Grain-oriented electrical steel sheet and method for producing same
By controlling the relationship between the laser groove and the thickness of the glass film, the problem of reducing magnetic flux density in the prior art is solved, and the iron loss reduction and magnetic domain subdividing effect of directional electromagnetic steel plate is achieved, the process is simplified and the production efficiency is improved. .
Patent Information
- Application Number
- CN202380029357.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-04
- Filing Date
- 2023-04-04
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, when forming a laser groove of a directional electromagnetic steel plate, the decrease in magnetic flux density leads to deterioration of iron losses, and the process is complicated and it is difficult to achieve high-speed processing.
By controlling the shape of the laser groove and the thickness of the glass film, it is ensured that the thickness of the glass film in the groove recess is thicker than that of the flat portion, and meets a specific thickness ratio relationship. Combined with the laser irradiation and annealing process, an optimized magnetic domain subdividing effect is formed.
The effect of reducing iron loss and magnetic domain subdividing is achieved, the performance of directional electromagnetic steel plate is improved, and the process is simplified and production efficiency is improved.
Smart Images

Figure CN118946681A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a grain-oriented electromagnetic steel sheet. Background Art
[0002] Grain-oriented electrical steel sheets are steel sheets whose crystal orientation is controlled by a combination of cold rolling and annealing so that the easy magnetization axis of the crystal grains is aligned with the rolling direction.
[0003] As a technology for reducing eddy current loss, which is one of the iron losses of grain-oriented electromagnetic steel sheets, it is known to form an insulating film on the surface of a base steel sheet with controlled crystal orientation. The insulating film not only has electrical insulation properties, but also has the functions of imparting tension and rust resistance to the base steel sheet.
[0004] In addition, as another method for reducing eddy current loss, the following magnetic domain control method is known: by forming strain regions or grooves formed in a direction intersecting the rolling direction at predetermined intervals along the rolling direction, the width of the 180° magnetic domain is narrowed (the 180° magnetic domain is subdivided). The magnetic domain control method is classified into a method of applying strain to the base steel sheet of the directional electromagnetic steel sheet and a method of forming grooves on the surface of the base steel sheet where a film that applies tension to the base steel sheet exists.
[0005] By using a grain-oriented electromagnetic steel sheet that has been subjected to magnetic domain control using grooves to manufacture the iron core (winding core) of the transformer, the grooves will not disappear even after strain relief annealing, so the magnetic domain segmentation effect can be maintained. Therefore, as a method for reducing eddy current loss for the winding core, a magnetic domain control method using groove formation is sometimes used.
[0006] Figure 1 This is a diagram schematically showing an electromagnetic steel sheet having grooves formed therein. Figure 1 , a state in which a plurality of grooves 2 are formed at intervals on the surface of a base steel plate 1 along the rolling direction of the base steel plate 1 is shown. Figure 1 In the figure, the symbol θ represents the angle between the direction (plate width direction) perpendicular to the rolling direction and the plate thickness direction of the base steel plate 1 and the length direction of the groove 2. The symbol W represents the width of the groove 2, the symbol D represents the depth of the groove 2, and the symbol P represents the interval between adjacent grooves 2 in the rolling direction.
[0007] Various methods for forming grooves in electromagnetic steel sheets have been proposed. For example, Patent Document 1 discloses an electrolytic etching method for forming grooves on the surface of a grain-oriented electromagnetic steel sheet by electrolytic etching. For example, Patent Document 2 discloses a gear pressing method for forming grooves on the surface of a grain-oriented electromagnetic steel sheet by mechanically pressing a gear on the surface of the steel sheet.
[0008] However, the electrolytic etching method requires masking, etching, and mask removal, and has a problem of being more complicated than the mechanical method. The gear pressing method has a problem of wearing out the gears in a short period of time due to the high hardness of the electromagnetic steel sheet. From the perspective of further high-speed processing, it is difficult to achieve a line speed of 100 mpm or more as required in the general steel manufacturing process.
[0009] In addition, for example, Patent Document 3 discloses a laser irradiation method for melting and evaporating a laser irradiated portion of a grain-oriented electrical steel sheet surface by laser irradiation. The laser irradiation method does not cause problems such as tooth wear or complicated processes, and can also be processed at high speed.
[0010] In the laser irradiation method, several groove forming processes are also disclosed. For example, Patent Document 4 proposes forming grooves on a cold-rolled steel sheet by laser irradiation. However, when the cold-rolled steel sheet is laser irradiated, a glass film formed of forsterite is formed at the bottom of the groove in the final product. Since the glass film is a non-magnetic oxide, the magnetic flux density of the steel sheet is reduced, and the deterioration of the iron loss caused by this is a problem.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Publication No. 62-54873
[0014] Patent Document 2: Japanese Patent Publication No. 62-53579
[0015] Patent Document 3: Japanese Patent Application Publication No. 2003-129135
[0016] Patent Document 4: International Publication No. 2019 / 156127
[0017] Patent Document 5: International Publication No. 2011 / 007771 Summary of the invention
[0018] Problems to be solved by the invention
[0019] The present invention has been developed in view of the above-mentioned actual situation, and an object of the present invention is to provide a grain-oriented electromagnetic steel sheet having further improved iron loss in magnetic domain control of laser grooves (grooves formed by laser irradiation) formed in a cold-rolled steel sheet.
[0020] Means for solving problems
[0021] The present inventors have repeatedly conducted in-depth research to solve the above-mentioned problems. In the process of repeatedly studying the laser irradiation conditions when forming laser grooves, it was found that the glass film formed on the surface of the steel plate has a magnetic domain control effect. Although the magnetic flux density is reduced, it has an effect of improving iron loss. The present invention is completed based on this knowledge, and its main purpose is as follows. [1]
[0023] A grain-oriented electromagnetic steel sheet according to one embodiment of the present invention is a grain-oriented electromagnetic steel sheet, characterized in that it comprises a base steel sheet having a plurality of grooves on the surface of the steel sheet and a glass film formed on the surface of the base steel sheet. When the angle θ formed by the direction perpendicular to the rolling direction and the plate thickness direction of the base steel sheet and the length direction of the groove is 0 to 40°, the width W of the groove is 20 to 300 μm, the depth D of the groove is 10 to 40 μm, the interval P of the groove in the rolling direction is 1.0 to 30 mm, the thickness of the glass film at the flat portion (the portion other than the groove) of the base steel sheet is set to t1, the thickness of the glass film at the deepest portion of the groove in the concave portion of the groove is set to t2, and the thickness of the glass film at the side portion of the groove is set to t3, the relationship of formula (1) is satisfied.
[0024] (t2+t3) / 2≥t1 Formula (1)
[0025] It is preferable that the relationship of formula (2) is further satisfied.
[0026] t1<t2 Formula (2) [2]
[0028] A method for manufacturing a directional electromagnetic steel sheet according to one embodiment of the present invention is a method for manufacturing a directional electromagnetic steel sheet, characterized in that it is a method for manufacturing the directional electromagnetic steel sheet described in [1] above, the manufacturing method comprising a groove forming step of irradiating a surface of a cold-rolled steel sheet with a laser to form a groove and an annealing step following the groove forming step, wherein as irradiation conditions of the laser in the groove forming step, a focal point diameter dL of the laser in the rolling direction and a focal point diameter dC in the plate width direction satisfy equation (3), and an oxygen potential (PH2O / PH2) in the annealing step is greater than 0.20 and less than 0.85.
[0029] 0.010≤dL / dC≤1.000 Formula (3)
[0030] Effects of the Invention
[0031] According to the present invention, the magnetic domain subdivision effect can be fully exerted, and a grain-oriented electrical steel sheet with good iron loss can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a schematic diagram showing an example of an electromagnetic steel sheet having grooves formed on the surface.
[0033] Figure 2 This is a diagram showing the relationship between an example of a cross section of a base steel plate including a groove and the film thickness.
[0034] Figure 3 This is a diagram showing an example of a cross-sectional photograph of a base steel plate including a groove. DETAILED DESCRIPTION
[0035] The inventors of the present invention have repeatedly conducted research to maximize the effect of magnetic domain segmentation, and found that the magnetic domain segmentation effect can be maximized by controlling the thickness of the glass film on the surface of the groove recess. The structure of the grain-oriented electromagnetic steel sheet (hereinafter referred to as the present electromagnetic steel sheet) according to the embodiment of the present invention is described below.
[0036] The electromagnetic steel sheet includes a base steel sheet having a plurality of grooves arranged in parallel on the surface thereof and a glass coating film formed on the surface of the base steel sheet (see Figure 1 to Figure 3 In the present electromagnetic steel sheet, a tension film (insulating film) may be formed on the surface of the glass film. Figure 1 As shown in , a plurality of grooves are formed on the surface of the base steel plate in parallel so as to be adjacent to each other in the rolling direction of the base steel plate. The direction (angle θ), the width W, the depth D, and the interval P of the grooves are determined in consideration of the iron loss in the same manner as in the conventional grain-oriented electromagnetic steel sheet.
[0037] <Angle θ between the rolling direction of the base steel plate and the length direction of the groove>
[0038] If the angle θ formed by the direction (plate width direction) orthogonal to the rolling direction and plate thickness direction of the parent steel plate and the length direction of the groove is too large, there will be no magnetic domain control effect, and the iron loss improvement effect cannot be obtained, so it is set to 40° or less. The angle θ is preferably smaller and can be set to less than 35°, less than 30°, less than 25°, less than 20°, less than 15°, less than 10°, less than 8°, less than 6°, or less than 5°. The lower limit of the angle θ is 0°, that is, when the length direction of the groove is parallel to the plate width direction. It should be noted that the direction of the angle θ is not limited, and refers to the angle on the acute angle side of the angle formed by the length direction of the groove and the plate width direction. A plurality of grooves are arranged roughly in parallel on the surface of the parent steel plate, but as long as the angle θ of each groove is in the above-mentioned range.
[0039] <Slot width W>
[0040] The groove width W refers to the width of the groove on the surface of the parent steel plate in the cross section (groove cross section) of the groove in the plane perpendicular to the length direction of the groove. Even if the groove width W is less than 20μm and too narrow, it will not become the starting point for the generation of magnetic poles, there is no magnetic domain control effect, and good iron loss cannot be obtained. On the other hand, if it exceeds 300μm and is too wide, it will not become the starting point for the generation of magnetic poles, there is no magnetic domain control effect, only the magnetic flux density is significantly reduced, and good iron loss cannot be obtained. Therefore, the groove width W can be set to more than 20μm and less than 300μm. The lower limit of the groove width W can preferably be set to 25μm, 30μm, or 35μm. The upper limit of the groove width W can preferably be set to 250μm, 200μm, 150μm, 100μm, or 80μm.
[0041] <Groove Depth D>
[0042] When the groove depth D is less than 10μm and too shallow, it will not become the starting point of the magnetic pole, there is no magnetic domain control effect, and good iron loss cannot be obtained. On the other hand, when it exceeds 40μm and is too deep, the magnetic domain control effect reaches saturation, and only the magnetic flux density is significantly reduced, so good iron loss cannot be obtained. Therefore, the depth D of the groove can be set to more than 10μm and less than 40μm. The lower limit of the groove depth D can be preferably set to 11μm, 12μm, 13μm, 14μm, or 15μm. The upper limit of the groove depth D can be preferably set to 38μm, 36μm, 34μm, 32μm, 30μm, 28μm, or 26μm.
[0043] <Slot spacing P>
[0044] The groove spacing P is the spacing between the center lines of adjacent grooves arranged approximately parallel to each other on the surface of the base steel plate in the longitudinal direction, and refers to the distance in the rolling direction of the base steel plate. The center line of the groove is a line parallel to the longitudinal direction of the groove passing through the midpoint of the groove on the surface of the base steel plate in the groove cross section.
[0045] When the slot spacing P is less than 1mm and too narrow, the magnetic domain control effect is saturated, and only the magnetic flux density is significantly reduced, so good iron loss cannot be obtained. On the other hand, when it exceeds 30mm and is too wide, the magnetic domain control effect cannot be fully obtained, and good iron loss cannot be obtained. Therefore, the slot spacing P can be greater than 1mm and less than 30mm. The slot spacing P may not be equally spaced, but the slot spacing P with adjacent slots may be within the above range. The lower limit of the slot spacing P may preferably be 1.2mm, 1.4mm, 1.5mm, 1.6mm, 1.8mm, or 2.0mm. The upper limit of the slot spacing P may preferably be 25mm, 20mm, 15mm, 10mm, 7mm, or 5mm.
[0046] <Glass film thickness>
[0047] The glass film on the surface of the flat portion (the portion without a groove, i.e., the portion outside the groove, hereinafter sometimes referred to as the "flat portion") and the laser groove (hereinafter sometimes referred to as the "groove") of the base steel sheet surface in the present electromagnetic steel sheet is described. Figure 2 This is a cross-sectional view of a base steel plate including a groove, and is a view obtained by observing a region including the groove from a cross section in the plate thickness direction perpendicular to the longitudinal direction of the groove (groove cross section). Portions connected to both sides of the groove are flat portions.
[0048] The present electromagnetic steel sheet is a directional electromagnetic steel sheet, characterized in that when the glass film thickness of the flat portion is set to t1, the glass film thickness of the bottom portion (deepest portion) of the groove in the recessed portion of the groove is set to t2, and the glass film thickness of the side portion of the groove is set to t3, the relationship of formula (1) is satisfied.
[0049] (t2+t3) / 2≥t1 Formula (1)
[0050] The thickness of the film t1, t2, and t3 of each part is explained. The glass film has an embedded structure. The so-called embedded structure refers to a structure in which the end of the glass film extends into the base steel plate like the root of a plant. Therefore, in the cross section of the steel plate, the end of the embedded structure sometimes appears separated from the glass film. For example, Figure 2 In the figure, the glass film can be confirmed like an isolated island at a location separated from the glass film on the flat portion or the surface of the groove recess, but this is because a cross section of the end portion of the embedded structure is observed. Figure 3 is equivalent to Figure 2 An example of a cross-sectional photograph of a steel plate containing a groove. Figure 3 In the figure, the portion that appears as a black spot in the steel sheet is the end portion of the embedded structure of the glass film. Hereinafter, the end of the glass film includes not only the glass film but also the embedded structure portion of the glass film that appears to be separated from the glass film in the cross section of the steel sheet, and refers to the portion farthest from the surface of the glass film.
[0051] The following is a method for measuring the thickness t1, t2, and t3 of the glass film at each portion using Figure 2 Provide explanation.
[0052] First, the thickness t1 of the glass film on the flat portion is explained. The intersection of the flat portion and the groove (i.e., the edge of the groove) is set as point A and point A'. The straight line passing through point A and point A' is set as L1U. That is, the straight line representing the surface of the glass film at the flat portion of the steel plate surface is set as L1U. Next, the lower end position (deepest position in the plate thickness direction) of the farthest point from the glass film surface (i.e., L1U) at the end of the glass film within 25 μm from point A and point A' in the flat portion is set as point a. Next, a straight line passing through point a and parallel to line L1U is set as L1L, and the distance between these L1U and L1L is set as t1.
[0053] Next, the glass film thickness t2 at the bottom portion (deepest portion) of the groove is described. The deepest portion (deepest portion in the plate thickness direction) of the groove concave surface is set as point B, and the line passing through point B and parallel to L1U is set as L2U. Next, the lower end position of the end of the glass film farthest from L2U in the plate thickness direction is set as point b, and the line passing through point b and parallel to L2U is set as L2L. The distance between these straight lines L2U and L2L is set as t2.
[0054] Finally, the glass film thickness t3 of the side surface of the groove is described. The intersection of the perpendicular bisector of the line segment AB connecting point A at the end of the groove and point B at the deepest part of the groove and the glass film surface on the side surface of the groove is set as point C, and the straight line passing through point A and point C is set as L3U. Next, the end of the glass film on the side surface of the groove that is farthest from the straight line L3U is determined, and the point farthest from the straight line L3U is set as point c. The line passing through point c and parallel to L3U is set as L3L, and the distance between these straight lines L3U and L3L is set as t3.
[0055] Since the glass film thickness on the sides of the groove is Figure 2 The side surface at point A and the side surface at point A' are almost the same, so only one side needs to be measured. Of course, the thickness of the glass film on both sides can also be measured, and their average value is set as the glass film thickness t3 on the groove side.
[0056] The thickness of the glass film can be measured, for example, by observing the cross section with an optical microscope or SEM after mirror polishing. The observation conditions of the optical microscope or SEM can be known conditions, and the field of view or observation magnification can be appropriately adjusted according to the size of the groove and the thickness of the glass film. In SEM observation, secondary electron images can be taken, and reflected electron images can also be taken.
[0057] Here, the effect of the glass film will be described.
[0058] The magnetic domain segmentation in grain-oriented electrical steel sheets is achieved by: the static magnetic energy increases due to the magnetic poles generated on the steel sheet surface, and a new 180° magnetic domain wall is generated to eliminate it, and the magnetic domain width becomes narrower. If the magnetic domain width is narrowed, the movement distance of the magnetic domain wall when the steel sheet is magnetized becomes shorter, the energy loss during the movement of the magnetic domain wall is reduced, and the iron loss is reduced.
[0059] By applying a glass film having a different expansion coefficient from that of the steel sheet at high temperature and baking it, after cooling, tensile tension is applied in the rolling direction due to the difference in expansion coefficients between the steel sheet and the glass film, thereby subdividing the magnetic domains and improving the iron loss.
[0060] Furthermore, since the glass film is made of non-magnetic oxide and has a different magnetic permeability from the steel sheet, magnetic poles are generated at the interface and the magnetic domains are subdivided. Therefore, it is believed that the glass film becomes the starting point for the generation of magnetic poles and reduces iron loss by promoting the subdivision of magnetic domains.
[0061] Although it is difficult to apply tension to the groove in the rolling direction, if the groove is formed at right angles to the rolling direction, magnetic poles are generated on the concave surface of the groove. The synergistic effect with the magnetic poles of the glass film can promote the subdivision of the magnetic domain.
[0062] On the other hand, the glass film is formed of non-magnetic oxides, so the magnetic flux density of the steel sheet is reduced. Therefore, there is a trade-off between iron loss and magnetic flux density. If the glass film is thicker, although the magnetic domain segmentation can be promoted in the groove part, the magnetic flux density on the entire surface of the steel sheet is reduced.
[0063] The present inventors found that making the glass film thickness on the concave surface of the groove relatively thick can achieve the magnetic domain segmentation effect in the groove, while making the glass film thickness on the flat portion relatively thin can suppress the reduction in the magnetic flux density of the entire steel sheet.
[0064] That is, as shown in the formula (1), the thickness of the glass film in the concave portion of the groove only needs to be thicker than the thickness of the glass film in the flat portion.
[0065] (t2+t3) / 2≥t1 Formula (1)
[0066] t1: Thickness of glass film on flat part
[0067] t2: The thickness of the glass film at the bottom (deepest part) of the groove in the concave part of the groove
[0068] t3: Glass film thickness on the side of the groove
[0069] Preferably, the ratio of the thickness of the glass film at the concave portion of the groove [(t2+t3) / 2] to the thickness of the glass film at the flat portion [t1], i.e., the film thickness ratio [film thickness ratio = {(t2+t3) / 2} / t1] can be set to 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, 1.6 or more, 1.7 or more, 1.8 or more, 1.9 or more, or 2.0 or more. The upper limit of the film thickness ratio [film thickness ratio = {(t2+t3) / 2} / t1] is not particularly limited, but in consideration of actual operation, the film thickness ratio can be set to 5.0 or less, 4.0 or less, or 3.0 or less.
[0070] It is further preferred that the glass film thickness t1 of the flat portion is thinner than the glass film thickness t2 of the bottom portion (deepest portion) of the groove (Formula (2)). By making the glass film of the bottom portion of the groove thicker than the flat portion, the decrease in the magnetic flux density of the entire steel plate can be suppressed, and the generation of magnetic poles using the groove and the glass film can be promoted, which can further improve the magnetic properties.
[0071] t1<t2 Formula (2)
[0072] <Manufacturing method>
[0073] First, a cold-rolled steel sheet for the present electromagnetic steel sheet is manufactured by a known method. The steel sheet composition and the method for manufacturing the cold-rolled steel sheet are not particularly limited, and a known method, for example, the steel sheet composition and the method for manufacturing the steel sheet described in Patent Document 5 can be used.
[0074] However, the groove forming step by laser irradiation is preferably set after cold rolling and before the decarburization annealing step. The shape of the groove formed by laser irradiation is decarburized and finished without cold rolling, so the controllability of the groove shape is improved.
[0075] <Laser irradiation conditions>
[0076] The groove forming process is described. By irradiating the cold-rolled steel sheet with laser, a plurality of grooves are formed on the surface of the steel sheet in a direction intersecting the rolling direction in such a manner that the groove width W, the groove depth D, and the prescribed interval (groove interval P) are within a prescribed range. The laser irradiation conditions are not particularly limited to the type of laser light source, the laser output power, the laser scanning speed, and the steel sheet moving speed during laser irradiation, but the conditions that the groove width W, the groove depth D, and the prescribed interval (groove interval P) of the grooves are within the prescribed range can be appropriately selected.
[0077] [Laser light source]
[0078] As the laser light source, for example, a high-output laser generally used in industry, such as a fiber laser, a YAG laser, a semiconductor laser, or a CO2 laser, can be used. As long as the groove can be formed stably, it can be a pulse laser or a continuous wave laser.
[0079] [Laser output power]
[0080] When the laser output power is lower than 200W, the laser scanning speed is significantly reduced in order to form the desired groove, and the industrial productivity is reduced, so it can be set to 200W or more. It can be preferably 1000W or more, and more preferably 1500W or more. In addition, when the laser output power exceeds 3000W, the power supply capacity becomes large and the equipment cost becomes huge, which is not realistic in industry, so it can be set to 3000W or less. It can be preferably 2800W or less, and more preferably 2500W or less.
[0081] [Laser scanning speed]
[0082] When the laser scanning speed is lower than 5 m / s, the steel plate passing speed must be slowed down, and the productivity is reduced, so it is set to 5 m / s or more. It can be preferably 20 m / s or more, and more preferably 40 m / s or more. In addition, when the laser scanning speed is higher than 100 m / s, a high output power is required, and the equipment cost increases, so it can be set to 100 m / s or less. It can be preferably 80 m / s or less, and more preferably 60 m / s or less.
[0083] [Laser spot shape]
[0084] The shape of the laser light spot can be circular or slightly widened in the plate width direction on the surface of the base steel plate. In order to avoid excessive widening, for example, the laser light spot diameter in the rolling direction: dL, the laser light spot diameter in the plate width direction: dC can satisfy equation (3). For example, the laser light spot diameter dL in the plate width direction can be set to 5 to 100 μm, the light spot diameter dC in the plate width direction can be set to 5 to 100 μm, the laser output power can be set to 200 to 3000 W, and the laser scanning speed V can be set to 5 to 100 m / s.
[0085] 0.010≤dL / dC≤1.000 Formula (3)
[0086] This is because, when dL / dC is larger than 1, the laser spot diameter becomes an elongated ellipse in the rolling direction, making it difficult to control the laser groove shape.
[0087] When dL / dC is less than 0.010, the laser spot diameter becomes an extremely elongated ellipse in the plate width direction, and in this case, it becomes difficult to control the laser groove shape.
[0088] The present inventors have repeatedly conducted experiments and found that the thickness of the molten layer in the laser irradiated portion can be controlled by the above laser irradiation conditions, and that the present electromagnetic steel sheet with the controlled glass film thickness as described above can be obtained by forming an internal oxide layer in the subsequent recrystallization annealing.
[0089] The mechanism by which the laser irradiation conditions contribute to the thickness control of the glass film in the groove recessed portion is considered to be as follows.
[0090] First, the glass film is an oxide formed by Mg2SiO4, which is formed by the reaction of the internal oxide layer SiO2 generated in the decarburization annealing and the annealing separator MgO coated on the surface of the steel sheet before the final annealing during the high temperature annealing of 1200°C in the final annealing process.
[0091] At this time, a glass film is also formed according to the thickness of the internal oxide layer. For example, the thickness of the internal oxide layer can be adjusted by increasing the dew point of the decarburization annealing.
[0092] By irradiating the cold-rolled steel sheet with laser, the laser-irradiated portion of the cold-rolled steel sheet (base steel sheet) melts to form grooves, and crystals grow in an oriented manner on the surface portions of the grooves, thereby generating columnar crystals.
[0093] It is confirmed that when the shape of the focal point is a moderate elliptical shape in the width direction of the steel plate as in the present invention, if dL / dC becomes smaller, the thickness of the molten layer on the surface of the groove concave portion becomes moderately thick. It is believed that if the laser spot shape is set to a moderately long elliptical shape in the width direction of the plate, when the laser is continuously irradiated at an angle of less than 40° relative to the width direction of the plate, the heat generated by the laser irradiation becomes easy to conduct in the groove forming direction, and the controllability of the columnar crystals formed on the surface of the groove concave portion is improved. Therefore, when dL and dC are within the above range, the heat input to the steel plate becomes larger, the molten layer is formed moderately thick, and therefore the columnar crystals are generated moderately thick. It is believed that in the subsequent decarburization annealing, the grown columnar crystals become the diffusion path of oxygen, the internal oxide layer is developed, and the glass film also becomes thicker in the finished annealing.
[0094] Therefore, it is preferred to satisfy the relationship of formula (3). The lower limit of dL / dC is set to 0.010, but it can be preferably 0.015, 0.020, 0.025, 0.030, 0.035, 0.040, 0.045, or 0.050. The upper limit of dL / dC is 1.000 (circular spot), but as long as the laser spot shape is formed, it can be set to an ellipse that is long in the plate width direction, and it can be preferably set to 0.980, 0.960, 0.940, 0.920, 0.900, 0.880, 0.860, 0.840, 0.820, 0.800, 0.780, 0.760, 0.740, 0.720, or 0.700.
[0095] On the other hand, in the flat portion, since there is no laser irradiation, no molten layer is generated, and therefore the internal oxide layer is not developed as in the groove portion, and as a result, the glass film is not generated as thickly as in the groove portion.
[0096] The focal spot diameter is not particularly limited as long as dL and dC satisfy the prescribed relationship, but the focal spot diameter is preferably smaller from the viewpoint of making the remaining recrystallized grains fine. The focal spot diameter can be selected based on the relationship with other properties of the electromagnetic steel sheet, and in practice, the upper limit of dC can be set to 300 μm, preferably 250 μm, 200 μm, 150 μm, or 100 μm.
[0097] <Assist gas>
[0098] It is also possible to blow auxiliary gas to the portion of the steel plate irradiated with the laser while irradiating the laser. The auxiliary gas plays the role of removing the components melted or evaporated from the steel plate by laser irradiation. By blowing the auxiliary gas, the laser stably reaches the steel plate, so that the groove is stably formed. The flow rate of the auxiliary gas is preferably set to 10 to 1000 liters per minute, for example.
[0099] Furthermore, the assist gas is preferably air or an inert gas.
[0100] <Steps after Groove Formation>
[0101] After the grooves are formed in the cold-rolled steel sheet in the groove forming step, the cold-rolled steel sheet is annealed (decarburization annealing), nitrided by a known method, and then coated with an annealing separator mainly composed of MgO, heated, maintained, and then cooled to form a glass film.
[0102] The decarburization conditions may be known conditions, but in order to further reduce the iron loss, it is effective to more precisely control the glass film formation behavior. For example, the decarburization annealing conditions are to heat the steel plate with grooves to 800-880°C, set the annealing atmosphere to a hydrogen-inert gas atmosphere, set the oxygen potential (PH2O / PH2) to 0.20-0.85, keep it for more than 60 seconds and then cool it. If the oxygen potential (PH2O / PH2) is lower than 0.20, decarburization cannot be fully performed, and the magnetic properties of the final product deteriorate. In addition, the supply of oxygen is insufficient, and the internal oxide layer is basically not generated. As a result, the glass film is basically not obtained, and the magnetic properties are significantly deteriorated. On the other hand, when the oxygen potential (PH2O / PH2) is greater than 0.85, the supply of oxygen becomes excessive, and not only the groove concave portion of the molten layer that becomes the diffusion path, but also the internal oxide layer is thickly formed on the flat portion. As a result, a thick glass film is formed outside the groove concave portion, and the iron loss is deteriorated due to the reduction in magnetic flux density. The glass film is a non-magnetic layer, and if it is formed too thickly, it will cause a decrease in magnetic flux density.
[0103] Furthermore, by also controlling the heating process conditions of the decarburization annealing, the internal oxidation of the groove recess is promoted in the subsequent decarburization annealing process, and a thick glass film can be generated in the subsequent finished annealing process. For example, the residence time of 200-700°C in the heating process of the decarburization annealing can be preferably set to less than 50 seconds. If the residence time is less than 50 seconds, internal oxidation can be promoted in the subsequent decarburization annealing soaking process, so it is preferred. In addition, the oxygen potential (PH2O / PH2) in the heating process of the decarburization annealing can also be preferably less than 0.85, and more preferably less than 0.60. If it is less than 0.85, internal oxidation becomes easy to promote in the subsequent decarburization annealing soaking process, so it is preferred.
[0104] The nitridation can be performed by a known method, and the nitridation amount can be set to, for example, a range of 50 to 400 ppm, and good characteristics can be obtained particularly when it is within a range of 180 to 250 ppm.
[0105] The glass film is formed by a process of coiling a steel sheet coated with an annealing separator into a coil, keeping it at a temperature of 1150 to 1250° C. for 10 to 30 hours, and then cooling it. The composition of the annealing separator can be a known composition, for example, it can be set to 100 parts by mass of MgO, 5 parts by mass of TiO2, and a composition in which FeCl2 is added as an additive in a manner of 200 ppm in terms of chlorine.
[0106] In order to further reduce the iron loss, the water release rate from the annealing separator during the finish annealing (room temperature to 700°C) may preferably be 0.5% or more and 6.0% or less. If the water release rate is 0.5% or more and 6.0% or less, the aggregation of the internal oxide layer to the surface side of the steel sheet can be suppressed during the temperature rise process of the finish annealing, and the formation of fine particles in the glass film can be promoted.
[0107] Tension can be applied to the steel sheet only by the glass coating, but a tension coating (insulating coating) may be formed on the glass coating to enhance the magnetic domain control effect. The tension coating may be composed mainly of aluminum phosphate, for example, and may have a thickness of about 1 μm.
[0108] Example
[0109] Next, examples of the present invention will be described. The examples are one embodiment of the present invention, and the present invention is not limited to this embodiment.
[0110] <Example 1>
[0111] A slab containing Si: 3.3 mass %, Mn: 0.10 mass %, S: 0.006 mass %, C: 0.060 mass %, acid-soluble Al: 0.027 mass %, N: 0.008 mass %, with the remainder consisting of Fe and impurities is used as a raw material, hot rolled by a known method, then annealed, and cold rolled to obtain a steel plate with a final plate thickness of 0.22 mm.
[0112] Next, the surface of the steel sheet is irradiated with laser light to form a plurality of grooves extending in a direction intersecting the rolling direction along the rolling direction. The groove forming direction is set to a direction inclined 0° to 50° along the rolling direction relative to the width direction of the steel sheet, the groove width is set to 3 to 320 μm, the groove depth is set to 5 to 50 μm, and the groove interval is set to 0.9 to 32 mm.
[0113] Regarding the laser irradiation conditions, the laser output power was set to 2000 W, the laser scanning speed was set to 45 m / s, and the focal spot diameter ratio of the laser in the rolling direction was set to 0.25 and 1.50.
[0114] During the laser irradiation, air was blown at 100 liters / minute as an assist gas in order to effectively remove the metal of the steel plate melted and evaporated by the laser.
[0115] The cold-rolled steel sheet with grooves is decarburized and further nitrided. The decarburization annealing conditions are set to heat up to 850°C, hold for 60 seconds and then cool. The decarburization annealing atmosphere is a hydrogen-nitrogen atmosphere, and the oxygen potential (PH2O / PH2) is set to 0.30-0.50. In addition, the nitriding amount is set to 200 ppm.
[0116] After that, the coating amount was adjusted to 4 g / m 2 An annealing separator mainly composed of MgO was applied in the following manner. The composition of the annealing separator was 100 parts by mass of MgO and 5 parts by mass of TiO2, and FeCl2 was added so as to be 200 ppm in terms of chlorine.
[0117] Next, the steel sheet coated with the annealing separator was coiled into a coil, kept at 1200°C for 20 hours, and then cooled to form a glass film on the surface. Furthermore, a tension film containing aluminum phosphate as a main component was formed to a thickness of 1 μm to obtain a grain-oriented electrical steel sheet. The tension at this time was 12 MPa with respect to the rolling direction including the glass film.
[0118] After the tensile insulation coating was applied, the iron loss W17 / 50 (energy loss measured under the excitation conditions of 1.7 T and 50 Hz) and the magnetic flux density B8 (magnetic flux density at a magnetizing force of 800 A / m) were measured. The results are shown in Table 1.
[0119] In No.A1 to A11 and a1 to a16, the magnetic flux density is similar. However, in No.A1 to A11, the iron loss is less than 0.750 W / kg, which is good, while in No.a1 to a16, the iron loss is more than 0.750 W / kg, which is poor, because the relationship between the groove shape and the glass film thickness is outside the range of the above-mentioned prescribed value.
[0120] <Example 2>
[0121] A slab containing Si: 3.3 mass %, Mn: 0.10 mass %, S: 0.006 mass %, C: 0.060 mass %, acid-soluble Al: 0.027 mass %, N: 0.008 mass %, with the remainder consisting of Fe and impurities is used as a raw material, hot rolled by a known method, then annealed, and cold rolled to obtain a steel plate with a final plate thickness of 0.22 mm.
[0122] Next, the surface of the steel sheet was irradiated with laser light to form a plurality of grooves extending in a direction intersecting the rolling direction at intervals of 3 mm along the rolling direction. The groove forming direction was set to a direction inclined 10° along the rolling direction relative to the width direction of the steel sheet, the groove width was set to 30 μm, and the groove depth was set to 25 μm.
[0123] Regarding the laser irradiation conditions, the laser output power was set to 1800 to 2000 W, the laser scanning speed was set to 40 to 60 m / s, and the laser focal spot diameter ratio in the rolling direction was controlled within the range of 0.03 to 27.
[0124] During laser irradiation, air was blown at 100 liters / minute as an assist gas in order to effectively remove the metal of the steel plate melted and evaporated by the laser.
[0125] The grooved cold-rolled steel sheet was decarburized and further subjected to nitriding treatment. The decarburization annealing conditions were set to heat up to 850°C, hold for 60 seconds, and then cool. The decarburization annealing atmosphere was a hydrogen-nitrogen atmosphere, and the oxygen potential (PH2O / PH2) was set to 0.12 to 1.10. In addition, the nitriding amount was set to 200 ppm.
[0126] After that, the coating amount is 4g / m per side. 2 An annealing separator mainly composed of MgO was applied in the following manner. The composition of the annealing separator was 100 parts by mass of MgO and 5 parts by mass of TiO2, and FeCl2 was added so as to be 200 ppm in terms of chlorine.
[0127] Next, the steel sheet coated with the annealing separator was coiled into a coil, kept at 1200°C for 20 hours, and then cooled to form a glass film on the surface. Furthermore, a tension film containing aluminum phosphate as a main component was formed to a thickness of 1 μm to obtain a grain-oriented electrical steel sheet. The tension at this time was 12 MPa with respect to the rolling direction including the glass film.
[0128] The iron loss W17 / 50 (energy loss measured under the excitation conditions of 1.7 T and 50 Hz) and the magnetic flux density B8 after the tensile insulation coating was applied were measured. The results are shown in Table 2.
[0129] In No.B1~B12 and b1~b4, the magnetic flux density is the same. However, for No.B1~B12, the relationship of the glass film thickness meets the above-mentioned requirements, the iron loss is less than 0.750W / kg and is good. On the other hand, for No.b1~b4, the relationship of the glass film thickness is outside the above-mentioned range, and the iron loss is more than 0.750W / kg and is poor. In addition, the relationship of the glass film thickness of b5 and b6 is outside the above-mentioned range, and the iron loss is significantly poor due to poor decarburization. Furthermore, the relationship of the glass film thickness of b7 and b8 is also outside the above-mentioned range, and the magnetic flux density is low, resulting in significantly poor iron loss.
[0130] Table 1
[0131]
[0132] Table 2
[0133]
[0134] Industrial Applicability
[0135] The present invention can be used for industrial equipment using a grain-oriented electromagnetic steel sheet, such as a winding core for a transformer.
[0136] Explanation of symbols
[0137] 1. Base steel plate
[0138] 2 slots
[0139] 3. Base steel plate
[0140] 4Glass coating
[0141] 5. Base steel plate
[0142] 6Glass coating
[0143] θ is the angle between the direction perpendicular to the rolling direction of the base steel plate (plate width direction) and the length direction of the groove.
[0144] Width of W groove
[0145] Depth of D groove
[0146] P slot spacing
[0147] t1 Glass film thickness on the flat part of the base steel plate
[0148] Glass film thickness at the deepest part of t2 groove
[0149] Glass film thickness on the side of t3 groove
Claims
1. A directional electromagnetic steel sheet, It is characterized in that The invention is a grain-oriented electromagnetic steel sheet including a base steel sheet having a plurality of grooves on a surface of the steel sheet and a glass film formed on the surface of the base steel sheet, wherein: The angle θ formed by the direction perpendicular to the rolling direction and the plate thickness direction of the base steel plate and the length direction of the groove is 0 to 40°, the width W of the groove is 20 to 300 μm, the depth D of the groove is 10 to 40 μm, and the interval P of the groove in the rolling direction is 1.0 to 30.0 mm. When the thickness of the glass film at the flat portion of the surface of the base steel plate is set to t1, the thickness of the glass film at the deepest portion of the groove in the concave portion of the groove is set to t2, and the thickness of the glass film at the side portion of the groove is set to t3, the relationship of formula (1) is satisfied. (t2+t3) / 2≥t1 formula (1).
2. A method for manufacturing a directional electromagnetic steel sheet, It is characterized in that The method is a method for manufacturing the grain-oriented electrical steel sheet according to claim 1. The manufacturing method comprises a groove forming step of irradiating a surface of a steel plate with laser light to form a groove and an annealing step following the groove forming step. As the irradiation conditions of the laser light in the groove forming step, the focal point diameter dL of the laser light in the rolling direction and the focal point diameter dC of the laser light in the plate width direction satisfy the formula (3). The oxygen potential (PH) in the annealing step is 2 O / PH 2 ) is 0.20 or more and 0.85 or less, 0.010≤dL / dC≤1.000Formula (3).