All-solid-state battery comprising silicon anode having concave spherical structure

By adopting a concave spherical silicon anode electrode in an all-solid-state battery pack, the pulsed DC magnetron sputtering technology is used to solve the shortcomings of the lithium-ion battery pack in extreme conditions and cycling performance, achieving higher power capacity and stability , simplifies the manufacturing process.

CN118919655APending Publication Date: 2024-11-08GM GLOBAL TECHNOLOGY OPERATIONS LLC
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310512515.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing lithium-ion battery packs have shortcomings in terms of extreme conditions, operating temperature range and power capacity, especially during the cycle process, the transmission rate performance and stability of the silicon anode electrode are poor.

Method used

Using silicon anode electrode with a concave spherical structure, a silicon layer is deposited on the anode current collector through pulsed DC magnetron sputtering technology, increasing the silicon/electrolyte interface area, simplifying the manufacturing process, adapting to the expansion and contraction of the silicon anode, and improving the battery Cyclic performance.

Benefits of technology

The power capacity and cycle stability of the all-solid-state battery pack are enhanced, the stress release capacity and cycle performance of the battery are improved, the manufacturing process is simplified, and the dependence on adhesives and solid electrolytes is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118919655A_ABST
    Figure CN118919655A_ABST
Patent Text Reader

Abstract

An all-solid-state battery including a silicon anode having a concave spherical structure is disclosed. A solid state battery cell includes a cathode electrode including a cathode current collector and a cathode active layer disposed on the cathode current collector and including a cathode active material and a solid electrolyte. The separator layer contains a solid electrolyte. The anode layer includes an anode current collector and a silicon layer disposed on the anode current collector and including a plurality of concave spherical surfaces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a solid-state battery pack. Background Art

[0002] The information provided in this section is for the purpose of generally presenting the background of the present disclosure. The work of the presently named inventors, to the extent described in this section, and aspects of the description that may not otherwise constitute prior art at the time of filing, are neither expressly nor impliedly admitted to be prior art against the present disclosure.

[0003] The present disclosure relates to all-solid-state batteries, and more particularly to all-solid-state batteries including a silicon anode electrode having a concave spherical structure.

[0004] Electric vehicles such as battery electric vehicles and hybrid vehicles are powered by a battery pack including one or more battery modules, each battery module having one or more battery cells. The battery cell includes an anode electrode, a cathode electrode, and a separator. The anode electrode includes an anode active layer disposed on an anode current collector. The cathode electrode typically includes a cathode active layer disposed on a cathode current collector.

[0005] All-solid-state batteries (ASSBs) have the potential to outperform state-of-the-art lithium-ion batteries in terms of abuse tolerance, operating temperature range, and power capability. Summary of the invention

[0006] A solid-state battery cell includes a cathode electrode, the cathode electrode includes a cathode current collector and a cathode active layer, the cathode active layer is arranged on the cathode current collector and contains a cathode active material and a solid electrolyte. The separator layer contains a solid electrolyte. The anode layer includes an anode current collector and a silicon layer arranged on the anode current collector and includes a plurality of concave spherical surfaces.

[0007] In other features, the silicon layer has a surface area of ​​105% to 300% of the corresponding flat surface. The anode current collector is made of one or more materials selected from copper, stainless steel, nickel, iron, titanium, tin (Sn) and alloys thereof. The anode current collector has a surface roughness Rz of 0.1 μm to 12 μm. The depth of the concave spherical surface is 0.1 μm to 20 μm. The anode current collector has a thickness of 4 μm to 30 μm.

[0008] In other features, the cathode active layer comprises 1 to 50 wt % of a solid electrolyte, 30 to 98 wt % of a cathode active material, 0 to 30 wt % of a conductive additive and 0 to 20 wt % of a binder. The cathode active material comprises one or more materials selected from the following: rock salt layered oxides, spinels, polyanionic cathodes, lithium transition metal oxides, surface-coated cathode materials, doped cathode materials and low voltage cathode materials. The conductive additive comprises one or more materials selected from carbon black, graphite, graphene, graphene oxide, Super P, acetylene black, carbon nanofibers and carbon nanotubes. The binder comprises one or more materials selected from the following: polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS) and styrene butadiene styrene copolymer (SBS).

[0009] In other features, the solid electrolyte is selected from pseudo binary sulfides, pseudo ternary sulfides, and pseudo quaternary sulfides. The solid electrolyte is selected from halide-based solid electrolytes and hydride-based solid electrolytes. The silicon layer is deposited using DC magnetron sputtering.

[0010] A solid-state battery cell, comprising: a cathode electrode, comprising a cathode current collector, and a cathode active layer, which is arranged on the cathode current collector and comprises a cathode active material and a solid electrolyte. The separator layer comprises a solid electrolyte. The solid electrolyte is selected from pseudo binary sulfides, pseudo ternary sulfides and pseudo quaternary sulfides. The anode layer comprises an anode current collector having a surface roughness Rz of 0.1 μm to 12 μm. The silicon layer is arranged on the anode current collector and comprises a plurality of concave spherical surfaces.

[0011] In other features, the silicon layer has a surface area of ​​105% to 300% of the corresponding flat surface. The anode current collector is made of one or more materials selected from copper, stainless steel, nickel, iron, titanium, tin (Sn) and alloys thereof.

[0012] In other features, the depth of the concave spherical surface is 0.1 μm to 20 μm. The anode current collector has a thickness of 4 μm to 30 μm.

[0013] In other features, the cathode active layer comprises 1 to 50 wt % solid electrolyte, 30 to 98 wt % cathode active material, 0 to 30 wt % conductive additive and 0 to 20 wt % binder. The cathode active material comprises one or more materials selected from the group consisting of rock salt layered oxides, spinels, polyanion cathodes, lithium transition metal oxides, surface coated cathode materials, doped cathode materials and low voltage cathode materials.

[0014] In other features, the conductive additive comprises one or more materials selected from the group consisting of carbon black, graphite, graphene, graphene oxide, SuperP, acetylene black, carbon nanofibers, and carbon nanotubes. The binder comprises one or more materials selected from the group consisting of polytetrafluoroethylene (PTFE), sodium carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), polyvinylidene fluoride (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS), and styrene butadiene styrene copolymer (SBS). The silicon layer is deposited using DC magnetron sputtering.

[0015] The present invention discloses the following embodiments:

[0016] 1. A solid-state battery cell, comprising:

[0017] A cathode electrode comprising:

[0018] a cathode current collector; and

[0019] a cathode active layer disposed on the cathode current collector and comprising a cathode active material and a solid electrolyte;

[0020] a separator layer comprising a solid electrolyte; and

[0021] An anode layer comprising:

[0022] an anode current collector; and

[0023] The silicon layer is disposed on the anode current collector and includes a plurality of concave spherical surfaces.

[0024] 2. The solid-state battery cell of embodiment 1, wherein the silicon layer has a surface area of ​​105% to 300% of the corresponding flat surface.

[0025] 3. The solid-state battery cell according to Embodiment 1, wherein the anode current collector is made of one or more materials selected from the group consisting of copper, stainless steel, nickel, iron, titanium, tin (Sn) and alloys thereof.

[0026] 4. The solid-state battery cell according to embodiment 1, wherein the anode current collector has a surface roughness Rz of 0.1 μm to 12 μm.

[0027] 5. The solid-state battery cell according to embodiment 1, wherein the depth of the concave spherical surface is 0.1 μm to 20 μm.

[0028] 6. The solid-state battery cell according to embodiment 1, wherein the anode current collector has a thickness of 4 μm to 30 μm.

[0029] 7. A solid-state battery cell according to embodiment 1, wherein the cathode active layer comprises 1 to 50 wt% of a solid electrolyte, 30 to 98 wt% of a cathode active material, 0 to 30 wt% of a conductive additive, and 0 to 20 wt% of a binder.

[0030] 8. A solid-state battery cell according to Embodiment 7, wherein the cathode active material comprises one or more materials selected from the group consisting of rock salt layered oxides, spinels, polyanion cathodes, lithium transition metal oxides, surface-coated cathode materials, doped cathode materials, and low voltage cathode materials.

[0031] 9. The solid-state battery cell according to Embodiment 7, wherein the conductive additive comprises one or more materials selected from the group consisting of carbon black, graphite, graphene, graphene oxide, Super P, acetylene black, carbon nanofibers, and carbon nanotubes.

[0032] 10. A solid-state battery cell according to embodiment 7, wherein the binder comprises one or more materials selected from the group consisting of polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), poly(vinylidene fluoride) (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS) and styrene butadiene styrene copolymer (SBS).

[0033] 11. The solid-state battery cell according to embodiment 1, wherein the solid electrolyte is selected from the group consisting of pseudo binary sulfides, pseudo ternary sulfides, and pseudo quaternary sulfides.

[0034] 12. The solid-state battery cell according to embodiment 1, wherein the solid electrolyte is selected from the group consisting of a halide-based solid electrolyte and a hydride-based solid electrolyte.

[0035] 13. The solid-state battery cell of embodiment 1, wherein the silicon layer is deposited using DC magnetron sputtering.

[0036] 14. A solid-state battery cell comprising:

[0037] A cathode electrode comprising:

[0038] a cathode current collector; and

[0039] a cathode active layer disposed on the cathode current collector and comprising a cathode active material and a solid electrolyte;

[0040] a separator layer comprising a solid electrolyte,

[0041] wherein the solid electrolyte is selected from pseudo binary sulfides, pseudo ternary sulfides and pseudo quaternary sulfides; and

[0042] An anode layer comprising:

[0043] an anode current collector having a surface roughness Rz of 0.1 μm to 12 μm; and

[0044] The silicon layer is disposed on the anode current collector and includes a plurality of concave spherical surfaces.

[0045] 15. The solid-state battery cell of embodiment 14, wherein:

[0046] The silicon layer has a surface area of ​​105% to 300% of the corresponding flat surface; and

[0047] The anode current collector is made of one or more materials selected from the group consisting of copper, stainless steel, nickel, iron, titanium, tin (Sn) and alloys thereof.

[0048] 16. The solid-state battery cell of embodiment 14, wherein:

[0049] The depth of the concave spherical surface is 0.1 μm to 20 μm; and

[0050] The anode current collector has a thickness of 4 μm to 30 μm.

[0051] 17. The solid-state battery cell of embodiment 14, wherein:

[0052] The cathode active layer comprises 1 to 50 wt % of a solid electrolyte, 30 to 98 wt % of a cathode active material, 0 to 30 wt % of a conductive additive, and 0 to 20 wt % of a binder; and

[0053] The cathode active material comprises one or more materials selected from the group consisting of rock salt layered oxides, spinels, polyanion cathodes, lithium transition metal oxides, surface coated cathode materials, doped cathode materials, and low voltage cathode materials.

[0054] 18. The solid-state battery cell of embodiment 17, wherein the conductive additive comprises one or more materials selected from the group consisting of carbon black, graphite, graphene, graphene oxide, Super P, acetylene black, carbon nanofibers, and carbon nanotubes.

[0055] 19. A solid-state battery cell according to embodiment 17, wherein the binder comprises one or more materials selected from the group consisting of polytetrafluoroethylene (PTFE), sodium carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), poly(vinylidene fluoride) (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS) and styrene butadiene styrene copolymer (SBS).

[0056] 20. The solid-state battery cell of embodiment 14, wherein the silicon layer is deposited using DC magnetron sputtering.

[0057] Further areas of applicability of the present disclosure will become apparent from the detailed description, claims and drawings.The detailed description and specific examples are intended for purposes of illustration only and are not intended to limit the scope of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0058] The present disclosure will become more fully understood from the detailed description and accompanying drawings, in which:

[0059] Figure 1 is a side cross-sectional view of an example of a battery cell;

[0060] Figure 2 is a side cross-sectional view of an example of a battery cell including an anode electrode having a concave spherical structure according to the present disclosure;

[0061] Figure 3 is a partial side cross-sectional view of an example of an anode electrode and separator layer according to the present disclosure;

[0062] Figure 4A and 4B are side cross-sectional views of examples of an anode electrode in a discharged and charged state, respectively, according to the present disclosure;

[0063] Figure 5 is a side cross-sectional view of an example of an anode electrode according to the present disclosure, illustrating the depth of the concave spherical structure;

[0064] Figure 6 is a functional block diagram of an example of a DC magnetron sputtering apparatus for depositing a silicon layer having a concave spherical structure on an anode current collector according to the present disclosure;

[0065] Figure 7 is a graph showing an example of capacity retention percentage as a function of cycles for a battery cell including a silicon anode having a concave spherical structure according to the present disclosure;

[0066] Figure 8 is a graph showing an example of capacity as a function of cycles for a battery cell including a silicon anode having a concave spherical structure according to the present disclosure;

[0067] Fig. 9 is a scanning electron microscope image of an example of a top surface of a silicon anode having a concave spherical structure according to the present disclosure; and

[0068] Fig.10 is a scanning electron microscope image of an example of a side view of a silicon anode having a concave spherical structure according to the present disclosure.

[0069] Among the drawings, reference numerals may be repeated to identify similar and / or identical elements. DETAILED DESCRIPTION

[0070] Although the present disclosure describes all-solid-state batteries for use in vehicle applications, the battery cells may be used in stationary or other types of applications.

[0071] Since silicon (Si) has more Li + Silicon (Si), which is abundant in nature, is a promising anode candidate due to its diffusion paths and high theoretical capacity. The development of high-performance anode electrodes including a silicon layer is important for constructing practical sulfide-based all-solid-state batteries (ASSBs). Typically, the Si layer of the anode electrode is manufactured using a wet coating method to form a sheet-type silicon layer on the anode current collector. However, the transport rate performance and cycling of the anode electrode with a sheet-type Si layer need to be enhanced.

[0072] The present disclosure relates to an ASSB including an anode electrode having a silicon layer with a concave spherical surface. In some examples, the silicon layer is deposited from a silicon target onto an anode current collector such as a roughened copper foil using pulsed DC magnetron sputtering. The concave spherical structure has an inverted bowl-like shape that increases the silicon / electrolyte interface area and enhances the power capability of the ASSB (even at 3C). The shape of the concave spherical structure also releases stress more effectively during cycling than a flat surface and is better able to withstand silicon expansion and contraction during cycling.

[0073] Compared to conventional wet coating methods, pulsed DC magnetron sputtering does not require the use of binders, solvents, and / or solid electrolytes for the anode electrode, which simplifies the manufacturing process.

[0074] Silicon is environmentally friendly and has reasonable electrochemical potential (~0.3 V vs Li / Li + ) and high theoretical capacity (for Li 4.4 When used in ASSBs containing sulfide electrolytes as solid electrolytes, the sulfide electrolytes can accommodate the expansion and contraction (eg, breathing) behavior of the silicon anode electrode during cycling.

[0075] Reference now Figure 1 , an all-solid-state battery (ASSB) cell 10 includes a cathode electrode 20, an anode electrode 40, and a separator layer 32 arranged in a predetermined order in a housing 50. The cathode electrodes 20-1, 20-2, .. and 20-C (where C is an integer greater than 1) include a cathode active layer 24 arranged on one or both sides of a cathode current collector 26. The anode electrodes 40-1, 40-2, ... and 40-A (where A is an integer greater than 1) include a silicon layer 42 on one or both sides of an anode current collector 46.

[0076] Reference now Figure 2 , the cathode electrode 20 includes a cathode current collector 26, a cathode active material 120, and a solid electrolyte 124 disposed on one or both sides of the cathode current collector 26. The separator layer 32 includes a solid electrolyte 132. The anode electrode 40 includes a silicon layer 42 having a concave spherical surface 142 disposed on one or both sides of the anode current collector 46.

[0077] Reference now Figures 3 to 5 The concave spherical surface 142 of the silicon layer 42 enhances the performance of the anode electrode 40. Figure 3 In FIG. 1 , the concave spherical surface 142 provides increased surface area for interfacing with the solid electrolyte 132 of the separator layer 32 to increase the ion conduction path and enhance power capability. Figure 4A and 4B In the embodiment of the present invention, the concave spherical surface 142 helps to relieve stress during cycling and accommodates the expansion and contraction of the silicon layer 42 during charging and discharging.

[0078] In some examples, the depths d1 and d2 of the concave spherical surface 142 ( Figure 5 ) is 0.1 μm to 20 μm. Depths d1 and d2 can be the same or different. In some examples, the complex 3D surface area of ​​silicon layer 42 is 105% to 300% of the flat 2D surface area (e.g., x dimension multiplied by y dimension). In some examples, the average thickness of silicon layer 42 is 1 μm to 50 μm (e.g., 8 μm).

[0079] In some examples, the anode current collector 46 is made of a material selected from the following: copper, stainless steel, nickel, iron, titanium, tin (Sn), alloys thereof and / or other conductive materials. For example, a coated foil, such as a graphene-coated or carbon-coated stainless steel foil (corrosion-resistant) can be used. In some examples, the anode current collector 46 includes a roughened copper current collector. The surface of the anode current collector 46 is a rough surface so as to be able to closely interface with the silicon layer 42. In some examples, the thickness of the anode current collector 46 is 4 μm to 30 μm (e.g., 18 μm), and the surface roughness Rz is 0.1 μm to 12 μm.

[0080] Reference now Figure 6 , shows a DC magnetron sputtering device 300 for depositing a silicon layer 42 having a concave spherical surface 142 on an anode current collector 46. The anode current collector 46 is arranged on a substrate support 314 in a process chamber 310. A magnetron cathode 316 including a magnet 320 and a target 318 is arranged above the substrate support 314.

[0081] During deposition, a process gas mixture such as argon (Ar) from a gas source 322 is introduced into the process chamber 310 while providing AC and / or DC power. In some examples, a mass flow controller 324 and a valve 326 are used to meter the process gas from the gas source 322. A throttle valve 334 and / or a pump 338 may be used to control the pressure within the process chamber 310 and / or to exhaust reactants from the process chamber 310. A DC source 344 provides a DC voltage to the magnetron cathode 316. An AC source 346 provides an AC voltage to the magnetron cathode 316.

[0082] During deposition, target material (Si) is ejected from target 318 and deposited on anode current collector 46. Material is also sputtered from the exposed surface of anode current collector 46, and in some examples, a silicon layer 42 having a concave spherical surface 142 is deposited using pulsed DC magnetron sputtering in an argon (Ar) atmosphere. In some examples, a silicon target (e.g., n-type; 99.995%) sputters silicon particles onto a roughened anode current collector (e.g., copper foil).

[0083] In some examples, the DC source 344 supplies a DC voltage of 200 V to 800 V (e.g., 450 V). In some examples, the cathode power from the AC source 346 is from 2 kW to 30 kW at a frequency of 20 kHz to 200 kHz. In some examples, the deposition time period is 20 to 840 minutes (e.g., 540 minutes).

[0084] Reference now Figure 7 and 8 , showing the performance of a battery cell including a bowl-shaped silicon layer. Figure 7 In the figure, the capacity retention percentage is shown as a function of the cycles. Figure 8 , the capacity is shown as a function of cycling. The battery cells with silicon layer 42 exhibit good rate performance and good battery cycling due to the unique concavity.

[0085] Reference now Fig. 9 and 10 , shows a scanning electron microscope image of the top surface of the silicon layer 42. The concave spherical structures are deposited in an adjacent manner on the exposed surface of the anode current collector 46. Fig. 9 In the example shown, the average diameter of the concave surface of the concave spherical structure is about 6 μm to 10 μm. Fig.10 In FIG. 5 , the recess has a depth of about 2 μm.

[0086] In some examples, the cathode active layer comprises a solid electrolyte (1 to 50 wt%), a cathode active material (30 to 98 wt%), a conductive additive (0 to 30 wt%), and a binder (0 to 20 wt%). In some examples, the cathode electrode has a thickness of 10 μm to 500 μm (e.g., 40 μm).

[0087] In some examples, the cathode active material comprises one or more materials selected from the group consisting of rock salt layered oxides, spinels, polyanion cathodes, lithium transition metal oxides, surface coated and / or doped cathode materials, and low voltage cathode materials.

[0088] Examples of rock salt layered oxides include LiCoO2, LiNixMn y Co 1-x-y O2、LiNixMn y Al 1-x-y O2、LiNixMn 1-x O2、Li 1+x MO2. Examples of spinels include LiMn2O4, LiNi 0.5 Mn 1.5 O4. Examples of polyanion cathodes include LiV2(PO4)3. Examples of surface-coated and / or doped cathode materials include LiNbO3-coated LiMn2O4, Li2ZrO3 or Li3PO4-coated LiNi x Mn y Co 1-x-y O2 and Al-doped LiMn2O4. Examples of low voltage cathode materials include lithiated metal oxides / sulfides (eg, LiTiS2), lithium sulfide, and sulfur.

[0089] In some examples, the conductive additive comprises one or more materials selected from the group consisting of carbon black, graphite, graphene, graphene oxide, SuperP, acetylene black, carbon nanofibers, carbon nanotubes, and other electronic conductive additives. Examples of binders include one or more materials selected from the group consisting of polytetrafluoroethylene (PTFE), sodium carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), poly(vinylidene fluoride) (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS), styrene butadiene styrene copolymer (SBS), and other suitable binders.

[0090] In some examples, the solid electrolyte in the separator layer and / or the cathode electrode is selected from pseudo binary sulfides, pseudo ternary sulfides, pseudo quaternary sulfides, halide-based solid electrolytes, and hydride-based solid electrolytes.

[0091] Examples of pseudo binary sulfides include the Li2S-P2S5 system (Li3PS4, Li7P3S 11 and Li 9.6 P3S 12), Li2S-SnS2 system (Li4SnS4), Li2S-SiS2 system, Li2S-GeS2 system, Li2S-B2S3 system, Li2S-Ga2S3 system, Li2S-P2S3 system, Li2S-Al2S3 system. Examples of pseudo-ternary sulfides include Li2O-Li2S-P2S5 system, Li2S-P2S5-P2O5 system, Li2S-P2S5-GeS2 system (Li 3.25 Ge 0.25 P 0.75 S4 and Li 10 GeP2S 12 )、Li2S-P2S5-LiX (X=F, Cl, Br, I) system (Li6PS5Br, Li6PS5Cl, L7P2S8I and Li4PS4I), Li2S-As2S5-SnS2 system (Li 3.833 Sn 0.833 As 0.166 S4), Li2S-P2S5-Al2S3 system, Li2S-LiX-SiS2 (X=F, Cl, Br, I) system, and 0.4LiI·0.6Li4SnS4 and Li 11 Si2PS 12 Examples of pseudo-quaternary sulfides include the Li2O-Li2S-P2S5-P2O5 system, Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 、Li7P 2.9 Mn 0.1 S 10.7 I 0.3 , and Li 10.35 [Sn 0.27 Si 1.08 ]P 1.65 S 12 .

[0092] Examples of halide-based solid electrolytes include Li3YCl6, Li3InCl6, Li3YBr6, LiI, Li2CdCl4, Li2MgCl4, Li2CdI4, Li2ZnI4, Li3OCl. Examples of hydride-based solid electrolytes include LiBH4, LiBH4-LiX (X = Cl, Br or I), LiNH2, Li2NH, LiBH4-LiNH2, Li3AlH6. In other examples, other types of solid electrolytes with low grain boundary resistance can be used.

[0093] The foregoing description is essentially only illustrative, and is by no means intended to limit the present disclosure, its application or use. The broad teaching of the present disclosure can be implemented in various forms. Therefore, although the present disclosure includes specific examples, the true scope of the present disclosure should not be so limited, because after studying the drawings, the specification and the appended claims, other modifications will become apparent. It should be understood that, without changing the principle of the present disclosure, one or more steps in the method can be performed in different orders (or simultaneously). In addition, although each of the embodiments is described above as having certain features, any one or more of those features described with respect to any embodiment of the present disclosure can be implemented in the features of any one in other embodiments and / or combined with the features of any one in other embodiments, even if the combination is not explicitly described. In other words, the described embodiments are not mutually exclusive, and the replacement of one or more embodiments with each other remains within the scope of the present disclosure.

[0094] Various terms are used to describe the spatial and functional relationships between elements (e.g., between modules, circuit elements, semiconductor layers, etc.), including "connected," "engaged," "coupled," "adjacent," "next to," "on top," "above," "below," and "disposed." Unless explicitly described as "direct," when describing the relationship between a first and a second element in the above disclosure, the relationship can be a direct relationship in which there are no other intervening elements between the first and second elements, but can also be an indirect relationship in which there are one or more intervening elements (spatially or functionally) between the first and second elements. As used herein, the phrase at least one of A, B, and C should be interpreted to mean a logical (A or B or C, AOR B OR C) using a non-exclusive logical OR, and should not be interpreted to mean "at least one of A, at least one of B, and at least one of C."

[0095] In the drawings, the direction of the arrows, as indicated by the arrows, generally represents the flow of information (e.g., data or instructions) of interest to the illustration. For example, when element A and element B exchange various information, but the information transmitted from element A to element B is relevant to the illustration, the arrow may be directed from element A to element B. This unidirectional arrow does not imply that no other information is transmitted from element B to element A. In addition, for information sent from element A to element B, element B may send a request for the information or an acknowledgment of receipt of the information to element A.

Claims

1. A solid-state battery cell, comprising: A cathode electrode comprising: a cathode current collector; and a cathode active layer disposed on the cathode current collector and comprising a cathode active material and a solid electrolyte; a separator layer comprising a solid electrolyte; and An anode layer comprising: an anode current collector; and The silicon layer is disposed on the anode current collector and includes a plurality of concave spherical surfaces.

2. The solid-state battery cell of claim 1, wherein the silicon layer has a surface area of ​​105% to 300% of the corresponding flat surface.

3. The solid-state battery cell according to claim 1, wherein the anode current collector is made of one or more materials selected from the group consisting of copper, stainless steel, nickel, iron, titanium, tin (Sn) and alloys thereof. 4 . The solid-state battery cell according to claim 1 , wherein the anode current collector has a surface roughness Rz of 0.1 μm to 12 μm. 5 . The solid-state battery cell according to claim 1 , wherein the depth of the concave spherical surface is 0.1 μm to 20 μm. 6 . The solid-state battery cell of claim 1 , wherein the anode current collector has a thickness of 4 μm to 30 μm.

7. The solid-state battery cell of claim 1, wherein the cathode active layer comprises 1 to 50 wt% solid electrolyte, 30 to 98 wt% cathode active material, 0 to 30 wt% conductive additive, and 0 to 20 wt% binder.

8. A solid-state battery cell according to claim 7, wherein the cathode active material comprises one or more materials selected from the group consisting of rock salt layered oxides, spinels, polyanion cathodes, lithium transition metal oxides, surface-coated cathode materials, doped cathode materials, and low voltage cathode materials.

9. The solid-state battery cell according to claim 7, wherein the conductive additive comprises one or more materials selected from the group consisting of carbon black, graphite, graphene, graphene oxide, Super P, acetylene black, carbon nanofibers, and carbon nanotubes.

10. The solid-state battery cell of claim 7, wherein the binder comprises one or more materials selected from the group consisting of polytetrafluoroethylene (PTFE), sodium carboxymethylcellulose (CMC), styrene-butadiene rubber (SBR), poly(vinylidene fluoride) (PVDF), nitrile rubber (NBR), styrene ethylene butylene styrene copolymer (SEBS), and styrene butadiene styrene copolymer (SBS).

Citation Information

Cited By

  • Solid-state secondary battery and electric device

    WO2026171258A1