Large-wall-thickness-difference multi-cavity wallboard aluminum alloy profile forming device and method

By using multi-component flow holes, two-stage welding chambers and step-shaped flow blocks in the forming process of aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels, the problem of uneven metal flow velocity is solved and the profile forming is improved Accuracy and mold life.

CN118926336APending Publication Date: 2024-11-12SHANDONG UNIV

Patent Information

Application Number
CN202411032137.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to ensure the uniformity of metal flow velocity and temperature during the forming of aluminum alloy profiles with large wall thickness difference and multiple cavity thickness, resulting in the occurrence of defects such as difficulty in forming the profile, deformation and cracking.

Method used

A forming device including multi-component flow holes, two-stage welding chambers and step-shaped flow blocks is designed. Material flow distribution is performed through reasonably distributed flow holes and flow bridges, and step-shaped flow arresting is provided on the thick wall side of the profile. The block balances the metal flow rate to avoid lateral deviation and deformation of the profile.

Benefits of technology

It improves the profile forming accuracy and mechanical properties, avoids lateral deviation and local warping of the profile, extends the service life of the mold, and ensures the uniformity of the metal flow rate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118926336A_ABST
    Figure CN118926336A_ABST
Patent Text Reader

Abstract

The invention relates to a large-wall-thickness-difference multi-cavity wallboard aluminum alloy profile forming device and method, and belongs to the technical field of profile extrusion forming. The device comprises an upper die and a lower die, an inner group shunting hole, an outer group shunting hole and a main shunting bridge are arranged at the feeding position of the upper die, and a die core protruding towards a die hole is arranged on the main shunting bridge; the mold core comprises a plurality of sub-mold cores, and drainage grooves are formed among the sub-mold cores; a first-level welding chamber is arranged on the periphery of a die hole of the lower die, a second-level welding chamber is arranged between the first-level welding chamber and the die hole, the bottom face of the second-level welding chamber is lower than the bottom face of the first-level welding chamber, and the bottom face of the second-level welding chamber on the thick wall side of a profile protrudes upwards to the position higher than the bottom face of the first-level welding chamber to form a flow stopping block. According to the invention, a plurality of groups of shunting holes and shunting bridges are reasonably distributed according to the wall thickness of a profile, and reasonable flow distribution is carried out on materials at a feed port; and two stages of welding chambers and flow choking blocks are arranged to balance metal flow on the thick-wall side and the thin-wall side of the sectional material, and the forming quality of the sectional material is improved through multi-aspect optimization means.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of profile extrusion forming, and in particular relates to a device and method for forming a multi-cavity wall panel aluminum alloy profile with a large wall thickness difference. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] In recent years, the requirements for lightweight structural parts in aerospace, high-speed rail transportation and other fields have been continuously improved. Large multi-cavity wall panel hollow aluminum alloy extruded profiles have become the main development direction of lightweight structural parts because of their dual advantages of lightweight materials and lightweight structures. This type of profile often has a large cross-section, a large wall thickness difference, and a complex shape. At the same time, it requires high dimensional accuracy and mechanical properties, and also requires the interface bonding quality of the longitudinal weld. The complexity of its geometric shape and the high requirements of the service environment for forming accuracy and performance have greatly increased the difficulty of mold design and optimization. In order to improve the dimensional accuracy and comprehensive performance of the profile, it is necessary to ensure that the metal of each part on the cross section of the profile is extruded from the die hole at the most consistent speed, temperature and required thickness during the extrusion process. However, when the wall thickness difference of the hollow profile is large and the cross-sectional shape is complex, it is often difficult to ensure the uniformity of the metal flow speed and temperature during the extrusion process. In the prior art, the forming mold generally contains a multi-component flow hole and a diverter bridge. The design and optimization of the diverter hole and the diverter bridge is one of the difficulties faced.

[0004] The size, shape, and distribution of the diverter holes, the direction of the diverter bridge, and the setting of the sinking bridge have a direct impact on the feed amount and material flow rate. During the extrusion process, excessive feed in a local area usually causes the metal to flow too fast, while too little feed will lead to a lack of sufficient material input. At the same time, the amount of feed also has an important impact on the extrusion load and die life. When the wall thickness difference of the profile is large and the cross-sectional shape is complex, it is often difficult to coordinate the relationship between the feed amount and the material flow rate at different wall thicknesses, resulting in difficulty in profile forming, or defects such as deformation and cracking.

[0005] In addition, the shape and depth of the welding chamber in the extrusion die are key factors affecting the quality of the longitudinal weld interface of the profile, and the design of the drainage groove, baffle block and working belt has an important influence on the balance of the flow velocity of each particle on the profile cross section. When the wall thickness difference of the profile is large, the difference in metal flow velocity and temperature on the profile cross section at the die outlet is large. However, the commonly used design and optimization methods of the welding chamber, drainage groove, baffle block and working belt have a small adjustment range for the metal flow velocity, which makes it difficult to effectively improve the uniformity of the metal flow velocity on the profile cross section at the die outlet, and cannot guarantee the forming accuracy of the profile. Summary of the invention

[0006] In view of the current technical problem that it is difficult to form aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels, the purpose of the present invention is to provide a device and method for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels, and to provide a multi-group flow hole, a two-stage welding chamber and a stepped flow block. The flow block is connected to the two-stage welding chamber to improve the uniformity of metal flow velocity on the thick-wall side and the thin-wall side of the profile, avoid lateral displacement and deformation, cracking and other defects of the profile, and improve the forming accuracy of the profile 14.

[0007] In order to achieve the above object, the technical solution of the present invention is:

[0008] In a first aspect, a device for forming a large wall thickness difference multi-cavity wall panel aluminum alloy profile comprises a mold, wherein the mold comprises an upper mold and a lower mold;

[0009] An inner group flow hole and an outer group flow hole are arranged at the material inlet of the upper mold, and the inner group flow hole and the outer group flow hole respectively include a plurality of flow diversion holes; a main flow diversion bridge is arranged between the inner group flow hole and the outer group flow diversion hole, and a mold core protruding toward the lower mold is arranged on the main flow diversion bridge; the mold core includes a plurality of sub-mold cores, and a drainage groove is arranged between the plurality of sub-mold cores;

[0010] The lower die is provided with a through die hole, and a welding chamber is provided on the periphery of the die hole, and the welding chamber includes a primary welding chamber and a secondary welding chamber, and the secondary welding chamber is provided between the primary welding chamber and the die hole, and the bottom surface of the secondary welding chamber is lower than the bottom surface of the primary welding chamber, and the bottom surface of the secondary welding chamber on the thick wall side of the profile protrudes upward to a position higher than the bottom surface of the primary welding chamber, forming a flow block;

[0011] The drainage groove is connected to the gaps between the mold core and the mold holes on both sides.

[0012] Optionally, the main diversion bridge is arranged along the distribution direction of the multiple inner cavities of the profile.

[0013] Optionally, in the inner group of diverter holes and the outer group of diverter holes, secondary diverter bridges are provided between the diverter holes in the group, and the width of the primary diverter bridge is greater than that of the secondary diverter bridge.

[0014] Optionally, the main shunt bridge is connected to the secondary shunt bridge.

[0015] Optionally, the diverter bridge between the diverter holes at the thin-wall side of the profile is set as a sinking bridge, and the diverter holes on both sides of the sinking bridge are set as sinking holes.

[0016] Optionally, the diversion holes are arranged along the distribution direction of the outer wall of the profile.

[0017] Optionally, the drainage groove is arranged along the distribution direction of the cavity wall inside the profile.

[0018] Optionally, the baffle block is stepped, which means that the baffle block increases in height near the thick-walled side of the profile where the wall thickness is relatively thicker, and decreases in height near the thick-walled side of the profile where the wall thickness is relatively thinner.

[0019] Optionally, the height of the baffle block is greater than the depth of the secondary welding chamber, the depth of the secondary welding chamber is the distance between the bottom surfaces of the secondary welding chamber and the primary welding chamber, and the baffle block is connected to the bottom surface of the primary welding chamber.

[0020] Optionally, the secondary welding chamber is arranged around the die hole, the baffle block is arranged on the bottom surface of the secondary welding chamber on the thick wall side of the profile, and the primary welding chamber is arranged around the secondary welding chamber and / or the baffle block.

[0021] Optionally, working belts are provided on the surfaces of the mold hole and the mold core.

[0022] In a second aspect, a method for forming a multi-cavity wall panel aluminum alloy profile with a large wall thickness difference is provided, using the above-mentioned multi-cavity wall panel aluminum alloy profile forming device with a large wall thickness difference, comprising the following steps:

[0023] S1, prepare a billet for extrusion of a set length and heat and keep it warm, heat the die used and keep it warm;

[0024] S2, the blank is extruded into the die through the diverter hole, divided into multiple metal streams by the diverter bridge, and welded in the primary welding chamber;

[0025] S3, the metal flow flows from the primary welding chamber to the gap between the die hole and the die core. The flow of the metal flow on the thick wall side is restricted by the flow block and the flow velocity is reduced. A part of the metal flow on the thin wall side flows into the drainage groove, and the rest flows into the secondary welding chamber.

[0026] S4. The metal flow is squeezed out from the gap between the die hole and the die core, and is formed into a multi-cavity wall panel aluminum alloy profile with a large wall thickness difference together with the metal flow flowing out through the drainage groove.

[0027] Optionally, in S1, the extrusion blank is made of aluminum or aluminum alloy.

[0028] Optionally, in S2, the blank is divided into multiple metal flows by the diverter bridge and the sinker bridge, and the metal flows enter the primary welding chamber through the diverter holes or the sinker holes.

[0029] Optionally, in S4, the metal flow is squeezed out from the channels between the working belts.

[0030] Optionally, the following steps are also included:

[0031] S5. Perform online air-cooling quenching and aging treatment on the profile extruded in S4.

[0032] The beneficial effects of the present invention are:

[0033] 1. In the forming device disclosed in the present invention, the forming mold is designed to solve the problem of difficulty in forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels, and multi-component flow holes and diversion bridges are reasonably distributed according to the wall thickness of the profile to reasonably distribute the material flow at the inlet and improve the uniformity of metal flow rate; in order to solve the problem that the metal flow rate is slow on the thin-wall side of the profile and fast on the thick-wall side, a two-stage welding chamber is set, and a stepped flow block is set on the bottom surface of the second-stage welding chamber on the thick-wall side of the profile to balance the metal flow on the thick-wall side and the thin-wall side of the profile, and avoid lateral deviation and local warping of the profile. The profile forming quality is improved through various optimization means.

[0034] 2. In the forming device disclosed in the present invention, the diverter bridge is configured as a main bridge and a plurality of diverter bridges coordinated with each other, a mold core is arranged on the main bridge, and a sinker bridge is arranged on the thin-wall side of the profile; the outer side of the baffle block is located on the bottom surface of the first-stage welding chamber, that is, the baffle block is connected to the two-stage welding chamber at the same time, which can improve the uniformity of the metal flow rate while balancing the mold force and extending the service life of the mold.

[0035] 3. In the forming method disclosed in the present invention, the material passes through the diverter hole, the primary welding chamber, the secondary welding chamber and the working belt of the mold in sequence; in the welding chamber, the flow of the thick-walled side material is hindered by the baffle block and the extrusion speed is reduced, while part of the material on the thin-walled side flows into the drainage groove to become the cavity wall inside the profile. Through comprehensive consideration and optimized design of the diverter hole, welding chamber, drainage groove, baffle block and working belt, the uniformity of the metal flow speed on the thick-walled side and the thin-walled side of the profile can be improved, and the profile forming accuracy can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0037] Figure 1 This is a schematic cross-sectional view of the aluminum alloy profile with large wall thickness difference and multi-cavity wall panel in Example 1.

[0038] Figure 2 It is a schematic longitudinal section diagram of the extrusion die for the aluminum alloy profile with large wall thickness difference and multi-cavity wall panel in Example 1.

[0039] Figure 3 This is a schematic diagram of the structure of the upper mold in Example 1.

[0040] Figure 4 This is a bottom view of the upper mold in Example 1.

[0041] Figure 5 This is a schematic diagram of the structure of the lower mold in Example 1.

[0042] Figure 6 This is a top view of the lower mold in Example 1.

[0043] Figure 7 This is a schematic diagram of the connection between the baffle block and the two-stage welding chamber from a first viewing angle of Example 1.

[0044] Figure 8 This is a schematic diagram of the connection between the baffle block and the two-stage welding chamber from a second viewing angle of Example 1.

[0045] Fig. 9 Schematic diagram of the welding chamber of Example 1.

[0046] Among them, 1. upper mold; 2. lower mold; 3. diverter hole; 31. diverter hole A; 32. diverter hole B; 33. diverter hole C; 34. diverter hole D; 35. diverter hole E; 36. diverter hole F; 37. diverter hole G; 38. diverter hole H; 39. diverter hole I; 310. diverter hole J; 311. diverter hole K; 312. diverter hole L; 4. diverter bridge; 41. diverter bridge A; 42. diverter bridge B; 43. diverter bridge C; 44. diverter bridge D; 45. diverter bridge E; 46. diverter bridge F; 47. diverter bridge G; 48. diverter bridge H; 49. diverter bridge I; 410. diverter bridge J; 411. diverter bridge K; 412. diverter bridge L; 413. diverter bridge M; 414. diverter bridge N; 415. 5. Diverter bridge O; 416. Diverter bridge P; 417. Diverter bridge Q; 5. Countersunk hole; 6. Mold core; 61. Sub-mold core A; 62. Sub-mold core B; 63. Sub-mold core C; 64. Sub-mold core D; 65. Sub-mold core E; 66. Sub-mold core F; 67. Sub-mold core G; 68. Sub-mold core H; 7. Drainage groove; 71. Drainage groove A; 72. Drainage groove B; 73. Drainage groove C; 74. Drainage groove D; 75. Drainage groove E; 76. Drainage groove F; 8. Welding chamber; 81. Primary welding chamber; 811. Bottom surface of primary welding chamber; 82. Secondary welding chamber; 821. Bottom surface of secondary welding chamber; 9. Block; 10. First working zone; 11. Second working zone; 12. Mold hole; 13. Empty knife; 14. Profile. DETAILED DESCRIPTION

[0047] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0048] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0049] Example 1

[0050] Profile 14 is a complex cross-section profile of a multi-cavity wall panel with a large wall thickness difference, having the following characteristics: Figure 1 The cross section shown includes an outer wall at the periphery; the upper outer wall is a straight thick wall, and the shapes on both sides are asymmetrical, the lower outer wall is an arc-shaped thin wall, the outer walls on both sides are thin walls, and the shapes of the thin walls on both sides are basically symmetrical; multiple cavities are arranged in an arc shape, the cavities are separated by thinner cavity walls, and the cavity walls connect the outer walls on opposite sides of the cavity; in the center of the cross section, the upper outer wall and the lower outer wall merge into a thick wall without cavities. This type of profile often has a large cross-section, many cavities, and a large difference in wall thickness, and has high requirements for dimensional accuracy and mechanical properties. Therefore, it is difficult to ensure that the metal on the thick wall side and the thin wall side of the profile section at the mold outlet is extruded at a consistent speed and the required thickness, and the forming is difficult, and defects such as lateral displacement, deformation, and cracking are prone to occur.

[0051] The 6005A aluminum alloy ingot used for the profile 14 is prepared by melting and casting, and the mass percentage of the alloy components is Mg0.62%, Si 0.65%, Mn 0.24%, Fe 0.13%, Cr 0.13%, Cu 0.06%, Ti 0.04%, Zn≤0.01%, and the rest is Al.

[0052] A device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels, comprising a die. In this embodiment, the die for extruding complex cross-section profiles with large wall thickness difference and multi-cavity wall panels is a split die, such as Figure 2 As shown, the mold includes an upper mold 1 and a lower mold 2; the upper and lower molds here are defined according to the flow direction of the metal flow during the profile forming process. During the extrusion process, the metal flow first flows into the diversion hole of the upper mold 1, and then is extruded through the gap between the mold hole 12 of the lower mold 2 and the mold core 6 of the upper mold 1.

[0053] like Figure 4 As shown, the inlet of the upper mold 1 is provided with an inner group flow hole and an outer group flow hole, and the inner group flow hole and the outer group flow hole respectively include a plurality of flow holes 3; a main flow bridge is provided between the inner group flow hole and the outer group flow hole, such as Figure 3 As shown, a mold core protruding toward the mold hole is provided on the main diversion bridge; the mold core 6 includes a plurality of sub-mold cores, and a drainage groove 7 is provided between the plurality of sub-mold cores; Figure 5As shown, the lower die 2 is provided with a through die hole 12, and a welding chamber 8 is provided on the periphery of the die hole 12. The welding chamber 8 includes a primary welding chamber 81 and a secondary welding chamber 82. The secondary welding chamber 82 is provided between the primary welding chamber 81 and the die hole 12, and a baffle block 9 is provided on the bottom surface of the secondary welding chamber 82 on the thick wall side of the profile 14; and the bottom surface of the secondary welding chamber 82 is lower than the bottom surface of the primary welding chamber 81, and the baffle block 9 is higher than the bottom surface of the primary welding chamber 81; as shown Figure 2 As shown, the drainage groove 7 connects the gap between the mold hole 12 and the mold core 6.

[0054] Through the above settings, reasonably distributed multi-component flow holes 3 and diverter bridges 4, as well as two-stage welding chambers 8, stepped baffles 9, and drainage grooves 7 of different volumes are arranged according to the geometric shape of the profile and the characteristics of the wall thickness, so as to balance the metal flow state during the extrusion forming process of complex cross-section profiles with multi-cavity wall panels with large wall thickness differences, improve the uniformity of the metal flow velocity on the thick-walled side and the thin-walled side of the profile cross section at the mold outlet, thereby improving the profile dimensional accuracy, forming quality and mechanical properties, while balancing the mold stress and extending the mold service life.

[0055] The mold is in the form of a combination of two mold units, an upper mold 1 and a lower mold 2. The specifications of the upper mold 1 are Φ898mm×240mm, and the specifications of the lower mold 2 are Φ898mm×180mm. It should be pointed out that in other embodiments, the mold can also be split or combined in other ways. When the internal structure of the mold is relatively simple, an integrated mold can be used. When the internal structure of the mold is relatively complex, three mold units can be used.

[0056] The main diverter bridge is arranged along the distribution direction of the multiple inner cavities of the profile. Since the multiple inner cavities of the profile 14 are basically distributed in an arc shape, the main diverter bridge is distributed in an arc shape. In the inner group diverter holes and the outer group diverter holes, a secondary diverter bridge is arranged between the diverter holes 3 in the group, and the width of the main diverter bridge is greater than that of the secondary diverter bridge; the diverter holes 3 are arranged along the distribution direction of the outer wall of the profile 14. Since the profile 14 is an arc shape surrounded by the outer wall, the inner group diverter holes and the outer group diverter holes are basically arranged in an arc shape, and the central diverter hole is designed to be a straight line, corresponding to the thick wall shape of the outer wall. The main diverter bridge is connected to the secondary diverter bridge, and the feed port is divided into multiple diverter holes 3, and the blank entering the feed port is reasonably distributed. At the same time, the force on the mold is balanced, and the service life of the mold is effectively extended.

[0057] The shunt bridge 4 includes Figure 4The main diverter bridge shown in the figure is connected with multiple secondary diverter bridges, and the main diverter bridge is formed by connecting multiple diverter bridges, and is reasonably arranged according to the geometric shape characteristics of the profile. In this embodiment, the main diverter bridge is connected by seven diverter bridges 41 to 47, of which 41 is diverter bridge A, 42 is diverter bridge B, 43 is diverter bridge C, 44 is diverter bridge D, 45 is diverter bridge E, 46 is diverter bridge F, and 47 is diverter bridge G. The direction of the main bridge is consistent with the outer contour geometry of the profile 14 and the internal cavity distribution characteristics. The seven diverter bridges represented by 41 to 47 are arranged in an arc shape; ten secondary diverter bridges are dispersed on both sides of the extension direction of the main diverter bridge, of which 48 is diverter bridge H, 49 is diverter bridge I, 410 is diverter bridge G, and 411 is diverter bridge H. The diverter bridge J, 411 is the diverter bridge K, 412 is the diverter bridge L, 413 is the diverter bridge M, 414 is the diverter bridge N, 415 is the diverter bridge O, 416 is the diverter bridge P, and 417 is the diverter bridge Q, wherein the diverter bridge D44 and the diverter bridge G47 are located at both ends and are sinking bridges; therefore, under the division of the two sinking bridges (diverter bridge D44 and diverter bridge G47), the diverter holes on both sides (including between the diverter hole F36 and the diverter hole G37, and between the diverter hole J310 and the diverter hole K311) are open at the end away from the core, and the bottom becomes the sinking hole 5. During the extrusion process, the billet enters from the feed port, and on the thick wall side of the profile, the billet is divided into four metal flows by the diverter bridge 4, which enter the diverter holes on the thick wall side (including: diverter hole A31, diverter hole B32, diverter hole C33 and diverter hole D34) respectively and then converge in the welding chamber 8.

[0058] On the thin-walled side of the profile, the blank is divided into eight metal flows by the diverter bridge 4, and enters the thin-walled side diverter holes (including: diverter hole E35, diverter hole F36, diverter hole G37, diverter hole H38, diverter hole I39, diverter hole J310, diverter hole K311 and diverter hole L312) respectively, and then merges in the welding chamber 8; wherein, the blank flowing into the diverter hole F36, diverter hole G37, diverter hole J310 and diverter hole K311 first enters the countersunk hole 5, and then is divided into four metal flows by the sinking bridge (including diverter bridge D44 and diverter bridge G47) to increase the flow speed of the metal in the thin-walled side welding chamber 8 of the profile and reduce the lateral force on the mold; this embodiment adopts the form of connecting and matching a main bridge composed of multiple main diverter bridges and multiple secondary diverter bridges, and the direction of the main bridge is designed to be consistent with the geometric shape of the profile 14 and the distribution characteristics of the inner hole.

[0059] The diverter bridge between the diverter holes at the feeding point on the thin-wall side of the profile is set as a sinker bridge, and the diverter holes on both sides of the sinker bridge are set as countersunk holes. When a sinker bridge or countersunk hole is used on the thin-wall side of the profile, it is not limited to only one sinker bridge or countersunk hole on one side, and two or more sinkers or countersunk holes can also be set. It needs to be adjusted according to the wall thickness distribution characteristics of the profile and the balance effect of metal flow on the thick-wall side and the thin-wall side.

[0060] Accordingly, due to Figure 1 The cross-section of the large wall thickness difference multi-cavity wall panel aluminum alloy profile 14 shown is asymmetrical on both ends of the thick wall side, while symmetrical on the thin wall side. Therefore, the diverter hole B32 / diverter hole E35 and diverter hole C33 / diverter hole I39 have slightly different shapes and sizes, while the diverter hole F36 / diverter hole G37 / diverter hole H38 and diverter hole J310 / diverter hole K311 / diverter hole L312 have the same shape and size and are symmetrically distributed on the left and right to obtain a profile with the required wall thickness requirements and forming accuracy. Countersunk holes are provided at the bottom of the diversion holes F36, diversion holes G37, diversion holes J310 and diversion holes K311 on the thin-walled side of the profile to increase the metal flow rate on the thin-walled side of the profile; in this embodiment, the depth of the countersunk holes is set to 30 mm. In other embodiments, the position and depth of the countersunk holes can be adjusted according to the wall thickness of the profile and the difference in the flow rate of the material in the forming channels on the thick-walled side and the thin-walled side to further increase the metal flow rate on the thin-walled side, improve the uniformity of the metal flow rate on the profile cross section at the mold outlet, and ultimately improve the profile forming accuracy.

[0061] A mold core 6 is provided on the main bridge, and the main bridge is connected to the mold core 6 as a structure for fixing the mold core 6.

[0062] In this embodiment, the mold core 6 includes eight sub-mold cores: one side of the sub-mold cores (including: sub-mold core A61, sub-mold core B62, sub-mold core C63 and sub-mold core D64) are located on the three diversion bridges (including: diversion bridge B42, diversion bridge C43 and diversion bridge D44) of the main bridge, and the other side of the sub-mold cores (including: sub-mold core E65, sub-mold core BF66, sub-mold core G67 and sub-mold core H68) are located on the three diversion bridges (including: diversion bridge E45, diversion bridge F46 and diversion bridge G47) of the main bridge. Figure 1 The thick-walled ends of the multi-cavity wall panel aluminum alloy profile 14 with a large wall thickness difference shown are asymmetrical on the left and right sides. Therefore, the left and right sub-mold cores are only partially symmetrical in structure, and some sub-mold cores have different precise shapes and sizes. For example, sub-mold core C63, sub-mold core D64, sub-mold core G67, and sub-mold core H68 are completely symmetrical, while sub-mold core A61, sub-mold core B62, sub-mold core E65, and sub-mold core F66 have slightly different structural features at both ends of the thick-walled side; in this embodiment, the height of the mold core 6 is set to 100 mm, that is, the top of the mold core 6 is 100 mm away from the surface of the upper mold 1.

[0063] like Figure 2 As shown, working belts are arranged on the surface of the die hole and the die core, and a first working belt 10 is arranged on the surface of the die core 6, the bottom of which is connected to the main bridge, and the top of which is inserted into the second working belt 11 of the lower die 2, and the final extrusion channel of the profile 14 is formed between the first working belt 10 and the second working belt 11. The upper die 1 is provided with a first working belt 10, and the lower die 2 is provided with a second working belt 11 matched with the first working belt 10. The blank is extruded from the gap between the first working belt 10 and the second working belt 11, and is formed as shown in FIG. Figure 1 The shown aluminum alloy profile 14 with large wall thickness difference and multi-cavity wall panel has a larger distance between the first working band 10 and the second working band 11 on the thick wall side of the profile, and a smaller distance between the first working band 10 and the second working band 11 on the thin wall side of the profile, so as to meet the wall thickness requirements of different parts of the profile.

[0064] A drainage groove 7 is provided between adjacent sub-mold cores, and the drainage groove 7 is arranged along the distribution direction of the cavity wall inside the profile 14. After the blank is pre-diverted by the countersunk hole 5 and the diverter hole 3, it converges at the periphery of the mold core 6 in the welding chamber 8. Part of the material passes through the drainage groove 7 and finally flows into the gap between the working belts to form the thin-walled rib plate of the profile, the cavity wall and other difficult-to-form locations. In this embodiment, as Figure 3 As shown, there are six drainage grooves (including drainage groove A71, drainage groove B72, drainage groove C73, drainage groove D74, drainage groove E75 and drainage groove F76) between the eight sub-mold cores. The volume, height and slope of the drainage groove can be adjusted according to the wall thickness of the thin-walled rib plate of the profile and the difference in the flow speed of the material in the welding chamber to adjust the flow rate of the metal entering the drainage groove and improve the forming accuracy of the thin-walled rib plate of the profile.

[0065] like Figure 2 As shown, since the distance between the first working zone 10 and the second working zone 11 on the thick-walled side of the profile 14 is greater than the distance between the first working zone 10 and the second working zone 11 on the thin-walled side of the profile, the volume of the final extrusion channel on the thick-walled side of the profile is larger, and the metal flow speed is faster, while the volume of the final extrusion channel on the thin-walled side of the profile is smaller, and the metal flow speed is slower, resulting in uneven metal flow speed on the profile cross section at the die outlet, which can easily cause lateral displacement of the profile, and even local warping and shape distortion; In order to solve the problem of uneven metal flow speed on the thick-walled side and the thin-walled side of the profile cross section at the die outlet, this embodiment adopts a design method in which the baffle block 9 is connected to the two-stage welding chamber, such as Figure 5 and Figure 6 As shown, a baffle block 9 is provided on the bottom surface of the secondary welding chamber 82 on the thick wall side of the profile 14 to reduce the flow velocity of the metal on the thick wall side of the profile 14 in the welding chamber 8, and further reduce its flow velocity in the final extrusion channel; it should be noted that the minimum height of the baffle block 9 is greater than the depth of the secondary welding chamber 82, and the outer side of the baffle block 9 (the side away from the mold core is the outer side) is located on the bottom surface of the primary welding chamber 81, as shown in FIG. Figure 7 and Figure 8As shown, the height direction of the baffle block 9 is arranged along the length direction of the working belt, the length direction of the baffle block 9 is arranged along the length direction of the secondary welding chamber 82, and the width direction of the baffle block 9 almost covers the secondary welding chamber 82, and only the inner side (the side close to the mold core is the inner side) is at a very small distance from the edge of the secondary welding chamber 82, that is, the inner side of the baffle block 9 in the width direction and the length direction are connected to the secondary welding chamber 82, and the outer side of the baffle block 9 in the width direction is connected to the primary welding chamber 81, and the baffle block 9 is designed to be connected to the two-stage welding chamber (including the primary welding chamber 81 and the secondary welding chamber 82); Fig. 9 (b) is a schematic diagram of a welding chamber without the baffle 9, and the height of the bottom surface 821 of the secondary welding chamber is lower than the height of the bottom surface 811 of the primary welding chamber; Fig. 9 (a) is a schematic diagram of a welding chamber including a baffle block 9, wherein the bottom surface 821 of the secondary welding chamber is partially raised to a height higher than the bottom surface 811 of the primary welding chamber on a side close to the bottom surface 811 of the primary welding chamber, thereby forming the baffle block 9, i.e., the baffle block 9 is formed by raising the bottom surface 821 of the secondary welding chamber; at the position where the baffle block is set, the width of the bottom surface 811 of the primary welding chamber remains unchanged, while the width of the bottom surface 821 of the secondary welding chamber becomes narrower, therefore, the baffle block 9 is surrounded by the primary welding chamber 81 and the secondary welding chamber 82; so as to balance the metal flow on the thick-walled side and the thin-walled side of the profile 14 in the welding chamber 8, thereby improving the uniformity of the metal flow velocity on the profile cross section at the mold outlet, and finally improving the profile forming accuracy.

[0066] The baffle block 9 is stepped, which means that the height of the baffle block increases near the thick-walled side of the profile where the wall thickness is relatively large, and decreases near the thick-walled side of the profile where the wall thickness is relatively small, that is, the height of the baffle block is positively correlated with the wall thickness of the thick-walled side of the profile. Figure 1 The upper outer wall of the profile 14 shown is a thick wall side, in which the wall thickness is relatively large in the center, relatively small at both ends, and slightly reduced in the middle of the center. Figure 7 and Figure 8 As shown, the height of the baffle block 9 increases near the center of the thick wall side, decreases near the two ends, and slightly decreases near the middle of the center of the thick wall side. By arranging the stepped baffle block 9 on the thick wall side of the profile 14 according to its wall thickness distribution characteristics, the metal flow on the thick wall side of the profile 14 is improved, and the uniformity of the metal flow speed at different wall thicknesses on the thick wall side of the profile cross section at the mold outlet is improved.

[0067] In this embodiment, the width of the baffle block 9 is set to 5.7 mm and 6.4 mm, the height is set to 20-32 mm, the width of the secondary welding chamber 82 is set to 10 mm, and the depth is set to 10 mm (the depth of the secondary welding chamber is the distance between the bottom surfaces of the secondary welding chamber and the primary welding chamber), and the minimum height of the baffle block 9 is greater than the depth of the secondary welding chamber 82; in other embodiments, the width, height of the baffle block 9 and the width and depth of the secondary welding chamber 82 can be adjusted according to the wall thickness of the profile 14 and the flow rate of the material in the welding chamber 8, but it is necessary to ensure that the minimum height of the baffle block 9 is greater than the depth of the secondary welding chamber 82, and the outer side of the baffle block 9 is located at the bottom surface of the primary welding chamber 81 to meet the design requirements of connecting the baffle block 9 with the two-stage welding chamber. During the profile extrusion process, the blank enters the countersunk hole 5 and the diverter hole 3 at the feed port, is divided into multiple metal flows by the diverter bridge 4 and the countersunk bridge, and is welded in the primary welding chamber 81; then, the material continues to flow in the welding chamber, and the flow rate of the material on the thick-walled side is limited by the baffle block 9, while part of the material on the thin-walled side flows into the drainage groove 7 between the sub-mold cores; finally, the material is extruded from the channel between the first working belt 10 and the second working belt 11 to be formed into a complex cross-section profile 14 of a multi-cavity wall panel with a large wall thickness difference, and ensures that the metal on the profile cross section at the mold outlet flows out at a speed as consistent as possible to improve the profile forming accuracy and mechanical properties.

[0068] like Figure 2 As shown, a hollow knife 13 is provided on the inner wall of the lower die 2 to support the second working belt 11 and avoid contact and friction between the die and the profile 14 material, thereby ensuring that the profile 14 can pass through the die hole 12 smoothly.

[0069] In this embodiment, the working band length range of the final extrusion channel on the thick-wall side is set to 20 to 45 mm, and the working band length range of the final extrusion channel on the thin-wall side is set to 4.5 to 17 mm; in other embodiments, the working band length can be adjusted according to the wall thickness distribution characteristics of the profile and the difference in flow velocity of the material in the final extrusion channels on the thick-wall side and the thin-wall side, so as to further reduce the difference in metal flow velocity on the profile cross section at the mold outlet and improve the profile forming accuracy.

[0070] The method for preparing the profile 14 using the mold in this embodiment includes the following steps:

[0071] S1. The molten 6005A aluminum alloy bar is homogenized and then sawed to obtain an extrusion billet with a diameter of Φ638 mm and an extrusion ratio of 34.42; the extrusion billet of a set length is prepared and heated to 510-520° C. and kept warm for 12-36 hours; the mold used is heated to 480-500° C. and kept warm for 12-36 hours.

[0072] S2, convey the billet for extrusion into the extrusion cylinder, and set the extrusion speed to 1.5 mm / s; under the push of the extrusion rod, the billet reaches the inlet of the extrusion die, enters the countersunk hole 5 and the diverter hole 3, and is divided into multiple metal flows by the diverter bridge 4 and the sinking bridge: on the thick-walled side of the profile, the billet is divided into four metal flows by the diverter bridge 4, and on the thin-walled side of the profile, the billet is divided into eight metal flows by the diverter bridge 4; the billet is extruded into the die through the diverter hole 3, and is divided into multiple metal flows by the diverter bridge 4, and is welded in the primary welding chamber 81;

[0073] S3. The metal flow flows from the primary welding chamber 81 to the gap between the die hole 12 and the die core 6. The flow of the metal flow on the thick-walled side is restricted by the baffle block 9 and the flow velocity is reduced. A part of the metal flow on the thin-walled side flows into the drainage groove 7, and the remaining part flows into the secondary welding chamber 82. Specifically, the blank flows in the primary welding chamber 81, wherein on the thick-walled side of the profile, the flow of the material is hindered by the baffle block 9, and on the thin-walled side of the profile, part of the material enters the drainage groove 7; then the blank enters the secondary welding chamber 82.

[0074] S4. The metal flow is extruded from the final extrusion channel between the first working belt 10 and the second working belt 11 between the die hole 12 and the die core 6, and is formed into a multi-cavity wall panel aluminum alloy profile 14 with a large wall thickness difference together with the metal flow flowing out through the drainage groove 7.

[0075] S5. The profile 14 extruded in S4 is subjected to online air-cooling quenching and aging treatment at 175±5°C / 8h.

[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels, comprising a mold, characterized in that: The mold comprises an upper mold and a lower mold; An inner group flow hole and an outer group flow hole are arranged at the material inlet of the upper mold, and the inner group flow hole and the outer group flow hole respectively include a plurality of flow holes; A main flow-dividing bridge is provided between the inner group flow-dividing holes and the outer group flow-dividing holes, and a mold core protruding toward the lower mold is provided on the main flow-dividing bridge; the mold core includes a plurality of sub-mold cores, and drainage grooves are provided between the plurality of sub-mold cores; The lower die is provided with a through die hole, a welding chamber is provided on the periphery of the die hole, the welding chamber includes a primary welding chamber and a secondary welding chamber, the secondary welding chamber is provided between the primary welding chamber and the die hole, and the bottom surface of the secondary welding chamber is lower than the bottom surface of the primary welding chamber, and the bottom surface of the secondary welding chamber on the thick wall side of the profile protrudes upward to a position higher than the bottom surface of the primary welding chamber to form a flow block; The drainage groove is connected to the gap between the mold hole and the mold core.

2. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1 is characterized in that: The main shunt bridge is arranged along the distribution direction of the multiple inner cavities of the profile; Optionally, in the inner group of diverter holes and the outer group of diverter holes, a secondary diverter bridge is provided between the diverter holes in the group, and the width of the primary diverter bridge is greater than that of the secondary diverter bridge; Optionally, the main shunt bridge is connected to the secondary shunt bridge.

3. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1 is characterized in that: The diverter bridge between the diverter holes at the thin-wall side of the profile is set as a sinking bridge, and the diverter holes on both sides of the sinking bridge are set as sinking holes.

4. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1, characterized in that: The diversion holes are arranged along the distribution direction of the outer wall of the profile.

5. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1, characterized in that: The drainage grooves are arranged along the distribution direction of the cavity wall inside the profile.

6. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1, characterized in that: The baffle block is in a stepped shape, which means that the baffle block is higher at a location where the wall thickness is relatively thicker near the thick-walled side of the profile, and is lower at a location where the wall thickness is relatively thinner near the thick-walled side of the profile; Optionally, the height of the baffle block is greater than the depth of the secondary welding chamber, and the baffle block is connected to the bottom surface of the primary welding chamber.

7. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1, characterized in that: The secondary welding chamber is arranged around the die hole, the baffle block is arranged on the bottom surface of the secondary welding chamber on the thick wall side of the profile, and the primary welding chamber is arranged around the secondary welding chamber and / or the baffle block.

8. The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in claim 1, characterized in that: Working belts are arranged on the surfaces of the mold hole and the mold core.

9. A method for forming a multi-cavity aluminum alloy profile with a large wall thickness difference, characterized in that: The device for forming aluminum alloy profiles with large wall thickness difference and multi-cavity wall panels as claimed in any one of claims 1 to 8 comprises the following steps: S1, prepare a billet for extrusion of a set length and heat and keep it warm, heat the die used and keep it warm; S2, the blank is extruded into the die through the diverter hole, divided into multiple metal streams by the diverter bridge, and welded in the primary welding chamber; S3, the metal flow flows from the primary welding chamber to the gap between the die hole and the die core. The flow of the metal flow on the thick wall side is restricted by the flow block and the flow velocity is reduced. A part of the metal flow on the thin wall side flows into the drainage groove, and the rest flows into the secondary welding chamber. S4. The metal flow is squeezed out from the gap between the die hole and the die core, and is formed into a multi-cavity wall panel aluminum alloy profile with a large wall thickness difference together with the metal flow flowing out through the drainage groove.

10. The method for forming a multi-cavity aluminum alloy profile with a large wall thickness difference as claimed in claim 9, characterized in that: In S1, the extrusion blank is made of aluminum or aluminum alloy; Optionally, in S2, the blank is divided into multiple metal flows by the diverter bridge and the sinker bridge, and the metal flows enter the primary welding chamber through the diverter holes or the sinker holes; Optionally, in S4, the metal flow is squeezed out from the channels between the working belts; Optionally, the following steps are also included: S5. Perform online air-cooling quenching and aging treatment on the profile extruded in S4.

Citation Information

Patent Citations

  • Protective type double-hole extrusion mould for aluminum section bar

    CN105170680A

  • Multi-core-head extrusion die

    CN216857794U

  • Hollow shape material extrusion die and thin thickness hollow shape material

    JP2001071025A

Cited By

  • Extrusion forming die and method for ultra-multi-cavity ultra-large-width-thickness-ratio ultra-thin component

    CN122538594A