Flexible sulfide solid electrolyte and all-solid-state battery comprising same

By adjusting the ratio of bromine and chlorine and polymer binder type, a high flexibility and high ionic conductivity sulfur silver germanium ore sulfide solid electrolyte layer was prepared, which solved the cracking of the thiophosphate-based electrolyte layer under high strain. The problem improves the safety and performance of the battery.

CN118922970APending Publication Date: 2024-11-08FACTORIAL INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029285.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-20
Filing Date
2023-07-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The existing thiophosphate-based solid electrolyte layer is prone to cracks and wrinkles under high strain, resulting in electronic contact between the positive electrode and the negative electrode, posing a safety hazard, and the traditional polymer electrolyte has low ionic conductivity and poor thermal stability.

Method used

By adjusting the ratio of bromine and chlorine, using different types of polymer binders and binder content, a flexible sulfide solid electrolyte layer based on sulfosilan germanium ore is prepared to achieve its high flexibility and high ionic conductivity.

Benefits of technology

The bending radius of the sulfide solid electrolyte layer under high strain is not more than 4 cm and the bending strain is not less than 0.1%, while the lithium ion conductivity is improved and the safety and performance of the battery are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922970A_ABST
    Figure CN118922970A_ABST
Patent Text Reader

Abstract

The present disclosure relates to flexible membranes for sulfide solid electrolytes. In one embodiment, the flexible film has a bending strain of not less than 0.1%. In one embodiment, the flexible film has a lithium ion conductivity of not less than 0.5 mS / cm. The bending strain is calculated according to the formula [epsilon] M = h / (2r), where h is the thickness of the film and r is the bending radius of the film corresponding to no observable kink, wrinkle, crack or damage.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references

[0002] This application claims priority to US Serial No. 63 / 390,699, filed on July 20, 2022, the entire contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates to a flexible sulfide solid electrolyte for an all-solid-state battery. Background Art

[0004] All-solid-state batteries (ASSBs) have attracted much attention due to their potential for better safety and higher energy density compared to conventional lithium-ion batteries based on organic liquid electrolytes. Among them, ASSBs containing thiophosphate-based solid electrolytes (SEs) are promising due to their high ionic conductivity and good mechanical compatibility. The SE layer, which is an alternative to traditional liquid electrolytes, is inserted between the positive electrode (cathode) and the negative electrode (anode). In addition, the SE layer also has the functions of both electrolyte and separator, which allows the transport or flow of ions and prevents electronic contact between the positive and negative electrodes.

[0005] General requirements for the solid electrolyte (SE) layer include: a) high ionic conductivity, b) good chemical / electrochemical stability to prevent its original phase from being oxidized or reduced, and c) physical / mechanical strength to prevent the positive and negative electrodes from making direct or electronic contact (which would usually result in catastrophic heat dissipation and fire or explosion).

[0006] So far, there is no or little research on the physical properties of thiophosphate SE layers. Mechanical flexibility is an important physical property of thiophosphate SE layers. During the processing process, the SE layer may be damaged or cracked. These defects and / or cracks may cause electronic contact between the positive and negative electrodes.

[0007] The present disclosure provides a flexible thiophosphate SE layer that is less likely to crack and wrinkle even under high strain.

[0008] U.S. Patent No. US11024876 B2 discloses a flexible composite membrane comprising a polymer porous support having pores filled with an inorganic solid electrolyte. The flexibility of the composite membrane is attributed to the flexible polymer support. However, the use of polymers may have disadvantages such as low ionic conductivity, low thermal stability, and poor safety due to their flammability.

[0009] WO 2021 / 016319 A1 discloses a stretchable flexible lithium-ion battery comprising a polymer-based flexible electrolyte, wherein the electrolyte is selected from sodium (Na) superionic conductor (NASICON), garnet, perovskite, lithium (Li) superionic conductor (LISICON), lithium phosphorus oxynitride (LiPON), Li3N, argyrodite sulfide and antiperovskite. It also discloses that a polymer-based thin electrolyte can be used to achieve an electrolyte with consistent shape, flexibility and high ionic conductivity. It does not provide any flexible inorganic electrolyte.

[0010] Eckert, Zhang and Kennedy conducted thermomechanical optimization experiments on the Li2S-P2S5 system and presented it as a whole sample without a single phase (Chem. of Mat. 1990, 2, 273-279). U.S. Patent No. 8075865B2 discloses a single-phase lithium silver germanium sulfide. However, the patent does not disclose any mechanical properties or any method for preparing a flexible SE. There is still a need for flexible SEs and solid-state batteries including flexible SEs. Summary of the invention

[0011] The present disclosure provides a flexible solid electrolyte layer based on argyrodite lithium ion conductive material. In one aspect, the flexibility of the argyrodite SE layer is achieved by adjusting the ratio of bromine (Br) to chlorine (Cl). In another aspect, the flexibility of the argyrodite SE layer is achieved by adjusting 1) the Br / Cl ratio, 2) the polymer binder type, and / or 3) the binder content in a mixture such as a slurry.

[0012] The present disclosure provides a flexible membrane of a sulfide solid electrolyte. In one embodiment, the sulfide solid electrolyte is argyrodite. In one embodiment, the flexible membrane has a bending radius of no more than 4 cm. In one embodiment, the flexible membrane has a bending strain of no less than 0.1%.

[0013] Definitions and Abbreviations

[0014] The following terms will be used to describe the present disclosure. In the absence of specific definitions set forth herein, the terms used to describe the present disclosure should be given their ordinary meanings as understood by those of ordinary skill in the art.

[0015] As used herein, "bending radius" is a parameter that characterizes the flexibility of a material and is typically measured by the radius of a sheet or film sample that corresponds to a bend or arc when the sheet or film sample can be bent without causing any observable damage (Kim T et al., "Bending Strain and Bending Fatigue Lifetime of Flexible Metal Electrodes on Polymer Substrates," Materials 2019, 12, 2490). Observable damage may include cracks, kinks, or wrinkles. In one embodiment, the sheet or film has a thickness of 10-200 μm. In one embodiment, the sheet or film has a width or length of 3.0 to 10 cm. In one embodiment, the sheet or film is a 5.4 cm×5.4 cm square sheet with a thickness of 90 μm. In one embodiment, bending strain can also be used to measure the bendability or flexibility of a layer or film. In one embodiment, the bending strain (ε M ) is typically calculated by the most commonly used single-layer model and can be measured by the following formula (Kim T et al., "Bending Strain and Bending Fatigue Lifetime of Flexible Metal Electrodes on Polymer Substrates," Materials 2019, 12, 2490):

[0016] ε M =h / (2r),

[0017] Where h is the thickness of the sample and r is the minimum bending radius without causing any damage (eg, cracks, wrinkles, or kinks).

[0018] Higher ε M A higher value indicates better flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figures 1A to 1D A representative measurement of the bending radius by using a solid electrolyte membrane having a size of 5.4 cm×5.4 cm and a thickness of 90 μm is shown.

[0020] Figure 2A It is shown that for the formula Li 5.8 PS 4.8 Cl a Br b Representative relationship between Br / Cl ratio and bending radius for compounds with a+b=1.2.

[0021] Figure 2BShows the representative relationship between the Br / Cl ratio and the bending radius for compounds of the formula Li 5.4 PS 4.4 Cl a Br b (where a + b = 1.6).

[0022] Figure 3 Shows the X-ray diffraction (XRD) patterns of Examples 2, 4, 8 and Comparative Examples 1 and 2.

[0023] Figure 4 Shows flexible SEs prepared with two representative binders at different Br / Cl ratios. Detailed Description

[0024] In one embodiment, the present disclosure provides a flexible electrolyte membrane of a sulfide solid electrolyte having a compound represented by Formula I and having a thiargillite-type crystal structure: Li x M1 y M2 z P 1- p M3 p S 6-a-b-q O q Cl a Br b (Formula I), where 4 ≤ x ≤ 8, 0 ≤ y < 1, 0 ≤ z < 1, 0 ≤ p < 1, 0 ≤ q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6, 0 < 1 - p ≤ 1, 0 ≤ b / a ≤ 3.5, and where M1 is at least one element of Group 1 or Group 11 of the periodic table other than H or Li, M2 is at least one element of Group 2 of the periodic table, and M3 is at least one element of Group 14 of the periodic table.

[0025] In one embodiment, the flexible electrolyte membrane as disclosed in the present disclosure has a cubic crystal structure. In one embodiment, the electrolyte has a crystal structure in the space group as verified by XRD.

[0026] In one aspect, the present disclosure provides a flexible electrolyte membrane of a sulfide solid electrolyte having the following formula: Li x M1 y M2 z P 1-p M3 p S 6-a-b-q O q Cl a Br b(Formula I), where 4 ≤ x ≤ 8, 0 ≤ y < 1, 0 ≤ z < 1, 0 ≤ p < 1, 0 ≤ q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6, 0 < 1 - p ≤ 1, 0 ≤ b / a ≤ 7, and where M1 is at least one element of Group 1 or Group 11 in the Periodic Table other than H or Li, M2 is at least one element of Group 2 in the Periodic Table, and M3 is at least one element of Group 14 in the Periodic Table.

[0027] In one embodiment, the bending strain (ε M ) of the flexible electrolyte membrane is not less than 0.1%, where the bending strain is calculated according to the following formula:

[0028] ε M = h / (2r),

[0029] where h is the thickness of the membrane, and r is the bending radius without causing observable damage (such as cracks, wrinkles or kinks) to the membrane.

[0030] In one embodiment, the thickness of the flexible electrolyte membrane is in the range of 5 μm to 300 μm, 10 μm to 300 μm, 20 μm to 300 μm, 50 μm to 300 μm, 2 μm to 500 μm, 5 μm to 500 μm, 10 μm to 500 μm, 10 μm to 500 μm, 20 μm to 500 μm, 50 μm to 500 μm, or any and all ranges and sub - ranges therebetween.

[0031] In some embodiments, the lithium - ion conductivity of the electrolyte membrane is not less than 0.02 mS / cm, not less than 0.05 mS / cm, not less than 0.1 mS / cm, not less than 0.2 mS / cm, not less than 0.5 mS / cm or not less than 1 mS / cm. In some embodiments, the lithium - ion conductivity of the flexible electrolyte membrane is in the range of 0.05 mS / cm to 10 mS / cm, 0.1 mS / cm to 10 mS / cm, 0.25 mS / cm to 10 mS / cm, 0.5 mS / cm to 10 mS / cm, 0.75 mS / cm to 10 mS / cm, 0.05 mS / cm to 20 mS / cm, 0.1 mS / cm to 20 mS / cm, 0.25 mS / cm to 20 mS / cm, 0.5 mS / cm to 20 mS / cm, 0.75 mS / cm to 20 mS / cm, 0.05 mS / cm to 50 mS / cm, 0.1 mS / cm to 50 mS / cm, 0.25 mS / cm to 50 mS / cm, 0.5 mS / cm to 50 mS / cm, 0.75 mS / cm to 50 mS / cm, or any and all ranges and sub - ranges therebetween.

[0032] In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.02 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.05 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.1 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.2 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.5 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.55 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.60 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.65 mS / cm. In some embodiments, the electrolyte membrane has a bending strain of not less than 0.1% and a lithium ion conductivity of not less than 0.7 mS / cm.

[0033] In one embodiment, the formula of the sulfide electrolyte comprises at least one element selected from the group consisting of M1, M2, M3, and O. In some embodiments, formula (I) comprises one element selected from the group consisting of M1, M2, M3, and O. In some embodiments, formula I is selected from the group consisting of:

[0034] 1) Li x PS 6-a-b-q O q Cl a Br b , where 4 ≤ x ≤ 8, 0 < q ≤ 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6;

[0035] 2) Li x M1 y PS 6-a-b Cl a Br b , where 4 ≤ x ≤ 8, 0 < y < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b < 6;

[0036] 3) Li x M2 z PS 6-a-b Cl a Br b , where 4 ≤ x ≤ 8, 0 < z ≤ 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b < 6; and

[0037] 4) Li x P 1-p M3 p S 6-a-b Cl a Br b where 4 ≤ x ≤ 8, 0 < p ≤ 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b < 6, 0 < 1 - p < 1.

[0038] In some embodiments, the molar amount value of Br in the formula is greater than zero, i.e., b > 0.

[0039] In some embodiments, M1 is at least one element of Group 1 or Group 11 in the Periodic Table other than H or Li. In some embodiments, M1 is at least one selected from the group consisting of Na, K, Rb, Cs, Cu, Ag, and Au. In some embodiments, M1 is selected from the group consisting of Na, Cu, and Ag. In some embodiments, M2 is at least one element of Group 2 in the Periodic Table. In some embodiments, M2 is at least one selected from the group consisting of Be, Mg, Ca, Sr, and Ba. In some embodiments, M3 is at least one element of Group 14 in the Periodic Table. In some embodiments, M3 is at least one selected from the group consisting of Si, Ge, Sn, and Pb.

[0040] Introducing oxygen into the formula makes such materials more stable and / or less sensitive to oxygen or water. In one embodiment, when the formula is Li x PS 6-a-b-q O q Cl a Br b where 4 ≤ x ≤ 8, 0 < q ≤ 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6, the molar amount value q of O is in the range of 0 to 0.1, 0 to 0.2, 0 to 0.3, 0 to 0.4, 0 to 0.5, 0 to 0.6, 0.001 to 0.1, 0.001 to 0.2, 0.001 to 0.3, 0.001 to 0.4, 0.001 to 0.5, 0.001 to 0.6, 0.002 to 0.1, 0.002 to 0.2, 0.002 to 0.3, 0.002 to 0.4, 0.002 to 0.5, 0.002 to 0.6, 0.005 to 0.1, 0.005 to 0.2, 0.005 to 0.3, 0.005 to 0.4, 0.005 to 0.5, 0.005 to 0.6, or any and all ranges and sub - ranges therebetween. In one embodiment, the formula is Li 5.8 PS 4.7 O 0.1 Cl 1.2 . In one embodiment, the formula is Li x PS6-a-b-q O q Cl a Br b , where 4 ≤ x ≤ 8, 0 < q ≤ 1, 0 < a ≤ 2, 0 < b < 2, 0 < 6 - a - b - q < 6. In some embodiments, the value of b / a ranges from 0 to 3.5. In some embodiments, the value of b / a ranges from 0 to 7. In some embodiments, the value of b / a ranges from 0 to 10, 0 to 15, or 0 to 20. In some embodiments, the value of b / a is greater than zero.

[0041] In one embodiment, when the formula is Li x M1 y PS 6-a-b-q Cl a Br b , 4 ≤ x ≤ 8, 0 < y < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b < 6, the value of b / a ranges from 0 to 3.5. In some embodiments, the value of b / a ranges from 0 to 7. In some embodiments, the value of b / a ranges from 0 to 10, 0 to 15, or 0 to 20. In some embodiments, the value of b / a is greater than zero.

[0042] In one embodiment, when the formula is Li x M2 z PS 6-a-b Cl a Br b , where 4 ≤ x ≤ 8, 0 < z ≤ 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b < 6, the value of b / a ranges from 0 to 3.5. In some embodiments, the value of b / a ranges from 0 to 7. In some embodiments, the value of b / a ranges from 0 to 10, 0 to 15, or 0 to 20. In some embodiments, the value of b / a is greater than zero.

[0043] In one embodiment, when the formula is Li x P 1-p M3 p S 6-a-b Cl a Br b , 4 ≤ x ≤ 8, 0 < p ≤ 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b < 6, 0 < 1 - p < 1, the value of b / a ranges from 0 to 3.5. In some embodiments, the value of b / a ranges from 0 to 7. In some embodiments, the value of b / a ranges from 0 to 10, 0 to 15, or 0 to 20. In some embodiments, the value of b / a is greater than zero.

[0044] In some embodiments, formula (I) contains O and one element selected from the group consisting of M1, M2, and M3. In some embodiments, the sulfide solid electrolyte has a formula selected from the group consisting of: Li x M1 y PS 6-a-b-q O q Cl a Br b (4 ≤ x ≤ 8, 0 < y < 1, 0 < q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6), Li x M2 z PS 6-a-b-q O q Cl a Br b (4 ≤ x ≤ 8, 0 < z < 1, 0 ≤ q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6), and Li x P 1-p M3 p S 6-a-b-q O q Cl a Br b (4 ≤ x ≤ 8, 0 < p < 1, 0 < q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6, 0 < 1 - p < 1). In one embodiment, formula (I) contains O and does not contain M1, M2, or M3. In one embodiment, the formula of the sulfide electrolyte is Li x PS 6-a-b-q O q Cl a Br b (4 ≤ x ≤ 8, 0 < q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6). In some embodiments, the value of the molar amount of Br in the formula is greater than zero, i.e., b > 0.

[0045] In one embodiment, the total molar amount of halogens in the formula of the sulfide electrolyte is not greater than 2, i.e., a + b ≤ 2. In one embodiment, the total molar amount of halogens in the formula is not less than 2 and not greater than 3, i.e., 2 ≤ a + b ≤ 3. In one embodiment, the total molar amount of halogens in the formula is not less than 2 and less than 4, i.e., 2 ≤ a + b < 4. In one embodiment, the total molar amount of Br and Cl in the formula is not greater than 2, i.e., a + b ≤ 2. In one embodiment, the total molar amount of Br and Cl in the formula is not less than 2 and not greater than 3, i.e., 2 ≤ a + b ≤ 3. In one embodiment, the total molar fraction of Br and Cl in the formula is not less than 2 and less than 4, i.e., 2 ≤ a + b < 4.

[0046] In one embodiment, the sulfide solid electrolyte has a formula selected from the group consisting of: Li 5.8PS 4.7 O 0.1 Cl 1.2 、Li 5.9 P 0.9 Ge 0.1 S 4.8 Cl 1.2 、Li 5.7 Na 0.1 PS 4.8 Cl 1.2 、Li 5.4 PS 4.4 Cl 0.4 Br 1.2 、Li 5.8 PS 4.8 Cl 0.4 Br 0.8 、Li 5.4 PS 4.4 Cl 0.6 Br 1.0 、Li 5.4 PS 4.4 Cl 0.8 Br 0.8 、Li 5.4 PS 4.4 Cl 0.8 Br 0.8 、Li 5.8 PS 4.8 Cl 0.6 Br 0.6 、Li 5.4 PS 4.4 Cl 1.0 Br 0.6 、Li 5.4 PS 4.4 Cl 1.2 Br 0.4 、Li 5.8 PS 4.8 Cl 0.8 Br 0.4 、Li 5.8 PS 4.8 Cl 1.0 Br 0.2 and Li 5.4 PS 4.4 Cl 1.4 Br 0.2 。

[0047] In some embodiments, the flexible SE film includes a binder, wherein the percentage of the binder is between 0.02 wt % and 5 wt %, 0.02 wt % and 10 wt %, 0.02 wt % and 15 wt %, 0.02 wt % and 20 wt %, 0.05 wt % and 5 wt %, 0.05 wt % and 10 wt %, 0.05 wt % and 15 wt %, 0.05 wt % and 20 wt %, 0.1 wt % and 5 wt %, 0.1 wt % and 10 wt %, 0.1 wt % and 15 wt % %, 0.1 wt % to 20 wt %, 0.2 wt % to 5 wt %, 0.2 wt % to 10 wt %, 0.2 wt % to 15 wt %, 0.2 wt % to 20 wt %, 0.5 wt % to 5 wt %, 0.5 wt % to 10 wt %, 0.5 wt % to 15 wt %, 0.5 wt % to 20 wt %, 1 wt % to 5 wt %, 1 wt % to 10 wt %, 1 wt % to 15 wt %, 1 wt % to 20 wt %, or any ranges and subranges therebetween.

[0048] In one aspect, the present disclosure provides an all-solid-state battery comprising a flexible electrolyte membrane as disclosed herein.

[0049] In one embodiment, the all-solid-state battery further comprises a positive electrode comprising a positive electroactive material.

[0050] In one embodiment, during operation of the all-solid-state battery, the positive electrode active material exhibits a redox reaction at a potential of 2 V or more based on a lithium electrode.

[0051] In one embodiment, the positive electrode active material comprises Li, Ni, and Co. In one embodiment, the positive electrode active material comprises Li, Ni, and Co, and at least one of Mn and Al.

[0052] In one embodiment, the positive electrode active material includes at least one of Fe and P.

[0053] In one embodiment, the all-solid-state battery further comprises a positive electrode layer containing a positive active material and a negative electrode layer, wherein the flexible electrolyte membrane is disposed between the positive electrode layer and the negative electrode layer.

[0054] In one embodiment, the negative electrode layer includes particles of a carbon-based conductive material having at least one selected from the group consisting of carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, natural graphite, and artificial graphite.

[0055] In one embodiment, the negative electrode layer includes a metal having at least one selected from the group consisting of lithium, sodium, magnesium, aluminum, silicon, calcium, titanium, manganese, iron, cobalt, nickel, zinc, molybdenum, silver, indium, tin, and tungsten.

[0056] In one aspect, the flexibility of the electrolyte membrane or layer disclosed herein is not only due to the polymer porous support layer (scaffold layer). In order to exclude the influence of the polymer porous support layer on the flexibility, the same polymer porous support was used in all examples in Table 1 to study other factors such as Br / Cl ratio, polymer binder type and polymer binder content.

[0057] In one aspect, the present disclosure provides a method for preparing a flexible electrolyte membrane by a wet process or a dry process. In one embodiment, the wet process may include:

[0058] 1) mixing particles of a sulfide electrolyte having formula (I), a binder and a solvent to obtain a slurry;

[0059] 2) coating the slurry on a substrate, and then vacuum drying at room temperature, wherein the substrate includes a film and a non-woven fabric, thereby obtaining a dry coating layer attached to the non-woven fabric; and

[0060] 3) The dried coating layer with the nonwoven fabric is peeled off from the membrane, thereby obtaining an electrolyte membrane.

[0061] In one embodiment, when the slurry is applied to the nonwoven fabric of the substrate, the pores of the nonwoven fabric are filled with a mixture comprising particles, a binder and a solvent. Once a dry coating is formed after substantially removing the solvent, the nonwoven fabric is attached to the electrolyte layer and forms a part of the electrolyte layer.

[0062] In one embodiment, the particles of the sulfide electrolyte are prepared by mixing raw precursor powders in a stoichiometric ratio in an inert atmosphere, followed by sintering at 400-700° C. for 4-24 hours and grinding. In some embodiments, the raw precursor powders include Li2S, Na2S, P2S5, LiCl, LiBr, Li2O, and GeS2.

[0063] In one embodiment, the binder used in the wet process can be a non-aqueous acrylate type binder, a rubber type binder, such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), poly(vinylidene fluoride) (PVDF), polyethylene (PE), vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride-co-trichloroethylene, polyacrylonitrile, polymethyl methacrylate, polyvinyl pyrrolidone, polyvinyl acetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, polysaccharide polymers and carboxymethyl cellulose, or a combination thereof.

[0064] In one embodiment, the solvent comprises xylene.

[0065] In one embodiment, the particles, binder, and solvent are mixed in a planetary centrifugal mixer.

[0066] In one embodiment, the film in the substrate is a PET film. In one embodiment, the nonwoven fabric is used as a support layer or a mechanical support layer. In one embodiment, the nonwoven fabric is made of polyester. Non-restrictive specific polyesters include polyethylene terephthalate (PET). In some embodiments, the thickness of the nonwoven fabric is about 7.5 μm, about 10 μm, about 12 μm, about 15 μm, about 17 μm or about 20 μm. In some embodiments, the porosity of the nonwoven fabric is about 70%, 73%, about 75%, about 78%, about 80%.

[0067] In some embodiments, the method further comprises peeling the dried coating having the scaffold layer from the membrane.

[0068] In another embodiment, a representative dry process may include:

[0069] 1) mixing particles of a sulfide electrolyte having formula (I) with a binder to obtain a mixture; and

[0070] 2) Forming the mixture into an electrolyte membrane.

[0071] In some embodiments, the binder is a fibrillizable binder. In some embodiments, the fibrillizable binder includes polytetrafluoroethylene (PTFE), ultra-high molecular weight (UHMW) polyethylene (PE) and combinations thereof. In some embodiments, the particles and the binder are mixed at a temperature below the melting point of the binder and sufficient to soften the binder. In some embodiments, the temperature is in the range of 70°C to 300°C, 80°C to 300°C, 90°C to 300°C, 100°C to 300°C, 110°C to 300°C, 120°C to 300°C, 130°C to 300°C, 150°C to 300°C, or all and any ranges and sub-ranges therebetween.

[0072] In some embodiments, the mixture is formed into an electrolyte membrane by calendaring. In one embodiment, calendaring is performed on a roller.

[0073] The present disclosure will be better understood by reference to the following experimental details, but those skilled in the art will readily appreciate that the specific experiments detailed are merely illustrative and are not meant to limit the present disclosure as described herein, which is defined by the appended claims.

[0074] It should be noted that the transitional term "comprising" is synonymous with "including," "containing," or "characterized by," is inclusive or open-ended, and does not exclude additional, unrecited elements or method steps.

[0075] Example

[0076] Synthesis of solid electrolyte materials

[0077] In a glove box with an inert argon atmosphere, raw material precursor powders were prepared in a stoichiometric ratio. Precursor examples include, but are not limited to, Li2S, Na2S, P2S5, LiCl, LiBr, Li2O, GeS2, and any combination thereof. These powders were ball milled for 4 hours using a planetary ball mill. Subsequently, these powders were sintered at 450°C for 12 hours.

[0078] Thus, a solid electrolyte material having an argyrodite type structure was obtained. After the milling process, the average particle size of the solid electrolyte particles was in the range of 1 to 10 μm and would be used for slurry preparation.

[0079] Preparation of solid electrolyte slurry

[0080] The solid electrolyte, binder, solvent and zirconium oxide grinding media are mixed using a planetary centrifugal mixer. The binder includes but is not limited to PTFE, a rubber-type binder (e.g., SBR) and a non-aqueous acrylate-type binder. The solvent includes but is not limited to xylene.

[0081] Preparation of solid electrolyte membrane

[0082] In a drying room with a dew point below -50 ° C, the obtained solid electrolyte slurry was coated on a release polyethylene terephthalate film (50 μm) using a scraper, and the film was then dried overnight at room temperature in a vacuum oven. Non-woven fabric was used as a support layer to provide the necessary mechanical support for the self-supporting solid electrolyte layer. The thickness of the solid electrolyte layer produced was about 90 μm. The solid electrolyte layer was cut into a film of 5.4 cm × 5.4 cm in size for testing.

[0083] Characterization and testing of solid electrolyte membranes

[0084] Powder X-ray diffraction (XRD) measurements were performed using an X-ray diffractometer with Cu-Kα radiation (SmartLab, Rigaku). -1The diffraction data were collected at a scan rate of 0.05° in the 2θ range of 5-60°. XRD measurements were performed using an airtight container to prevent air exposure to the electrolyte powder. For ionic conductivity: the SE membrane was first punched into a disc with a diameter of 1.2 cm and pressed at a stacking pressure of 375 MPa in a torque unit (PEEK). Titanium plungers were used as current collectors. The ionic conductivity of the solid electrolyte membrane was measured by electrochemical impedance spectroscopy (EIS) and collected in the range of 1 Hz to 7 MHz using a potentiostat (SP200, Biologic) with an applied AC voltage of 10 mV. All measurements were performed at room temperature.

[0085] Figures 1A to 1D A typical process for measuring the bending radius according to one embodiment of the present disclosure is provided. First, a solid electrolyte membrane ( Figure 1A ). A bending force is applied to the membrane, and the two opposite edges approach each other ( Figure 1B ).like Figure 1C As shown, the flexibility of the membrane is reflected by the distance between the two opposite edges when there are no observable wrinkles or cracks in the membrane, or by the bending radius (r) corresponding to the curved or curved membrane. Once the membrane is overbent, the membrane will have a Figure 1D The observable wrinkles or cracks are shown by the arrows in the figure. The smaller the value of the bending radius, the higher the flexibility of the film. In one embodiment, the bending test is performed with the naked eye or under a microscope or optical magnifier.

[0086] Table 1 summarizes the bending radius (r), bending strain (ε M ) and lithium ion conductivity.

[0087] Figure 2A The formula is Li 5.8 PS 4.8 Cl a Br b Representative relationship between Br / Cl ratio and bending radius of SE sheets or films, where the total mole fraction of halogen, i.e., a+b, is 1.2. Figure 2B The formula is Li 5.4 PS 4.4 Cl a Br b Figure 2 shows a representative relationship between the Br / Cl ratio and the bending radius of a SE sheet or film, where the total mole fraction of halogen, i.e., a+b, is 1.6. These two figures clearly show that when the Br / Cl molar ratio is not greater than 4, the film exhibits better flexibility, i.e., the bending radius (r) is not greater than 4 cm and the bending strain is not less than 0.1%.

[0088] As also shown in Table 1, SE may include other elements, including but not limited to O and Ge. In one embodiment, SE does not include Br.

[0089] Table 1 Bending radius (r), bending strain (ε M ) and lithium ion conductivity

[0090]

[0091] a: A sheet was prepared using 1.25 wt% of Binder 1, which was an acrylate binder.

[0092] like Figure 4 As shown, a flexible SE film (bending strain of at least 0.1%) was obtained. This clearly shows that increasing the amount of polymer binder makes the SE film flexible. For binder 1, the curve fitting yields the equation,

[0093] Br / Cl = 183x - 2.11 (Equation 1),

[0094] where x is the weight percent of binder in the SE film.

[0095] Equation 1 describes the highest Br / Cl ratio that results in SE film flexibility at different weight percentages of Binder 1. All compositions falling within or below the equation can produce flexible SE films.

[0096] For Binder 2, the curve fit yields the equation,

[0097] Br / Cl = 345x - 1.94 (Equation II),

[0098] where x is the weight percentage of binder 2 in the SE film.

[0099] Equation II describes the highest Br / Cl ratio that results in SE film flexibility at different weight percentages of Binder 2.

[0100] This clearly demonstrates that the structure of the binder plays an important role in determining the flexibility of the SE film.

[0101] The solid electrolyte material was prepared according to the steps in Example 1. The solid electrolyte particles were mixed with a binder 2 and PTFE to form a mixture, and each mixture was then formed into a solid electrolyte membrane having a desired thickness by calendering. The weight percentage of the binder in the mixture ranged from 0.5 wt % to 7 wt %. The flexibility of the membrane is summarized in Table 2.

[0102] Table 2 Bending radius (r) and bending strain (ε) of SE films or sheets with different compositions M )

[0103] SE composition Br / Cl r(cm) <![CDATA[ε M (%)]]> Example 1 <![CDATA[Li 5.8 PS 4.8 Cl 1.2 ]]> 0 <0.75 >0.6 Embodiment 11 <![CDATA[Li 5.8 PS 4.8 Cl 0.4 Br 0.8 ]]> 2 <0.75 >0.6 Comparative Example 1 <![CDATA[Li 5.4 PS 4.4 Cl 0.2 Br 1.4 ]]> 7 <0.75 >0.6

[0104] In one aspect of the present disclosure, the electrolyte membrane comprises:

[0105] a) a sulfide solid electrolyte having the formula Li x M1 y M2 z P 1-p M3 p S 6-a-b-q O q Cl a Br b (Formula I), where 4 ≤ x ≤ 8, 0 ≤ y < 1, 0 ≤ z < 1, 0 ≤ p < 1, 0 ≤ q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6, 0 < 1 - p ≤ 1, 0 ≤ b / a ≤ 20, and where M1 is at least one element of Group 1 or Group 11 of the periodic table other than H or Li, M2 is at least one element of Group 2 of the periodic table, and M3 is at least one element of Group 14 of the periodic table; and

[0106] b) a binder, the weight percentage of which in the flexible electrolyte membrane ranges from 0.05 wt% to 10 wt%,

[0107] wherein the electrolyte membrane has a bending strain (ε M ) of not less than 0.1%, and wherein the bending strain is calculated according to the following formula:

[0108] ε M = h / (2r),

[0109] where h is the thickness of the membrane and r is the bending radius of the membrane obtained without causing any damage to the membrane.

[0110] In a second aspect, the value of b / a is not higher than the threshold determined by the equation.

[0111] In a third aspect according to the second aspect, for an acrylate binder, the equation is b / a = 183x - 2.11 (Equation I), where x refers to the weight percentage of the acrylate binder in the electrolyte membrane.

[0112] In a fourth aspect according to the second aspect, for a PTFE binder, the equation is b / a = 345x - 1.94 (Equation II), where x refers to the weight percentage of the PTFE binder in the electrolyte membrane.

[0113] In a fifth aspect according to the first aspect, the lithium ion conductivity of the electrolyte membrane ranges from 0.05 to 20 mS / cm.

[0114] In a sixth aspect according to the first aspect, the electrolyte membrane has a lithium ion conductivity of not less than 0.5 mS / cm.

[0115] In a seventh aspect according to the first aspect, the thickness of the electrolyte membrane is in the range of 5 μm to 300 μm.

[0116] In an eighth aspect according to the first aspect, the electrolyte membrane further includes a nonwoven fabric or an equivalent as a support layer.

[0117] In a ninth aspect according to the first aspect, Formula I is selected from the group consisting of:

[0118] a)Li x PS 6-a-b Cl a Br b , where 4≤x≤8, 0 <a≤2、0≤b<2、0<6-a-b<6;

[0119] b)Li x M1 y PS 6-a-b Cl a Br b , where 4≤x≤8, 0 <y<1、0<a≤2、0≤b<2、0<6-a-b<6;

[0120] c)Li x M2 z PS 6-a-b Cl a Br b , where 4≤x≤8, 0 <z<1、0<a≤2、0≤b<2、0<6-a-b<6;

[0121] d)Li x P 1-p M3 p S 6-a-b Cl a Br b , where 4≤x≤8, 0 <p<1、0<a≤2、0≤b<2、0<6-a-b<6、0<1-p<1;

[0122] e)Li x PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0 <q≤1、0<a≤2、0≤b<2、0<6-a-b-q<6;

[0123] f)Li x M1 y PS 6-a-b-q Oq Cl a Br b , where 4 ≤ x ≤ 8, 0 < y < 1, 0 < q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6;

[0124] g) Li x M2 z PS 6-a-b-q O q Cl a Br b , where 4 ≤ x ≤ 8, 0 < z < 1, 0 ≤ q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6; and

[0125] h) Li x P 1-p M3 p S 6-a-b-q O q Cl a Br b , where 4 ≤ x ≤ 8, 0 < p < 1, 0 < q < 1, 0 < a ≤ 2, 0 ≤ b < 2, 0 < 6 - a - b - q < 6, 0 < 1 - p < 1.

[0126] In the tenth aspect according to the first aspect, the total molar amount of Br and Cl is less than 2, i.e., a + b ≤ 2.

[0127] In the eleventh aspect according to the first aspect, the sulfide solid electrolyte has a formula selected from the group consisting of: Li 5.8 PS 4.7 O 0.1 Cl 1.2 , Li 5.9 P 0.9 Ge 0.1 S 4.8 Cl 1.2 , Li 5.7 Na 0.1 PS 4.8 Cl 1.2 , Li 5.4 PS 4.4 Cl 0.4 Br 1.2 , Li 5.8 PS 4.8 Cl 0.4 Br 0.8 , Li 5.4 PS 4.4 Cl 0.6 Br 1.0 , Li 5.4 PS 4.4 Cl 0.8 Br 0.8 , Li5.4 PS 4.4 Cl 0.8 Br 0.8 , Li 5.8 PS 4.8 Cl 0.6 Br 0.6 , Li 5.4 PS 4.4 Cl 1.0 Br 0.6 , Li 5.4 PS 4.4 Cl 1.2 Br 0.4 , Li 5.8 PS 4.8 Cl 0.8 Br 0.4 , Li 5.8 PS 4.8 Cl 1.0 Br 0.2 and Li 5.4 PS 4.4 Cl 1.4 Br 0.2 .

[0128] In a twelfth aspect of the present disclosure, an all-solid-state battery comprises the electrolyte membrane as disclosed herein.

[0129] In a thirteenth aspect of the present disclosure, the all-solid-state battery further includes a positive electrode comprising a positive electrode electroactive material.

[0130] In a fourteenth aspect according to the thirteenth aspect, during operation of the all-solid-state battery, the positive electrode active material is + At a potential of 2 V or more, a redox reaction is exhibited.

[0131] In a fifteenth aspect of the present disclosure, a method for preparing an electrolyte membrane includes mixing particles of a sulfide solid electrolyte and a polymer binder to obtain a mixture.

[0132] In the sixteenth aspect according to the fifteenth aspect of the present disclosure, particles of a sulfide solid electrolyte are synthesized by mixing raw precursor powders in a stoichiometric ratio in an inert atmosphere, followed by sintering at 400-700° C. for 4-24 hours and grinding. The raw precursor powders include Li2S, Na2S, P2S5, LiCl, LiBr, Li2O and GeS2.

[0133] In a seventeenth aspect according to the fifteenth aspect of the present disclosure, wherein the mixture comprises a solvent and the mixture is a slurry.

[0134] In an eighteenth aspect according to the seventeenth aspect of the present disclosure, the method further comprises:

[0135] a) coating the mixture onto a substrate, followed by vacuum drying at room temperature, wherein the substrate comprises a film and a nonwoven fabric, thereby obtaining a dry coating layer attached to the nonwoven fabric; and

[0136] b) peeling the dry coating layer from the membrane, thereby obtaining an electrolyte membrane including the dry coating layer and the nonwoven fabric.

[0137] In a nineteenth aspect according to the eighteenth aspect of the present disclosure, the film in the substrate is a PET film, and the nonwoven fabric is made of polyester having a thickness of about 10 μm.

[0138] In a twentieth aspect according to the fifteenth aspect of the present disclosure, the mixture is substantially free of solvent, and the mixture is formed into a film by calendaring.

Claims

1. An electrolyte membrane comprising: a) has the formula Li x M1 y M2 z P 1-p M3 p S 6-a-b-q O q Cl a Br b (Formula I) sulfide solid electrolyte, wherein 4≤x≤8, 0≤y<1, 0≤z<1, 0≤p<1, 0≤q<1, 0<a≤2, 0≤b<2, 0<6-abq<6, 0<1-p≤1, 0≤b / a≤20, and wherein M1 is at least one element of Group 1 or Group 11 in the periodic table other than H or Li, M2 is at least one element of Group 2 in the periodic table, and M3 is at least one element of Group 14 in the periodic table; and b) a binder, the weight percentage of which in the flexible electrolyte membrane is in the range of 0.05 wt % to 10 wt %, The electrolyte membrane has a bending strain (ε M ), and wherein the bending strain is calculated according to the following formula: ε M =h / (2r), Wherein h is the thickness of the film and r is the bending radius of the film obtained without causing any observable damage to the film. 2 . The electrolyte membrane according to claim 1 , wherein the value of b / a is not higher than a threshold value determined by an equation.

3. The electrolyte membrane according to claim 2, wherein for the acrylate binder, the equation is b / a=183x-2.11 (Equation I), wherein x refers to the weight percentage of the acrylate binder in the electrolyte membrane.

4. The electrolyte membrane according to claim 2, wherein for the PTFE binder, the equation is b / a=345x-1.94 (Equation II), wherein x refers to the weight percentage of the PTFE binder in the electrolyte membrane. 5 . The electrolyte membrane according to claim 1 , wherein the lithium ion conductivity of the electrolyte membrane is in the range of 0.05 to 20 mS / cm. 6 . The electrolyte membrane according to claim 1 , wherein the electrolyte membrane has a lithium ion conductivity of not less than 0.5 mS / cm. 7 . The electrolyte membrane according to claim 1 , wherein a thickness of the electrolyte membrane is in a range of 5 μm to 300 μm. The electrolyte membrane according to claim 1 , further comprising a nonwoven fabric as a support layer.

9. The electrolyte membrane according to claim 1, wherein Formula I is selected from the group consisting of: a)Li x PS 6-a-b Cl a Br b , where 4≤x≤8, 0 <a≤2、0≤b<2、0<6-a-b<6; b)Li x M1 y PS 6-a-b Cl a Br b , where 4≤x≤8, 0 <y<1、0<a≤2、0≤b<2、0<6-a-b<6; c)Li x M2 z PS 6-a-b Cl a Br b, where 4≤x≤8, 0 <z<1、0<a≤2、0≤b<2、0<6-a-b<6; d)Li x P 1-p M3 p S 6-a-b Cl a Br b , where 4≤x≤8, 0 <p<1、0<a≤2、0≤b<2、0<6-a-b<6、 0<1-p<1; e)Li x PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0 <q≤1、0<a≤2、0≤b<2、0<6-a-b-q<6; f)Li x M1 y PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0 <y<1、0<q<1、0<a≤2、0≤b<2、 0<6-abq<6; g)Li x M2 z PS 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0 <z<1、0≤q<1、0<a≤2、0≤b<2、 0<6-abq<6; and h)Li x P 1-p M3 p S 6-a-b-q O q Cl a Br b , where 4≤x≤8, 0 <p<1、0<q<1、0<a≤2、0≤b<2、 0<6-abq<6, 0<1-p<1. 10 . The electrolyte membrane according to claim 1 , wherein a+b≤2.

11. The electrolyte membrane according to claim 1, wherein the sulfide solid electrolyte has a formula selected from the group consisting of: Li 5.8 PS 4.7 O 0.1 Cl 1.2 , Li5.9 P 0.9 Ge 0.1 S 4.8 Cl 1.2 , Li 5.7 Na 0.1 PS 4.8 Cl 1.2 , Li 5.4 PS 4.4 Cl 0.4 Br 1.2 , Li 5.8 PS 4.8 Cl 0.4 Br 0.8 , Li 5.4 PS 4.4 Cl 0.6 Br 1.0 , Li 5.4 PS 4.4 Cl 0.8 Br 0.8 , Li 5.4 PS 4.4 Cl 0.8 Br 0.8 , Li 5.8 PS 4.8 Cl 0.6 Br 0.6 , Li 5.4 PS 4.4 Cl 1.0 Br 0.6 , Li 5.4 PS 4.4 Cl 1.2 Br 0.4 , Li 5.8 PS 4.8 Cl 0.8 Br 0.4 , Li 5.8 PS 4.8 Cl 1.0 Br 0.2 and Li 5.4 PS 4.4 Cl 1.4 Br 0.2 . 12 . An all-solid-state battery comprising the electrolyte membrane according to claim 1 .

13. The all-solid-state battery according to claim 12, further comprising a positive electrode comprising a positive electrode electroactive material.

14. The all-solid-state battery according to claim 13, wherein during operation of the all-solid-state battery, the cathode active material is + At a potential of 2 V or more, a redox reaction is exhibited.

15. A method for preparing the electrolyte membrane according to claim 1, comprising: The particles of the sulfide solid electrolyte and a polymer binder are mixed to obtain a mixture.

16. The method according to claim 15, wherein the particles of the sulfide solid electrolyte are synthesized by mixing raw precursor powders in a stoichiometric ratio in an inert atmosphere, followed by sintering at 400-700° C. for 4-24 hours and grinding, wherein the raw precursor powders are selected from the group consisting of Li2S, Na2S, P2S5, LiCl, LiBr, Li2O, GeS2, and combinations thereof.

17. The method of claim 15, wherein the mixture comprises a solvent and the mixture is a slurry.

18. The method according to claim 17, further comprising: a) coating the mixture onto a substrate and then vacuum drying at room temperature, wherein the substrate comprises a film and a non-woven fabric, thereby obtaining a dry coating layer attached to the non-woven fabric; and b) peeling the dry coating layer from the membrane, thereby obtaining an electrolyte membrane including the dry coating layer and the nonwoven fabric.

19. The method according to claim 18, wherein the film in the substrate is a PET film, and the nonwoven fabric is made of polyester having a thickness of about 10 μm.

20. The method of claim 15, wherein the mixture is substantially free of solvent and the mixture is formed into a film by calendaring.