.
[0028] Figure 7 In the drawings, (a), (b), (c), and (d) are photographs showing the results of appearance evaluation. DETAILED DESCRIPTION
[0029] The following describes the embodiments of the present invention with reference to the accompanying drawings, but the present invention is not limited to the embodiments. In order to more clearly describe the drawings, the width, thickness, shape, etc. of each part are schematically shown compared to the embodiments, but this is only an example and is not used to limit the interpretation of the present invention. In addition, with respect to the drawings, the same or equivalent elements are sometimes given the same reference numerals, and repeated descriptions are omitted.
[0030] (Definition of Terms and Symbols)
[0031] The definitions of terms and symbols in this specification are as follows.
[0032] (1) Refractive index (nx, ny, nz)
[0033] "nx" is the refractive index in the direction where the in-plane refractive index is maximum (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis (ie, the fast axis direction) in the plane, and "nz" is the refractive index in the thickness direction.
[0034] (2) In-plane phase difference (Re)
[0035] "Re(λ)" is the in-plane phase difference measured at 23°C with light of wavelength λnm. For example, "Re(550)" is the in-plane phase difference measured at 23°C with light of wavelength 550nm. Re(λ) is calculated by the formula: Re(λ) = (nx-ny) × d when the thickness of the layer (thin film) is d (nm).
[0036] (3) Retardation in the thickness direction (Rth)
[0037] "Rth(λ)" is the phase difference in the thickness direction measured at 23°C with light of wavelength λnm. For example, "Rth(550)" is the phase difference in the thickness direction measured at 23°C with light of wavelength 550nm. Rth(λ) is calculated using the formula: Rth(λ) = (nx-nz) × d when the thickness of the layer (film) is d (nm).
[0038] (4) Nz coefficient
[0039] The Nz coefficient is obtained by Nz=Rth / Re.
[0040] (5) Angle
[0041] When an angle is mentioned in this specification, unless otherwise specified, the angle includes both clockwise and counterclockwise directions relative to a reference direction. Therefore, for example, "45°" means ±45°.
[0042] Figure 1This is a schematic diagram showing a schematic configuration of a display system according to an embodiment of the present invention. Figure 1 , the arrangement and shape of each component of the display system 2 are schematically illustrated. The display system 2 includes: a display element 12, a reflective polarizing member 14, a first lens unit 16, a half mirror 18, a first phase difference member 20, a second phase difference member 22, and a second lens unit 24. The reflective polarizing member 14 is arranged on the display surface 12a side of the display element 12, that is, in front, and can reflect the light emitted from the display element 12. The first lens unit 16 is arranged on the optical path between the display element 12 and the reflective polarizing member 14, and the half mirror 18 is arranged between the display element 12 and the first lens unit 16. The first phase difference member 20 is arranged on the optical path between the display element 12 and the half mirror 18, and the second phase difference member 22 is arranged on the optical path between the half mirror 18 and the reflective polarizing member 14.
[0043] The components arranged forward from the half mirror (in the example of the figure, the half mirror 18, the first lens unit 16, the second phase difference member 22, the reflective polarizing member 14 and the second lens unit 24) are sometimes collectively referred to as a lens unit (lens unit 4).
[0044] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12a for displaying images. Light emitted from the display surface 12a passes through a polarizing member (typically a polarizing film) that the display element 12 may include, and then is emitted to become first linearly polarized light.
[0045] The first phase difference member 20 includes a first λ / 4 member, which can convert the first linear polarization incident on the first phase difference member 20 into a first circular polarization. When the first phase difference member does not include a member other than the first λ / 4 member, the first phase difference member is equivalent to the first λ / 4 member. The first phase difference member 20 can also be provided on the display element 12 as a whole.
[0046] The half mirror 18 transmits the light emitted from the display element 12, and reflects the light reflected by the reflective polarizing member 14 toward the reflective polarizing member 14. The half mirror 18 is provided integrally with the first lens portion 16.
[0047] The second phase difference member 22 includes a second λ / 4 member, which allows the light reflected by the reflective polarizing member 14 and the half mirror 18 to pass through the reflective polarizing member 14. When the second phase difference member does not include a member other than the second λ / 4 member, the second phase difference member is equivalent to the second λ / 4 member. The second phase difference member 22 may also be provided on the first lens portion 16 as a whole.
[0048] The first circularly polarized light emitted from the first λ / 4 member included in the first phase difference member 20 passes through the half mirror 18 and the first lens unit 16, and is converted into the second linearly polarized light by the second λ / 4 member included in the second phase difference member 22. The second linearly polarized light emitted from the second λ / 4 member does not pass through the reflective polarizing member 14 but is reflected toward the half mirror 18. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing member 14 is the same direction as the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14.
[0049] The second linear polarization reflected by the reflective polarization member 14 is converted into a second circular polarization by the second λ / 4 member included in the second phase difference member 22, and the second circular polarization emitted from the second λ / 4 member is reflected by the half mirror 18 through the first lens unit 16. The second circular polarization reflected by the half mirror 18 passes through the first lens unit 16 and is converted into a third linear polarization by the second λ / 4 member included in the second phase difference member 22. The third linear polarization is transmitted through the reflective polarization member 14. At this time, the polarization direction of the third linear polarization incident on the reflective polarization member 14 is in the same direction as the transmission axis of the reflective polarization member 14. Therefore, the third linear polarization incident on the reflective polarization member 14 is transmitted through the reflective polarization member 14.
[0050] The light from the transflective polarizing element 14 passes through the second lens portion 24 and enters the eye 26 of the user.
[0051] For example, the absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 may be arranged to be substantially parallel to each other, or may be arranged to be substantially orthogonal. The angle formed by the absorption axis of the polarizing member included in the display element 12 and the slow axis of the first λ / 4 member included in the first phase difference member 20 is, for example, 40° to 50°, 42° to 48°, or approximately 45°. The angle formed by the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second λ / 4 member included in the second phase difference member 22 is, for example, 40° to 50°, 42° to 48°, or approximately 45°.
[0052] The in-plane phase difference Re(550) of the first λ / 4 component is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The Re(450) / Re(550) of the first λ / 4 component is, for example, not less than 0.75 and less than 1, or not less than 0.8 and not more than 0.95.
[0053] The in-plane phase difference Re(550) of the second λ / 4 component is, for example, 100 nm to 190 nm, 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The second λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. The Re(450) / Re(550) of the second λ / 4 component is, for example, not less than 0.75 and less than 1, or not less than 0.8 and not more than 0.95.
[0054] In the lens portion 4, a space may be formed between the first lens portion 16 and the second lens portion 24. At this time, the component arranged between the first lens portion 16 and the second lens portion 24 is preferably provided on either the first lens portion 16 or the second lens portion 24 to form an integral body. For example, it is preferred that the component arranged between the first lens portion 16 and the second lens portion 24 is provided on either the first lens portion 16 or the second lens portion 24 via an adhesive layer to form an integral body. According to the described form, for example, the handling properties of each component can be excellent. The adhesive layer can be formed by an adhesive or an adhesive. Specifically, the adhesive layer can be an adhesive layer or an adhesive layer. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm.
[0055] Figure 2 Yes means Figure 1 Schematic cross-sectional view of an example of the details of the lens portion of the display system shown. Specifically, Figure 2 The lens unit 4 includes a first lens unit 16 , a first laminated unit 100 disposed adjacent to the first lens unit 16 , a second lens unit 24 , and a second laminated unit 200 disposed adjacent to the second lens unit 24 . Figure 2 In the example shown, the first build-up portion 100 and the second build-up portion 200 are arranged separately. Although not shown, the half mirror may be provided on the first lens portion 16 so as to be integrated therewith.
[0056] The first laminated part 100 includes a second phase difference member 22, and an adhesive layer (e.g., adhesive layer) 41 disposed between the first lens portion 16 and the second phase difference member 22, and is integrally provided on the first lens portion 16 through the adhesive layer 41. The first laminated part 100 further includes a first protective member 31 disposed in front of the second phase difference member 22. The first protective member 31 is laminated on the second phase difference member 22 via an adhesive layer (e.g., adhesive layer) 42. The first protective member 31 may be located on the outermost surface of the first laminated part 100.
[0057] Figure 2In the example shown, the second phase difference component 22 includes a component (so-called positive C plate) 22b whose refractive index characteristic can show the relationship of nz>nx=ny in addition to the second λ / 4 component 22a. The second phase difference component 22 has a laminated structure of the second λ / 4 component 22a and the positive C plate 22b. By using the positive C plate, light leakage (for example, oblique light leakage) can be prevented. Figure 2 As shown, in the second phase difference member 22, the second λ / 4 member 22a is preferably located in front of the positive C plate 22b. The second λ / 4 member 22a and the positive C plate 22b are laminated via an adhesive layer (not shown), for example.
[0058] The second λ / 4 component preferably has a refractive index characteristic showing a relationship of nx>ny≥nz. Here, "ny=nz" includes not only the case where ny and nz are completely the same, but also the case where they are substantially the same. Therefore, there may be a case where ny<nz within a range that does not impair the effect of the present invention. The Nz coefficient of the second λ / 4 component is preferably 0.9 to 3, more preferably 0.9 to 2.5, more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0060] The second λ / 4 member is formed of any appropriate material that can satisfy the above characteristics. The second λ / 4 member can be, for example, a stretched film of a resin film or an oriented solidified layer of a liquid crystal compound.
[0061] The resin contained in the above-mentioned resin film can be listed as follows: polycarbonate resin, polyester carbonate resin, polyester resin, polyvinyl acetal resin, polyarylate resin, cyclic olefin resin, cellulose resin, polyvinyl alcohol resin, polyamide resin, polyimide resin, polyether resin, polystyrene resin, acrylic resin, etc. These resins can be used alone or in combination. The combination method can be, for example, blending and copolymerization. When the second λ / 4 component exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate resin or a polyester carbonate resin (hereinafter sometimes simply referred to as a polycarbonate resin) can be preferably used.
[0062] Any appropriate polycarbonate resin can be used for the above-mentioned polycarbonate resin. For example, the polycarbonate resin includes: a structural unit derived from a fluorene dihydroxy compound; a structural unit derived from an isosorbide dihydroxy compound; and a structural unit derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanols, di-, tri- or polyethylene glycols, and alkylene glycols or spiroglycerol. The polycarbonate resin preferably includes: a structural unit derived from a fluorene dihydroxy compound; a structural unit derived from an isosorbide dihydroxy compound; a structural unit derived from alicyclic dimethanol; and / or a structural unit derived from di-, tri- or polyethylene glycol; more preferably includes: a structural unit derived from a fluorene dihydroxy compound; a structural unit derived from an isosorbide dihydroxy compound; and a structural unit derived from di-, tri- or polyethylene glycol. The polycarbonate resin may also include structural units derived from other dihydroxy compounds as needed. In addition, the details of the polycarbonate-based resin that can be preferably used for the second λ / 4 component and the method for forming the second λ / 4 component are recorded in, for example, (Japan) Patent Gazette No. 2014-10291, (Japan) Patent Gazette No. 2014-26266, (Japan) Patent Gazette No. 2015-212816, (Japan) Patent Gazette No. 2015-212817, and (Japan) Patent Gazette No. 2015-212818, and this specification cites the records of these gazettes as reference.
[0063] The thickness of the second λ / 4 member formed of a stretched film of a resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.
[0064] The oriented solidified layer of the liquid crystal compound is a layer in which the liquid crystal compound is oriented in a predetermined direction within the layer and its oriented state is fixed. In addition, the concept of "oriented solidified layer" includes an oriented hardened layer obtained by hardening the liquid crystal monomer as described later. For the second λ / 4 member, it represents that the upper rod-shaped liquid crystal compound is oriented (oriented along the surface) in a state of being arranged along the slow axis direction of the second λ / 4 member. Examples of the rod-shaped liquid crystal compound include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the liquid crystal compound can be polymerized after being oriented, thereby fixing the oriented state of the liquid crystal compound.
[0065] The above-mentioned oriented solidified layer of liquid crystal compound (liquid crystal oriented solidified layer) can be formed by the following method: subjecting the surface of a predetermined substrate to an oriented treatment, and applying a coating liquid containing a liquid crystal compound to the surface, so that the liquid crystal compound is oriented in the direction corresponding to the above-mentioned oriented treatment, and fixing the oriented state. Any appropriate oriented treatment can be used for the oriented treatment. Specifically, mechanical oriented treatment, physical oriented treatment, and chemical oriented treatment can be mentioned. Specific examples of mechanical oriented treatment include friction treatment and stretching treatment. Specific examples of physical oriented treatment include magnetic field oriented treatment and electric field oriented treatment. Specific examples of chemical oriented treatment include oblique evaporation method and optical oriented treatment. The processing conditions of various oriented treatments can adopt any appropriate conditions according to the purpose.
[0066] The liquid crystal compound can be oriented by treating it at a temperature that can exhibit a liquid crystal phase according to the type of the liquid crystal compound. The liquid crystal compound changes into a liquid crystal state by the temperature treatment, and the liquid crystal compound is oriented according to the orientation treatment direction of the substrate surface.
[0067] In one embodiment, the alignment state is fixed by cooling the aligned liquid crystal compound. When the liquid crystal compound is polymerizable or cross-linkable, the alignment state is fixed by subjecting the aligned liquid crystal compound to a polymerization treatment or a cross-linking treatment.
[0068] The above-mentioned liquid crystal compound can use any appropriate liquid crystal polymer and / or liquid crystal monomer. Liquid crystal polymer and liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for preparing liquid crystal directional solidification layers are described in, for example, (Japan) Patent Publication No. 2006-163343, (Japan) Patent Publication No. 2006-178389, and International Publication No. 2018 / 123551. This specification refers to the records of these publications as reference.
[0069] The thickness of the second λ / 4 member formed of a liquid crystal alignment solidification layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and further preferably 1 μm to 4 μm.
[0070] The thickness direction phase difference Rth(550) of the positive C plate is preferably -50nm to -300nm, more preferably -70nm to -250nm, more preferably -90nm to -200nm, and particularly preferably -100nm to -180nm. Here, "ny=nz" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane phase difference Re(550) of the positive C plate is, for example, less than 10nm.
[0071] The positive C plate can be formed of any appropriate material, and the positive C plate is preferably composed of a film containing a liquid crystal material fixed in a homeotropic orientation. The liquid crystal material (liquid crystal compound) that can achieve homeotropic orientation can be a liquid crystal monomer or a liquid crystal polymer. Specific examples of the formation method of the liquid crystal compound and the positive C plate include the liquid crystal compound and the formation method of the phase difference layer described in paragraphs
[0020] to
[0028] of the (Japanese) Patent Gazette No. 2002-333642. At this time, the thickness of the positive C plate is preferably 0.5μm to 5μm.
[0072] The first protective member may be a laminated film having a substrate and a surface treatment layer. The first protective member having a surface treatment layer may be arranged such that the surface treatment layer is located at the front side. Specifically, the surface treatment layer may be located at the outermost surface of the first laminated portion.
[0073] The maximum value of the 30° normal reflectance spectrum of the first protective component in the wavelength range of 420nm to 680nm is greater than 0% and less than 1.4%, preferably less than 1.2%, and more preferably less than 1.0%. By locating the protective component having the above-mentioned reflective characteristics on the outermost surface of the laminated portion, the visibility can be significantly improved. Specifically, by satisfying the above-mentioned reflective characteristics in the protective component connected to the space formed between the first lens portion 16 and the second lens portion 24, the light loss caused by reflection at the interface between the air and the protective component can be extremely well suppressed. Specifically, light will diffuse in the display system 2, and the diffused light may be incident on the protective component from an oblique direction. The light loss can be extremely well suppressed. In the display system 2 using a large number of components, the amount of light required is large, so that the effect of suppressing light loss can be significantly obtained. As mentioned above, Figure 1 In the display system 2 shown, light can pass three times through the member disposed between the half mirror 18 and the reflective polarizing member 14, so that the effect of suppressing light loss can be significantly obtained. In addition, by satisfying the above-mentioned reflection characteristics of the protective member, it is possible to suppress the visual perception of ghosts due to reflection.
[0074] As mentioned above, when the amount of light used is large, hue management is important. For example, the balance of reflectance in the visible light region is important. The normal reflectance of the first protective member at a wavelength of 450nm at 30° is, for example, 0.01% or more and 0.6% or less, preferably 0.5% or less, more preferably 0.4% or less, and more preferably 0.3% or less. The normal reflectance of the first protective member at a wavelength of 600nm at 30° is, for example, 0.01% or more and 0.6% or less, preferably 0.5% or less, more preferably 0.4% or less, and more preferably 0.3% or less.
[0075] The 30° normal reflectivity spectrum of the first protective member in the wavelength range of 420nm to 680nm may also have a minimum value in the wavelength range of 430nm to 470nm and in the wavelength range of 550nm to 590nm. For example, the ratio of the average value Ave (430-470nm) of the 30° normal reflectivity in the wavelength range of 430nm to 470nm to the average value Ave (480-510nm) of the 30° normal reflectivity in the wavelength range of 480nm to 510nm is preferably 0.10 or more and less than 1.0, and may also be 0.80 or less. Moreover, the ratio of the average value Ave (580-620nm) of the 30° normal reflectivity in the wavelength range of 580nm to 620nm to the average value Ave (480-510nm) of the 30° normal reflectivity in the wavelength range of 480nm to 510nm is preferably 0.10 or more and less than 1.0, and may also be 0.80 or less. The average value of the 30° normal reflectance can be obtained, for example, by sampling measured values at 5 nm intervals in each wavelength range and dividing the total by the number of the selected wavelengths.
[0076] The surface smoothness of the first protective member is preferably less than 0.5 arcmin, more preferably less than 0.4 arcmin. By using a protective member that satisfies the above smoothness, the occurrence of stray light can be suppressed, and the image can be suppressed from becoming unclear. In fact, the surface smoothness of the first protective member is, for example, greater than 0.1 arcmin. The thickness of the first protective member is preferably 10 μm to 80 μm, more preferably 15 μm to 60 μm, and more preferably 20 μm to 45 μm.
[0077] Figure 3 Schematic cross-sectional view showing the schematic structure of a laminated film according to one embodiment of the present invention. The laminated film 34 has a substrate 36 and a surface treatment layer 38 disposed above the substrate 36. The thickness of the substrate 36 is preferably 5 μm to 80 μm, more preferably 10 μm to 50 μm, and more preferably 15 μm to 40 μm. The surface smoothness of the substrate 36 is preferably 0.7 arcmin or less, more preferably 0.6 arcmin or less, and more preferably 0.5 arcmin or less. In addition, the surface smoothness can be measured by focusing the irradiated light on the surface of the object.
[0078] The substrate 36 can be made of any appropriate film. The material of the main component of the film constituting the substrate 36 can be listed, for example: cellulose resins such as triacetyl cellulose (TAC), polyester resins, polyvinyl alcohol resins, polycarbonate resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polynorbornene resins and other cycloolefin resins, polyolefin resins, (meth) acrylic resins and acetate resins. Here, (meth) acrylic acid means acrylic acid and / or methacrylic acid. In one embodiment, the substrate 36 is preferably made of (meth) acrylic resin. By adopting (meth) acrylic resin, the above-mentioned surface smoothness can be well satisfied. Specifically, by adopting (meth) acrylic resin, a substrate with excellent surface smoothness can be formed by extrusion molding.
[0079] The thickness of the surface treatment layer 38 is preferably 0.5 μm to 10 μm, more preferably 1 μm to 7 μm, and even more preferably 2 μm to 5 μm. The surface treatment layer 38 includes, for example, a hard coating layer 38 a and a functional layer 38 b having an anti-reflection function.
[0080] The hard coating layer 38a is typically formed by coating a hard coating forming material on the substrate 36 and curing the coating layer. The hard coating forming material typically includes a curable compound as a layer forming component. The curing mechanism of the curable compound can be, for example, a thermal curing type and a light curing type. The curable compound can be, for example, a monomer, an oligomer, and a prepolymer. Preferably, a multifunctional monomer or oligomer can be used as the curable compound. The multifunctional monomer or oligomer can be, for example, a monomer or oligomer having two or more (meth)acryloyl groups, a urethane (meth)acrylate or an oligomer of a urethane (meth)acrylate, an epoxy-based monomer or oligomer, and a polysilicone-based monomer or oligomer.
[0081] The thickness of the hard coating layer 38 a is preferably 0.5 μm to 10 μm, more preferably 1 μm to 7 μm, and further preferably 2 μm to 5 μm.
[0082] The functional layer 38b preferably has a laminated structure including a high refractive index layer and a low refractive index layer. The functional layer 38b preferably has a high refractive index layer and a low refractive index layer in this order from the substrate 36 side. By having such a laminated structure, the above-mentioned reflection characteristics can be satisfactorily satisfied.
[0083] For example, the high refractive index layer may be formed by a high refractive index resin (e.g., a refractive index of 1.55 or more measured at a wavelength of 550 nm). In this case, the high refractive index layer may be a coating layer. In another example, the high refractive index layer may be formed by an inorganic film. In this case, the high refractive index layer may be formed by physical evaporation such as vacuum evaporation or sputtering, or chemical evaporation.
[0084] The thickness of the high refractive index layer is preferably 10 nm to 200 nm, more preferably 20 nm to 150 nm.
[0085] The thickness of the low refractive index layer is preferably 10 nm to 200 nm, more preferably 20 nm to 150 nm.
[0086] The low refractive index layer (anti-reflection layer) can be obtained, for example, by applying a coating liquid for forming a low refractive index layer (anti-reflection layer) and drying the resulting coating to harden the coating film. The coating liquid for forming an anti-reflection layer can also contain, for example, a resin component (hardening compound), a fluorine-containing additive, hollow particles, solid particles, and a solvent, and can be obtained by mixing these, for example.
[0087] The curing mechanism of the resin component (curable compound) contained in the coating solution for forming the anti-reflection layer can be, for example, a heat-curing type or a light-curing type. The resin component can use, for example, a curable compound having at least one of an acrylate group and a methacrylate group, such as a polysilicone resin, a polyester resin, a polyether resin, an epoxy resin, a urethane resin, an alkyd resin, a spiroacetal resin, a polybutadiene resin, a polythiol polyene resin, an oligomer or prepolymer such as an acrylate or methacrylate of a multifunctional compound such as a polyol, etc. These can be used alone or in combination of two or more.
[0088] Reactive diluents having at least one of an acrylate group and a methacrylate group may also be used in the above-mentioned resin component. Reactive diluents may be, for example, reactive diluents described in (Japan) Patent Gazette No. 2008-88309, for example, monofunctional acrylates, monofunctional methacrylates, multifunctional acrylates, multifunctional methacrylates, etc. From the viewpoint of obtaining excellent hardness, reactive diluents may preferably use acrylates having three or more functions and methacrylates having three or more functions. Reactive diluents may also include, for example, butanediol glycerol ether diacrylate, acrylates of isocyanuric acid, methacrylates of isocyanuric acid, etc. These may be used alone or in combination of two or more. For the hardening of the above-mentioned resin component, for example, a hardener may also be used. For example, a known polymerization initiator (for example, a thermal polymerization initiator, a photopolymerization initiator, etc.) may be used as a hardener.
[0089] The above-mentioned fluorine-containing additive may be, for example, a fluorine-containing organic compound or a fluorine-containing inorganic compound. Examples of the fluorine-containing organic compound include fluorine-containing antifouling coating agents, fluorine-containing acrylic compounds, and fluorine-containing and silicon-containing acrylic compounds. Commercially available fluorine-containing organic compounds may be used. Specific examples of commercially available products include the trade name "KY-1203" manufactured by Shin-Etsu Chemical Co., Ltd. and the trade name "MEGAFACE" manufactured by DIC Co., Ltd. Relative to 100 parts by weight of the above-mentioned resin component, the content of the fluorine-containing additive may be, for example, 0.05 parts by weight or more, 0.1 parts by weight or more, 0.15 parts by weight or more, 0.20 parts by weight or more, or 0.25 parts by weight or more, and may be less than 20 parts by weight, less than 15 parts by weight, less than 10 parts by weight, less than 5 parts by weight, or less than 3 parts by weight.
[0090] The hollow particles may be, for example, silica particles, acrylic particles, and acrylic-styrene copolymer particles. Commercially available hollow silica particles may be used (e.g., trade names "THRULYA5320" and "THRULYA4320" manufactured by JGC Catalysts & Chemicals Co., Ltd.). The weight average particle size of the hollow particles may be, for example, greater than 30 nm, greater than 40 nm, greater than 50 nm, greater than 60 nm, or greater than 70 nm, or less than 150 nm, less than 140 nm, less than 130 nm, less than 120 nm, or less than 110 nm. The shape of the hollow particles is not particularly limited, and is preferably roughly spherical. Specifically, the aspect ratio of the hollow particles is preferably less than 1.5. Relative to 100 parts by weight of the above-mentioned resin component, the content of the hollow particles can be, for example, more than 30 parts by weight, more than 50 parts by weight, more than 70 parts by weight, more than 90 parts by weight or more than 100 parts by weight, or less than 300 parts by weight, less than 270 parts by weight, less than 250 parts by weight, less than 200 parts by weight or less than 180 parts by weight.
[0091] The solid particles may be, for example, silicon oxide particles, zirconium oxide particles, and titanium oxide particles. Solid silicon oxide particles may be commercially available (e.g., trade names "MEK-2140Z-AC", "MIBK-ST", "IPA-ST" manufactured by Nissan Chemical Industries, Ltd.). The weight average particle size of the solid particles may be, for example, 5 nm or more, 10 nm or more, 15 nm or more, 20 nm or more, or 25 nm or more, and may be 330 nm or less, 250 nm or less, 200 nm or less, 150 nm or less, or 100 nm or less. The shape of the hollow particles is not particularly limited, and is preferably roughly spherical. Specifically, the aspect ratio of the hollow particles is preferably 1.5 or less. Relative to 100 parts by weight of the above-mentioned resin component, the content of the solid particles may be, for example, 5 parts by weight or more, 10 parts by weight or more, 15 parts by weight or more, 20 parts by weight or more, or 25 parts by weight or more, or may be 150 parts by weight or less, 120 parts by weight or less, 100 parts by weight or less, or 80 parts by weight or less.
[0092] Any appropriate solvent can be used for the above-mentioned solvent. Examples of the solvent include alcohols such as methanol, ethanol, isopropanol, butanol, TBA (tertiary butanol), and 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, MIBK (methyl isobutyl ketone), and cyclopentanone; esters such as methyl acetate, ethyl acetate, butyl acetate, and PMA (propylene glycol monomethyl ether acetate); ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellulosides such as ethyl cellulosides and butyl cellulosides; aliphatic hydrocarbons such as hexane, heptane, and octane; and aromatic hydrocarbons such as benzene, toluene, and xylene. These can be used alone or in combination of two or more. Regarding the content of the solvent, for example, the weight of the solid component can be set to, for example, 0.1% by weight or more, 0.3% by weight or more, 0.5% by weight or more, 1.0% by weight or more, or 1.5% by weight or less, relative to the total weight of the above-mentioned anti-reflection layer forming coating liquid. It can also be set to the weight of the solid component to be 20% by weight or less, 15% by weight or less, 10% by weight or less, 5% by weight or less, or 3% by weight or less.
[0093] The coating method of the anti-reflection layer forming coating liquid can use a known coating method such as a jet coating method, a die coating method, a spin coating method, a spray coating method, a gravure coating method, a roller coating method, a rod coating method, etc. The drying temperature of the above-mentioned coating film is, for example, 30°C to 200°C, and the drying time is, for example, 30 seconds to 90 seconds. The curing of the above-mentioned coating film can be carried out, for example, by heating or light irradiation (typically, ultraviolet irradiation). The light source of the light irradiation can be, for example, a high-pressure mercury lamp. The irradiation amount of ultraviolet irradiation is preferably 50mJ / cm in terms of the cumulative exposure amount at an ultraviolet wavelength of 365nm. 2 ~500mJ / cm 2 .
[0094] The second lamination section 200 includes a reflective polarizing member 14 and an adhesive layer (e.g., an adhesive layer) disposed between the reflective polarizing member 14 and the second lens portion 24. For example, from the perspective of improving visibility, the second lamination section 200 further includes an absorptive polarizing member 28 disposed between the reflective polarizing member 14 and the second lens portion 24. The absorptive polarizing member 28 is laminated in front of the reflective polarizing member 14 via an adhesive layer (e.g., an adhesive layer) 44. The reflection axis of the reflective polarizing member 14 and the absorption axis of the absorptive polarizing member 28 can be disposed substantially parallel to each other, and the transmission axis of the reflective polarizing member 14 and the transmission axis of the absorptive polarizing member 28 can be disposed substantially parallel to each other. By laminating via the adhesive layer, the reflective polarizing member 14 and the absorptive polarizing member 28 are fixed, and the axis arrangement deviation of the reflection axis and the absorption axis (transmission axis and transmission axis) can be prevented. Furthermore, it is possible to suppress adverse effects caused by an air layer that may be formed between the reflective polarizing member 14 and the absorptive polarizing member 28 .
[0095] The second laminated part 200 further includes a second protective member 32 disposed behind the reflective polarizing member 14. The second protective member 32 is laminated on the reflective polarizing member 14 via an adhesive layer (e.g., an adhesive layer) 43. The second protective member 32 may be located on the outermost surface of the second laminated part 200. The first protective member 31 and the second protective member 32 are disposed in a manner facing each other with a space therebetween. Like the first protective member described above, the second protective member may be a laminated film having a substrate and a surface treatment layer. In this case, the surface treatment layer may be located on the outermost surface of the second laminated part. The same description as that of the first protective member described above may be applied to the details of the second protective member. Specifically, the same description as that of the first protective member described above may be applied to the reflective characteristics and effects, smoothness, composition, thickness, and constituent materials of the second protective member.
[0096] exist Figure 2 In the example shown, the second laminated portion 200 further includes a third phase difference member 30 disposed between the absorption type polarizing member 28 and the second lens portion 24. The third phase difference member 30 is laminated on the absorption type polarizing member 28 via an adhesive layer (e.g., an adhesive layer) 45. In addition, the third phase difference member 30 is laminated on the second lens portion 24 via an adhesive layer (e.g., an adhesive layer) 46, and the second laminated portion 200 is provided on the second lens portion 24 to form a single body. The third phase difference member 30 includes, for example, a third λ / 4 member. The angle formed by the absorption axis of the absorption type polarizing member 28 and the slow axis of the third λ / 4 member included in the third phase difference member 30 is, for example, 40° to 50°, 42° to 48°, or about 45°. By providing the above member, for example, reflection of external light from the second lens portion 16 side can be prevented. When the third phase difference member does not include a member other than the third λ / 4 member, the third phase difference member is equivalent to the third λ / 4 member.
[0097] The above-mentioned reflective polarizing member can transmit polarized light (typically linear polarized light) parallel to its transmission axis while maintaining its polarized state, and reflect light in other polarized states. The reflective polarizing member is typically composed of a film having a multilayer structure (sometimes referred to as a reflective polarizing film). In this case, the thickness of the reflective polarizing member is, for example, 10 μm to 150 μm, preferably 20 μm to 100 μm, and more preferably 30 μm to 60 μm.
[0098] Figure 4 It is a schematic stereogram showing an example of a multilayer structure contained in a reflective polarizing film. The multilayer structure 14a alternately has a layer A having birefringence and a layer B having substantially no birefringence. The total number of layers constituting the multilayer structure may also be 50 to 1000. For example, the refractive index nx of layer A in the x-axis direction is greater than the refractive index ny in the y-axis direction, while the refractive index nx of layer B in the x-axis direction is substantially the same as the refractive index ny in the y-axis direction; the refractive index difference between layer A and layer B is large in the x-axis direction, and is substantially zero in the y-axis direction. As a result, the x-axis direction becomes the reflection axis, and the y-axis direction becomes the transmission axis. The refractive index difference between layer A and layer B in the x-axis direction is preferably 0.2 to 0.3.
[0099] The above-mentioned A layer is typically composed of a material that exhibits birefringence by stretching. Examples of the material include naphthalene dicarboxylic acid polyesters (e.g., polyethylene naphthalate), polycarbonate, and acrylic resins (e.g., polymethyl methacrylate). The above-mentioned B layer is typically composed of a material that does not substantially exhibit birefringence even when stretched. Examples of the material include, for example, copolyesters of naphthalene dicarboxylic acid and terephthalic acid. The above-mentioned multilayer structure can be formed by combining coextrusion and stretching. For example, after the material constituting the A layer and the material constituting the B layer are extruded, they are multilayered (e.g., using a multiplier). Then, the obtained multilayer laminate is stretched. The x-axis direction of the diagram example can correspond to the stretching direction.
[0100] Examples of commercially available reflective polarizing films include "DBEF" and "APF" manufactured by 3M Co., Ltd. and "APCF" manufactured by Nitto Denko Corporation.
[0101] The orthogonal transmittance (Tc) of the reflective polarizing member (reflective polarizing film) can be, for example, 0.01% to 3%. The single transmittance (Ts) of the reflective polarizing member (reflective polarizing film) can be, for example, 43% to 49%, preferably 45% to 47%. The polarization degree (P) of the reflective polarizing member (reflective polarizing film) can be, for example, 92% to 99.99%.
[0102] The above-mentioned orthogonal transmittance, single transmittance and polarization degree can be measured, for example, using an ultraviolet visible light spectrophotometer. The polarization degree P can be measured using an ultraviolet visible light spectrophotometer to measure the single transmittance Ts, parallel transmittance Tp and orthogonal transmittance Tc, and the obtained Tp and Tc can be calculated using the following formula. In addition, Ts, Tp and Tc are measured with a 2-degree field of view (C light source) of JIS Z 8701 and the Y value after the visual sensitivity correction.
[0103] Polarization degree P (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100
[0104] The absorption type polarizing member may include a resin film containing a dichroic substance (sometimes referred to as an absorption type polarizing film). The thickness of the absorption type polarizing film is, for example, 1 μm to 20 μm, 2 μm to 15 μm, 12 μm to 10 μm, 8 μm to 8 μm, or 5 μm to 5 μm.
[0105] The above-mentioned absorption-type polarizing film can be made of a single-layer resin film, or can be made of a laminate of two or more layers.
[0106] When the film is made of a single-layer resin film, for example, a hydrophilic polymer film such as a polyvinyl alcohol (PVA) film, a partially formalized PVA film, or a partially saponified ethylene-vinyl acetate copolymer film is subjected to dyeing treatment with a dichroic substance such as iodine or a dichroic dye, stretching treatment, etc., to obtain an absorption-type polarizing film. Among them, an absorption-type polarizing film obtained by dyeing a PVA film with iodine and uniaxially stretching is preferred.
[0107] The dyeing using iodine can be performed, for example, by immersing the PVA film in an iodine aqueous solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching can be performed after the dyeing treatment or while dyeing. Furthermore, the dyeing can be performed after the stretching. If necessary, the PVA film can be subjected to swelling treatment, cross-linking treatment, cleaning treatment, drying treatment, etc.
[0108] As a laminated body produced using the above-mentioned two or more layers, the following laminated bodies can be listed: a laminated body of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate; or a laminated body of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. The absorption-type polarizing film obtained by using a laminated body of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by the following steps: a PVA-based resin solution is coated on a resin substrate and dried to form a PVA-based resin layer on the resin substrate to obtain a laminated body of the resin substrate and the PVA-based resin layer; and the PVA-based resin layer is made into an absorption-type polarizing film by stretching and dyeing the laminated body. In the present embodiment, it is preferred to form a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin on one side of the resin substrate. Stretching typically includes stretching the laminated body by immersing it in an aqueous boric acid solution. And as required, the stretching may further include stretching the laminate at a high temperature (e.g., above 95°C) in the air before stretching in a boric acid aqueous solution. And, in this embodiment, it is preferred that the laminate is subjected to a drying shrinkage treatment, which heats the laminate while conveying it in the long side direction so that it shrinks by more than 2% in the width direction. Representatively, the manufacturing method of this embodiment includes sequentially performing an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, the crystallinity of PVA can be improved even when PVA is coated on a thermoplastic resin, and high optical properties can be achieved. And, by simultaneously improving the orientation of PVA in advance, problems such as reduction in orientation or dissolution of PVA can be prevented when it is immersed in water in a subsequent dyeing step or stretching step, and high optical properties can be achieved. And, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and reduction in orientation of the polyvinyl alcohol molecules can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. Thus, the optical properties of the absorption type polarizing film obtained by the treatment steps of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved. In addition, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment. The obtained resin substrate / absorption type polarizing film laminate can be used directly (that is, the resin substrate can be used as a protective layer for the absorption type polarizing film), or it can be used on the peeling surface after peeling the resin substrate from the resin substrate / absorption type polarizing film laminate, or on the surface opposite to the peeling surface. The details of the method for manufacturing the absorption type polarizing film are described in, for example, (Japan) Patent Gazette No. 2012-73580 and (Japan) Patent No. 6470455. The entire contents of these gazettes are cited in this specification as a reference.
[0109] The orthogonal transmittance (Tc) of the absorption type polarizing member (absorption type polarizing film) is preferably 0.5% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The single transmittance (Ts) of the absorption type polarizing member (absorption type polarizing film) is, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarization degree (P) of the absorption type polarizing member (absorption type polarizing film) is, for example, 99.0% to 99.997%, and preferably 99.9% or more.
[0110] The in-plane phase difference Re(550) of the third λ / 4 component is, for example, 100nm to 190nm, 110nm to 180nm, 130nm to 160nm, or 135nm to 155nm. The third λ / 4 component preferably exhibits an inverse dispersion wavelength characteristic in which the phase difference value increases with the wavelength of the measurement light. Re(450) / Re(550) of the third λ / 4 component is, for example, greater than 0.75 and less than 1, or greater than 0.8 and less than 0.95. The third λ / 4 component preferably exhibits a refractive index characteristic showing the relationship of nx>ny≥nz. The Nz coefficient of the third λ / 4 component is preferably 0.9 to 3, more preferably 0.9 to 2.5, more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0111] The third λ / 4 member is formed of any appropriate material that can satisfy the above characteristics. The third λ / 4 member can be, for example, a stretched film of a resin film or a directional solidified layer of a liquid crystal compound. The same description as the second λ / 4 member can be applied to the third λ / 4 member composed of a stretched film of a resin film or a directional solidified layer of a liquid crystal compound. The second λ / 4 member and the third λ / 4 member can be members of the same structure (e.g., forming material, thickness, optical characteristics, etc.) or members of different structures.
[0112] Example
[0113] The present invention is specifically described below using examples, but the present invention is not limited to these examples. In addition, the thickness and surface smoothness are values measured by the following measurement methods. And, unless otherwise specified, "parts" and "%" are weight basis.
[0114] <Thickness>
[0115] The thickness of 10 μm or less was measured using a scanning electron microscope (manufactured by JEOL Ltd., product name “JSM-7100F”). The thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu Ltd., product name “KC-351C”).
[0116] <Surface smoothness>
[0117] The measurement was performed using a scanning white interferometer (manufactured by Zygo Corporation, product name "NewView9000"). Specifically, the measurement sample was placed on a measurement table with an anti-vibration table, and interference fringes were generated using a single white LED illumination. The interference objective lens (1.4 times) with a reference surface was scanned along the Z direction (thickness direction), thereby selectively obtaining the smoothness of the outermost surface of the measurement object within the field of view of 12.4 mm□ (surface smoothness). A 5 μm thick acrylic adhesive layer with few bumps was formed on a glass slide (manufactured by Matsunami Glass Industries, product name "S200200"), and a thin film of the measurement object was laminated to the adhesive surface in a manner that prevented the entry of foreign matter, bubbles, or deformed streaks, and the smoothness of the surface opposite to the adhesive layer was measured.
[0118] Regarding the analysis, the value obtained by multiplying the angle index "Slope magnitude RMS" by 2 (equivalent to 2σ) is defined as the surface smoothness (unit: arcmin).
[0119] [Example 1]
[0120] (Preparation of Hard Coat Layer Forming Material)
[0121] A hard coat forming material was prepared by mixing 50 parts of a urethane acrylate oligomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "NKOligo UA-53H"), 30 parts of a polyfunctional acrylate having pentaerythritol triacrylate as the main component (manufactured by Osaka Organic Chemical Co., Ltd., trade name "Viscoat#300"), 20 parts of 4-hydroxybutyl acrylate (manufactured by Osaka Organic Chemical Co., Ltd.), 1 part of a leveling agent (manufactured by DIC Corporation, "GRANDIC PC4100"), and 3 parts of a photopolymerization initiator (manufactured by Chiba Japan Co., Ltd., "IRGACURE907"), and diluting with methyl isobutyl ketone to a solid content concentration of 50%.
[0122] (Preparation of coating liquid for forming high refractive index layer)
[0123] 100 parts by weight of a multifunctional acrylate (manufactured by Arakawa Chemical Industries, Ltd., trade name "OPSTAR KZ6728", solid content 20% by weight), 3 parts by weight of a leveling agent (manufactured by DIC Corporation, "GRANDIC PC4100"), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF Corporation, trade name "OMNIRAD907", solid content 100% by weight) were mixed. In this mixture, butyl acetate was used as a diluent solvent to adjust the solid content to 12% by weight and stirred to prepare a coating liquid for forming a high refractive index layer.
[0124] (Preparation of coating liquid A for forming low refractive index layer)
[0125] 100 parts by weight of a multifunctional acrylate containing pentaerythritol triacrylate as a main component (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300", solid content 100% by weight), 150 parts by weight of hollow nano-silica particles (manufactured by JGC Catalysts & Chemicals Co., Ltd., trade name "THRULYA5320", solid content 20% by weight, weight average particle size 75 nm), 50 parts by weight of solid nano-silica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle size 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight) and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD 907", solid content 100% by weight) were mixed. To the mixture, a mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 was added as a diluent solvent so that the overall solid content became 4 weight %, and the mixture was stirred to prepare a coating liquid for forming a low refractive index layer.
[0126] The hard coating forming material was coated on an acrylic film having a lactone ring structure (thickness 40 μm, surface smoothness 0.45 arcmin) and heated at 90°C for 1 minute. The heated coating layer was then irradiated with a high pressure mercury lamp with a cumulative light intensity of 300 mJ / cm 2 The coating layer was cured by ultraviolet rays to produce an acrylic film (thickness 44 μm, surface smoothness 0.4 arcmin on the hard coating side) having a hard coating layer having a thickness of 4 μm.
[0127] Next, the high refractive index layer-forming coating liquid was applied onto the hard coating layer using a wire bar, and the applied coating liquid was heated at 80°C for 1 minute to dry it, thereby forming a coating film. The dried coating film was irradiated with a high pressure mercury lamp at a cumulative light intensity of 300 mJ / cm 2 The ultraviolet rays harden the coating to form a high refractive index layer with a thickness of 140nm.
[0128] Next, the coating liquid for forming the low refractive index layer was applied onto the high refractive index layer using a wire bar, and the applied coating liquid was heated at 80°C for 1 minute to dry it, thereby forming a coating film. The dried coating film was irradiated with a high pressure mercury lamp at a cumulative light intensity of 300 mJ / cm 2 The ultraviolet rays harden the coating to form a low refractive index layer with a thickness of 105nm.
[0129] In the above manner, a laminated film having a thickness of 44 μm and a surface smoothness of 0.4 arcmin was obtained.
[0130] [Comparative Example 1]
[0131] A laminated film having a thickness of 44 μm and a surface smoothness of 0.4 arcmin was obtained in the same manner as in Example 1 except that no high refractive index layer was formed and the following coating liquid B was used as the coating liquid for forming a low refractive index layer to form a low refractive index layer having a thickness of 100 nm.
[0132] (Preparation of coating liquid B for forming low refractive index layer)
[0133] 100 parts by weight of a multifunctional acrylate containing pentaerythritol triacrylate as the main component (manufactured by Osaka Organic Chemical Industry Co., Ltd., trade name "Viscoat #300", solid content 100% by weight), 100 parts by weight of hollow nano-silica particles (manufactured by JGC Catalysts & Chemicals Co., Ltd., trade name "THRULYA5320", solid content 20% by weight, weight average particle size 75 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight) and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD 907", solid content 100% by weight) were mixed. To the mixture, a mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone) and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 was added as a diluent solvent so that the overall solid content became 4 weight %, and the mixture was stirred to prepare a coating liquid B for forming an anti-reflective low-refractive layer.
[0134] [Comparative Example 2]
[0135] A laminated film having a thickness of 44 μm and a surface smoothness of 0.4 arcmin was obtained in the same manner as in Example 1 except that the high refractive index layer and the low refractive index layer were not formed.
[0136] <Evaluation>
[0137] (1) 30° normal reflectivity
[0138] A test piece of 50 mm × 50 mm size was cut out from the laminated film of Example 1, Comparative Example 1 and Comparative Example 2, and attached to a black acrylic plate using an adhesive to obtain a measurement sample. A spectrophotometer (manufactured by Hitachi High-Tech Co., trade name "U-4100") was used as a measurement device to measure the normal reflectance spectrum. The measurement wavelength was set to the range of 420 nm to 680 nm, and the incident angle of light on the measurement sample was set to 30°.
[0139] The 30° normal reflectance spectra of the laminated films of Example 1, Comparative Example 1 and Comparative Example 2 are shown in FIG. Figure 5 .like Figure 5 As shown, the maximum value of the 30° normal reflectance spectrum of the laminated film of Example 1 in the wavelength range of 420nm to 680nm is 0.85%. In addition, the 30° normal reflectance at a wavelength of 450nm is 0.15%, and the 30° normal reflectance at a wavelength of 600nm is 0.13%. In addition, the results of Comparative Examples 1 and 2 are as follows.
[0140] [Table 1]
[0141] Reflectivity Example 1 Comparative Example 1 Comparative Example 2 Maximum 0.85 1.4 4.8 450nm 0.15 1.0 4.7 600nm 0.13 1.1 3.9
[0142] (2) Appearance 1
[0143] The laminated films of Example 1, Comparative Example 1 and Comparative Example 2 were attached to a black acrylic plate using an adhesive to obtain a measurement plate. In a dark room, a surface light emitting unit (LED light box "LLBK1" manufactured by Altec Corporation) was set at a distance of 18 cm from the measurement plate so as to face the measurement plate. When light was irradiated from the surface light emitting unit to the measurement plate using a dimmer 1, the appearance of the measurement plate was confirmed with the naked eye (reflection visual appearance). Figure 6 (a) Figure 6 (b) and Figure 6 (c) shows the reflective visual appearance. Specifically, Figure 6 (a) shows the result when irradiating with white light. Figure 6 (b) shows the result when irradiated with blue light (wavelength 450nm±30nm), Figure 6 (c) shows the result when irradiated with red light (wavelength 630nm±30nm).
[0144] (3) Appearance 2
[0145] The laminated films of Example 1, Comparative Example 1 and Comparative Example 2 were attached to a transparent glass plate using an adhesive to obtain a test plate. A surface light-emitting unit (LED light box "LLBK1" manufactured by Altec Corporation) was set in a dark room and the test plate was placed on its light-emitting surface. The appearance of the test plate when light was irradiated from the surface light-emitting unit with a dimmer 1 was confirmed with the naked eye (transmitted visual appearance). Figure 7 (a) Figure 7 (b) Figure 7 (c) and Figure 7 (d) shows the transmission visual appearance. Figure 7 (a) shows the result when irradiated with white light. Figure 7 (b) shows the result when irradiated with blue light (wavelength 450nm±30nm), Figure 7 (c) shows the result when irradiated with red light (wavelength 630nm±30nm), Figure 7(d) shows the result when green light (wavelength 530 nm ± 30 nm) is irradiated.
[0146] like Figure 6 (a) Figure 6 (b) and Figure 6 As shown in (c), the reflected visual appearance of Example 1 is particularly excellent compared to Comparative Examples 1 and 2. In the above evaluation, it is assumed that a black acrylic plate is used in combination with an absorption-type polarizing member, but the difference in reflected visual appearance can also be confirmed when a transparent glass plate is used. According to Example 1, it is believed that the problem of ghosting that may occur due to reflected light can be solved very well in the display system of the embodiment of the present invention. In addition, Figure 7 (a) Figure 7 (b) Figure 7 (c) and Figure 7 As shown in (d), the transmission visual appearance of Example 1, Comparative Example 1 and Comparative Example 2 does not change much.
[0147] The present invention is not limited to the above-described embodiments, and various modifications are possible. For example, the present invention may be replaced by a configuration substantially the same as that shown in the above-described embodiments, a configuration that can exert the same effects, or a configuration that can achieve the same purpose.
[0148] Industrial Applicability
[0149] The lens portion according to the embodiment of the present invention can be used for a display body such as VR goggles, for example.
[0150] Description of Reference Numerals
[0151] 2: display system; 4: lens unit; 12: display element; 14: reflective polarizing component; 16: first lens unit; 18: half mirror; 20: first phase difference component; 22: second phase difference component; 24: second lens unit; 28: absorption polarizing component; 30: third phase difference component; 31: first protective component; 32: second protective component; 34: laminated film; 36: substrate; 38: surface treatment layer; 41: adhesive layer; 42: adhesive layer; 43: adhesive layer; 44: adhesive layer; 45: adhesive layer; 46: adhesive layer; 100: first laminated unit; 200: second laminated unit.
Claims
1. A lens unit for displaying an image to a user, comprising: A reflective polarizing member that reflects light emitted forward from a display surface of a display element that displays an image and passes through the polarizing member and the first λ / 4 member; A first lens portion disposed on an optical path between the display element and the reflective polarizing member; a half mirror disposed between the display element and the first lens portion, the half mirror transmitting light emitted from the display element and reflecting light reflected by the reflective polarizing member toward the reflective polarizing member; a second lens portion disposed in front of the reflective polarizing element; A second λ / 4 element disposed on an optical path between the half mirror and the reflective polarizing element; as well as A first protective member and a second protective member, which are arranged on an optical path between the half mirror and the reflective polarizing member; The first protection member and the second protection member are arranged to face each other with a space therebetween; The maximum value of each of the first protective member and the second protective member in a 30° normal reflectance spectrum in a wavelength range of 420 nm to 680 nm is 1.4% or less.
2. The lens portion according to claim 1, The first protective member and the second protective member each have a normal reflectivity of 0.5% or less at 30° at a wavelength of 450 nm.
3. The lens portion according to claim 1, The first protective member and the second protective member each have a normal reflectivity of 0.5% or less at 30° at a wavelength of 600 nm.
4. The lens portion according to claim 1, The surface smoothness of each of the first protection member and the second protection member is 0.5 arcmin or less.
5. The lens portion according to claim 1, The second λ / 4 member satisfies Re(450)<Re(550).
6. The lens unit according to claim 1, comprising: a first laminated portion including the second λ / 4 member and the first protective member; and a second laminated portion including the reflective polarizing member and the second protective member.
7. The lens portion according to claim 6, The second stacked portion includes an absorptive polarizing member disposed between the reflective polarizing member and the second lens portion.
8. The lens portion according to claim 6, The second stacked portion includes a third λ / 4 member disposed between the reflective polarizing member and the second lens portion.
9. The lens portion according to claim 8, The third λ / 4 member satisfies Re(450)<Re(550).
10. A laminated film for use in a display method comprising the following steps: The step of allowing the light of the display image emitted through the polarizing element and the first λ / 4 element to pass through the half mirror and the first lens portion; a step of allowing the light that has passed through the half mirror and the first lens portion to pass through a second λ / 4 member; a step of reflecting the light that has passed through the second λ / 4 member toward the half mirror using a reflective polarizing member; A step of allowing the light reflected by the reflective polarizing member and the half mirror to pass through the second λ / 4 member and transmit through the reflective polarizing member; and allowing the light transmitted through the reflective polarizing member to pass through a second lens portion; The laminated film is arranged on an optical path between the half mirror and the reflective polarizing member and is in contact with a space formed between the first lens portion and the second lens portion; The maximum value of the 30° normal reflectance spectrum of the laminated film in the wavelength range of 420 nm to 680 nm is 1.4% or less.