Grain-oriented electrical steel sheet and method for producing same

By forming grooves of specific angles and depths on the cold-rolled steel sheet surface of the directional electromagnetic steel sheet, and introducing fine particles into the glass film on the recessed grooves, the grooves are formed by laser irradiation, and the process complexity and magnetic flux density in the prior art are solved in the prior art. The problem of reduction has achieved full play to the effect of magnetic domain subdividing and a significant reduction in iron loss.

CN118922574APending Publication Date: 2024-11-08NIPPON STEEL CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029358.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-04
Filing Date
2023-04-04
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the magnetic domain control of forming directional electromagnetic steel plates, the laser groove method has problems such as complex processes, tooth wear and magnetic flux density reduction, making it difficult to achieve high-speed processing and good iron loss reduction.

Method used

By forming a groove with an angle of 0 to 40°, a width of 20 to 300 μm and a depth of 10 to 40 μm on the surface of the cold-rolled steel sheet, and fine particles with an angle of 1 to 20 μm or less are introduced into the glass film on the recessed portion of the groove, and irradiation with laser light is used. Form grooves to control the shape and irradiation conditions of laser focus spots to optimize the magnetic domain subdividing effect.

Benefits of technology

The magnetic domain subdividing effect is fully utilized, which significantly reduces iron losses and improves the performance of directional electromagnetic steel plates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922574A_ABST
    Figure CN118922574A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a grain-oriented electrical steel sheet in which iron loss is further improved in magnetic domain control for forming a laser groove in a cold-rolled steel sheet. The present invention is a grain-oriented electrical steel sheet provided with the following requirements for achieving the above-mentioned purpose. Namely, the grain-oriented electrical steel sheet is characterized in that the grain-oriented electrical steel sheet is provided with a base material steel sheet having a plurality of grooves in the surface of the steel sheet, and a glass coating film positioned on the surface of the base material steel sheet, the absolute value of the angle (theta) formed by the direction orthogonal to the rolling direction and the thickness direction of the base steel plate and the longitudinal direction of the groove is 0-40 DEG, the width (W) of the groove is 20-300 [mu] m, the depth (D) of the groove is 10-40 [mu] m, the interval (P) of the groove in the rolling direction is 1-30 mm, and the thickness of the groove is 10-30 [mu] m in the interior of the glass coating film located directly below the surface of the recess of the groove. One or more microparticles having a long axis of 1 [mu] m or more and 20 [mu] m or less are present in a cross section orthogonal to the longitudinal direction of the groove.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a grain-oriented electromagnetic steel sheet. Background Art

[0002] Grain-oriented electrical steel sheets are steel sheets whose crystal orientation is controlled by a combination of cold rolling and annealing so that the easy magnetization axis of the crystal grains is aligned with the rolling direction.

[0003] As a technology for reducing eddy current loss, which is one of the iron losses of grain-oriented electromagnetic steel sheets, it is known to form an insulating film on the surface of a base steel sheet with controlled crystal orientation. The insulating film not only has electrical insulation properties, but also has the functions of imparting tension and rust resistance to the base steel sheet.

[0004] In addition, as another method for reducing eddy current loss, the following magnetic domain control method is known: by forming strain regions or grooves formed in a direction intersecting the rolling direction at predetermined intervals along the rolling direction, the width of the 180° magnetic domain is narrowed (the 180° magnetic domain is subdivided). The magnetic domain control method is classified into a method of applying strain to the base steel sheet of the directional electromagnetic steel sheet and a method of forming grooves on the surface of the base steel sheet where a film that applies tension to the base steel sheet exists.

[0005] By using a grain-oriented electromagnetic steel sheet that has been subjected to magnetic domain control using grooves to manufacture the iron core (winding core) of the transformer, the grooves will not disappear even after strain relief annealing, so the magnetic domain segmentation effect can be maintained. Therefore, as a method for reducing eddy current loss for the winding core, a magnetic domain control method using groove formation is sometimes used.

[0006] Figure 1 This is a diagram schematically showing an electromagnetic steel sheet having grooves formed therein. Figure 1 , a state in which a plurality of grooves 2 are formed at intervals on the surface of a base steel plate 1 along the rolling direction of the base steel plate 1 is shown. Figure 1 In the figure, the symbol θ represents the angle between the direction (plate width direction) perpendicular to the rolling direction and the plate thickness direction of the base steel plate 1 and the length direction of the groove 2. The symbol W represents the width of the groove 2, the symbol D represents the depth of the groove 2, and the symbol P represents the interval between adjacent grooves 2 in the rolling direction.

[0007] Various methods for forming grooves in electromagnetic steel sheets have been proposed. For example, Patent Document 1 discloses an electrolytic etching method for forming grooves on the surface of a grain-oriented electromagnetic steel sheet by electrolytic etching. For example, Patent Document 2 discloses a gear pressing method for forming grooves on the surface of a grain-oriented electromagnetic steel sheet by mechanically pressing a gear on the surface of the steel sheet.

[0008] However, the electrolytic etching method requires masking, etching, and mask removal, and has a problem of being more complicated than the mechanical method. The gear pressing method has a problem of wearing out the gears in a short period of time due to the high hardness of the electromagnetic steel sheet. From the perspective of further high-speed processing, it is difficult to achieve a line speed of 100 mpm or more as required in the general steel manufacturing process.

[0009] In addition, for example, Patent Document 3 discloses a laser irradiation method for melting and evaporating a laser irradiated portion of a grain-oriented electrical steel sheet surface by laser irradiation. The laser irradiation method does not cause problems such as tooth wear or complicated processes, and can also be processed at high speed.

[0010] In the laser irradiation method, several groove forming processes are also disclosed. For example, Patent Document 4 proposes forming grooves on a cold-rolled steel sheet by laser irradiation. However, when the cold-rolled steel sheet is laser irradiated, a glass film formed of forsterite is formed at the bottom of the groove in the final product. Since the glass film is a non-magnetic oxide, the magnetic flux density of the steel sheet is reduced, and the deterioration of the iron loss caused by this is a problem.

[0011] Prior art literature

[0012] Patent Literature

[0013] Patent Document 1: Japanese Patent Publication No. 62-54873

[0014] Patent Document 2: Japanese Patent Publication No. 62-53579

[0015] Patent Document 3: Japanese Patent Application Publication No. 2003-129135

[0016] Patent Document 4: International Publication No. 2019 / 156127

[0017] Patent Document 5: International Publication No. 2011 / 007771 Summary of the invention

[0018] Problems to be solved by the invention

[0019] The present invention has been developed in view of the above-mentioned actual situation, and an object of the present invention is to provide a grain-oriented electromagnetic steel sheet having further improved iron loss in magnetic domain control of laser grooves (grooves formed by laser irradiation) formed in a cold-rolled steel sheet.

[0020] Means for solving problems

[0021] The present inventors have repeatedly conducted in-depth research to solve the above-mentioned problems. In the process of repeatedly studying the laser irradiation conditions when forming the laser groove, it was found that if fine particles exist inside the glass film formed on the groove surface, the iron loss is improved. The present invention is completed based on this knowledge, and its main purpose is as follows. [1]

[0023] A grain-oriented electromagnetic steel sheet according to one embodiment of the present invention is a grain-oriented electromagnetic steel sheet, characterized in that it comprises a base steel sheet having a plurality of grooves on its surface and a glass film formed on the surface of the base steel sheet. The angle θ formed by the direction perpendicular to the rolling direction and the thickness direction of the base steel sheet and the longitudinal direction of the groove is 0 to 40°, the width W of the groove is 20 to 300 μm, the depth D of the groove is 10 to 40 μm, and the spacing P of the grooves in the rolling direction is 1 to 30 mm. Inside the glass film on the concave surface of each groove, there are at least one fine grain having a major axis of 1 μm or more and 20 μm or less in a cross section perpendicular to the longitudinal direction of the groove. [2]

[0025] The grain-oriented electrical steel sheet according to [1] is characterized in that the crystal orientation of fine grains inside the glass film on the surface of the recessed portion of the groove deviates from the Goss orientation, which is the crystal orientation of the adjacent base material, by 5° or more. [3]

[0027] A method for manufacturing a directional electromagnetic steel sheet according to one embodiment of the present invention is a method for manufacturing a directional electromagnetic steel sheet, characterized in that it is a method for manufacturing the directional electromagnetic steel sheet described in [1] or [2] above, wherein the manufacturing method includes a groove forming step of irradiating a surface of a cold-rolled steel sheet with a laser to form a groove, and as laser irradiation conditions, a focal point diameter dL of the laser in the rolling direction and a focal point diameter dC in the plate width direction satisfy equation (1).

[0028] 0.010≤dL / dC≤1.000 Formula (1)

[0029] Effects of the Invention

[0030] According to the present invention, the magnetic domain subdivision effect can be fully exerted, and a grain-oriented electrical steel sheet with good iron loss can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram showing an example of an electromagnetic steel sheet having grooves formed on the surface.

[0032] Figure 2 This is a diagram showing an example of an IPF map from the ND direction obtained by SEM-EBSD of fine particles existing in the glass film on the surface of the concave portion of the groove.

[0033] Figure 3 This is a diagram showing an example of a SEM image obtained by SEM-EBSD of fine particles existing in the glass film on the surface of the concave portion of the groove.

[0034] Figure 4 It is a schematic diagram showing an example of a cross section of a glass film on the surface of a concave portion of a groove. DETAILED DESCRIPTION

[0035] The inventors of the present invention have repeatedly studied to maximize the effect of magnetic domain segmentation, and found that the magnetic domain segmentation effect can be maximized by forming fine particles in the glass film on the surface of the concave portion of the groove. The structure of the grain-oriented electromagnetic steel sheet (hereinafter referred to as the present electromagnetic steel sheet) according to the embodiment of the present invention is described below.

[0036] The electromagnetic steel sheet includes a base steel sheet having a plurality of grooves arranged in parallel on the surface thereof and a glass coating film formed on the surface of the base steel sheet (see Figure 1 to Figure 4 In the present electromagnetic steel sheet, a tension film (insulating film) may be formed on the surface of the glass film. Figure 1 As shown in , a plurality of grooves are formed on the surface of the base steel plate in parallel so as to be adjacent to each other in the rolling direction of the base steel plate. The direction (angle θ), the width W, the depth D, and the interval P of the grooves are determined in consideration of the iron loss in the same manner as in the conventional grain-oriented electromagnetic steel sheet.

[0037] <Angle θ between the rolling direction of the base steel plate and the length direction of the groove>

[0038] If the angle θ formed by the direction (plate width direction) orthogonal to the rolling direction and plate thickness direction of the parent steel plate and the length direction of the groove is too large, there will be no magnetic domain control effect, and the iron loss improvement effect cannot be obtained, so it is set to 40° or less. The angle θ is preferably smaller and can be set to less than 35°, less than 30°, less than 25°, less than 20°, less than 15°, less than 10°, less than 8°, less than 6°, or less than 5°. The lower limit of the angle θ is 0°, that is, when the length direction of the groove is parallel to the plate width direction. It should be noted that the direction of the angle θ is not limited, and refers to the angle on the acute angle side of the angle formed by the length direction of the groove and the plate width direction. A plurality of grooves are arranged roughly in parallel on the surface of the parent steel plate, but as long as the angle θ of each groove is in the above-mentioned range.

[0039] <Slot width W>

[0040] The groove width W refers to the width of the groove on the surface of the parent steel plate in the cross section (groove cross section) of the groove in the plane perpendicular to the length direction of the groove. Even if the groove width W is less than 20μm and too narrow, it will not become the starting point for the generation of magnetic poles, there is no magnetic domain control effect, and good iron loss cannot be obtained. On the other hand, if it exceeds 300μm and is too wide, it will not become the starting point for the generation of magnetic poles, there is no magnetic domain control effect, only the magnetic flux density is significantly reduced, and good iron loss cannot be obtained. Therefore, the groove width W can be set to more than 20μm and less than 300μm. The lower limit of the groove width W can preferably be set to 25μm, 30μm, or 35μm. The upper limit of the groove width W can preferably be set to 250μm, 200μm, 150μm, 100μm, or 80μm.

[0041] <Groove Depth D>

[0042] When the groove depth D is less than 10 μm and too shallow, it will not become the starting point of the magnetic pole, there is no magnetic domain control effect, and good iron loss cannot be obtained. On the other hand, when it exceeds 40 μm and is too deep, the magnetic domain control effect reaches saturation, and only the magnetic flux density is significantly reduced, so good iron loss cannot be obtained. Therefore, the groove depth D can be set to more than 10 μm and less than 40 μm. The lower limit of the groove depth D can be preferably set to 11 μm, 12 μm, 13 μm, 14 μm, or 15 μm. The upper limit of the groove depth D can be preferably set to 38 μm, 36 μm, 34 μm, 32 μm, 30 μm, 28 μm, or 26 μm.

[0043] <Slot spacing P>

[0044] The groove spacing P is the spacing between the center lines of adjacent grooves arranged approximately parallel to each other on the surface of the base steel plate in the longitudinal direction, and refers to the distance in the rolling direction of the base steel plate. The center line of the groove is a line parallel to the longitudinal direction of the groove passing through the midpoint of the groove on the surface of the base steel plate in the groove cross section.

[0045] When the slot spacing P is less than 1mm and too narrow, the magnetic domain control effect is saturated, and only the magnetic flux density is significantly reduced, so good iron loss cannot be obtained. On the other hand, when it exceeds 30mm and is too wide, the magnetic domain control effect cannot be fully obtained, and good iron loss cannot be obtained. Therefore, the slot spacing P can be greater than 1mm and less than 30mm. The slot spacing P may not be equally spaced, but the slot spacing P with adjacent slots may be within the above range. The lower limit of the slot spacing P may preferably be 1.2mm, 1.4mm, 1.5mm, 1.6mm, 1.8mm, or 2.0mm. The upper limit of the slot spacing P may preferably be 25mm, 20mm, 15mm, 10mm, 7mm, or 5mm.

[0046] <Fine Particles in the Glass Film on the Surface of the Concave Part of the Groove>

[0047] The fine particles in the glass film on the surface of the concave portion of the groove in the present electromagnetic steel sheet will be described. Figure 2 to Figure 4 It is a cross-sectional view of the groove portion of the present electromagnetic steel sheet, and more specifically, it is a view obtained by observing a region including the groove in a cross section perpendicular to the longitudinal direction of the groove.

[0048] In the present electromagnetic steel sheet, the glass film on the surface of the concave portion of the groove formed on the surface of the base steel sheet is controlled so that fine particles exist inside the glass film. Specifically, Figure 2 As shown in , the glass film on the surface of the concave portion of the groove is controlled so that fine particles with a major axis of 1 μm or more and less than 20 μm are present. Furthermore, the crystal orientation of the fine particles is controlled so that it differs from the crystal orientation of the base material, i.e., the Goss orientation, by 5° or more.

[0049] Observation of fine particles of the glass film on the surface of the concave portion of the groove Figure 2 As shown in , the cross section of the groove perpendicular to the length direction of the groove (groove cross section) is mirror-polished and electrolytically polished, and the inverse pole figure (IPF) surface distribution diagram (crystal orientation diagram) is obtained using SEM-EBSD (Electron BackScattered Diffraction Pattern), which can confirm the fine particles 4 in the glass film 6. SEM and EBSD measurements can be performed under known conditions, and the measurement field or observation magnification, and EBSD measurement steps can be appropriately adjusted according to the size of the groove or fine particles. Figure 2 In the IPF diagram of FIG. 1 , when it is difficult to confirm the interface between the glass film 6 and the groove 2 , the interface can be confirmed using, for example, a SEM image of the same field of view. Figure 3 Representation and Figure 2 SEM images of the same field of view. Figure 4 The cross section of the groove is schematically shown. Figure 2 and Figure 3 In the figure, the island-shaped black part 6' in the base material 3 is a glass film. The glass film itself exists in a way that it is rooted in the base material, and the interface between the envelope below these glass films (including the parts that appear to be island-shaped) and the groove can be considered to be a glass film. As described above, the IPF map of EBSD can identify the microparticles in the glass film, and further confirm the crystal orientation of the microparticles and the Gauss orientation of the base material.

[0050] The reason why the fine particles inside the glass film on the concave surface of the groove reduce the iron loss is considered to be as follows. The magnetic domain segmentation in the grain-oriented electromagnetic steel sheet is achieved as follows: the static magnetic energy becomes higher due to the magnetic poles generated on the surface of the steel sheet, and a new 180° magnetic domain wall is generated to eliminate it, and the magnetic domain width becomes narrower. If the magnetic domain width is narrowed, the movement distance of the magnetic domain wall when the steel sheet is magnetized becomes shorter, and the energy loss when the magnetic domain wall moves is reduced, that is, the iron loss is reduced. Therefore, for the magnetic domain segmentation, magnetic poles must be generated, and an interface between the steel sheet and a material with different magnetic permeability must be generated. It is believed that the fine particles inside the glass film on the concave surface of the groove will become the starting point for the generation of magnetic poles, and the iron loss is reduced by promoting the magnetic domain segmentation.

[0051] If the long axis of the fine particles inside the glass film on the surface of the concave portion of the groove becomes longer, the magnetic properties may be significantly deteriorated, so the long axis of the fine particles may be 20 μm or less. Preferably, the upper limit of the long axis of the fine particles can be set to 19 μm, 18 μm, 17 μm, 16 μm, 15 μm, 14 μm, 13 μm, 12 μm, 11 μm, 10 μm, or 9 μm. The lower limit of the long axis length of the fine particles is not particularly limited, but can also be set to 1 μm or more according to the spatial resolution of SEM-EBSD.

[0052] In addition, it is preferable that the fine particles are flat in shape relative to the rolling direction. This is because it is believed that when the fine particles are flat, magnetic pole generation can be effectively achieved. Therefore, with respect to the fine particles observed in the groove cross section, the ratio of the major axis (the maximum length of the fine particles: La) to the minor axis (the maximum length of the fine particles in the direction perpendicular to the major axis: Lb) (aspect ratio = major axis length La / minor axis length Lb) can be greater than 1.0, preferably 1.1 or more, and more preferably 1.2 or more.

[0053] As for the fine particles, as long as there are more than one fine particle in the glass film on the surface of the concave portion of each groove, magnetic poles will be generated, and the effect of magnetic domain segmentation will be obtained. Therefore, it is not necessary for a plurality of fine particles to be arranged in a linear shape, and even if there is only one fine particle, excellent magnetic properties can be achieved. As long as there is a starting point for the generation of magnetic poles in each groove, there is no upper limit to the number of fine particles present in the glass film on the surface of the concave portion of each groove. That is, it is believed that by precisely controlling the groove shape and the fine particles in the glass film of the groove concave portion, magnetic poles can be effectively generated, and an excellent effect of magnetic domain segmentation can be obtained.

[0054] Regarding the number of fine particles in the glass film on the surface of the concave portion of each groove, at least one arbitrary groove is selected from the surface of the electromagnetic steel sheet, 10 arbitrary groove cross sections are selected from the selected groove, and the 10 selected groove cross sections are observed by SEM-EBSD as described above, and the number is set as the average value of the number of fine particles in the groove cross sections at the 10 locations. The number only needs to be 1.0 or more.

[0055] In order to make the fine grains the starting point for the generation of magnetic poles, the fine grains inside the glass film on the surface of the concave portion of the groove and the adjacent base material have a crystal orientation, that is, a Goss orientation {110} <001> (hereinafter sometimes referred to as "parent material Gaussian orientation.") The orientation difference can be 5° or more. Because when the orientation difference is less than 5°, the orientation difference with the parent material Gaussian orientation is too small and may not become the starting point for the generation of magnetic poles. In addition, as long as it becomes the starting point for the generation of magnetic poles, there is no upper limit on the crystal orientation difference between the fine particles and the parent material.

[0056] <Manufacturing method>

[0057] First, a cold-rolled steel sheet for the present electromagnetic steel sheet is manufactured by a known method. The steel sheet composition and the method for manufacturing the cold-rolled steel sheet are not particularly limited, and a known method, for example, the steel sheet composition and the method for manufacturing the steel sheet described in Patent Document 5 can be used.

[0058] However, the groove forming step by laser irradiation is preferably set after cold rolling and before the decarburization annealing step. The shape of the groove formed by laser irradiation is decarburized and finished without cold rolling, so the controllability of the groove shape is improved.

[0059] <Laser irradiation conditions>

[0060] The groove forming process is described. By irradiating the cold-rolled steel sheet with laser, a plurality of grooves are formed on the surface of the steel sheet in a direction intersecting the rolling direction in such a manner that the groove width W, the groove depth D, and the prescribed interval (groove interval P) are within a prescribed range. The laser irradiation conditions are not particularly limited to the type of laser light source, the laser output power, the laser scanning speed, and the steel sheet moving speed during laser irradiation, but the conditions that the groove width W, the groove depth D, and the prescribed interval (groove interval P) of the grooves are within the prescribed range can be appropriately selected.

[0061] [Laser light source]

[0062] As the laser light source, for example, a high-output laser generally used in industry, such as a fiber laser, a YAG laser, a semiconductor laser, or a CO2 laser, can be used. As long as the groove can be formed stably, it can be a pulse laser or a continuous wave laser.

[0063] [Laser output power]

[0064] When the laser output power is lower than 200W, the laser scanning speed is significantly reduced in order to form the desired groove, and the industrial productivity is reduced, so it can be set to 200W or more. It can be preferably 1000W or more, and more preferably 1500W or more. In addition, when the laser output power exceeds 3000W, the power supply capacity becomes large and the equipment cost becomes huge, which is not realistic in industry, so it can be set to 3000W or less. It can be preferably 2800W or less, and more preferably 2500W or less.

[0065] [Laser scanning speed]

[0066] When the laser scanning speed is lower than 5 m / s, the steel plate passing speed must be slowed down, and the productivity is reduced, so it is set to 5 m / s or more. It can be preferably 20 m / s or more, and more preferably 40 m / s or more. In addition, when the laser scanning speed is higher than 100 m / s, a high output power is required, and the equipment cost increases, so it can be set to 100 m / s or less. It can be preferably 80 m / s or less, and more preferably 60 m / s or less.

[0067] [Laser spot shape]

[0068] The shape of the laser light spot can be circular on the surface of the base steel plate or slightly widened in the plate width direction. In order to avoid excessive widening, for example, the laser light spot diameter in the rolling direction: dL, the laser light spot diameter in the plate width direction: dC can satisfy equation (1). For example, the laser light spot diameter dL in the rolling direction can be set to 5 to 100 μm, the light spot diameter dC in the plate width direction can be set to 5 to 100 μm, the laser output power can be set to 200 to 3000 W, and the laser scanning speed V can be set to 5 to 100 m / s.

[0069] 0.010≤dL / dC≤1.000 Formula (1)

[0070] This is because when dL / dC is larger than 1.000, the laser spot diameter becomes an elongated ellipse in the rolling direction, making it difficult to control the laser groove shape.

[0071] When dL / dC is less than 0.010, the laser spot diameter becomes an extremely elongated ellipse in the plate width direction, and in this case, it becomes difficult to control the laser groove shape.

[0072] Furthermore, the inventors have repeatedly conducted experiments and found that dL / dC affects the thickness of the molten layer on the surface of the groove recess. More specifically, it is confirmed that when the shape of the focal point is a moderate elliptical shape in the width direction of the steel plate as in the present invention, if dL / dC becomes smaller, the thickness of the molten layer on the surface of the groove recess becomes moderately thicker. It is believed that this is because: if the laser spot shape is set to a moderately long elliptical shape in the plate width direction, when the laser is continuously irradiated at an angle of less than 40° relative to the plate width direction, the heat generated by the laser irradiation becomes easy to conduct in the groove formation direction, and the controllability of the columnar crystals formed on the surface of the groove recess is improved.

[0073] The formation mechanism of fine particles is described below, but since the thickness of the molten layer has a strong influence on the formation of fine particles, it is preferably not too thick. Furthermore, if the thickness of the molten layer becomes too thick, recrystallization will occur not only from the base material during decarburization annealing (primary annealing), but also from within the molten layer, thereby generating grains with different orientations from the recrystallized grains from the base material. If there are many recrystallized crystals in the molten layer, the so-called secondary recrystallization, which preferentially grows in the Gaussian orientation during the finished annealing (secondary annealing), will be adversely affected, resulting in deterioration of the properties of the electromagnetic steel sheet. Therefore, it is necessary to control the thickness of the molten layer so that it does not become too thick, that is, so that dL / dC does not become too small.

[0074] Therefore, it is preferred to satisfy the relationship of formula (1). The lower limit of dL / dC is set to 0.01, but it can be preferably 0.015, 0.020, 0.025, 0.030, 0.035, 0.040, 0.045, or 0.050. The upper limit of dL / dC is 1 (circular spot), but as long as the laser spot shape is formed, it can be set to an ellipse that is appropriately long in the plate width direction, and it can be preferably set to 0.980, 0.960, 0.940, 0.920, 0.900, 0.880, 0.860, 0.840, 0.820, 0.800, 0.750, 0.700, 0.650, 0.600, 0.550, or 0.500.

[0075] In the above groove forming process, a groove is formed on the laser irradiated portion of the steel plate, and the thickness of the molten layer on the concave surface of the groove can be controlled. In the subsequent recrystallization annealing treatment, fine particles can be nucleated, and fine particles can be present inside the glass film on the concave surface of the groove as described above.

[0076] The generation mechanism of fine particles inside the glass film on the concave surface of the groove is considered to be as follows. The laser irradiated part of the cold-rolled steel sheet (parent steel sheet) is melted by laser irradiation to form a groove. After the surface of the groove is partially melted, the crystal grows in an oriented manner during the solidification process, so columnar crystals are generated from the cold-rolled steel sheet (parent material) side. The columnar crystals existing on the surface of the groove of the cold-rolled steel sheet are largely eroded by the crystal grains recrystallized from the internal structure of the cold-rolled steel sheet during the decarburization annealing in the next process. On the other hand, an internal oxide layer is formed from the surface of the cold-rolled steel sheet toward the inner layer, and the columnar crystals become covered and blocked by oxides. Therefore, the oxide functions as a pinning and becomes less likely to be eroded by the crystal grains recrystallized from the inside of the steel sheet. As a result, a part of the columnar crystals exists in the internal oxide layer, is not eroded, and remains as fine particles. In the subsequent secondary recrystallization, the internal oxide layer also becomes a glass film, and the fine particles in the glass film are not eroded by the Gauss orientation that grows preferentially in the secondary recrystallization, and remain to the final product.

[0077] As mentioned above, from the perspective of the fine particle generation mechanism, it is also clear that if the molten layer thickness is thicker, the size of the remaining fine particles will also become larger. Furthermore, if the molten layer thickness becomes too thick, as mentioned above, a large number of recrystallized grains will also be generated from the molten layer, which will have an adverse effect on the secondary recrystallization, specifically hindering the preferential growth of the Goss orientation, so it is important to control the molten layer thickness.

[0078] When dL and dC satisfy the prescribed relationship, the thickness of the molten layer does not become too thick, and the columnar crystals become fine. If the crystal grains are fine, the distance of oxide formation from the surface to the inner layer is short, and the recrystallized grains grow from the inside of the steel plate, forming pinning oxides before the columnar crystals that erode the surface layer, and become easy to remain. The remaining fine grains here are not eroded even in the secondary recrystallization of high-temperature annealing at 1200°C. It is believed that this is because: the internal oxide layer is transformed into a glass film during high-temperature annealing, so the pinning of the oxide still functions and is not eroded.

[0079] The focal spot diameter is not particularly limited as long as dL and dC satisfy the prescribed relationship, but the focal spot diameter is preferably smaller from the viewpoint of making the remaining recrystallized grains fine. The focal spot diameter can be selected based on the relationship with other properties of the electromagnetic steel sheet, and in practice, the upper limit of dC can be set to 300 μm, preferably 250 μm, 200 μm, 150 μm, or 100 μm.

[0080] [Assist gas]

[0081] It is also possible to blow auxiliary gas to the portion of the steel plate irradiated with the laser while irradiating the laser. The auxiliary gas plays the role of removing the components melted or evaporated from the steel plate by laser irradiation. By blowing the auxiliary gas, the laser stably reaches the steel plate, so that the groove is stably formed. The flow rate of the auxiliary gas is preferably set to 10 to 1000 liters per minute, for example.

[0082] Furthermore, the assist gas is preferably air or an inert gas.

[0083] <Steps after Groove Formation>

[0084] After the grooves are formed in the cold-rolled steel sheet, the cold-rolled steel sheet is decarburized and nitrided by a known method, and then an annealing separator mainly composed of MgO is applied, heated, maintained, and then cooled to form a glass film.

[0085] The decarburization conditions may be known conditions, but in order to further reduce the iron loss, it is effective to more precisely control the glass film formation behavior. For example, after heating to 850°C, the temperature is kept for 60 seconds and then cooled. The decarburization atmosphere is a hydrogen-inert gas atmosphere, and the oxygen potential (PH 2 O / PH 2 ) is set in the range of 0.15 to 0.80, and good characteristics can be obtained particularly in the range of 0.30 to 0.60.

[0086] Furthermore, by controlling the heating process conditions of the decarburization annealing, the internal oxidation of the columnar crystals in the groove recesses is promoted in the subsequent decarburization annealing process, and the fine particles can be stably ensured in the glass film in the subsequent final annealing process. For example, the residence time of 200 to 700°C during the heating process of the decarburization annealing can be preferably set to 50 seconds or less. If the residence time is less than 50 seconds, internal oxidation can be promoted in the subsequent decarburization annealing soaking process, so it is preferred. In addition, the oxygen potential (PH) during the heating process of the decarburization annealing 2 O / PH 2 ) may also be preferably 0.80 or less, and more preferably 0.60 or less. If it is 0.80 or less, internal oxidation is easily promoted in the subsequent decarburization annealing soaking process, so it is preferred.

[0087] The nitridation can also be performed by a known method. The nitridation amount can be set to, for example, a range of 50 to 400 ppm. In particular, good characteristics can be obtained when the nitridation amount is set to a range of 180 to 250 ppm.

[0088] For example,

[0089] The glass film is formed by a process of rolling up a steel sheet coated with an annealing separator into a coil, holding it at 1150 to 1250°C (finish annealing) for 10 to 30 hours, and then cooling it. The composition of the annealing separator can be a known composition, for example, it can be set to 100 parts by mass of MgO, 100 parts by mass of TiO 2 : 5 parts by mass, for example, FeCl is added so as to be 200 ppm in terms of chlorine 2 As a composition of additives. In order to further reduce iron loss, the water release rate from the annealing separator in the final annealing (room temperature to 700°C) can be preferably 0.5% or more and 6.0% or less. If the water release rate is 0.5% or more and 6.0% or less, the internal oxide layer can be suppressed from agglomerating to the surface of the steel sheet during the temperature rise process of the final annealing, and the formation of fine particles in the glass film can be promoted.

[0090] Tension can be applied to the steel sheet only by the glass coating, but a tension coating (insulating coating) may be formed on the glass coating to enhance the magnetic domain control effect. The tension coating may be composed mainly of aluminum phosphate, for example, and may have a thickness of about 1 μm.

[0091] Example

[0092] Next, examples of the present invention will be described. The examples are one embodiment of the present invention, and the present invention is not limited to this embodiment.

[0093] <Example 1>

[0094] A slab containing Si: 3.3 mass %, Mn: 0.10 mass %, S: 0.006 mass %, C: 0.060 mass %, acid-soluble Al: 0.027 mass %, and N: 0.008 mass % was hot rolled, hot-rolled sheet annealed, and cold rolled in sequence by a known method to obtain a steel sheet with a final sheet thickness of 0.22 mm.

[0095] Next, the laser output power was adjusted to 1800-2000W, the laser scanning speed was adjusted to 40-60m / s, and the laser was irradiated on the surface of the steel plate to form the laser grooves shown in Table 1. At this time, the focal point diameter dL of the laser in the rolling direction was adjusted within the range of 3-1000μm, and the focal point diameter dC of the laser in the plate width direction was adjusted within the range of 3-800μm, and the aspect ratio (dL / dC) of the focal point was adjusted as shown in Table 1.

[0096] Regarding the formed grooves, the groove angle θ is set to a direction inclined 0 to 80° in the rolling direction relative to the width direction of the steel plate, the groove depth D is set to 5 to 50 μm, the groove interval P is set to 0.4 to 50 mm, and the groove width W is set to 10 to 350 μm.

[0097] Furthermore, during the laser irradiation, air was blown at 100 liters / minute as an assist gas in order to effectively remove the metal of the steel plate melted and evaporated by the laser.

[0098] The grooved cold-rolled steel sheet was decarburized and further nitrided. The decarburization conditions were heating to 850°C, holding for 60 seconds and then cooling. The decarburization atmosphere was a hydrogen-nitrogen atmosphere, and the pH 2 O / PH 2 The nitriding amount was set to 200 ppm.

[0099] After that, the coating amount was adjusted to 4 g / m 2 The composition of the annealing separator is 100 parts by mass of MgO, 100 parts by mass of TiO 2 : 5 parts by mass FeCl was added so as to be 200 ppm in terms of chlorine 2 .

[0100] Next, the steel sheet coated with the annealing separator was coiled into a coil, kept at 1200°C for 20 hours, and then cooled to form a glass film on the surface. Furthermore, a tension film containing aluminum phosphate as a main component was formed to a thickness of 1 μm to obtain a grain-oriented electrical steel sheet. The tension at this time was 12 MPa with respect to the rolling direction including the glass film.

[0101] The iron loss W17 / 50 (energy loss measured under the excitation conditions of 1.7T and 50Hz) after the tensile insulation film was applied was measured. The results are shown in Table 1. In symbols B1 to B20 and symbols b1 to b11, b15, b16, b18, and b19, the magnetic flux density is the same, while in symbols B1 to B20, the iron loss is confirmed to be less than 0.750W / kg and is good. Regarding symbols b12, b13, b14, and b17, there is no secondary recrystallization, the number of fine particles cannot be counted, and the iron loss and magnetic flux density are significantly deteriorated.

[0102] <Example 2>

[0103] The slab described in Example 1 was used to form the laser grooves shown in Table 2 under the laser irradiation conditions shown in Table 2. A grain-oriented electrical steel sheet was manufactured by the same manufacturing method as described in Example 1 except for the laser irradiation conditions and the laser groove formation state shown in Table 2. For symbols C1 to C10 in which the crystal orientation of fine particles inside the glass film on the surface of the concave portion of the groove deviates from the crystal orientation of the base material by 5° or more, it was confirmed that the iron loss was 0.730 W / kg or less, which was better.

[0104] Table 1

[0105] Table 2

[0106]

[0107] Industrial Applicability

[0108] The present invention can be used in industrial equipment using a grain-oriented electromagnetic steel sheet, such as a winding core for a transformer.

[0109] Explanation of symbols

[0110] 1: Steel plate

[0111] 2: Slot

[0112] θ: Slot angle

[0113] W: Slot width

[0114] D: Groove depth

[0115] P: Slot spacing

[0116] 3: Base material

[0117] 4: Fine particles

[0118] 5: Base material

[0119] 6: Glass coating

[0120] 6': Glass coating

[0121] 7: Insulation film

[0122] 8: Fine particles

Claims

1. A directional electromagnetic steel sheet, characterized in that: The invention is a grain-oriented electromagnetic steel sheet having a base steel sheet having a plurality of grooves on its surface and a glass film formed on the surface of the base steel sheet, wherein: The angle θ formed by the direction perpendicular to the rolling direction and the plate thickness direction of the base steel plate and the length direction of the groove is 40° or less, the width W of the groove is 20 μm or more and 300 μm or less, the depth D of the groove is 10 μm or more and 40 μm or less, and the interval P of the groove in the rolling direction is 1.0 mm or more and 30.0 mm or less, In a cross section perpendicular to the longitudinal direction of the groove, 1.0 or more fine particles having a major axis of 1 μm or more and 20 μm or less exist inside the glass film on the surface of the concave portion of the groove.

2. The grain-oriented electrical steel sheet according to claim 1, characterized in that: The crystal orientation of the fine grains differs from the crystal orientation of the adjacent base steel plate, that is, the Goss orientation, by 5° or more.

3. A method for manufacturing a grain-oriented electromagnetic steel sheet, characterized in that: The method is a method for producing a grain-oriented electrical steel sheet according to claim 1 or 2, The manufacturing method includes a groove forming step of irradiating a surface of a steel plate with laser light to form a groove. As the irradiation conditions of the laser light, the focal point diameter dL of the laser light in the rolling direction and the focal point diameter dC of the laser light in the plate width direction satisfy the formula (1): 0.010≤dL / dC≤1.000Formula (1).