Liquid crystal aligning agent, liquid crystal alignment film and method for producing same, and liquid crystal element

By combining specific polymers and diamines in the liquid crystal alignment agent to form a liquid crystal alignment film, the problems of scintillation and afterimage during driving are solved, and the display quality and charge management capabilities are significantly improved.

CN118931556APending Publication Date: 2024-11-12JICC 02 LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410455480.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-04-16
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing liquid crystal components are prone to flickering and afterimage problems during driving, especially in the edge field switching technology of asymmetric electrode structures, it is difficult to effectively suppress the accumulation of charge and affect the display quality.

Method used

A liquid crystal alignment agent is used, which comprises a first polymer and a second polymer, the first polymer comprises a specific compound structural unit, and the second polymer consists of a specific diamine, which is treated by coating and light or friction A liquid crystal alignment film is formed to prepare liquid crystal components.

Benefits of technology

It effectively suppresses flickering and afterimage generation in the liquid crystal element, improves the liquid crystal orientation, and improves the charge accumulation and relieving characteristics, and improves the display quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931556A_ABST
    Figure CN118931556A_ABST
Patent Text Reader

Abstract

The invention provides a liquid crystal aligning agent, a liquid crystal alignment film and a manufacturing method thereof, and a liquid crystal element. The liquid crystal element which shows good liquid crystal aligning property and meanwhile, generation of flicker and residual images is fully reduced can be obtained. A liquid crystal aligning agent contains a first polymer and a second polymer, the first polymer includes a structural unit (U1) derived from a compound represented by formula (1), and the second polymer includes a structural unit (U2) derived from at least one selected from a group consisting of diamine (D1) and diamine (D2). Diamine (D1): a diamine having a nitrogen atom to which a releasable group is bonded, and diamine (D2): a specific diamine having at least one type selected from the group consisting of an aromatic condensed ring structure and a linking ring structure, said diamine (D1) being a diamine having a nitrogen atom to which a releasable group is bonded, and said diamine (D2) being a specific diamine having a partial structure (a) that is at least one type selected from the group consisting of an aromatic condensed ring structure and a linking ring structure. In formula (1), X1 represents-O-,-S-,-SO2-,-CO-, an alkanediyl group having 1-20 carbon atoms, or the like. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a liquid crystal alignment agent, a liquid crystal alignment film and a method for manufacturing the same, and a liquid crystal element. Background Art

[0002] Liquid crystal elements are used in a wide range of applications, from larger display devices such as LCD TVs and information displays to smaller display devices such as smartphones. The performance of liquid crystal elements is determined by various characteristics such as the orientation of the liquid crystal, the size of the pretilt angle, and the voltage holding rate. In order to improve the performance of liquid crystal elements, in addition to the improvement of liquid crystal materials, the improvement of liquid crystal alignment films used to align liquid crystals in a certain direction has also been promoted.

[0003] In a liquid crystal element, when electric charge accumulates in the liquid crystal unit, it is visible to the observer in the form of an afterimage (direct current (DC) afterimage), or it may cause flicker (flicker) during the driving of the liquid crystal element, so there is a concern that the display quality of the liquid crystal element will be reduced. Therefore, as one of the characteristics required of the liquid crystal alignment film, it can be listed that the amount of accumulated electric charge can be reduced. As the cause of the accumulation of electric charge in the liquid crystal unit, it can be considered that the application of positive and negative asymmetric voltages caused by AC driving, or the absorption of backlight by the liquid crystal alignment film, etc. In particular, in a fringe field switching technology (FFS) type liquid crystal display element with an asymmetric electrode structure, it is prone to produce DC afterimages or flicker.

[0004] Therefore, various technologies for suppressing the accumulation of charges in the liquid crystal unit and improving the display quality of the liquid crystal element have been proposed in the past (for example, refer to Patent Document 1 or Patent Document 2). Patent Document 1 discloses that the reduction of accumulated charge is achieved by making the liquid crystal aligning agent contain the following polyamic acid, that is, a polyamic acid obtained by reacting a diamine compound containing a nitrogen-containing diamine such as N4,N4'-bis(4-aminophenyl)-benzidine with tetracarboxylic dianhydride. Patent Document 2 discloses that the liquid crystal aligning agent contains the following diamine, that is, a polymer obtained from a diamine having a structure in which a carbazole structure and a benzene ring are bonded through an amino group, thereby obtaining a liquid crystal aligning film that has a fast relaxation of accumulated charge and is not prone to flicker (flicker) during driving.

[0005] [Prior art literature]

[0006] [Patent Document]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2008-107811

[0008] [Patent Document 2] International Publication No. 2018 / 110354 Summary of the invention

[0009] [Problems to be solved by the invention]

[0010] In order to meet the requirements of further high performance in recent years, it is important that the flicker of the liquid crystal element during driving is fully suppressed (i.e., the flicker characteristics are good) and the generation of residual images is small. Therefore, it is required to develop a liquid crystal alignment agent that can form the following liquid crystal alignment film, which can not easily accumulate charges in the liquid crystal cell and more quickly relieve the accumulated residual charges while well maintaining the liquid crystal orientation as one of the basic characteristics.

[0011] The present invention has been made in view of the above-mentioned problems, and a main object of the present invention is to provide a liquid crystal aligning agent which can obtain a liquid crystal element in which the occurrence of flicker and afterimage is sufficiently reduced while showing good liquid crystal alignment.

[0012] [Technical means to solve the problem]

[0013] The present invention adopts the following means to solve the above-mentioned problems.

[0014] <1> A liquid crystal aligning agent comprising a first polymer and a second polymer different from the first polymer,

[0015] The first polymer comprises a structural unit (U1) derived from a compound represented by the following formula (1),

[0016] [Chemistry 1]

[0017]

[0018] (In formula (1), A 1 and A 2 are independently trivalent aromatic ring groups; X 1 -O-, -S-, -SO2-, -CO-, an alkanediyl group having 1 to 20 carbon atoms, or a portion of the methylene group in an alkanediyl group having 1 to 20 carbon atoms replaced by -O-, -S-, -SO2-, -CO-, -COO- or -CONR 10 -substituted divalent group; R 10 is a hydrogen atom or a monovalent hydrocarbon group)

[0019] The second polymer includes a structural unit (U2) derived from at least one selected from the group consisting of diamines (D1) and diamines (D2) shown below.

[0020] Diamine (D1): a diamine having a nitrogen atom to which a leaving group is bonded (wherein, a diamine having a partial structure in which a nitrogen atom to which a leaving group is bonded is bonded to a pyridine ring, and 1In the case of an alkanediyl group having 1 to 20 carbon atoms, the group having "-R 11 -N(R 12 )(R 13 )" represented by the monovalent group (R 11 is an alkanediyl group, R 12 For the detached radical, R 13 (except for diamines whose partial structure is formed by bonding a hydrogen atom or a leaving group to a benzene ring)

[0021] Diamine (D2): a diamine having two or more partial structures (a) in one molecule, or having the partial structure (a) and an aromatic ring structure different from the partial structure (a) in one molecule, wherein the partial structure (a) is at least one selected from the group consisting of an aromatic condensed ring structure and a linked ring structure in which two or more aromatic rings are directly linked

[0022] <2> A liquid crystal alignment film formed using the liquid crystal aligning agent according to <1>.

[0023] <3> A method for producing a liquid crystal alignment film, comprising applying the liquid crystal alignment agent according to <1> on a substrate, and performing a photo-alignment treatment or a rubbing treatment after the application to impart liquid crystal alignment capability.

[0024] <4> A liquid crystal element comprising the liquid crystal alignment film according to <2>.

[0025] [Effects of the Invention]

[0026] The liquid crystal aligning agent of the present invention can provide a liquid crystal element in which a good liquid crystal orientation is exhibited, flickering during driving is sufficiently suppressed, and generation of an afterimage is sufficiently reduced. DETAILED DESCRIPTION

[0027] Liquid crystal alignment agent

[0028] Hereinafter, each component contained in the liquid crystal aligning agent of this indication, and other components mix|blend arbitrarily as needed are demonstrated.

[0029] In addition, in this specification, the so-called "hydrocarbon group" includes the meaning of chain hydrocarbon groups, alicyclic hydrocarbon groups and aromatic hydrocarbon groups. The so-called "chain hydrocarbon group" refers to a straight-chain hydrocarbon group and a branched hydrocarbon group whose main chain does not contain a cyclic structure and is only composed of a chain structure. Among them, the chain hydrocarbon group may be saturated or unsaturated. The so-called "alicyclic hydrocarbon group" refers to a hydrocarbon group that only contains the structure of alicyclic hydrocarbon as a ring structure and does not contain an aromatic ring structure. Among them, the alicyclic hydrocarbon group does not need to be composed only of the structure of alicyclic hydrocarbon, and also includes a group having a chain structure in a part thereof. The so-called "aromatic hydrocarbon group" refers to a hydrocarbon group containing an aromatic ring structure as a ring structure. Among them, the aromatic hydrocarbon group does not need to be composed only of the aromatic ring structure, and may also contain a chain structure or alicyclic hydrocarbon structure in a part thereof. The so-called "aliphatic hydrocarbon group" refers to a chain hydrocarbon group and an alicyclic hydrocarbon group. "Aromatic ring" means an aromatic hydrocarbon ring and an aromatic heterocycle. The "organic group" refers to an atomic group formed by removing any hydrogen atom from a compound containing carbon (ie, an organic compound).

[0030] The liquid crystal aligning agent of the present disclosure contains a first polymer and a second polymer different from the first polymer. Hereinafter, the first polymer and the second polymer contained in the liquid crystal aligning agent of the present disclosure, and components prepared as needed will be described.

[0031] <First polymer>

[0032] The first polymer includes a structural unit (U1) derived from a compound represented by the following formula (1).

[0033] [Chemistry 2]

[0034]

[0035] (In formula (1), A 1 and A 2 are independently trivalent aromatic ring groups; X 1 -O-, -S-, -SO2-, -CO-, an alkanediyl group having 1 to 20 carbon atoms, or a portion of the methylene group in an alkanediyl group having 1 to 20 carbon atoms replaced by -O-, -S-, -SO2-, -CO-, -COO- or -CONR 10 -substituted divalent group; R 10 is a hydrogen atom or a monovalent hydrocarbon group)

[0036] In the formula (1), A 1 or A 2 The trivalent aromatic ring group represented by is a group formed by removing three hydrogen atoms from the ring part of a substituted or unsubstituted aromatic ring. Examples of the aromatic ring include aromatic hydrocarbon rings such as a benzene ring, a naphthalene ring, an anthracene ring, and a phenanthrene ring; and aromatic heterocyclic rings such as a pyridine ring, a pyridazine ring, a pyrimidine ring, a pyrazine ring, and a triazine ring. 1 or A 2When the trivalent aromatic ring group represented by has a substituent in the ring part, examples of the substituent include an alkyl group, an alkoxy group, a halogen atom, and the like. 1 or A 2 The aromatic ring of the trivalent aromatic ring group represented by is preferably a benzene ring or a naphthalene ring, and more preferably a benzene ring.

[0037] In X 1 When X is an alkanediyl group having 1 to 20 carbon atoms, the alkanediyl group may be linear or branched. 1 The alkanediyl group having 1 to 20 carbon atoms represented by the above-mentioned group is preferably in a straight chain form. In addition, the alkanediyl group having 1 to 20 carbon atoms preferably has 1 to 12 carbon atoms, and more preferably has 1 to 10 carbon atoms.

[0038] In X 1 In the case of a divalent group in which a part of the methylene group in an alkanediyl group having 1 to 20 carbon atoms is substituted with -O- or the like, the above explanations on preferred specific examples of the alkanediyl group having 1 to 20 carbon atoms can be applied. 10 The monovalent hydrocarbon group represented is preferably an alkyl group, more preferably a methyl group or an ethyl group.

[0039] About X 1 From the perspective of further improving the effect of reducing flicker and DC afterimage, and the availability of the compound represented by the formula (1), among the above, preferably, -O-, -S-, -SO2- or a divalent group in which a part of the methylene group in an alkanediyl group having 1 to 12 carbon atoms is substituted by -O-, -S- or -COO-, and from the perspective of electrical properties, -O- or -S- is more preferred.

[0040] Specific examples of the compound represented by the formula (1) include compounds represented by the following formulas (t1-1) to (t1-14).

[0041] [Chemistry 3]

[0042]

[0043] Relative to the total amount of the structural units constituting the first polymer, the content ratio of the structural unit (U1) in the first polymer is preferably 1 mol% or more, more preferably 2 mol% or more, and further preferably 5 mol% or more. In addition, relative to the total amount of the structural units constituting the first polymer, the content ratio of the structural unit (U1) is, for example, 50 mol% or less, and from the perspective of electrical properties, preferably 35 mol% or less. By setting the content ratio of the structural unit (U1) in the first polymer to the range, a liquid crystal element with less flicker and DC afterimage while showing good liquid crystal orientation can be obtained.

[0044] The first polymer may contain only the structural unit (U1) as a structural unit derived from tetracarboxylic dianhydride, or may further contain a structural unit different from the structural unit (U1) (hereinafter also referred to as "structural unit (T1)"). Examples of monomers providing the structural unit (T1) include aliphatic tetracarboxylic dianhydride, aromatic tetracarboxylic dianhydride, and the like. Examples of aliphatic tetracarboxylic dianhydride include chain tetracarboxylic dianhydride and alicyclic tetracarboxylic dianhydride.

[0045] Specific examples of the monomer providing the structural unit (T1) include 1,2,3,4-butanetetracarboxylic dianhydride and ethylenediaminetetraacetic dianhydride as chain tetracarboxylic dianhydride. Examples of the alicyclic tetracarboxylic dianhydride include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentanetetracarboxylic dianhydride, and cyclohexanetetracarboxylic dianhydride. As the aromatic tetracarboxylic dianhydride, pyromellitic dianhydride, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride, etc. can be cited. In addition, as the tetracarboxylic dianhydride providing the structural unit (T1), in addition to the above, a compound different from the compound represented by the formula (1) and the tetracarboxylic dianhydride described in Japanese Patent Laid-Open No. 2010-97188 can also be used. As the tetracarboxylic dianhydride providing the structural unit (T1), one kind can be used alone or two or more kinds can be used in combination.

[0046] The first polymer preferably also includes a structural unit derived from an aliphatic tetracarboxylic dianhydride (hereinafter also referred to as "structural unit (T1-1)"). By the first polymer also including the structural unit (T1-1), the solubility of the first polymer can be improved, or the organic film formed by the liquid crystal aligning agent can be given photo-orientation, which is preferred in this regard. Relative to the total amount of structural units derived from tetracarboxylic dianhydride contained in the first polymer, the content ratio of the structural unit (T1-1) in the first polymer is preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 30 mol% or more. In addition, relative to the total amount of structural units derived from tetracarboxylic dianhydride contained in the first polymer, the content ratio of the structural unit (T1-1) is preferably 95 mol% or less, more preferably 90 mol% or less.

[0047] In particular, when forming a liquid crystal aligning film by a photo-alignment method, it is preferable that tetracarboxylic dianhydride having a cyclobutane ring structure is contained as tetracarboxylic dianhydride which provides a structural unit (T1).

[0048] As long as the first polymer includes the structural unit (U1), its main skeleton is not particularly limited. In terms of the aspect that a liquid crystal alignment film having high affinity with liquid crystal and high mechanical strength and excellent voltage retention characteristics can be formed, and the aspect that the structural unit (U1) is relatively easy to introduce, the first polymer is preferably a condensation product of a tetracarboxylic acid derivative and a diamine compound, specifically, preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide. Here, "tetracarboxylic acid derivative" includes tetracarboxylic dianhydride, tetracarboxylic acid diester and tetracarboxylic acid diester dihalide.

[0049] (Polyamic acid)

[0050] When the first polymer is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [P1]") can be produced by, for example, a method of reacting a tetracarboxylic dianhydride containing a compound represented by the formula (1) with a diamine compound.

[0051] As tetracarboxylic dianhydride used in synthesizing the first polymer, the compounds represented by the above-mentioned formula (1) and monomers providing the structural unit (T1) can be listed. When synthesizing the first polymer, the proportion of the compound represented by the above-mentioned formula (1) is preferably 2 mol% or more, more preferably 5 mol% or more, and further preferably 10 mol% or more relative to the total amount of tetracarboxylic dianhydride used in the synthesis of the first polymer. By setting the proportion of the compound represented by the above-mentioned formula (1) to the above-mentioned range, a liquid crystal element having good liquid crystal orientation, flicker characteristics and DC afterimage characteristics that are balanced and improved can be obtained. In addition, from the viewpoint of suppressing the reduction of DC afterimage characteristics caused by the excessive amount of the structural unit (U1) in the first polymer, the proportion of the compound represented by the above-mentioned formula (1) is preferably 90 mol% or less, more preferably 80 mol% or less, and further preferably 70 mol% or less relative to the total amount of tetracarboxylic dianhydride used in the synthesis of the first polymer.

[0052] As the diamine compound used in the synthesis of polyamic acid [P1], a compound known as a diamine compound of a polymer component constituting a liquid crystal alignment film can be suitably used. As the diamine compound, aliphatic diamines, aromatic diamines, diaminoorganosiloxanes, etc. can be listed. Aliphatic diamines include chain diamines and alicyclic diamines. As the diamine compound, one can be used alone or two or more can be used in combination.

[0053] Specific examples of diamine compounds include meta-xylylenediamine, 1,3-propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, and 1,3-bis(aminomethyl)cyclohexane as chain diamines, and 1,4-diaminocyclohexane and 4,4'-methylenebis(cyclohexylamine) as alicyclic diamines.

[0054] Examples of the aromatic diamine include dodecyloxydiaminobenzene, tetradecyloxydiaminobenzene, pentadecyloxydiaminobenzene, hexadecyloxydiaminobenzene, octadecyloxydiaminobenzene, cholesteryloxydiaminobenzene, cholesteryl diaminobenzoate, cholesteryl diaminobenzoate, lanosteryl diaminobenzoate, 3,6-bis(4-aminobenzoyloxy)cholestane, 3,6-bis(4-aminophenoxy)cholestane, 1,1-bis(4-((amino)-)- Orienting group-containing diamines such as 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenoxy)methyl)phenyl)-4-heptylcyclohexane, 1,1-bis(4-((aminophenyl)methyl)phenyl)-4-(4-heptylcyclohexyl)cyclohexane, N-(2,4-diaminophenyl)-4-(4-heptylcyclohexyl)benzamide, and a compound represented by the following formula (E-1):

[0055] [Chemistry 4]

[0056]

[0057] (In formula (E-1), X I and X II are independently a single bond, -O-, *-COO- or *-OCO- (wherein "*" represents a bond to the diaminophenyl side); R I is an alkanediyl group having 1 to 3 carbon atoms; R II is a single bond or an alkanediyl group having 1 to 3 carbon atoms; R III is an alkyl group, an alkoxy group, a fluoroalkyl group or a fluoroalkoxy group having 1 to 20 carbon atoms; a is 0 or 1; b is an integer from 0 to 3; c is an integer from 0 to 2; d is 0 or 1; wherein 1≦a+b+c≦3),

[0058] p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylamine, 4,4'-diaminodiphenyl sulfide, 4-aminophenyl-4'-aminobenzoate, 4,4'-diaminoazobenzene, 1,2-bis(4-aminophenoxy)ethane, 1,5-bis(4-aminophenoxy)pentane, bis[2-(4-aminophenyl)ethyl]adipic acid, N,N-bis(4-aminophenyl)methylamine, 1,5-diaminonaphthalene, 2,2'-dimethyl-4, 4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 9,9-bis(4-aminophenyl)fluorene, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-(isopropylidene)dianiline, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis-(4-aminophenyl)-piperazine, 3,5-diaminobenzoic acid, 4,4'-diaminodiphenylethyl urea, etc.;

[0059] Examples of the diaminoorganosiloxane include 1,3-bis(3-aminopropyl)-tetramethyldisiloxane, and other diamines described in JP-A-2010-97188 may also be used.

[0060] As "-X" in the formula (E-1) I -(R I -X II ) d Examples of the divalent group represented by "-" include an alkanediyl group having 1 to 3 carbon atoms, -O-, *-COO-, -O-C2H4-O- (where the bond with "*" is bonded to a diaminophenyl group), etc. III The group represented by is preferably linear. The two amino groups in the diaminophenyl group are preferably located at the 2, 4-position or the 3, 5-position relative to the other groups.

[0061] Specific examples of the compound represented by the formula (E-1) include compounds represented by the following formulas (E-1-1) to (E-1-4), respectively.

[0062] [Chemistry 5]

[0063]

[0064] The liquid crystal alignment agent disclosed in the present invention comprises a first polymer and a second polymer, and a structural unit (U2) is introduced into the second polymer as a structural unit derived from diamine. The first polymer may include the structural unit (U2) or may not include the structural unit (U2). The content ratio of the structural unit (U2) in the first polymer is preferably less than that of the second polymer, specifically, relative to the total amount of the structural units derived from the diamine compound constituting the first polymer, preferably 10 mol% or less, more preferably 5 mol% or less, and further preferably 1 mol% or less. By introducing the structural unit (U2) into the second polymer, on the other hand, the content ratio of the structural unit (U2) in the first polymer is set to the range, it is easier to produce phase separation between the first polymer and the second polymer when forming a film, and the liquid crystal orientation, flicker characteristics and DC afterimage characteristics of the liquid crystal element are improved in a balanced manner, which is preferred from this point of view.

[0065] (Synthesis of Polyamic Acid)

[0066] Polyamic acid [P1] can be obtained by reacting tetracarboxylic dianhydride and diamine compound with molecular weight modifier as needed. In the synthesis reaction of polyamic acid [P1], the ratio of tetracarboxylic dianhydride to diamine compound is preferably a ratio of 0.2 equivalent to 2 equivalents of the anhydride group of tetracarboxylic dianhydride relative to 1 equivalent of the amino group of the diamine compound. As molecular weight modifiers, for example, acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride, monoamine compounds such as aniline, cyclohexylamine, and n-butylamine, monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate, etc. The ratio of molecular weight modifier is preferably set to 20 parts by mass or less relative to a total of 100 parts by mass of the tetracarboxylic dianhydride and diamine compound used.

[0067] The synthesis reaction of polyamic acid [P1] is preferably carried out in an organic solvent. The reaction temperature at this time is preferably -20°C to 150°C, and the reaction time is preferably 0.1 hour to 24 hours. As organic solvents for the reaction, for example, non-protonic polar solvents, phenolic solvents, alcoholic solvents, ketone solvents, ester solvents, ether solvents, halogenated hydrocarbons, hydrocarbons, etc. can be cited. As specific examples thereof, it is preferred to use one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphoric triamide, meta-cresol, dimethyl phenol and halogenated phenol as a reaction solvent, or use a mixture of one or more of these solvents and other organic solvents (such as butyl cellosolve, diethylene glycol diethyl ether, etc.). It is preferable that the usage-amount of an organic solvent is the amount which makes the total amount of tetracarboxylic dianhydride and diamine into 0.1 mass % - 50 mass % with respect to the whole amount of a reaction solution.

[0068] In this manner, a polymer solution in which the polyamic acid [P1] is dissolved can be obtained. The polymer solution may be used directly for the preparation of a liquid crystal aligning agent, or the polyamic acid [P1] contained in the polymer solution may be separated and then used for the preparation of a liquid crystal aligning agent.

[0069] (Polyamic acid ester)

[0070] When the first polymer is polyamic acid ester, the polyamic acid ester (hereinafter also referred to as "polyamic acid ester [P1]") can be obtained, for example, by the following methods: [I] a method of reacting polyamic acid [P1] with an esterifying agent; [II] a method of reacting a tetracarboxylic acid diester with a diamine compound; [III] a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound. Polyamic acid ester [P1] may have only an amic acid ester structure, or may be a partial ester in which an amic acid structure and an amic acid ester structure coexist. The reaction solution obtained by dissolving polyamic acid ester [P1] may be directly used for the preparation of a liquid crystal aligning agent, or may be used for the preparation of a liquid crystal aligning agent after separating the polyamic acid ester [P1] contained in the reaction solution.

[0071] (Polyimide)

[0072] When the first polymer is a polyimide, the polyimide (hereinafter also referred to as "polyimide [P1]") can be obtained, for example, by dehydrating and ring-closing the polyamic acid [P1] synthesized in the above manner and imidizing it. The polyimide [P1] may be a completely imidized product in which all the amic acid structures of the polyamic acid [P1] as its precursor are dehydrated and ring-closed, or it may be a partially imidized product in which only a part of the amic acid structure is dehydrated and ring-closed so that the amic acid structure and the imide ring structure coexist. The polyimide [P1] preferably has an imidization rate of 20% to 99%, and more preferably 30% to 90%. In addition, the imidization rate is expressed as a percentage of the ratio of the number of imide ring structures to the total number of amic acid structures and the number of imide ring structures of the polyimide. Here, a part of the imide ring may be an isoimide ring.

[0073] The dehydration ring-closure of polyamic acid [P1] is preferably carried out by the following method: dissolving polyamic acid [P1] in an organic solvent, adding a dehydrating agent and a dehydration ring-closure catalyst to the solution, and heating as needed. In the method, as a dehydrating agent, for example, an anhydride such as acetic anhydride, propionic anhydride, trifluoroacetic anhydride, etc. can be used. The amount of the dehydrating agent used is preferably set to 0.01 mol to 20 mol relative to 1 mol of the amic acid structure of polyamic acid [P1]. As a dehydration ring-closure catalyst, for example, tertiary amines such as pyridine, coltidine, dimethylpyridine, and triethylamine can be used. The amount of the dehydration ring-closure catalyst used is preferably set to 0.01 mol to 10 mol relative to 1 mol of the dehydrating agent used. As the organic solvent used in the dehydration ring-closure reaction, the organic solvents exemplified as organic solvents for synthesizing polyamic acid [P1] can be cited. The reaction temperature of the dehydration ring-closure reaction is preferably 0°C to 180°C. The reaction time is preferably 1.0 hour to 120 hours. Moreover, the reaction solution containing the polyimide [P1] may be used for preparation of a liquid crystal aligning agent as it is, and you may use it for preparation of a liquid crystal aligning agent after isolating the polyimide [P1].

[0074] <Second polymer>

[0075] The second polymer includes a structural unit (U2) derived from at least one selected from the group consisting of diamines (D1) and diamines (D2) shown below.

[0076] Diamine (D1): a diamine having a nitrogen atom to which a leaving group is bonded (wherein, a diamine having a partial structure in which a nitrogen atom to which a leaving group is bonded is bonded to a pyridine ring, and 1 In the case of an alkanediyl group having 1 to 20 carbon atoms, the group having "-R 11 -N(R 12 )(R 13 )" (wherein R 11 is an alkanediyl group, R 12 For the detached radical, R 13 (except for diamines whose partial structure is formed by bonding a hydrogen atom or a leaving group to a benzene ring)

[0077] Diamine (D2): a diamine having two or more partial structures (a) in one molecule, or having the partial structure (a) and an aromatic ring structure different from the partial structure (a) in one molecule, wherein the partial structure (a) is at least one selected from the group consisting of an aromatic condensed ring structure and a linked ring structure in which two or more aromatic rings are directly linked

[0078] ·Diamine (D1)

[0079] Diamine (D1) is a diamine having two primary amino groups participating in the polymerization reaction and a nitrogen atom bonded with a detachable group. The detachable group bonded to the nitrogen atom is a group that is detached by heat or light and replaced by a hydrogen atom. The detachable group is preferably a group that is detached by heat and replaced by a hydrogen atom (hereinafter, also referred to as a "thermal detachable group"). In the case, in the process of applying the liquid crystal alignment agent to the substrate and heating it to form a liquid crystal alignment film, the detachable group bonded to the nitrogen atom can be detached, and the process can be simplified, which is preferred in this respect. From the perspective of detachment in the process of forming a liquid crystal alignment film, the thermal detachable group is preferably a group that decomposes at a temperature of 120°C to 300°C and is replaced by a hydrogen atom.

[0080] Specific examples of the detachable group include tert-butyloxycarbonyl (Boc (t-Butyloxy carbonyl) group), benzyloxycarbonyl group, 1,1-dimethyl-2-halogenoethyloxycarbonyl group, allyloxycarbonyl group, 2-(trimethylsilyl)ethoxycarbonyl group, 9-fluorenylmethyloxycarbonyl group, etc. Among these, the Boc group is preferred in terms of excellent thermal detachability and the ability to reduce the amount of detached structures remaining in the film.

[0081] The diamine (D1) does not have a partial structure in which a nitrogen atom having a leaving group is bonded to a pyridine ring. In addition, the monomer of the structural unit (U1) in the first polymer is X in the formula (1). 1 In the case of a compound of an alkanediyl group having 1 to 20 carbon atoms, the diamine (D1) does not have "-R 11 -N(R 12 )(R 13 )" (wherein R 11 is an alkanediyl group, R 12 For the detached radical, R 13 The partial structure formed by the bond between a hydrogen atom or a leaving group and a benzene ring.

[0082] Specifically, the diamine (D1) preferably has -B 1 -NR 1 -B 2 -、-NR 1 -CO-、-NR 1 -CO-NR 2 -、-NR 1 -CO-O- or * 1 -B 3 -NR 1 R 2 (Among them, R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 1 and B2 are independently a divalent aromatic ring group or an aliphatic hydrocarbon group; 3 is a single bond or a divalent organic group; "*1" indicates a bond to the main chain) is a partial structure including a nitrogen atom to which a leaving group is bonded.

[0083] About R 1 or R 2 Examples and preferred examples of the monovalent thermally detachable group represented by are as described above. 1 or B 2 The divalent aromatic ring group represented by may be a substituted or unsubstituted aromatic hydrocarbon group or an aromatic heterocyclic group. 1 or B 2 When the aromatic ring part has a substituent, examples of the substituent include an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a hydroxyl group, and a halogen atom. 1 or B 2 It is preferably a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted nitrogen-containing aromatic heterocyclic group, and more preferably a substituted or unsubstituted aromatic hydrocarbon group.

[0084] About B 1 or B 2 Specific examples of the divalent aromatic ring groups represented by the aromatic hydrocarbon groups include groups formed by removing two arbitrary hydrogen atoms bonded to carbon atoms constituting each ring of a benzene ring, a biphenyl ring, a naphthalene ring and anthracene ring; and groups formed by removing two arbitrary hydrogen atoms bonded to carbon atoms constituting each ring of a pyridine ring, a pyrimidine ring, a pyridazine ring, a pyrazine ring, a quinoline ring, an isoquinoline ring and an acridine ring as nitrogen-containing aromatic heterocyclic groups.

[0085] In terms of further improving the liquid crystal orientation, 1 or B 2 Among them, the divalent aromatic ring group represented by is preferably a group formed by removing two hydrogen atoms from a ring portion of a substituted or unsubstituted benzene ring, biphenyl ring, naphthalene ring, pyridine ring or pyrimidine ring, and more preferably a substituted or unsubstituted phenylene group.

[0086] As B 1 or B 2 The divalent aliphatic hydrocarbon group represented by may be a divalent chain hydrocarbon group or a divalent alicyclic hydrocarbon group. The divalent chain hydrocarbon group may be saturated or unsaturated. 1 or B 2 In the case of a divalent chain hydrocarbon group, the chain hydrocarbon group is preferably saturated, more preferably an alkanediyl group having 1 to 10 carbon atoms, and further preferably a linear alkanediyl group having 1 to 6 carbon atoms. 1 or B 2In the case of a divalent alicyclic hydrocarbon group, examples of the alicyclic hydrocarbon group include substituted or unsubstituted cyclohexylene and the like. 1 or B 2 The divalent aliphatic hydrocarbon group represented is preferably a divalent chain hydrocarbon group among these, more preferably an alkanediyl group having 1 to 10 carbon atoms, and still more preferably a linear alkanediyl group having 1 to 6 carbon atoms.

[0087] In B 3 In the case of a divalent organic group, examples of the organic group include a divalent hydrocarbon group having 1 to 10 carbon atoms. 3 It is preferably a single bond or an alkanediyl group having 1 to 10 carbon atoms, more preferably a single bond or an alkanediyl group having 1 to 6 carbon atoms, and still more preferably a single bond. 1 -B 3 -NR 1 R 2 " represents a group that is bonded to the main chain. 1 -B 3 -NR 1 R 2 The group represented by " may be bonded to the chain structure constituting the main chain or to the ring structure. From the viewpoint of making the liquid crystal orientation better, the group represented by "* 1 -B 3 -NR 1 R 2 The group represented by " is preferably bonded to the chain structure constituting the main chain.

[0088] Specifically, the diamine (D1) is preferably at least one selected from the group consisting of a compound represented by the following formula (d1-1), a compound represented by the following formula (d1-2), a compound represented by the following formula (d1-3), and a compound represented by the following formula (d1-4).

[0089] [Chemistry 6]

[0090] H2N-Ar 1 -Y 1 -Ar 2 -NH2 (d1-1)

[0091] (In formula (d1-1), Ar 1 and Ar 2 are independently a divalent aromatic ring group; Y 1 A portion of the methylene groups in an alkanediyl group having 2 to 20 carbon atoms is replaced by -NR 1 -、-NR 1 -CO-、-NR 1 -CO-NR 2 -or-NR 1 -CO-O-substituted divalent group; R 1It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; wherein the nitrogen atom bonded to the leaving group and Ar 1 In the case of adjacent 1 is an aromatic hydrocarbon ring group; the nitrogen atom bonded to the leaving group and Ar 2 In the case of adjacent 2 is an aromatic hydrocarbon ring group)

[0092] [Chemistry 7]

[0093]

[0094] (In formula (d1-2), Ar 3 is a substituted or unsubstituted divalent aromatic hydrocarbon group; Ar 4 is a divalent aromatic ring group; R 1a It is a monovalent leaving group; Y 2 is a divalent hydrocarbon group having 1 to 20 carbon atoms; 1b and Y 3 , R 1b is a monovalent leaving group, and Y 3 is a single bond or a divalent organic group, or represents R 1b With Y 3 Combined with R 1b and Y 3 The nitrogen atom to which the ring is bonded together forms a ring structure; m is an integer from 0 to 3; when m is 2 or more, multiple Y 3 Same or different, multiple R 1b The same or different; wherein m is greater than 1 and R 1b When Ar is a monovalent leaving group, 4 is a substituted or unsubstituted divalent aromatic hydrocarbon group)

[0095] [Chemistry 8]

[0096]

[0097] (In formula (d1-3), Ar 5 and Ar 6 are independently divalent aromatic ring groups; R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 3 is a single bond or a divalent organic group; B 4 is a hydrogen atom or a monovalent organic group; Y 4 and Y 5 are independently a single bond or a divalent organic group; r is an integer from 1 to 3)

[0098] [Chemistry 9]

[0099]

[0100] (In formula (d1-4), Ar 7 and Ar 8 are independently trivalent aromatic ring groups; 6 is a divalent organic group; 7 For-B 3 -NR 1 R 2 ; Y 8 A hydrogen atom or -B 4 -NR 1 R 2 ; R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 3 and B 4 are independently a single bond or a divalent organic group; j is an integer from 0 to 2; wherein X in the formula (1) 1 In the case of an alkanediyl group having 1 to 20 carbon atoms, B 3 and B 4 is a single key)

[0101] Regarding the above formulas (d1-1) to (d1-4), for Ar 1 ,Ar 2 ,Ar 4 ,Ar 5 or Ar 6 Specific examples and preferred examples of the divalent aromatic ring group represented by include the following: 1 or B 2 The groups exemplified as the divalent aromatic ring groups represented by .

[0102] As Ar 3 The divalent aromatic hydrocarbon group represented by can be exemplified as B 1 or B 2 The divalent aromatic hydrocarbon group represented by the embodiment is the same as the group exemplified.

[0103] As Ar 7 or Ar 8 The trivalent aromatic ring group represented by can be exemplified by 1 or B 2 A group obtained by further removing one hydrogen atom from the groups exemplified as the divalent aromatic ring group represented by .

[0104] About R 1 , R 1a or R 1b Specific examples and preferred examples of the monovalent leaving group represented are the same as those described as the leaving group possessed by the diamine (D1).

[0105] In R 2 In the case of a monovalent organic group, examples of the monovalent organic group include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent thermally desorbable group. 2 It is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent thermally detachable group, and more preferably a monovalent thermally detachable group.

[0106] In the formula (d1-2), Y 2 The divalent hydrocarbon group having 1 to 20 carbon atoms represented by may be a chain hydrocarbon group, an alicyclic hydrocarbon group, or an aromatic hydrocarbon group. 2 It is preferably a chain hydrocarbon group, and more preferably an alkanediyl group having 1 to 10 carbon atoms.

[0107] In Y 3 In the case of a divalent organic group, examples of the divalent organic group include a divalent hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group in which a portion of the methylene groups is replaced by -O-, -CO-, -COO-, -S-, -NR 20 -、-NR 20 -CO-、-NR 20 -CO-NR 21 -or-NR 20 -CO-O-substituted divalent group. 20 and R 21 Each of them is independently a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a monovalent thermally detachable group (hereinafter the same). From the viewpoint of obtaining a liquid crystal alignment film showing good liquid crystal alignment, Y 3 The divalent organic group represented by is preferably an alkanediyl group having 1 to 10 carbon atoms, or an alkanediyl group having 2 to 10 carbon atoms in which a part of the methylene groups is replaced by -NR 20 -、-NR 20 -CO-、-NR 20 -CO-NR 21 -or-NR 20 A divalent group formed by substitution with -CO-O-.

[0108] In R 1b and Y 3 Represents R 1b With Y 3 Combined with R 1b and Y 3 In the case of a ring structure formed together with the nitrogen atoms to which the ring is bonded, examples of the ring structure include a piperidine structure and a piperazine structure.

[0109] In the formula (d1-3), in B 4 In the case of a monovalent organic group, examples of the monovalent organic group include an alkyl group and an alkoxy group having 1 to 10 carbon atoms. 4A hydrogen atom or an alkyl group having 1 to 5 carbon atoms is preferred.

[0110] In Y 4 or Y 5 In the case of a divalent organic group, the divalent organic group includes the same as Y in the formula (d1-2): 3 In the case of a divalent organic group, Y is the same group as shown in the specific examples. 4 or Y 5 The divalent organic group represented by is preferably an alkanediyl group having 1 to 10 carbon atoms among these, or an alkanediyl group having 2 to 10 carbon atoms in which a part of the methylene groups is replaced by -O-, -CO-, -COO- or -CONR 22 -(where R 22 A divalent group substituted with a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

[0111] In the formula (d1-4), Y 6 The divalent organic group represented by can be exemplified by the following as Y in the formula (d1-2): 3 In the case of a divalent organic group, the groups are the same as those shown as specific examples.

[0112] When j is 0, Y 7 B 3 Preferably, a single bond is present. When j is 1 or 2, B 3 and B 4 It is preferably a single bond or an alkanediyl group having 1 to 10 carbon atoms, more preferably a single bond or an alkanediyl group having 1 to 5 carbon atoms, and still more preferably a single bond.

[0113] As a specific example of diamine (D1), the compound etc. represented by each of following formula (d1-1-1) - formula (d1-1-23) are mentioned.

[0114] [Chemistry 10]

[0115]

[0116] [Chemistry 11]

[0117]

[0118] (In formula (d1-1-1) to formula (d1-1-23), "Boc" represents a tert-butoxycarbonyl group; t is an integer from 1 to 18)

[0119] In terms of further improving the liquid crystal orientation, flicker characteristics and DC afterimage characteristics, the diamine (D1) is preferably a compound represented by each of the formulas (d1-1) to (d1-3) in the formulas (d1-1) to (d1-4), more preferably at least one selected from the group consisting of the compound represented by the formula (d1-2) and the compound represented by the formula (d1-3), and further preferably a compound represented by the formula (d1-3).

[0120] ·Diamine (D2)

[0121] The diamine (D2) is a diamine having two or more partial structures (a) in one molecule, or having a partial structure (a) and an aromatic ring structure different from the partial structure (a) in one molecule, wherein the partial structure (a) is at least one selected from the group consisting of an aromatic condensed ring structure and a linked ring structure in which two or more aromatic rings are directly linked.

[0122] Examples of the aromatic condensed ring structure in the partial structure (a) include a naphthalene ring structure, an anthracene ring structure, a phenanthrene ring structure, a quinoline ring structure, an isoquinoline ring structure, an acridine ring structure, a benzofuran ring structure, and a benzothiophene ring structure. From the viewpoint of the ease of synthesis of the diamine (D2) and the interaction with liquid crystals, the aromatic condensed ring structure in the diamine (D2) is preferably a naphthalene ring structure or an anthracene ring structure.

[0123] From the viewpoint of easy synthesis of diamine (D2) and interaction with liquid crystal, the linked ring structure formed by directly linking two or more aromatic rings in partial structure (a) is preferably a biphenyl ring structure or a triphenyl ring structure, and more preferably a biphenyl ring structure.

[0124] From the viewpoint of the ease of synthesis of diamine (D2) and the interaction with liquid crystal, as for partial structure (a), preferably at least one selected from the group consisting of biphenyl ring structure, triphenyl ring structure, naphthalene ring structure, anthracene ring structure, phenanthrene ring structure, quinoline ring structure, isoquinoline ring structure, acridine ring structure, benzofuran ring structure and benzothiophene ring structure, more preferably at least one selected from the group consisting of biphenyl ring structure, triphenyl ring structure, naphthalene ring structure, anthracene ring structure and phenanthrene ring structure, and further preferably at least one selected from the group consisting of biphenyl ring structure, naphthalene ring structure and anthracene ring structure. In addition, the ring constituting partial structure (a) may have a substituent. As the substituent, an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, etc. can be listed.

[0125] The diamine (D2) may also have an aromatic ring structure different from the partial structure (a). The aromatic ring structure is preferably a monocyclic structure. In addition, the aromatic ring constituting the aromatic ring structure different from the partial structure (a) may be an aromatic hydrocarbon ring or an aromatic heterocyclic ring. Specific examples of aromatic hydrocarbon rings and aromatic heterocyclic rings include benzene rings, pyrrole rings, pyridine rings, pyrimidine rings, pyridazine rings, pyrazine rings, furan rings, thiophene rings, etc. Among these, at least one selected from the group consisting of benzene rings, pyridine rings and pyrimidine rings is preferred, and at least one selected from the group consisting of benzene rings and pyridine rings is more preferred. In addition, the aromatic ring possessed by the aromatic ring structure different from the partial structure (a) may also have a substituent. In the case where the diamine (D2) has an aromatic ring structure different from the partial structure (a), the total number of aromatic ring structures different from the partial structure (a) is, for example, 1 to 4, preferably 1 to 3.

[0126] Specifically, the diamine (D2) is preferably at least one selected from the group consisting of the following diamines (D2-1) and diamines (D2-2).

[0127] Diamine (D2-1): a diamine having two or more partial structures (a)

[0128] Diamine (D2-2): a diamine having one partial structure (a) and one or more aromatic ring structures different from the partial structure (a) (specifically, a monocyclic aromatic ring structure)

[0129] From the viewpoint of sufficiently obtaining the effects of improving the liquid crystal orientation, flicker characteristics and DC afterimage characteristics of the liquid crystal element in a balanced manner, the diamine (D2) preferably has a partial structure (a) in the main chain, thereby having a structure capable of introducing the partial structure (a) into the main chain of the second polymer.

[0130] Specifically, the diamine (D2) is preferably a compound represented by the following formula (d2).

[0131] [Chemistry 12]

[0132]

[0133] (In formula (d2), Ar 9 and Ar 10 are independently divalent aromatic ring groups; wherein Ar 9 and Ar 10 At least one of Z has a biphenyl structure or a condensed ring structure; 1 and Z 2 are independently single bonds, -NR 5 -、-O-、-S-、-CO-、* 3 -NR 5 -CO-,*3 -CO-NR 5 -、-NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-; R 5 and R 6 are independently a hydrogen atom or a monovalent organic group; "* 3 " indicates that the 9 or Ar 10 The bonding bond of L 1 For-NR 7 -、-O-、-S-、-CO-、* 4 -NR 7 -CO-,* 4 -CO-NR 7 -、-NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-; R 7 and R 8 are independently a hydrogen atom or a monovalent organic group; "* 4 " indicates that 5 The bonding bond of B 5 and B 6 are independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms; k is an integer of 0 to 3; when k is 2 or 3, a plurality of B 5 Same or different, multiple L 1 Same or Different)

[0134] In the formula (d2), Ar 9 or Ar 10 The divalent aromatic ring group represented by may be a substituted or unsubstituted aromatic hydrocarbon group or an aromatic heterocyclic group. 9 or Ar 10 When the aromatic ring part has a substituent, examples of the substituent include an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a hydroxyl group, and a halogen atom. 9 or Ar 10 It is preferably a substituted or unsubstituted aromatic hydrocarbon group or a substituted or unsubstituted nitrogen-containing aromatic heterocyclic group, and more preferably a substituted or unsubstituted aromatic hydrocarbon group. 9 or Ar 10 Specific examples of the divalent aromatic ring group represented by include the following: 1 or B 2 The groups exemplified as the divalent aromatic ring groups represented by .

[0135] In terms of further improving the liquid crystal orientation while maintaining the flicker characteristics and DC afterimage characteristics of the liquid crystal element well, the Ar 9 or Ar 10 The divalent aromatic ring group represented by is preferably Ar 9 and Ar 10 One of them is a group formed by removing two hydrogen atoms from a ring portion of a substituted or unsubstituted benzene ring, biphenyl ring, naphthalene ring or anthracene ring, and the other is a group formed by removing two hydrogen atoms from a ring portion of a substituted or unsubstituted biphenyl ring, naphthalene ring or anthracene ring.

[0136] In Z 1 or Z 2 For-NR 5 -, * 3 -NR 5 -CO-,* 3 -CO-NR 5 -or-NR 5 -CO-NR 6 -In the case of R 5 or R 6 The monovalent organic group represented by may include a monovalent hydrocarbon group having 1 to 10 carbon atoms and a monovalent leaving group. Examples of the monovalent hydrocarbon group having 1 to 10 carbon atoms include a monovalent chain hydrocarbon group having 1 to 10 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 10 carbon atoms, and a monovalent aromatic hydrocarbon group having 6 to 10 carbon atoms. Among these, an alkyl group having 1 to 6 carbon atoms, a cycloalkyl group, or a phenyl group is preferred, and an alkyl group having 1 to 3 carbon atoms is more preferred from the viewpoint of further improving the film density. 5 or R 6 Examples of the monovalent leaving group represented include the same groups as exemplified as the leaving group of the diamine (D1).

[0137] About R 5 and R 6 Among these, a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a Boc group is preferred.

[0138] When a photo-alignment site (preferably a cyclobutane ring structure) is introduced into the main chain of the second polymer, from the viewpoint of improving the photoreactivity of the second polymer, Z 1 and Z 2 Preferably, the Z 1 or Z 2 The adjacent aromatic group (Ar 9 ,Ar 10 ) is an electron-donating group with an electron density of . Specifically, Z 1 and Z 2 At least one of -O-, -S- or -NR 56-(R 56 is a hydrogen atom or a monovalent organic group; in Z 1 In the case of R 5 , in Z 2 In the case of R 6 ), more preferably -O-. In addition, from the above viewpoint, Z 1 and Z 2 Of these two, -O-, -S- or -NR 56 -, and more preferably -O-.

[0139] As B 5 or B 6 The divalent aliphatic hydrocarbon group represented by can be a chain hydrocarbon group having 1 to 20 carbon atoms and an alicyclic hydrocarbon group having 3 to 20 carbon atoms. Among these, the chain hydrocarbon group having 1 to 20 carbon atoms can be a straight chain or branched saturated chain hydrocarbon group having 1 to 20 carbon atoms and a straight chain or branched unsaturated chain hydrocarbon group having 2 to 20 carbon atoms. The alicyclic hydrocarbon group having 3 to 20 carbon atoms may be saturated or unsaturated, and may be monocyclic or polycyclic. 5 or B 6 In the case of an alicyclic hydrocarbon group, the alicyclic hydrocarbon group is preferably a monocyclic saturated alicyclic hydrocarbon group, and examples thereof include a group obtained by removing two hydrogen atoms from the ring portion of each of a cyclopentane ring and a cyclohexane ring.

[0140] About B 5 or B 6 The divalent aliphatic hydrocarbon group represented by is preferably a divalent straight-chain or branched hydrocarbon group having 1 to 10 carbon atoms, and more preferably a straight-chain alkanediyl group having 1 to 10 carbon atoms, from the viewpoint of obtaining a liquid crystal element that can fully obtain the effect of improving the flicker characteristics and the afterimage characteristics and exhibits good liquid crystal orientation. 5 and B 6 The carbon number of is preferably 8 or less, more preferably 5 or less, further preferably 3 or less, and further preferably 1 or 2.

[0141] In L 1 For-NR 7 -, * 4 -NR 7 -CO-,* 4 -CO-NR 7 -or-NR 7 -CO-NR 8 -In the case of R 7 or R 8 Specific examples and preferred examples of the monovalent organic group represented by include the same as those in R 5or R 6 The monovalent organic groups represented are the same groups as described above.

[0142] k is preferably 0 to 2, more preferably 0 or 1, from the viewpoint of obtaining a liquid crystal element that sufficiently improves the effect of improving the flicker characteristics and the afterimage characteristics and exhibits good liquid crystal orientation.

[0143] In addition, the structural unit (U2) may be a structural unit derived from a diamine having a partial structure (a) and a leaving group bonded to a nitrogen atom in the same molecule. In this specification, a diamine having a partial structure (a) and a leaving group bonded to a nitrogen atom in the same molecule is classified as a diamine (D2).

[0144] As a specific example of diamine (D2), the compound etc. represented by each of following formula (d2-1) - formula (d2-12) are mentioned.

[0145] [Chemistry 13]

[0146]

[0147] (In formula (d2-1) to formula (d2-8), s is an integer of 3 to 10)

[0148] In addition, the compounds represented by the formula (d2-1), formula (d2-2), formula (d2-7) to formula (d2-9) among the compounds represented by the formula (d2-1) to formula (d2-12) are equivalent to diamines having a linked ring structure as a partial structure (a). In addition, the compounds represented by the formula (d2-3) to formula (d2-7), formula (d2-10) to formula (d2-12) are equivalent to diamines having a condensed ring structure as a partial structure (a).

[0149] In terms of making the liquid crystal orientation better while maintaining the flicker characteristics and afterimage characteristics of the liquid crystal element, the structural unit (U2) is particularly preferably at least one selected from the group consisting of the compound represented by the formula (d1-3) and the compound represented by the formula (d2).

[0150] The content ratio of the structural unit (U2) in the second polymer is preferably 5 mol% or more relative to the total amount of the structural unit derived from the diamine compound possessed by the second polymer. From the viewpoint of making the liquid crystal orientation more excellent while maintaining the flicker characteristics and afterimage characteristics of the liquid crystal element well, the content ratio of the structural unit (U2) relative to the total amount of the structural unit derived from the diamine compound possessed by the second polymer is more preferably 10 mol% or more, and further preferably 20 mol% or more. In addition, the structural unit (U2) possessed by the second polymer may be only one type or two or more types.

[0151] The main skeleton of the second polymer is not particularly limited as long as it contains the structural unit (U2). In terms of being able to form a liquid crystal alignment film having high affinity with liquid crystals and mechanical strength and excellent voltage retention characteristics, and in terms of being relatively easy to introduce the structural unit (U2), the second polymer is preferably a condensation product of a tetracarboxylic acid derivative and a diamine compound, and specifically, is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide.

[0152] (Polyamic acid)

[0153] When the first polymer is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [P2]") can be produced by, for example, a method of reacting tetracarboxylic dianhydride with a diamine compound containing a monomer providing the structural unit (U2).

[0154] The tetracarboxylic dianhydride used in the synthesis of the second polymer is not particularly limited. As the tetracarboxylic dianhydride used in the synthesis of the second polymer, for example, the compound represented by the formula (1) and the monomer providing the structural unit (T1) can be listed. In the case where the compound represented by the formula (1) is used for the synthesis of the second polymer, the content ratio of the structural unit (U1) in the second polymer is preferably less than that of the first polymer. Specifically, in the second polymer, the content ratio of the structural unit (U1) is preferably 20 mol% or less, more preferably 10 mol% or less, and further preferably 5 mol% or less, relative to the total amount of the structural units derived from tetracarboxylic dianhydride constituting the second polymer. By introducing the structural unit (U1) into the first polymer and setting the content ratio of the structural unit (U1) in the second polymer to the range, a liquid crystal element can be obtained in which the flicker characteristics and DC afterimage characteristics are further reduced while showing good liquid crystal orientation.

[0155] The second polymer may contain only the structural unit (U2) as a structural unit derived from the diamine compound, but may also contain a structural unit different from the structural unit (U2) (hereinafter also referred to as "structural unit (A1)"). As monomers providing the structural unit (A1), aliphatic diamines, aromatic diamines, etc. can be cited. As aliphatic diamines, chain diamines and alicyclic diamines can be cited. As specific examples thereof, the same compounds as those exemplified as diamine compounds that can be used in the synthesis of the first polymer can be cited.

[0156] Polyamic acid [P2] can be obtained by reacting tetracarboxylic dianhydride with a diamine compound and an optional molecular weight modifier. The details of the synthesis method of polyamic acid [P2] can be applied to the description of polyamic acid [P1]. In addition, in the case where the second polymer is polyamic acid ester or polyimide, the description of polyamic acid ester [P1] and polyimide [P1] can also be applied respectively.

[0157] When a solution with a concentration of 10% by mass is prepared, the solution viscosity of the first polymer and the second polymer used in the preparation of the liquid crystal alignment agent is preferably a solution viscosity of 10mPa·s to 800mPa·s, and more preferably a solution viscosity of 15mPa·s to 500mPa·s. In addition, the solution viscosity (mPa·s) is a value measured at 25°C using an E-type rotational viscometer for a polymer solution with a concentration of 10% by mass prepared using a good solvent for the polymer (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).

[0158] For each of the first polymer and the second polymer, the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, more preferably 2,000 to 300,000. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) in terms of polystyrene measured by GPC is preferably 7 or less, more preferably 5 or less.

[0159] Relative to the total amount of solid components contained in the liquid crystal alignment agent (i.e., the total mass of components other than the solvent of the liquid crystal alignment agent) 100 parts by mass, the total content of the first polymer and the second polymer in the liquid crystal alignment agent is preferably 50 parts by mass or more, more preferably 60 parts by mass or more, and further preferably 70 parts by mass or more. In addition, when preparing the liquid crystal alignment agent, as the first polymer, one may be used alone, or two or more may be used in combination. In addition, as the second polymer, one may be used alone, or two or more may be used in combination.

[0160] The ratio of the first polymer to the second polymer contained in the liquid crystal alignment agent is preferably set to first polymer: second polymer = 40: 60 to 95: 5 in terms of mass ratio. By setting the ratio of the first polymer to the second polymer within the above range, the liquid crystal orientation, flicker characteristics and afterimage characteristics of the liquid crystal element can be balanced. From this point of view, the ratio of the first polymer to the second polymer contained in the liquid crystal alignment agent is more preferably set to first polymer: second polymer = 50: 50 to 90: 10, and more preferably set to 50: 50 to 85: 15.

[0161] From the perspective of improving the liquid crystal orientation, flicker characteristics and afterimage characteristics of the liquid crystal element in a balanced manner, the combination of the first polymer and the second polymer is preferably that the first polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, and the second polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide. Among these, it is particularly preferred that the first polymer is polyamic acid and the second polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide. In the case described above, it is believed that when the liquid crystal alignment agent of the present disclosure containing the first polymer and the second polymer is applied to the substrate, the first polymer is easily biased to the substrate side, thereby further improving the effect of the present disclosure.

[0162] <Other ingredients>

[0163] The liquid crystal aligning agent of the present disclosure may contain a component different from the first polymer and the second polymer (hereinafter also referred to as “other component”) as necessary, in addition to the first polymer and the second polymer.

[0164] Other polymers

[0165] The liquid crystal alignment agent of the present disclosure may also contain a polymer different from the first polymer and the second polymer (hereinafter, also referred to as "other polymers") as a polymer component. The main skeleton of other polymers is not particularly limited. As other polymers, for example, polyamic acid, polyamic acid ester, polyimide, polysiloxane, polyester, polyenamine (polyenamine), polyurea, polyamide, polyamideimide, polybenzoxazole precursor, polybenzoxazole, cellulose derivatives, polyacetal, addition polymer, etc. As addition polymers, (meth) acrylic polymers, styrene polymers, maleimide polymers, styrene-maleimide copolymers, etc. can be listed.

[0166] From the viewpoint of obtaining a liquid crystal element with high reliability, among the above, the other polymer is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester, polyimide, polyorganosiloxane, and addition polymer.

[0167] When other polymers are contained in the liquid crystal aligning agent, the content of the other polymers is preferably 20 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the total amount of the first polymer, the second polymer and the other polymers. As other polymers, one type may be used alone or two or more types may be used in combination.

[0168] Cross-linking agent

[0169] The liquid crystal alignment agent of the present disclosure may further contain a crosslinking agent. As the crosslinking agent, there may be listed compounds having at least one crosslinking group selected from the group consisting of the following groups: a group having a polymerizable carbon-carbon bond, a cyclic ether group, a cyclic thioether group, an isocyanate group, a protected isocyanate group, a hydroxymethyl group, a protected hydroxymethyl group, a hydroxyalkylamide group, a protected hydroxyalkylamide group, a cyclic carbonate group, a group "-CR 30 =CR 31 -R 32 -”(where R 30 It is a monovalent organic group that is separated by reaction with an amino group; R 31 is a hydrogen atom or an alkyl group, R 32 is an electron-withdrawing group), a silanol group, an amino group, a protected amino group, and an alkoxysilyl group.

[0170] Among the crosslinking groups, groups having a polymerizable carbon-carbon bond include (meth)acryloyl, maleimide, alkenyl, vinylphenyl, vinyl ether, 3-methylenetetrahydrofuran-2(3H)-one-5-yl, etc. As the crosslinking agent, among the above, a compound having a functional group capable of reacting with an amino group or a carboxyl group can be preferably used, and among them, a compound having a total of two or more selected from the group consisting of a cyclic ether group, a hydroxyalkylamide group, a protected hydroxyalkylamide group, a hydroxymethyl group, a protected hydroxymethyl group, a protected isocyanate group, an amino group, and a protected amino group can be preferably used.

[0171] From the viewpoint of improving the liquid crystal orientation, voltage holding characteristics and film strength of the liquid crystal element in a balanced manner, the number of crosslinking groups in one molecule of the crosslinking agent is preferably 2 to 12, more preferably 2 to 10. From the viewpoint of ensuring good storage stability, the molecular weight of the crosslinking agent is preferably 3,000 or less, more preferably 2,000 or less, and further preferably 1,000 or less.

[0172] Specific examples of the crosslinking agent include compounds having a cyclic ether group, such as N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenylmethane, N,N,N',N'-tetraglycidyl-4,4'-diaminodiphenyl ether, N,N-diglycidyl-aminomethylcyclohexane, N,N-diglycidyl-cyclohexylamine, and epoxidation reaction products of pentaerythritol tetraallyl ether and hydrogen peroxide.

[0173] Examples of the compound having a hydroxyalkylamide group or a protected hydroxyalkylamide group include compounds represented by the following formulas (c-1) to (c-3);

[0174] Examples of the compound having a hydroxymethyl group or a protected hydroxymethyl group include compounds represented by the following formulae (c-4) to (c-9);

[0175] Examples of the compound having a protected isocyanate group include compounds represented by the following formulae (c-10) to (c-14);

[0176] Examples of the compound having an amino group or a protected amino group include compounds represented by the following formula (c-15) to (c-18).

[0177] [Chemistry 14]

[0178]

[0179] [Chemistry 15]

[0180]

[0181] (In formula (c-8), Ac is an acetyl group)

[0182] [Chemistry 16]

[0183]

[0184] (In formula (c-10) and formula (c-11), R 34 is tert-butoxy)

[0185] [Chemistry 17]

[0186]

[0187] In the case of making the liquid crystal aligning agent of the present disclosure contain a cross-linking agent, from the viewpoint of making the liquid crystal orientation and voltage holding characteristics better, relative to the total amount of the polymer components contained in the liquid crystal aligning agent (that is, the total amount of the first polymer and the second polymer and other polymers) 100 parts by mass, the content ratio of the cross-linking agent is preferably 0.2 parts by mass or more. Relative to the total amount of 100 parts by mass of the polymer component, the content ratio of the cross-linking agent is more preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more. In addition, from the viewpoint of satisfying the liquid crystal orientation and voltage holding characteristics of the liquid crystal element, or the storage stability of the liquid crystal aligning agent, relative to the total amount of 100 parts by mass of the polymer component, the content ratio of the cross-linking agent is preferably 20 parts by mass or less, more preferably 15 parts by mass or less. As a cross-linking agent, one can be used alone, or two or more can be used in combination.

[0188] Solvent

[0189] The liquid crystal aligning agent of the present disclosure is prepared as a liquid composition in which the first polymer, the second polymer, and other components used as necessary are preferably dispersed or dissolved in an appropriate solvent.

[0190] As the solvent, an organic solvent can be preferably used. Specific examples thereof include: N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,2-dimethyl-2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone, phenol, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, diacetone alcohol, 1-hexanol, 2-hexanol, propane-1,2-diol, 3-methoxy-1-butanol, ethylene glycol monomethyl ether, methyl lactate, ethyl lactate, butyl lactate, methyl acetate, ethyl acetate, butyl acetate, acetoacetic acid Methyl ester, ethyl acetoacetate, ethyl propionate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, ethylene glycol-isopropyl ether, ethylene glycol-n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisoamyl ether, ethylene carbonate, propylene carbonate, propylene glycol monomethyl ether (propylene glycol monomethyl ether, PGME), diethylene glycol diethyl ether acetate, propylene glycol monomethyl ether acetate (propylene glycol monomethyl ether acetate, PGMEA), propylene glycol diacetate, cyclopentanone, cyclohexanone, etc. As the solvent, one kind may be used alone or two or more kinds may be used in mixture.

[0191] Other components contained in the liquid crystal alignment agent include, in addition to the above, antioxidants, metal chelate compounds, curing accelerators, surfactants, fillers, dispersants, photosensitizers, etc. The proportion of other components can be appropriately selected according to each compound within the range that does not impair the effects of the present disclosure.

[0192] The solid content concentration in the liquid crystal aligning agent (the ratio of the total mass of the components other than the solvent of the liquid crystal aligning agent to the total mass of the liquid crystal aligning agent) is appropriately selected in consideration of viscosity, volatility, etc., preferably in the range of 1% to 10% by mass. If the solid content concentration is 1% by mass or more, the film thickness of the coating can be fully ensured, and a liquid crystal aligning film showing a better liquid crystal orientation can be obtained, which is suitable in this respect. On the other hand, if the solid content concentration is 10% by mass or less, there is a tendency that the coating can be set to a moderate thickness, and it is easy to obtain a liquid crystal aligning film showing a good liquid crystal orientation. In addition, there is a tendency that the viscosity of the liquid crystal aligning agent becomes moderate, which can make the coating property good.

[0193] 《Liquid crystal alignment film and liquid crystal element》

[0194] The liquid crystal alignment film of the present invention can be manufactured using the liquid crystal alignment agent prepared as described above. In addition, the liquid crystal element of the present invention includes a liquid crystal alignment film formed using the liquid crystal alignment agent described above. The driving mode of the liquid crystal in the liquid crystal element is not particularly limited, for example, it can be applied to twisted nematic (Twisted Nematic, TN) type, super twisted nematic (Super-twisted Nematic, STN) type, vertical alignment (Vertical Alignment, VA) type (including vertical alignment-multi-domain vertical alignment (Vertical Alignment-Multi-domain Vertical Alignment, VA-MVA) type, vertical alignment-patterned vertical alignment (Vertical Alignment-Patterned Vertical Alignment, VA-PVA) type, etc.), in-plane switching (In-Plane Switching, IPS) type, fringe field switching (Fringe Field Switching, FFS) type, optically compensated bend (Optically Compensated Bend, OCB) type, polymer stabilized alignment (Polymer Sustained Alignment, PSA) type and other modes. The liquid crystal element can be produced, for example, by a method including the following steps 1 to 3. The substrate used in step 1 varies depending on the desired operation mode. Steps 2 and 3 are common to each operation mode.

[0195] <Step 1: Formation of coating film>

[0196] First, a coating film is formed on the substrate by coating a liquid crystal alignment agent on the substrate, preferably by heating the coated surface. As a substrate, for example, glass such as float glass and soda glass can be used; a transparent substrate containing plastics such as polyethylene terephthalate, polybutylene terephthalate, polyethersulfone, polycarbonate, and poly(alicyclic olefin). In the case of manufacturing a TN type, STN type or VA type liquid crystal element, two substrates provided with patterned transparent conductive films are used. On the other hand, in the case of manufacturing an IPS type or FFS type liquid crystal element, a substrate provided with electrodes patterned into a comb-shaped shape and an opposing substrate without electrodes are used. As a transparent conductive film, a NESA film (registered trademark of PPG Company, USA) containing tin oxide (SnO2), an indium tin oxide (Indium Tin Oxide, ITO) film containing indium oxide-tin oxide (In2O3-SnO2), etc. can be used.

[0197] The method for applying the liquid crystal alignment agent to the substrate is not particularly limited. The liquid crystal alignment agent can be applied to the substrate by, for example, spin coating, printing (e.g., offset printing, flexographic printing, etc.), inkjet, slit coating, rod coating, extrusion die, direct gravure coater, chamber doctor coater, offset gravure coater, impregnation coater, MB coater, etc.

[0198] After applying the liquid crystal alignment agent, it is preferred to perform preheating (prebaking) for the purpose of preventing the applied liquid crystal alignment agent from sagging. The prebaking temperature is preferably 30°C to 200°C, and the prebaking time is preferably 0.25 minutes to 10 minutes. Then, the solvent is completely removed, and a calcination (post-baking) process is performed as needed for the purpose of thermal imidization of the amide acid structure present in the polymer. The calcination temperature (post-baking temperature) at this time is preferably 80°C to 280°C, and more preferably 80°C to 250°C. The post-baking time is preferably 5 minutes to 200 minutes. The film thickness of the formed film is preferably 0.001μm to 1μm.

[0199] <Step 2: Orientation treatment>

[0200] In the case of manufacturing TN type, STN type, IPS type or FFS type liquid crystal elements, the coating formed in the process 1 is subjected to a process (orientation treatment) of imparting liquid crystal orientation ability. Thus, the orientation ability of the liquid crystal molecules is imparted to the coating to form a liquid crystal orientation film. As an orientation treatment, it is preferred to use a friction treatment in which the surface of the coating formed on the substrate is wiped with cotton or nylon, or to perform a light irradiation treatment on the coating to impart a light orientation ability to it. In the case of manufacturing a vertically oriented liquid crystal element, the coating formed in process 1 can be directly used as a liquid crystal orientation film, and in order to further improve the liquid crystal orientation ability, the coating formed in process 1 can also be subjected to an orientation treatment.

[0201] Light irradiation for photo-orientation can be performed by the following methods, etc.: a method of irradiating the coating after the post-baking process; a method of irradiating the coating after the pre-baking process and before the post-baking process; a method of irradiating the coating during the heating process of the coating in at least one of the pre-baking process and the post-baking process. As radiation irradiated to the coating, for example: ultraviolet rays and visible light containing light with a wavelength of 150nm to 800nm ​​can be used. Preferably, ultraviolet rays containing light with a wavelength of 200nm to 400nm are used. When the radiation is polarized, it can be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the irradiation can be performed from a direction perpendicular to the substrate surface, from an oblique direction, or these directions can be combined. The irradiation direction for non-polarized radiation is set to an oblique direction.

[0202] Examples of the light source include a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, and an excimer laser. The radiation dose is preferably 200 J / m 2 ~30,000J / m 2 , more preferably 500 J / m 2 ~10,000J / m 2 After irradiation with light for imparting alignment ability, the substrate surface may be cleaned using water, an organic solvent (e.g., methanol, isopropanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.

[0203] <Step 3: Construction of liquid crystal cell>

[0204] A pair of substrates formed with liquid crystal alignment films are arranged opposite to each other, and a liquid crystal unit is manufactured by arranging liquid crystal between the two oppositely arranged substrates. When manufacturing a liquid crystal unit, for example, the following methods can be cited: arranging two substrates opposite to each other with a gap in a manner that the liquid crystal alignment films face each other, bonding the peripheral portions of the two substrates with a sealant, injecting and filling liquid crystal into the cell gap surrounded by the substrate surface and the sealant and sealing the injection hole, and a method using a liquid crystal dripping (One Drop Fill, ODF) method. As a sealant, for example, an epoxy resin containing a hardener and alumina balls as a spacer can be used. As liquid crystals, nematic liquid crystals and smectic liquid crystals can be cited, among which nematic liquid crystals are preferred.

[0205] When manufacturing a liquid crystal display device, a polarizing plate is then attached to the outer surface of the liquid crystal cell. Examples of the polarizing plate include a polarizing plate formed by sandwiching a polarizing film called "H film" in which polyvinyl alcohol is stretched and oriented on one side and iodine is absorbed on the other side, with a cellulose acetate protective film, or a polarizing plate containing the H film itself.

[0206] The liquid crystal element disclosed in the present invention can be effectively applied to various purposes. Specifically, for example, it can be used as a clock, a portable game console, a word processor, a notebook personal computer, a car navigation system, a camcorder, a personal digital assistant (PDA), a digital camera, a mobile phone, a smart phone, various monitors, a liquid crystal television, an information display, and other display devices or dimming devices, a phase difference film, etc.

[0207] The present disclosure described in detail above can provide the following means.

[0208] [Means 1] A liquid crystal alignment agent comprising a first polymer and a second polymer different from the first polymer,

[0209] The first polymer includes a structural unit (U1) derived from the compound represented by the formula (1), and the second polymer includes a structural unit (U2) derived from at least one selected from the group consisting of the diamine (D1) and diamine (D2) shown above.

[0210] [Means 2] The liquid crystal aligning agent according to [Means 1], wherein the diamine (D1) has -B 1 -NR 1 -B2 -、-NR 1 -CO-、-NR 1 -CO-NR 2 -、-NR 1 -CO-O- or * 1 -B 3 -NR 1 R 2 (R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 1 and B 2 are independently a divalent aromatic ring group or an aliphatic hydrocarbon group; 3 is a single bond or a divalent organic group; "* 1 ” represents a partial structure represented by a bond to the main chain).

[0211] [Means 3] A liquid crystal alignment agent according to [Means 1] or [Means 2], wherein the diamine (D1) is at least one selected from the group consisting of a compound represented by the formula (d1-1), a compound represented by the formula (d1-2), a compound represented by the formula (d1-3) and a compound represented by the formula (d1-4).

[0212] [Means 4] The liquid crystal aligning agent according to any one of [Means 1] to [Means 3], wherein the diamine (D2) is represented by the formula (D2).

[0213] [Means 5] The liquid crystal alignment agent according to any one of [Means 1] to [Means 4], wherein the first polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.

[0214] [Means 6] The liquid crystal alignment agent according to any one of [Means 1] to [Means 5], wherein the second polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.

[0215] [Means 7] The liquid crystal alignment agent according to any one of [Means 1] to [Means 6], wherein the first polymer is polyamic acid, and the second polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide.

[0216] [Means 8] The liquid crystal aligning agent according to any one of [Means 1] to [Means 7], wherein the first polymer further includes a structural unit derived from an aliphatic tetracarboxylic dianhydride.

[0217] [Means 9] A liquid crystal alignment film formed using the liquid crystal alignment agent according to any one of [Means 1] to [Means 8].

[0218] [Means 10] A method for producing a liquid crystal alignment film, comprising applying the liquid crystal alignment agent according to any one of [Means 1] to [Means 8] on a substrate, and performing a photo-alignment treatment or a rubbing treatment after the application to impart liquid crystal alignment ability.

[0219] [Means 11] A liquid crystal element comprising the liquid crystal alignment film according to [Means 9].

[0220] [Example]

[0221] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0222] <Structure and abbreviation of the compound>

[0223] The structures and abbreviations of the main compounds used in the following examples are as follows.

[0224] [Tetracarboxylic dianhydride]

[0225] Compound (TA-1) to Compound (TA-13): Compounds represented by the following formula (TA-1) to (TA-13)

[0226] [Chemistry 18]

[0227]

[0228] [Diamine (D1)]

[0229] Compound (DA-1) to Compound (DA-8): Compounds represented by the following formula (DA-1) to (DA-8)

[0230] [Chemistry 19]

[0231]

[0232] [Diamine (D2)]

[0233] Compound (DB-1) to Compound (DB-6): Compounds represented by the following formula (DB-1) to (DB-6)

[0234] [Chemistry 20]

[0235]

[0236] [Other diamines]

[0237] Compound (DC-1) to Compound (DC-7): Compounds represented by the following formula (DC-1) to (DC-7)

[0238] [Chemistry 21]

[0239]

[0240] [additive]

[0241] Compound (AD-1) to Compound (AD-3): Compounds represented by the following formula (AD-1) to (AD-3)

[0242] [Chemistry 22]

[0243]

[0244] [Solvent]

[0245] NMP: N-methyl-2-pyrrolidone

[0246] BC: Butyl Cellosolve (BC)

[0247] <Polymer Synthesis>

[0248] A polymer was synthesized in each of the following Synthesis Examples 1 to 43. In the following examples, the imidization ratio of the polyimide in the polymer solution was measured by the following method.

[0249] ·Determination of imidization rate of polyimide

[0250] The polyimide solution was put into pure water, the obtained precipitate was fully dried under reduced pressure at room temperature, and then dissolved in deuterated dimethyl sulfoxide. The hydrogen nuclear magnetic resonance (HNMR) was performed at room temperature using tetramethylsilane as a reference substance. 1 H-nuclear magnetic resonance, 1 H-NMR) determination. 1 The imidization ratio [%] was determined by using the following formula (1) using H-NMR spectrum (400 MHz).

[0251] Imidization rate [%] = (1-(A1 / (A2×α)))×100…(1)

[0252] (In formula (1), A1 is the peak area of ​​protons derived from amide groups appearing around a chemical shift of 10 ppm, A2 is the peak area of ​​protons derived from aromatic groups appearing around a chemical shift of 6 ppm to 9 ppm, and α is the ratio of the number of protons of aromatic groups to one proton of amide groups in the precursor of the polymer (polyamic acid))

[0253] [Synthesis example 1]

[0254] Diamine (DC-1) was dissolved in NMP, and 0.95 molar equivalent of tetracarboxylic dianhydride (TA-2) was added based on the total amount of diamine, and the mixture was reacted at room temperature for 6 hours to obtain a 15 mass % solution of a polyamic acid (hereinafter referred to as "polymer (PA-1)").

[0255] [Synthesis Example 2 to Synthesis Example 31]

[0256] The types and amounts of tetracarboxylic dianhydride and diamine were changed as described in Table 1 below, and polyamic acids (polymers (PA-2) to (PA-31)) were obtained in the same manner as in Synthesis Example 1. In addition, the amount of tetracarboxylic dianhydride used (the total amount when two or more types are used) was 0.95 molar equivalents relative to the total amount of diamines used in each synthesis.

[0257] [Synthesis Example 32]

[0258] The diamine (50 molar parts of diamine (DA-1) and 50 molar parts of diamine (DC-1) relative to 100 molar parts of all diamines) was dissolved in NMP, and 0.95 molar equivalent of tetracarboxylic dianhydride (TA-1) was added relative to the total amount of diamines, and the reaction was carried out at room temperature for 6 hours to obtain a solution of polyamic acid. 1-Methylpiperidine and acetic anhydride were added as dehydrating agents to the obtained solution in an amount of 1.5 molar equivalents relative to the carboxyl group of the polyamic acid, respectively, and heated and stirred at 60°C for 3 hours. For the obtained solution, reduced pressure concentration and dilution with NMP were repeated to obtain a 10 mass % solution of polyimide (set to "polymer (PI-1)"). The imidization rate of polymer (PI-1) is 80%.

[0259] [Synthesis Example 33 to Synthesis Example 50]

[0260] Except having changed the kind and amount of tetracarboxylic dianhydride and diamine as described in the following Table 2, respectively, it carried out similarly to Synthesis Example 32, and obtained the polyimide (it was called polymer (PI-2) - polymer (PI-19)).

[0261] [Table 1]

[0262]

[0263] [Table 2]

[0264]

[0265] The numerical values ​​in Tables 1 and 2 indicate the usage ratio (mol %) of each compound relative to the total amount (100 mol %) of tetracarboxylic dianhydride used in the synthesis for acid dianhydrides, and indicate the usage ratio (mol %) of each compound relative to the total amount (100 mol %) of diamines used in the synthesis for diamines.

[0266] <Preparation and evaluation of liquid crystal alignment agents>

[0267] [Example 1: Photo-aligned FFS-type liquid crystal display element]

[0268] (1) Preparation of Liquid Crystal Alignment Agent

[0269] The polymer components (solid content conversion: polymer (PI-1) 15 parts by mass, polymer (PA-9) 85 parts by mass) and 5 parts by mass of the additive (AD-2) were mixed and diluted with NMP and BC to obtain a solution having a solid content concentration of 3.5% by mass and a solvent composition ratio of NMP:BC = 65:35 (mass ratio). The solution was filtered with a filter having a pore size of 0.2 μm to prepare a liquid crystal aligning agent (AL-1).

[0270] (2) Formation of a liquid crystal alignment film by a photo-alignment method

[0271] The liquid crystal alignment agent (AL-1) prepared in (1) was applied to the glass substrate on which a flat electrode, an insulating layer and a comb-shaped electrode were sequentially stacked on one side and the opposite glass substrate without an electrode using a spin coater, and heated on a 90°C hot plate for 1 minute, and then heated in a 230°C oven in which the air in the chamber was replaced with nitrogen for 20 minutes to form a coating film with an average film thickness of 100 nm. The coating film surface was irradiated with ultraviolet rays containing a linearly polarized 254 nm bright line at 500 mJ / cm2 from the normal direction of the substrate using a Hg-Xe lamp. 2 The coating film subjected to the photo-alignment treatment was heated for 40 minutes in an oven at 230° C. in which the interior of the chamber was substituted with nitrogen to perform heat treatment, thereby forming a liquid crystal alignment film.

[0272] (3) Manufacturing of FFS type liquid crystal display elements

[0273] A liquid crystal injection port is reserved on the periphery of the surface with a liquid crystal orientation film of one of the substrates with a liquid crystal orientation film prepared in the above (2), and an epoxy resin adhesive containing alumina balls with a diameter of 3.5 μm is applied by a dispenser, and then the surfaces with a liquid crystal orientation film of a pair of substrates are made to face each other, and the orientation treatment directions of each substrate are crimped in an anti-parallel manner, and the adhesive is thermally cured at 150°C for 1 hour. Then, after the positive nematic liquid crystal (Merck, LCCC-18-514) is filled into the gap between the substrates from the liquid crystal injection port, the liquid crystal injection port is sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, it is heated at 120°C and then slowly cooled to room temperature. Secondly, the polarizing plate is attached to the outer two surfaces of the substrate in a manner in which its polarization directions are orthogonal to each other and are at an angle of 45° to the orientation treatment direction of the liquid crystal orientation film, thereby manufacturing an FFS type liquid crystal display element.

[0274] (4) Evaluation of Liquid Crystal Orientation

[0275] For the FFS type liquid crystal display element manufactured in (3), the presence or absence of abnormal domain in the light and dark change when the voltage of 7.2V is applied / released (ON / OFF) is observed using a microscope at a magnification of 50 times. Regarding the evaluation, the case where no abnormal domain is observed at all is set as "excellent", the case where the abnormal domain is partially observed is set as "good", and the case where the abnormal domain is fully observed is set as "poor". The result is "excellent" in this embodiment.

[0276] (5) Evaluation of flicker at room temperature (flicker characteristics)

[0277] The FFS type liquid crystal display element manufactured in (3) was placed in an environment of 23°C and 1 atmosphere. 2 Under the backlight irradiation, the pixels of the FFS type liquid crystal display element are driven by applying an alternating current (AC) voltage with a relative transmittance of 25%. Flicker is generated in the pixel by the gradually accumulated charge. The flicker of light is detected using RD-80S (manufactured by TOPCON TECHNOHOUSE). The case where the flicker change ratio from the initial state after 30 minutes from the start of self-driving is less than 2% is set to "excellent", the case where it is more than 2% and less than 4% is set to "good", and the case where it is more than 4% is set to "unacceptable". The result is an "excellent" evaluation in this embodiment.

[0278] (6) Evaluation of high-temperature short-term afterimage (DC accumulation and relaxation characteristics)

[0279] The FFS type liquid crystal display element manufactured in (3) was placed in an environment of 65°C and 1 atmosphere. After being driven by an alternating current rectangular wave (AC) with a frequency of 30 Hz and a relative transmittance of 100% and the brightness difference between any two pixels was set to 0, the luminance difference between any two pixels was set to 5000 cd / m 2 Under the backlight illumination, only one pixel is AC driven, thereby accumulating charge. When the two pixels are restored to AC drive with a relative transmittance of 25%, a brightness difference occurs between the two pixels due to the accumulated charge. When AC drive is continued, the accumulated charge is released, and the brightness difference between the two pixels gradually decreases. The brightness difference when AC drive with a relative transmittance of 25% is continued for three minutes is set to ΔL. In addition, as a general tendency, it is easier to accumulate charge in the liquid crystal unit at high temperature than at room temperature. Therefore, in order to compare the ease of charge accumulation of the liquid crystal unit between samples under more severe conditions, the ease of charge accumulation of the liquid crystal element was evaluated by a method that reflects the initial amount of accumulated charge under a high temperature environment (short-term afterimage evaluation). It can be said that the smaller the brightness difference ΔL, the less likely it is to accumulate charge, or the easier it is to release the accumulated charge, or the less likely it is to accumulate charge and the easier it is to release the accumulated charge, and the better the afterimage characteristics. The value obtained by dividing the brightness difference ΔL by the average brightness of the two pixels was evaluated as "excellent" when it was less than 1%, "good" when it was 1% or more and less than 3%, and "unacceptable" when it was 3% or more. The result was evaluated as "excellent" in this example.

[0280] [Example 2 to Example 37 and Comparative Example 1 to Comparative Example 17]

[0281] In Example 1, the types and amounts of the polymer components and additives contained in the liquid crystal aligning agent were changed as shown in Table 3 below. In addition, the liquid crystal aligning agent was prepared in the same manner as in Example 1, and a liquid crystal aligning film was formed by a photo-alignment method, and an FFS type liquid crystal display element was manufactured and various evaluations were performed. The evaluation results are shown in Tables 3 and 4 below.

[0282] [Table 3]

[0283]

[0284] [Table 4]

[0285]

[0286] [Example 38: Rubbing-aligned FFS-type liquid crystal display element]

[0287] (1) Preparation of Liquid Crystal Alignment Agent

[0288] The polymer components (solid content conversion: polymer (PI-28) 10 parts by mass, polymer (PA-7) 90 parts by mass) were mixed and diluted with NMP and BC to obtain a solution having a solid content concentration of 3.5% by mass and a solvent composition ratio of NMP:BC = 65:35 (mass ratio). The solution was filtered with a filter having a pore size of 0.2 μm to prepare a liquid crystal aligning agent (AL-55).

[0289] (2) Formation of liquid crystal alignment film by rubbing method

[0290] The liquid crystal alignment agent (AL-55) prepared in (1) is applied to the glass substrate on which a flat electrode, an insulating layer and a comb-shaped electrode are sequentially stacked on one side and the opposite glass substrate on which no electrode is set, using a spin coater, and heated on a hot plate at 80°C for 1 minute, and then heated in a 230°C oven in which nitrogen is replaced in the storehouse for 30 minutes to form a coating with an average film thickness of 100 nm. For the surface of the coating, a friction machine having a roller wound with a nylon cloth is used, and the friction treatment is performed twice at a roller speed of 1000 rpm, a platform moving speed of 30 mm / second, and a hair pressing length of 0.3 mm. After the coating subjected to the friction orientation treatment is ultrasonically cleaned in ultrapure water for 1 minute, it is dried in an oven at 100°C for 10 minutes to form a liquid crystal alignment film.

[0291] (3) Manufacturing of FFS type liquid crystal display elements

[0292] A FFS type liquid crystal display element was produced in the same manner as in Example 1 except that a pair of substrates having the liquid crystal alignment film produced by the rubbing method in (2) was used as the substrate having the liquid crystal alignment film.

[0293] (4) Evaluation of Liquid Crystal Orientation

[0294] The FFS liquid crystal display element produced in (3) was evaluated for liquid crystal orientation in the same manner as in Example 1. The result was evaluated as "excellent" in this example.

[0295] (5) Evaluation of flicker characteristics at room temperature

[0296] The FFS liquid crystal display element produced in (3) was evaluated for flicker characteristics in the same manner as in Example 1. The result was evaluated as "excellent" in this example.

[0297] (6) Evaluation of high-temperature short-term afterimage (DC accumulation characteristics)

[0298] The FFS liquid crystal display element produced in (3) was evaluated for high-temperature short-term image retention in the same manner as in Example 1. The result was evaluated as "excellent" in this example.

[0299] [Example 39 to Example 46 and Comparative Example 18 to Comparative Example 32]

[0300] In Example 38, the types and amounts of the polymer components and additives contained in the liquid crystal aligning agent were changed as shown in Table 5 below. Otherwise, the liquid crystal aligning agent was prepared in the same manner as in Example 38, a liquid crystal aligning film was formed by a rubbing method, and an FFS type liquid crystal display element was manufactured and various evaluations were performed. The evaluation results are shown in Table 5 below.

[0301] [Table 5]

[0302]

[0303] As is clear from Tables 3 to 5, by using the liquid crystal alignment agents of Examples 1 to 46 comprising a first polymer containing a structural unit (U1) and a second polymer containing a structural unit (U2), a liquid crystal element can be obtained in which the liquid crystal orientation, flicker characteristics and afterimage characteristics are balancedly improved.

[0304] In contrast, the liquid crystal orientation agents of Comparative Examples 1 to 32, which contain only one of the first polymer containing the structural unit (U1) and the second polymer containing the structural unit (U2), or neither of them, have one or more of poor liquid crystal orientation, flicker characteristics, and DC afterimage characteristics, which are worse than those of Examples 1 to 46.

Claims

1. A liquid crystal alignment agent comprising a first polymer and a second polymer different from the first polymer, The first polymer comprises a structural unit (U1) derived from a compound represented by the following formula (1), In formula (1), A 1 and A 2 are independently trivalent aromatic ring groups; X 1 -O-, -S-, -SO2-, -CO-, an alkanediyl group having 1 to 20 carbon atoms, or a portion of the methylene group in an alkanediyl group having 1 to 20 carbon atoms replaced by -O-, -S-, -SO2-, -CO-, -COO- or -CONR 10 -substituted divalent group; R 10 is a hydrogen atom or a monovalent hydrocarbon group; The second polymer includes a structural unit (U2) derived from at least one selected from the group consisting of diamines (D1) and diamines (D2) shown below, Diamine (D1): a diamine having a nitrogen atom to which a leaving group is bonded, wherein The diamine having a partial structure in which a nitrogen atom having a leaving group is bonded to a pyridine ring, and the X 1 In the case of an alkanediyl group having 1 to 20 carbon atoms, the group having "-R 11 -N(R 12 )(R 13 )" is a diamine with a partial structure formed by bonding a monovalent group represented by a benzene ring; wherein the "-R 11 -N(R 12 )(R 13 )" represents a monovalent group R 11 is an alkanediyl group, R 12 For the detached radical, R 13 A hydrogen atom or a free radical; Diamine (D2): a diamine having two or more partial structures (a) in one molecule, or having the partial structure (a) and an aromatic ring structure different from the partial structure (a) in one molecule, wherein the partial structure (a) is at least one selected from the group consisting of an aromatic condensed ring structure and a linked ring structure in which two or more aromatic rings are directly linked.

2. The liquid crystal alignment agent according to claim 1, wherein The diamine (D1) has -B 1 -NR 1 -B 2 -、-NR 1 -CO-、-NR 1 -CO-NR 2 -、-NR 1 -CO-O- or * 1 -B 3 -NR 1 R 2 The partial structure represented by 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 1 and B 2 are independently a divalent aromatic ring group or an aliphatic hydrocarbon group; 3 is a single bond or a divalent organic group; "* 1 ” indicates the bond to the main chain.

3. The liquid crystal alignment agent according to claim 1, wherein The diamine (D1) is at least one selected from the group consisting of a compound represented by the following formula (d1-1), a compound represented by the following formula (d1-2), a compound represented by the following formula (d1-3), and a compound represented by the following formula (d1-4), <h2 style=";text-align:left;direction:ltr">H2N-Ar<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> -Y<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> -Ar<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> -NH2(d1-1) In formula (d1-1), Ar 1 and Ar 2 are independently a divalent aromatic ring group; Y 1 A portion of the methylene groups in an alkanediyl group having 2 to 20 carbon atoms is replaced by -NR 1 -、-NR 1 -CO-、-NR 1 -CO-NR 2 -or-NR 1 -CO-O-substituted divalent group; R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; Among them, the nitrogen atom bonded to the leaving group and Ar 1 In the case of adjacent 1 is an aromatic hydrocarbon ring group; the nitrogen atom bonded to the leaving group and Ar 2 In the case of adjacent 2 is an aromatic hydrocarbon ring group; In formula (d1-2), Ar 3 is a substituted or unsubstituted divalent aromatic hydrocarbon group; Ar 4 is a divalent aromatic ring group; R 1a It is a monovalent leaving group; Y 2 is a divalent hydrocarbon group having 1 to 20 carbon atoms; 1b and Y 3 , R 1b is a monovalent leaving group, and Y 3 is a single bond or a divalent organic group, or represents R 1b With Y 3 Combined with R 1b and Y 3 The nitrogen atom to which the ring is bonded together forms a ring structure; m is an integer from 0 to 3; when m is 2 or more, multiple Y 3 Same or different, multiple R 1b The same or different; wherein m is greater than 1 and R 1b When Ar is a monovalent leaving group, 4 is a substituted or unsubstituted divalent aromatic hydrocarbon group; In formula (d1-3), Ar 5 and Ar 6 are independently a divalent aromatic ring group; R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 3 is a single bond or a divalent organic group; B 4 is a hydrogen atom or a monovalent organic group; Y 4 and Y 5 are independently a single bond or a divalent organic group; r is an integer from 1 to 3; In formula (d1-4), Ar 7 and Ar 8 are independently trivalent aromatic ring groups; 6 is a divalent organic group; 7 For-B 3 -NR 1 R 2 ; Y 8 A hydrogen atom or -B 4 -NR 1 R 2 ; R 1 It is a monovalent leaving group; R 2 is a hydrogen atom or a monovalent organic group; B 3 and B 4 are independently a single bond or a divalent organic group; j is an integer from 0 to 2; wherein X in the formula (1) 1 In the case of an alkanediyl group having 1 to 20 carbon atoms, B 3 and B 4 For a single key.

4. The liquid crystal alignment agent according to claim 1, wherein The diamine (D2) is represented by the following formula (D2): In formula (d2), Ar 9 and Ar 10 are independently divalent aromatic ring groups; wherein Ar 9 and Ar 10 At least one of Z has a biphenyl structure or a condensed ring structure; 1 and Z 2 are independently single bonds, -NR 5 -、-O-、-S-、-CO-、* 3 -NR 5 -CO-,* 3 -CO-NR 5 -、-NR 5 -CO-NR 6 -, * 3 -CO-O- or * 3 -O-CO-; R 5 and R 6 are independently a hydrogen atom or a monovalent organic group; "* 3 " indicates that the 9 or Ar 10 The bonding bond of L 1 For-NR 7 -、-O-、-S-、-CO-、* 4 -NR 7 -CO-,* 4 -CO-NR 7 -、-NR 7 -CO-NR 8 -, * 4 -CO-O- or * 4 -O-CO-; R 7 and R 8 are independently a hydrogen atom or a monovalent organic group; "* 4 " indicates that 5 The bonding bond of B 5 and B 6 are independently a divalent aliphatic hydrocarbon group having 1 to 20 carbon atoms; k is an integer of 0 to 3; when k is 2 or 3, a plurality of B 5 Same or different, multiple L 1 Same or different.

5. The liquid crystal alignment agent according to claim 1, wherein The first polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.

6. The liquid crystal alignment agent according to claim 1, wherein The second polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.

7. The liquid crystal alignment agent according to claim 1, wherein: The first polymer is polyamic acid, The second polymer is at least one selected from the group consisting of polyamic acid, polyamic acid ester, and polyimide.

8. The liquid crystal alignment agent according to claim 1, wherein The first polymer further includes a structural unit derived from an aliphatic tetracarboxylic dianhydride. 9 . A liquid crystal alignment film, formed using the liquid crystal alignment agent according to claim 1 . 10 . A method for producing a liquid crystal alignment film, comprising applying the liquid crystal alignment agent according to claim 1 on a substrate, and performing a photo-alignment treatment or a rubbing treatment after the application to impart liquid crystal alignment capability. 11 . A liquid crystal element comprising the liquid crystal alignment film according to claim 9 .