Flip light-emitting diode preparation method and flip light-emitting diode
By forming a metal reflective layer and a transverse conductive layer on the Bragg reflective layer of the flip-mounted light-emitting diode chip, the partition mask technology maximizes the reflectivity while minimizing the use of precious metal Au, the contradiction between high reflectivity and low cost is solved. Reduces chip manufacturing costs.
Patent Information
- Application Number
- CN202410954565.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-08
Smart Images

Figure CN118919611A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of optoelectronic technology, and in particular to a method for preparing an inverted light emitting diode and the inverted light emitting diode. Background Art
[0002] Flip-chip LED chips are widely used due to their advantages such as back-emitting light, strong heat dissipation, good weldability, large thrust, and strong reliability. Initially, people used Bragg reflectors as reflectors to enable flip-chip LEDs to emit light from the back. In recent years, people have begun to add high-reflectivity metals to the Bragg reflectors to form total reflectors in combination with the Bragg reflector layer, thereby improving the reflectivity of the reflector and ultimately improving the external quantum efficiency of the flip-chip LED chip.
[0003] The larger the metal area of the high reflector on the Bragg reflector, the better the effect of increasing the external quantum efficiency of the light-emitting diode chip. However, the larger the metal area of the high reflector on the Bragg reflector of the light-emitting diode, the larger the area of precious metal Au that needs to be set above the metal for connecting multiple N-type semiconductor layers, and the higher the chip cost, which affects the further use of the product. Summary of the invention
[0004] Based on this, the purpose of the present invention is to provide a method for preparing a flip-chip light emitting diode and a flip-chip light emitting diode to solve the problems existing in the prior art.
[0005] The present invention provides a method for preparing a flip-chip light-emitting diode, comprising the following steps:
[0006] S10, providing a substrate, and depositing an epitaxial layer on a surface of the substrate, wherein the epitaxial layer comprises an N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate;
[0007] S20, etching a partial area of the surface of the epitaxial layer to a depth down to the N-type semiconductor layer to form a conductive step of the N-type semiconductor layer, and preparing a current spreading layer on other unetched areas of the surface of the epitaxial layer;
[0008] S30, evaporating a plurality of overlapping layers of SiO2 and Ti3O5 as Bragg reflection layers on the surface of the epitaxial layer after the N-type semiconductor layer conductive step and the current spreading layer are prepared, and etching the Bragg reflection layer to form corresponding Bragg reflection layer through holes on the current spreading layer and the N-type semiconductor layer conductive step, respectively;
[0009] S40, coating a negative photoresist on the surface of the epitaxial layer forming the Bragg reflector layer, performing exposure and development processing using a partitioned mask, forming two opening areas of different sizes in the negative photoresist, and depositing conductive metals in the two opening areas in sequence to form a metal reflective layer in the large-size opening area and a lateral conductive layer in the small-size opening area;
[0010] S50, preparing an insulating passivation layer and a pad layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer to obtain a target flip-chip light emitting diode.
[0011] Preferably, after the P-type GaN layer is deposited, the method for preparing a flip-chip light-emitting diode further comprises: cleaning the epitaxial wafer with an acetone ultrasonic solution, an isopropanol solution, and a sulfuric acid-hydrogen peroxide mixed solution in sequence.
[0012] Preferably, etching a partial area of the surface of the epitaxial layer to a depth up to the N-type semiconductor layer to form a conductive step of the N-type semiconductor layer, and preparing a current spreading layer on other unetched areas of the surface of the epitaxial layer specifically includes:
[0013] Coating a photoresist on the surface of the P-type semiconductor layer, then exposing and developing to remove a portion of the photoresist and expose a portion of the P-type semiconductor layer;
[0014] Performing ICP etching on the exposed P-type semiconductor layer, removing the exposed P-type semiconductor layer and the active light-emitting layer and the N-type semiconductor layer at the bottom thereof in sequence, and then removing the remaining photoresist on the P-type semiconductor layer to form a conductive step of the N-type semiconductor layer;
[0015] Depositing an indium tin oxide layer on the surface of the epitaxial layer forming the conductive step of the N-type semiconductor layer by using a magnetron sputtering process, coating the indium tin oxide layer with a photoresist, exposing and developing to remove a portion of the photoresist, and exposing a portion of the indium tin oxide layer;
[0016] An indium tin oxide etching solution is used to remove the exposed indium tin oxide layer, and then the remaining photoresist on the indium tin oxide layer is removed to form a current spreading layer on the P-type semiconductor layer.
[0017] Preferably, only an N-type semiconductor layer is deposited on the edge of the substrate, and after forming the conductive step of the N-type semiconductor layer, the method for preparing a flip-chip light-emitting diode further comprises:
[0018] Coating photoresist on the surface of the epitaxial layer, and then exposing and developing to remove the photoresist on the N-type semiconductor layer at the edge of the epitaxial layer;
[0019] ICP etching is performed on the upper surface of the N-type semiconductor layer at the edge of the epitaxial layer until the substrate is etched, and the remaining photoresist is removed to form an isolation groove at the edge of the epitaxial layer.
[0020] Preferably, the step of evaporating a plurality of overlapping layers of SiO2 and Ti3O5 as Bragg reflection layers on the surface of the epitaxial layer after preparing the N-type semiconductor layer conductive step and the current spreading layer, and etching the Bragg reflection layer to form corresponding Bragg reflection layer through holes on the current spreading layer and the N-type semiconductor layer conductive step, respectively, specifically comprises:
[0021] After preparing the N-type semiconductor layer conductive step and the current spreading layer, 15-40 groups of overlapping layers of SiO2 and Ti3O5 are evaporated on the surface of the epitaxial layer as a Bragg reflection layer;
[0022] Coating a photoresist on the Bragg reflection layer, exposing and developing to remove a portion of the photoresist, thereby exposing a portion of the Bragg reflection layer;
[0023] Using an ICP etching process to remove the exposed Bragg reflection layer to form a Bragg reflection layer through hole, wherein the Bragg reflection layer through hole includes a P-type Bragg reflection layer through hole located on the current spreading layer and an N-type Bragg reflection layer through hole located on the conductive step of the N-type semiconductor layer;
[0024] The plasma formed by argon gas is used to process the current spreading layer under the through hole of the P-type Bragg reflection layer and the conductive step of the N-type semiconductor layer under the through hole of the N-type Bragg reflection layer, and finally the remaining photoresist is removed.
[0025] Preferably, the process of coating a negative photoresist on the surface of the epitaxial layer forming the Bragg reflector layer, performing exposure and development processing using a partitioned mask, forming two opening areas of different sizes in the negative photoresist, and sequentially depositing conductive metals in the two opening areas to form a metal reflective layer in the large-size opening area and forming a lateral conductive layer in the small-size opening area specifically includes:
[0026] A negative photoresist is coated on the surface of the epitaxial layer forming the Bragg reflection layer, and then a partitioned mask is used for exposure processing, wherein the partitioned mask is provided with an opaque graphic area on the end face away from the epitaxial layer, and a semi-transparent graphic area and a fully transparent graphic area on the end face close to the epitaxial layer;
[0027] Using a developer to develop, so as to form two opening regions with different sizes in the negative photoresist, wherein the large-size opening region is located above the Bragg reflection layer, and the small-size opening region is located above the large-size opening region and communicates with the large-size opening region;
[0028] Depositing a reflective metal and a reflective metal protection metal in the large-size opening area by a magnetron sputtering process to form a metal reflective layer, wherein the thickness of the metal reflective layer is equal to the depth of the large-size opening area;
[0029] Conductive metal is further deposited on the metal reflective layer as a lateral conductive layer, and then a blue film stripping process is used to remove all metal on the negative photoresist, and finally the remaining negative photoresist is removed.
[0030] Preferably, the thickness of the negative photoresist is 6 μm-10 μm, and the transmittance of the semi-transparent pattern area is 20%-80%.
[0031] Preferably, the reflective metal is Al or Ag, the reflective metal protective metal is one or more of Ti, Pt, Ni, TiW, and TiNi, and the conductive metal deposited to form the lateral conductive layer is Au.
[0032] Preferably, the lateral conductive layer includes a conductive plate and conductive fingers, the conductive plate is electrically connected to the pad layer, the conductive fingers are used to transmit current laterally to multiple Bragg reflection layer through holes, and the width of the conductive fingers is smaller than the diameter of the Bragg reflection layer through holes.
[0033] Preferably, the step of preparing an insulating passivation layer and a pad layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer to obtain the target flip-chip light-emitting diode specifically includes:
[0034] Depositing an insulating passivation layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer, wherein the insulating passivation layer is deposited from SiO2 or SiN or a mixture of SiO2 and SiN;
[0035] Coating a photoresist on the surface of the insulating passivation layer, exposing and developing to remove a portion of the photoresist, exposing a portion of the insulating passivation layer, removing the exposed insulating passivation layer by a plasma etching process to form an insulating passivation layer through hole, and removing the remaining photoresist;
[0036] Photoresist is coated on the surface of the insulating passivation layer and in the through holes of the insulating passivation layer, and then part of the photoresist is removed by exposure and development. Al, Ti, Pt, Ni, and Au metals are sequentially evaporated using an electron beam evaporation process, and then excess metal is removed using a blue film stripping process. Finally, the remaining photoresist is removed to form the pad layer.
[0037] The present application also provides a flip-chip light emitting diode, which is prepared using the above-mentioned flip-chip light emitting diode preparation method.
[0038] The beneficial effects of the present invention are as follows: the method for preparing a flip-chip light-emitting diode provided by the present application first provides a substrate, and deposits an epitaxial layer on the surface of the substrate; prepares an N-type semiconductor layer conductive step and a current spreading layer on the surface of the epitaxial layer; then evaporates a plurality of groups of overlapping layers of SiO2 and Ti3O5 on the surface of the epitaxial layer as a Bragg reflection layer, and etches to form a P-type Bragg reflection layer through hole and an N-type Bragg reflection layer through hole; then coats a negative photoresist on the surface of the epitaxial layer, performs a development process after a partitioned mask exposure, forms two opening areas of different sizes in the photoresist, and deposits metal in the two opening areas respectively, so as to form a metal reflection layer in the large-size opening area and a lateral conductive layer in the small-size opening area, so as to achieve the maximum area of the metal with high reflectivity and the minimum area of the precious metal Au of the lateral conductive layer when the same equipment is operated at the same time, thereby reducing the manufacturing cost of the flip-chip light-emitting diode chip; finally, prepares an insulating layer and a pad layer on the surface of the epitaxial layer to obtain a target light-emitting diode.
[0039] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 A flow chart of the method for preparing a flip-chip light-emitting diode provided by the present invention;
[0041] Figure 2 The AA cross-sectional structure diagram of the diode after the epitaxial layer is deposited on the substrate;
[0042] Figure 3 for Figure 2 AA cross-sectional structure diagram of the diode after the isolation trench is prepared;
[0043] Figure 4 for Figure 3 AA cross-sectional structure diagram of the diode after the current spreading layer is prepared;
[0044] Figure 5 for Figure 4 AA cross-sectional structure diagram of the diode after the Bragg reflection layer is prepared;
[0045] Figure 6 is a top view of the partitioned mask;
[0046] Figure 7(a)-Figure 7(d) for Figure 5 BB cross-sectional structure diagram of the diode during the preparation of the metal reflective layer and the lateral conductive layer;
[0047] Figure 8 FIG7 is a cross-sectional structural diagram of the diode taken along the line AA after the metal reflective layer and the lateral conductive layer are prepared;
[0048] Fig. 9 for Figure 8 AA cross-sectional structure diagram after preparing the insulating passivation layer;
[0049] Fig.10 for Fig. 9 AA cross-sectional structure diagram after preparing the pad layer;
[0050] Fig.11 This is a top view of the flip-chip light-emitting diode prepared by the present invention.
[0051] Description of main component symbols:
[0052] 10. Substrate; 111. N-type semiconductor layer; 112. Active light-emitting layer; 113. P-type semiconductor layer; 114. N-type semiconductor layer conductive step; 115. Isolation groove; 12. Current spreading layer; 13. Bragg reflection layer; 131. P-type Bragg reflection layer through hole; 132. N-type Bragg reflection layer through hole; 14. Negative photoresist; 141. Large-size opening area; 142. Small-size opening area; 15. Partitioned mask; 151. Optical-impermeable graphic area; 152. Semi-transparent graphic area; 153. Fully transparent graphic area; 161. Metal reflection layer; 162. Lateral conductive layer; 1621. Conductive disk; 1622. Conductive finger strip; 17. Insulating passivation layer; 171. Insulating passivation layer through hole; 18. Pad layer.
[0053] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0054] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0055] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0056] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing optional embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0057] Example 1
[0058] The present invention provides a method for preparing a flip-chip light-emitting diode, such as Figure 1 As shown, the method for preparing a flip-chip light-emitting diode includes S10 to S50:
[0059] S10, providing a substrate, and depositing an epitaxial layer on a surface of the substrate, wherein the epitaxial layer comprises an N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate;
[0060] In a specific implementation, the epitaxial layer can be deposited by metal chemical vapor deposition (MOCVD), such as Figure 2 As shown, an N-type semiconductor layer 111 , an active light-emitting layer 112 , and a P-type semiconductor layer 113 are sequentially prepared on a substrate 10 .
[0061] S20, etching a partial area of the surface of the epitaxial layer to a depth down to the N-type semiconductor layer to form a conductive step of the N-type semiconductor layer, and preparing a current spreading layer on other unetched areas of the surface of the epitaxial layer;
[0062] Optionally, S20 specifically includes:
[0063] Coating a photoresist on the surface of the P-type semiconductor layer, then exposing and developing to remove a portion of the photoresist and expose a portion of the P-type semiconductor layer;
[0064] The exposed P-type semiconductor layer is subjected to ICP etching to sequentially remove the exposed P-type semiconductor layer and the active light-emitting layer and the N-type semiconductor layer at the bottom thereof, and then the remaining photoresist on the P-type semiconductor layer is removed. Figure 2 As shown, a conductive step of the N-type semiconductor layer is formed;
[0065] Only an N-type semiconductor layer is deposited on the edge of the epitaxial layer. After forming a conductive step of the N-type semiconductor layer, the method for preparing a flip-chip light-emitting diode further includes:
[0066] A photoresist is coated on the surface of the epitaxial layer, and then the photoresist on the N-type semiconductor layer at the edge of the epitaxial layer is removed by exposure and development; an ICP etching is performed on the upper surface of the N-type semiconductor layer at the edge of the epitaxial layer until the substrate is etched, and the remaining photoresist is removed to form an isolation groove 115 at the edge of the epitaxial layer. Figure 3 As shown, the isolation groove 115 is to prevent the solder paste on the P-type pad from contacting with the N-type semiconductor during the subsequent chip packaging process to cause a short circuit. Therefore, the isolation groove is set in advance, and the isolation groove is protected by an insulating protective layer during the subsequent chip preparation process, which can prevent the solder paste on the P-type pad from contacting with the N-type semiconductor during the subsequent chip packaging process.
[0067] An indium tin oxide layer is deposited on the surface of the epitaxial layer forming the conductive step of the N-type semiconductor layer by using a magnetron sputtering process; in this embodiment, an indium tin oxide layer is deposited on the P-type semiconductor layer 113, the N-type semiconductor layer conductive step 114 and the isolation groove 115 by using a magnetron sputtering process; then a photoresist is coated on the indium tin oxide layer, and a part of the photoresist is removed by exposure and development to expose a part of the indium tin oxide layer;
[0068] The exposed indium tin oxide layer is removed by using an indium tin oxide etching solution, and then the remaining photoresist on the indium tin oxide layer is removed. Figure 4 As shown, a current spreading layer 12 is formed on the P-type semiconductor layer, and the current spreading layer 12 only exists on the surface of the P-type semiconductor layer 113 .
[0069] S30, evaporating a plurality of overlapping layers of SiO2 and Ti3O5 as Bragg reflection layers on the surface of the epitaxial layer after the N-type semiconductor layer conductive step and the current spreading layer are prepared, and etching the Bragg reflection layer to form corresponding Bragg reflection layer through holes on the current spreading layer and the N-type semiconductor layer conductive step, respectively;
[0070] Optionally, S30 specifically includes:
[0071] After preparing the N-type semiconductor layer conductive step and the current spreading layer, 15-40 groups of overlapping layers of SiO2 and Ti3O5 are evaporated on the surface of the epitaxial layer as the Bragg reflection layer 13;
[0072] Coating a photoresist on the Bragg reflection layer, exposing and developing to remove a portion of the photoresist, thereby exposing a portion of the Bragg reflection layer;
[0073] The exposed Bragg reflector layer is removed by ICP etching process to form a Bragg reflector through hole, such as Figure 5 As shown, the Bragg reflection layer through hole includes a P-type Bragg reflection layer through hole 131 located on the current spreading layer and an N-type Bragg reflection layer through hole 132 located on the conductive step of the N-type semiconductor layer;
[0074] The plasma formed by argon gas is used to process the current spreading layer under the through hole of the P-type Bragg reflection layer and the conductive step of the N-type semiconductor layer under the through hole of the N-type Bragg reflection layer, and finally the remaining photoresist is removed.
[0075] S40, coating a negative photoresist on the surface of the epitaxial layer forming the Bragg reflector layer, performing exposure and development processing using a partitioned mask, forming two opening areas of different sizes in the negative photoresist, and depositing conductive metals in the two opening areas in sequence to form a metal reflective layer in the large-size opening area and a lateral conductive layer in the small-size opening area;
[0076] Optionally, S40 specifically includes:
[0077] A negative photoresist 14 is coated on the surface of the epitaxial layer forming the Bragg reflection layer, and then a partition mask 15 is used for exposure processing. The partition mask 15 is provided with an opaque graphic area 151 on the end surface away from the epitaxial layer, and a semi-transparent graphic area 152 and a fully transparent graphic area 153 on the end surface close to the epitaxial layer;
[0078] Optional, such as Figure 6 As shown, the partitioned mask 15 includes a completely opaque graphic area 151 disposed on the front side of the partitioned mask 15, a semi-transparent graphic area 152 and a fully transparent graphic area 153 disposed on the back side. Optionally, in this embodiment, the thickness of the negative photoresist 14 is 6μm-10μm, and the transmittance of the semi-transparent graphic area is 20%-80%.
[0079] The developer is used to develop the negative photoresist to form two opening areas with different sizes in the negative photoresist, wherein Figure 7(a)-Figure 7(d) As shown, the large-sized opening area 141 is located above the Bragg reflection layer 13, the small-sized opening area 142 is located above the large-sized opening area 141 and communicates with the large-sized opening area 141, and the depth of the large-sized opening area 141 is L;
[0080] Depositing a reflective metal and a reflective metal protection metal in the large-size opening area by a magnetron sputtering process to form a metal reflective layer, wherein the thickness of the metal reflective layer is equal to the depth of the large-size opening area;
[0081] Optionally, during implementation, a magnetron sputtering process is used to first deposit highly reflective metal Al or Ag, and then continue to deposit highly reflective metal protective metal, the protective metal can be one or more of Ti, Pt, Ni, TiW, and TiNi; the highly reflective metal and the highly reflective metal protective metal together constitute a metal reflective layer 161, and the thickness of the metal reflective layer 161 is equal to the depth L of the large-size opening area 141; in some optional embodiments, an electron beam evaporation process can also be used to deposit the reflective metal and the protective metal.
[0082] Conductive metal is further deposited on the metal reflective layer as a lateral conductive layer, and then a blue film stripping process is used to remove all metal on the negative photoresist, and finally the remaining negative photoresist is removed.
[0083] Optional, in implementation, such as Figure 8 As shown, high-conductivity metal Au is continuously deposited as the lateral conductive layer 162, and then a blue film stripping process is used to remove all metals on the negative photoresist, and finally the remaining negative photoresist.
[0084] Through the above steps, the large-area metal reflective layer 161 and the small-area lateral conductive layer 162 are prepared on the Bragg reflective layer 13 at the same time, so that the metal area with high reflectivity is maximized while the area of the precious metal Au is minimized when the same equipment is operated at the same time, thereby reducing the manufacturing cost of the flip-chip light-emitting diode chip; further, Fig.11 As shown, the lateral conductive layer 162 includes a conductive plate 1621 and a conductive finger strip 1622. The conductive plate 1621 is responsible for forming an electrical connection with the subsequently prepared packaging pad layer 18, and the conductive finger strip 1622 is responsible for transmitting the current laterally to each Bragg reflection layer through hole. The width of the conductive finger strip is smaller than the diameter of the Bragg reflection layer through hole, and the central axis of the conductive finger strip coincides with the center of the Bragg reflection layer through hole.
[0085] S50, preparing an insulating passivation layer and a pad layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer to obtain a target flip-chip light emitting diode.
[0086] Optionally, S50 specifically includes:
[0087] Depositing an insulating passivation layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer, wherein the insulating passivation layer is deposited from SiO2 or SiN or a mixture of SiO2 and SiN;
[0088] In specific implementation, Fig. 9 As shown, PECVD (plasma enhanced chemical vapor deposition technology) can be used to deposit SiO2 or SiN or a mixture of SiO2 and SiN on the surface of the epitaxial layer as the insulating passivation layer 17;
[0089] Coating photoresist on the surface of the insulating passivation layer, exposing and developing to remove part of the photoresist, exposing part of the insulating passivation layer, removing the exposed insulating passivation layer by plasma etching process to form an insulating passivation layer through hole 171, and removing the remaining photoresist;
[0090] Optionally, the insulating passivation layer through hole 171 and the conductive plate 1621 of the lateral conductive metal layer are projected as concentric circles;
[0091] Photoresist is coated on the surface of the insulating passivation layer and in the through hole of the insulating passivation layer, and then part of the photoresist is removed by exposure and development, and Al, Ti, Pt, Ni, and Au metals are sequentially evaporated by electron beam evaporation process, and then the excess metal is removed by blue film stripping process, and finally the remaining photoresist is removed, such as Fig.10As shown, the pad layer 18 is formed.
[0092] Optionally, the pad layer 18 is electrically connected to the conductive pad 1621 through the insulating passivation layer through hole 171 .
[0093] In summary, the method for preparing a flip-chip light-emitting diode provided by the present application first provides a substrate, and deposits an epitaxial layer on the surface of the substrate; prepares an N-type semiconductor layer conductive step and a current spreading layer on the surface of the epitaxial layer; then evaporates a plurality of overlapping layers of SiO2 and Ti3O5 on the surface of the epitaxial layer as a Bragg reflection layer, and etches to form a P-type Bragg reflection layer through hole and an N-type Bragg reflection layer through hole; then coats a negative photoresist on the surface of the epitaxial layer, performs a zoned mask exposure and a development process, forms two opening areas of different sizes in the photoresist, and deposits metal in the two opening areas respectively, so as to form a metal reflection layer in the large-size opening area and a lateral conductive layer in the small-size opening area, so as to achieve the maximum area of the metal with high reflectivity and the minimum area of the precious metal Au in the lateral conductive layer when the same equipment is operated at the same time, thereby reducing the manufacturing cost of the flip-chip light-emitting diode chip; finally, prepares an insulating layer and a pad layer on the surface of the epitaxial layer to obtain a target light-emitting diode.
[0094] Example 2
[0095] The present application also provides a flip-chip light emitting diode, which is prepared according to the above-mentioned flip-chip light emitting diode preparation method.
[0096] It should be noted that the above implementation process is only to illustrate the feasibility of the present application, but it does not mean that the flip-chip light-emitting diode of the present application has only the above-mentioned implementation processes. On the contrary, as long as the flip-chip light-emitting diode of the present application can be implemented, it can be included in the feasible implementation scheme of the present application. In addition, the structural part in the embodiment of the present invention corresponds to the preparation method part of the present invention, and the specific implementation details are also the same, which will not be repeated here.
[0097] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0098] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present invention. It should be pointed out that, for a person of ordinary skill in the art, several modifications and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the present invention patent shall be subject to the attached claims.
Claims
1. A method for preparing a flip-chip light-emitting diode, characterized in that: The following steps are involved: S10, providing a substrate, and depositing an epitaxial layer on a surface of the substrate, wherein the epitaxial layer comprises an N-type semiconductor layer, an active light-emitting layer, and a P-type semiconductor layer sequentially deposited on the substrate; S20, etching a partial area of the surface of the epitaxial layer to a depth down to the N-type semiconductor layer to form a conductive step of the N-type semiconductor layer, and preparing a current spreading layer on other unetched areas of the surface of the epitaxial layer; S30, evaporating a plurality of overlapping layers of SiO2 and Ti3O5 as Bragg reflection layers on the surface of the epitaxial layer after the N-type semiconductor layer conductive step and the current spreading layer are prepared, and etching the Bragg reflection layer to form corresponding Bragg reflection layer through holes on the current spreading layer and the N-type semiconductor layer conductive step, respectively; S40, coating a negative photoresist on the surface of the epitaxial layer forming the Bragg reflector layer, performing exposure and development processing using a partitioned mask, forming two opening areas of different sizes in the negative photoresist, and depositing conductive metals in the two opening areas in sequence to form a metal reflective layer in the large-size opening area and a lateral conductive layer in the small-size opening area; S50, preparing an insulating passivation layer and a pad layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer to obtain a target flip-chip light emitting diode.
2. The method for preparing a flip-chip light-emitting diode according to claim 1, characterized in that: The etching of a part of the surface area of the epitaxial layer to a depth of the N-type semiconductor layer to form a conductive step of the N-type semiconductor layer, and the preparation of a current spreading layer on other unetched areas on the surface of the epitaxial layer specifically includes: Coating a photoresist on the surface of the P-type semiconductor layer, then exposing and developing to remove a portion of the photoresist and expose a portion of the P-type semiconductor layer; Performing ICP etching on the exposed P-type semiconductor layer, removing the exposed P-type semiconductor layer and the active light-emitting layer and the N-type semiconductor layer at the bottom thereof in sequence, and then removing the remaining photoresist on the P-type semiconductor layer to form a conductive step of the N-type semiconductor layer; Depositing an indium tin oxide layer on the surface of the epitaxial layer forming the conductive step of the N-type semiconductor layer by using a magnetron sputtering process, coating the indium tin oxide layer with a photoresist, exposing and developing to remove a portion of the photoresist, and exposing a portion of the indium tin oxide layer; An indium tin oxide etching solution is used to remove the exposed indium tin oxide layer, and then the remaining photoresist on the indium tin oxide layer is removed to form a current spreading layer on the P-type semiconductor layer.
3. The method for preparing a flip-chip light-emitting diode according to claim 2, characterized in that: The edge of the substrate is only deposited with an N-type semiconductor layer. After forming the conductive step of the N-type semiconductor layer, the method for preparing a flip-chip light-emitting diode further includes: Coating photoresist on the surface of the epitaxial layer, and then exposing and developing to remove the photoresist on the N-type semiconductor layer at the edge of the epitaxial layer; ICP etching is performed on the upper surface of the N-type semiconductor layer at the edge of the epitaxial layer until the substrate is etched, and the remaining photoresist is removed to form an isolation groove at the edge of the epitaxial layer.
4. The method for preparing a flip-chip light-emitting diode according to claim 1, characterized in that: The method of evaporating a plurality of overlapping layers of SiO2 and Ti3O5 as Bragg reflection layers on the surface of the epitaxial layer after preparing the N-type semiconductor layer conductive step and the current spreading layer, and etching the Bragg reflection layer to form corresponding Bragg reflection layer through holes on the current spreading layer and the N-type semiconductor layer conductive step, respectively, specifically comprises: After preparing the N-type semiconductor layer conductive step and the current spreading layer, 15-40 groups of overlapping layers of SiO2 and Ti3O5 are evaporated on the surface of the epitaxial layer as a Bragg reflection layer; Coating a photoresist on the Bragg reflection layer, exposing and developing to remove a portion of the photoresist, thereby exposing a portion of the Bragg reflection layer; Using an ICP etching process to remove the exposed Bragg reflection layer to form a Bragg reflection layer through hole, wherein the Bragg reflection layer through hole includes a P-type Bragg reflection layer through hole located on the current spreading layer and an N-type Bragg reflection layer through hole located on the conductive step of the N-type semiconductor layer; The plasma formed by argon gas is used to process the current spreading layer under the through hole of the P-type Bragg reflection layer and the conductive step of the N-type semiconductor layer under the through hole of the N-type Bragg reflection layer, and finally the remaining photoresist is removed.
5. The method for preparing a flip-chip light-emitting diode according to claim 1, characterized in that: The method of coating a negative photoresist on the surface of the epitaxial layer forming the Bragg reflector layer, performing exposure and development processing using a partitioned mask, forming two opening areas of different sizes in the negative photoresist, and depositing conductive metal in the two opening areas in sequence to form a metal reflective layer in the large-size opening area and a lateral conductive layer in the small-size opening area specifically includes: A negative photoresist is coated on the surface of the epitaxial layer forming the Bragg reflection layer, and then a partitioned mask is used for exposure processing, wherein the partitioned mask is provided with an opaque graphic area on the end face away from the epitaxial layer, and a semi-transparent graphic area and a fully transparent graphic area on the end face close to the epitaxial layer; Using a developer to develop, so as to form two opening regions with different sizes in the negative photoresist, wherein the large-size opening region is located above the Bragg reflection layer, and the small-size opening region is located above the large-size opening region and communicates with the large-size opening region; Depositing a reflective metal and a reflective metal protection metal in the large-size opening area by a magnetron sputtering process to form a metal reflective layer, wherein the thickness of the metal reflective layer is equal to the depth of the large-size opening area; Conductive metal is further deposited on the metal reflective layer as a lateral conductive layer, and then a blue film stripping process is used to remove all metal on the negative photoresist, and finally the remaining negative photoresist is removed.
6. The method for preparing a flip-chip light-emitting diode according to claim 5, characterized in that: The thickness of the negative photoresist is 6 μm-10 μm, and the light transmittance of the semi-transparent pattern area is 20%-80%.
7. The method for preparing a flip-chip light-emitting diode according to claim 5, characterized in that: The reflective metal is Al or Ag, the reflective metal protective metal is one or more of Ti, Pt, Ni, TiW, and TiNi, and the conductive metal deposited to form the lateral conductive layer is Au.
8. The method for preparing a flip-chip light-emitting diode according to claim 5, characterized in that: The lateral conductive layer includes a conductive plate and conductive fingers, the conductive plate is electrically connected to the pad layer, the conductive fingers are used to transmit current laterally to multiple Bragg reflection layer through holes, and the width of the conductive fingers is smaller than the diameter of the Bragg reflection layer through holes.
9. The method for preparing a flip-chip light-emitting diode according to claim 1, characterized in that: The step of preparing an insulating passivation layer and a pad layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer to obtain the target flip-chip light-emitting diode specifically includes: Depositing an insulating passivation layer on the surface of the epitaxial layer forming the metal reflective layer and the lateral conductive layer, wherein the insulating passivation layer is deposited from SiO2 or SiN or a mixture of SiO2 and SiN; Coating a photoresist on the surface of the insulating passivation layer, exposing and developing to remove a portion of the photoresist, exposing a portion of the insulating passivation layer, removing the exposed insulating passivation layer by a plasma etching process to form an insulating passivation layer through hole, and removing the remaining photoresist; Photoresist is coated on the surface of the insulating passivation layer and in the through holes of the insulating passivation layer, and then part of the photoresist is removed by exposure and development. Al, Ti, Pt, Ni, and Au metals are sequentially evaporated using an electron beam evaporation process, and then excess metal is removed using a blue film stripping process. Finally, the remaining photoresist is removed to form the pad layer.
10. A flip-chip light emitting diode, characterized in that: The flip-chip light-emitting diode is prepared according to any one of claims 1 to 9.
Citation Information
Cited By
Flip silver mirror light-emitting diode chip preparation method and flip silver mirror light-emitting diode chip
CN121013517A