Solid state battery

By using printable lithium compositions in lithium-ion batteries for lithiation or prelithiation, the problems of lithium metal tree crystal formation and irreversible capacity loss are solved, the energy density and safety of the battery are improved, and more efficient electricity is achieved Chemical properties.

CN118970043APending Publication Date: 2024-11-15LIVENT USA CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411005068.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-03-20
Filing Date
2019-03-21
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the circulation process, existing lithium-ion batteries have safety hazards and irreversible capacity loss problems caused by lithium metal tree crystals, which affect their energy density and safety.

Method used

Using a printable lithium composition, including lithium metal powder, polymer binder and rheology modifier, lithiation or prelithiation is applied to the current collector, electrode or solid electrolyte of the battery by printing technology to form stable lithium Metal layer, improving battery energy density and safety.

Benefits of technology

The energy density and safety improvement of lithium-ion batteries have been achieved, the irreversible consumption of lithium is reduced, and the circulation performance and manufacturing properties of the batteries have been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970043A_ABST
    Figure CN118970043A_ABST
Patent Text Reader

Abstract

The present application provides a solid state battery comprising a positive electrode, a negative electrode, and a solid electrolyte. In one embodiment, the positive electrode, the negative electrode, and / or the solid electrolyte are formed from a printable lithium composition, wherein the printable lithium composition comprises a lithium metal powder, a polymeric binder compatible with the lithium metal powder, a rheology modifier compatible with the lithium metal powder, and a solvent compatible with the lithium metal powder and with the polymeric binder. In another embodiment, lithium is deposited on the solid electrolyte using a lithium printable lithium composition, wherein the lithium printable lithium composition comprises a lithium metal powder, a polymeric binder compatible with the lithium metal powder, a rheology modifier compatible with the lithium metal powder, and a solvent compatible with the lithium metal powder and with the polymeric binder.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the invention patent application with application number 201980030085.9 and the application date of March 21, 2019, entitled “Solid State Battery”.

[0002] Related applications

[0003] The following application claims priority to U.S. Non-Provisional No. 16 / 359,707 filed on March 20, 2019, U.S. Non-Provisional No. 16 / 359,725 filed on March 20, 2019, U.S. Non-Provisional No. 16 / 359,733 filed on March 20, 2019, U.S. Provisional 62 / 646,521 filed on March 22, 2018, and U.S. Provisional 62 / 691,819 filed on June 29, 2018, the disclosures of which are hereby incorporated by reference in their entireties. Technical Field

[0004] The present invention relates to solid-state batteries comprising printable lithium compositions. Background Art

[0005] Lithium and lithium-ion secondary or rechargeable batteries have been used in certain applications, such as in cell phones, camcorders and laptop computers, and even more recently in higher power applications, such as in electric and hybrid electric vehicles. In these applications, it is preferred that the secondary battery have as high a specific capacity as possible, but still provide safe operating conditions and good cyclability, thereby maintaining the high specific capacity during subsequent charge and discharge cycles.

[0006] Although there are many configurations of secondary batteries, each configuration includes a positive electrode (or cathode), a negative electrode (or anode), a separator separating the positive electrode and the negative electrode, and an electrolyte that is electrochemically connected to the positive electrode and the negative electrode. For a secondary lithium battery, when the secondary battery is discharged, that is, when used for its specific application, lithium ions are transferred from the negative electrode to the positive electrode through the electrolyte. During the discharge process, electrons are collected from the negative electrode and transferred to the positive electrode through an external circuit. When the secondary battery is charged or recharged, lithium ions are transferred from the positive electrode to the negative electrode through the electrolyte.

[0007] Historically, secondary lithium batteries have been produced using non-lithiated compounds with high specific capacity as positive electrode active materials, such as TiS2, MoS2, MnO2, and V2O5. These positive electrode active materials are coupled with a lithium metal negative electrode. When the secondary battery is discharged, lithium ions are transferred from the lithium metal negative electrode to the positive electrode through the electrolyte. Unfortunately, during cycling, lithium metal forms dendrites, which eventually lead to unsafe conditions in the battery. As a result, the production of such secondary batteries was stopped in the early 1990s and switched to lithium-ion batteries.

[0008] Lithium-ion batteries generally use lithium metal oxides, such as LiCoO2 and LiNiO2, as positive electrode active materials, coupled with active negative electrode materials, such as carbon-based materials. Other negative electrode types based on silicon oxide, silicon particles, etc. are recognized. In batteries using carbon-based negative electrode systems, the formation of lithium dendrites on the negative electrode is essentially avoided, making the battery safer. However, the lithium, whose amount determines the battery capacity, is completely supplied by the positive electrode. This limits the choice of positive electrode active materials because the active materials must contain removable lithium. In addition, the Li-ion battery formed during charging and overcharging is x CoO2、Li x The corresponding delithiation products of NiO2 are not stable. Specifically, these delithiation products tend to react with the electrolyte and generate heat, which may cause safety hazards.

[0009] A new lithium-ion cell or battery is initially in a discharged state. During the first charge of a lithium-ion battery, lithium moves from the positive electrode material to the negative electrode active material. The lithium that moves from the positive electrode to the negative electrode reacts with the electrolyte material on the surface of the graphite negative electrode to form a passivation film on the negative electrode. The passivation film formed on the graphite negative electrode is a solid electrolyte interface (SEI). In subsequent discharges, the lithium consumed by the formation of the SEI does not return to the positive electrode. This causes the lithium-ion battery to have a smaller capacity compared to the initial charge capacity because some of the lithium has been consumed by the formation of the SEI. The available lithium that is partially consumed in the first cycle reduces the capacity of the lithium-ion battery. This phenomenon is called irreversible capacity and is known to consume about 10% to more than 20% of the capacity of the lithium-ion battery. Therefore, after the initial charge of the lithium-ion battery, the lithium-ion battery loses about 10% to more than 20% of its capacity.

[0010] One solution is to use stabilized lithium metal powder to pre-lithiate the negative electrode. For example, the lithium powder can be stabilized by passivating the metal powder surface with carbon dioxide, such as described in U.S. Patents 5,567,474, 5,776,369 and 5,976,403, the disclosures of which are hereby incorporated by reference in their entirety. CO2-passivated lithium metal powder can only be used for a limited time in air with a low moisture content before the lithium metal content decreases because of the reaction of lithium metal with air. Another solution is to apply a coating such as fluorine, wax, phosphorus or polymer to the lithium metal powder, such as described in U.S. Patents Nos. 7,588,623, 8,021,496, 8,377,236 and U.S. Patent Publication 2017 / 0149052.

[0011] However, there remains a need for solid-state batteries having lithiated or pre-lithiated components to achieve increased energy density as well as improved safety and manufacturability. Summary of the invention

[0012] To this end, the present invention provides a solid-state battery having one or more components pre-lithiated or lithiated with a printable lithium composition. The solid-state battery containing the printable lithium composition has increased energy density and improved safety and manufacturability.

[0013] The printable lithium composition of the present invention comprises lithium metal powder, a polymer binder, and a rheology modifier compatible with the lithium powder and the polymer binder, wherein the polymer binder is compatible with the lithium powder. The printable lithium composition may include a solvent, wherein the solvent is compatible with the lithium powder and compatible with the polymer binder (e.g., capable of forming a suspension or dissolving therein). The solvent may be included as a component during the initial preparation of the printable lithium composition, or added after the preparation of the printable lithium composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 is a schematic diagram of a solid-state battery according to one embodiment of the present invention;

[0015] Figure 2 is a temperature and pressure profile for reactivity testing of a SLMP / styrene butadiene / toluene printable lithium composition; and

[0016] Figure 3 is a graph showing the cycling performance of pouch cells with printable lithium-derived thin lithium film as negative electrode versus commercial thin lithium foil. DETAILED DESCRIPTION

[0017] The foregoing and other aspects of the present invention will now be described in more detail with respect to the description and methods provided herein. It should be understood that the present invention can be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. Moreover, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the present invention to those skilled in the art.

[0018] Here, the terms used in the description of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the description of the embodiments of the present invention in the claims, the singular forms "a", "an", and "the" are also intended to include plural forms unless otherwise explicitly stated. Moreover, as used herein, "and / or" refers to and covers any and all possible combinations of one or more associated listed items.

[0019] As used herein, the term "about" when referring to a measurable value (e.g., amount of a compound, dosage, time, temperature, etc.) is meant to include variations of 20%, 10%, 5%, 1%, 0.5%, or even 0.1% of the specified amount, wherein the measurable value is, for example, a compound, dosage, time, temperature, etc. Unless otherwise defined, all terms, including technical and scientific terms used in the specification, have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.

[0020] As used herein, the terms "comprising", "including", "comprising", "include", "including" and "comprising" specify the presence of stated features, integers, steps, operations, elements and / or components, but do not preclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.

[0021] As used herein, the term "consisting essentially of (and grammatical variations thereof), when applied to the compositions and methods of the present invention, means that the composition / method may contain other components, as long as the other components do not substantially alter the composition / method. The term "substantially alters" as applied to a composition / method means that the effectiveness of the composition / method is increased or decreased by at least about 20% or more.

[0022] All patents, patent applications, and publications cited herein are hereby incorporated by reference in their entirety. In the event of a conflict in terminology, the present specification controls.

[0023] Existing references Figure 1 According to one embodiment of the present invention, a solid-state battery 10 is provided, which includes a negative electrode 12, a positive electrode 14 and a solid electrolyte 16. The solid-state battery may further include a negative electrode collector 20 and a positive electrode collector 22. The printable lithium composition is applied or deposited on the current collector, electrode and / or solid electrolyte of the solid-state battery. For example, the printable lithium composition can be used to form a single lithium metal negative electrode with different thicknesses and widths for a solid-state battery, including solid-state batteries as described in U.S. Patents 8,252,438 and 9,893,379, the disclosures of which are incorporated by reference in their entirety. In another embodiment, the printable lithium composition can be applied or deposited to form a solid electrolyte for a solid-state battery, and includes combining an ink composition with a polymer or ceramic material to form a solid electrolyte. The printable lithium composition comprises lithium metal powder, one or more polymer binders, one or more rheology modifiers, and may further comprise a solvent or a cosolvent.

[0024] The printable lithium composition can be applied to a current collector, electrode or solid electrolyte by different methods, including extrusion, coating, printing, smearing, dipping and spraying. For example, the negative electrode can be lithiated or pre-lithiated by printing the printable lithium composition on the negative electrode or current collector, wherein a thin lithium film with controlled thickness and width can be formed, or the negative electrode can be coated with the printable lithium composition.

[0025] In one embodiment, the printable lithium composition can be used for pre-lithiation solid electrolytes, as described in U.S. Pat. No. 7,914,930, which is incorporated herein by reference in its entirety. An example of a solid-state secondary battery may include a positive electrode capable of electrochemically absorbing and desorbing lithium; and a negative electrode capable of electrochemically absorbing and desorbing lithium, the negative electrode comprising an active material layer containing an active material and a non-aqueous electrolyte, the active material layer being supported on a current collector. The method includes the steps of: reacting lithium with the active material of the negative electrode by contacting the printable lithium composition with the surface of the active material layer of the negative electrode; and then combining the negative electrode with the positive electrode to form an electrode assembly.

[0026] The printable lithium composition comprises lithium metal powder, a polymer binder, a rheology modifier, and may further include a solvent. The polymer binder may be compatible with the lithium metal powder. The rheology modifier may be compatible with the lithium metal powder and the polymer binder. The solvent may be compatible with the lithium metal powder and the polymer binder.

[0027] The lithium metal powder may be in the form of a finely divided powder. The average particle size of the lithium metal powder is generally less than about 80 microns, usually less than about 40 microns, and sometimes less than about 20 microns. The lithium metal powder may be a low pyrophoric stabilized lithium metal powder commercially available from FMC Lithium Corp. The lithium metal powder may also include a substantially continuous layer or coating of fluorine, wax, phosphorus, or polymer, or combinations thereof (as disclosed in US Pat. Nos. 5,567,474, 5,776,369, and 5,976,403). The lithium metal powder has significantly reduced reactivity with moisture and air.

[0028] The lithium metal powder can also be alloyed with metals. For example, the lithium metal powder can be alloyed with elements of I-VIII groups. Suitable elements from IB group can, for example, include copper, silver or gold. Suitable elements from IIB group can, for example, include zinc, cadmium or mercury. Suitable elements from IIA group of the periodic table can include beryllium, magnesium, calcium, strontium, barium and radium. Elements from IIIA group that can be used in the present invention can, for example, include boron, aluminum, gallium, indium or thallium. Elements from IVA group that can be used in the present invention can, for example, include carbon, silicon, germanium, tin or lead. Elements from VA group that can be used in the present invention can, for example, include nitrogen, phosphorus or bismuth. Suitable elements from VIIIB group can, for example, include nickel, palladium or platinum.

[0029] The polymer binder should be selected to be compatible with the lithium metal powder. "Compatible with" or "compatibility" is intended to mean that the polymer binder will not react violently with the lithium metal powder, thereby causing safety hazards. The lithium metal powder and the polymer binder may react to form a lithium-polymer complex, however, the complex should be stable at a variety of temperatures. It is recognized that the amount (concentration) of lithium and polymer binder contributes to stability and reactivity. The polymer binder can have a molecular weight of about 1,000 to about 8,000,000, and typically has a molecular weight of 2,000,000 to 5,000,000. Suitable polymer binders can include one or more of polyethylene oxide, polystyrene, polyisobutylene, natural rubber, butadiene rubber, styrene-butadiene rubber, polyisoprene rubber, butyl rubber, hydrogenated nitrile rubber, epichlorohydrin rubber, acrylate rubber, silicone rubber, nitrile rubber, polyacrylic acid, polyvinylidene chloride, polyvinyl acetate, ethylene-propylene diene trimer, ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-propylene terpolymer, and polybutene. The binder can also be wax.

[0030] The selection of rheology modifiers should make them compatible with lithium metal powder and polymer binder. The rheology modifier provides rheological properties, such as viscosity. Depending on the selection of rheology modifiers, the rheology modifiers can also provide conductivity, improved capacity and / or improved stability / safety. To this end, the rheology modifier can be a composition of two or more compounds to provide different properties or to provide additive properties. Exemplary rheology modifiers can include one or more of carbon black, carbon nanotubes, graphene, silicon nanotubes, graphite, hard carbon and mixtures thereof, fumed silica, titanium dioxide, zirconium dioxide and other IIA, IIIA, IVB, VB and VIA group elements / compounds and mixtures or blends thereof.

[0031] Solvents compatible with lithium can include acyclic hydrocarbons, cyclic hydrocarbons, aromatic hydrocarbons, symmetrical ethers, asymmetrical ethers, cyclic ethers, alkanes, sulfones, mineral oils and mixtures, blends or cosolvents thereof. Examples of suitable acyclic and cyclic hydrocarbons include n-hexane, n-heptane, cyclohexane, etc. Examples of suitable aromatic hydrocarbons include toluene, ethylbenzene, xylene, isopropylbenzene (cumene), etc. Examples of suitable symmetrical, asymmetrical and cyclic ethers include di-n-butyl ether, methyl tert-butyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, etc. Commercially available isoparaffin synthetic hydrocarbon solvents with a specified boiling point range, such as Shell (Shell Chemicals) or (Exxon) is also suitable.

[0032] The polymer binder and solvent are selected so that they are compatible with each other and with the lithium metal powder. Typically, the binder or solvent should not react with the lithium metal powder, or react in an amount to keep any reaction to a minimum and avoid violent reactions. The binder and solvent should be compatible with each other at the temperature of manufacture and application of the printable lithium composition. Preferably, the solvent (or co-solvent) has sufficient volatility to evaporate easily from the printable lithium composition (e.g., in the form of a slurry) to dry the printable lithium composition (slurry) after application.

[0033] The components of the printable lithium composition can be mixed together as a slurry or paste to have a high concentration of solids. Therefore, the slurry / paste can be in the form of a concentrate, and all of the solvent does not have to be added before deposition or application. In one embodiment, the lithium metal powder should be uniformly suspended in the solvent so that when applied or deposited, a substantially uniform distribution of lithium metal powder is deposited or applied. The dried lithium powder can be dispersed, for example, by vigorous stirring or stirring to apply high shear forces.

[0034] In another embodiment, a mixture of polymer binders, rheology modifiers, coating agents, and other potential additives for lithium metal powders can be formed and added to contact the lithium droplets during the dispersion process at a temperature above the melting point of lithium, or at a lower temperature after the lithium dispersion has cooled, such as described in U.S. Patent 7,588,623, the disclosure of which is incorporated by reference in its entirety. The lithium metal so modified can be added in crystalline form or in the form of a solution in a selected solvent. It should be understood that a combination of different process parameters can be used to achieve specific coating and lithium powder properties for a specific application.

[0035] Conventional pre-lithiation surface treatments require compositions with very low binder content and very high lithium; see, e.g., U.S. Patent 9,649,688, the disclosure of which is incorporated by reference in its entirety. However, embodiments of the printable lithium compositions of the present invention can accommodate higher binder ratios, including up to 20% on a dry basis. Various properties of the printable lithium composition, such as viscosity and fluidity, can be altered by increasing the binder and modifier content up to 50% on a dry basis without losing the electrochemical activity of the lithium. The increase in binder content facilitates the loading and flow of the printable lithium composition during printing. For example, in one embodiment, the printable lithium composition comprises approximately 70% lithium metal powder and approximately 30% polymer binder and rheology modifier. In another embodiment, the printable lithium composition may comprise approximately 85% lithium metal powder and approximately 15% polymer binder and rheology modifier.

[0036] An important aspect of the printable lithium composition is the rheological stability of the suspension. Since lithium metal has a low density of 0.534 g / cc, it is difficult to prevent the lithium powder from separating from the solvent suspension. By selecting the loading of lithium metal powder, the type and amount of polymer binder and conventional modifier, the viscosity and rheology can be adjusted to produce a stable suspension of the present invention. A preferred embodiment shows no separation for greater than 90 days. This can be achieved by designing a 1×10 4 cps to 1×10 7 However, it is very important for the present application method that the composition exhibits viscosity characteristics within the required range when subjected to shear.

[0037] The resulting printable lithium composition is preferably prepared within 10 s -1 The viscosity at this viscosity is about 20 to about 20,000 cps, and typically about 100 to about 10,000 cps. At this viscosity, the printable lithium composition is a flowable suspension or gel. The printable lithium composition preferably has an extended shelf life at room temperature and is stable to loss of metallic lithium at temperatures up to 60°C, often up to 120°C, and sometimes up to 180°C. The printable lithium composition will separate somewhat over time, but can be put back into suspension by gentle stirring and / or heating.

[0038] In one embodiment, the printable lithium composition comprises about 5 to 50% lithium metal powder, about 0.1 to 20% polymer binder, about 0.1 to 30% rheology modifier and about 50 to 95% solvent based on solution. In one embodiment, the printable lithium composition comprises about 15 to 25% lithium metal powder, about 0.3 to 0.6% polymer binder with a molecular weight of 4,700,000, about 0.5 to 0.9% rheology modifier and about 75 to 85% solvent based on solution. Generally speaking, the printable lithium composition is applied or deposited to a thickness of about 50 microns to 200 microns before pressing. After pressing, the thickness can be reduced to about 1 to 50 microns. Examples of pressing techniques are described, for example, in U.S. Patents 3,721,113 and 6,232,014, which are incorporated herein by reference in their entirety.

[0039] In one embodiment, the printable lithium composition is deposited or applied to an active negative electrode material on a current collector, i.e., a pre-lithiated negative electrode is formed. Suitable active negative electrode materials include graphite and other carbon-based materials, alloys, such as tin / cobalt, tin / cobalt / carbon, silicon-carbon, a variety of silicone / tin-based composite compounds, germanium-based composite materials, titanium-based composite materials, elemental silicon and germanium. The negative electrode material can be a foil, a mesh or a foam. It can be applied via spraying, extrusion, coating, printing, brushing, dipping and spraying.

[0040] In one embodiment, the active negative electrode material and the printable lithium composition are provided together and extruded onto a current collector (e.g., copper, nickel, etc.). For example, the active negative electrode material and the printable lithium composition can be mixed and coextruded together. Examples of the active negative electrode material include graphite, graphite-SiO, graphite-SnO, SiO, hard carbon and other lithium ion battery and lithium ion capacitor negative electrode materials. In another embodiment, the active negative electrode material and the printable lithium composition are coextruded to form a printable lithium composition layer on the current collector. The deposition of the printable lithium composition including the above-mentioned extrusion technology can include deposition into various patterns (e.g., dots, stripes), thickness, width, etc. For example, the printable lithium composition and the active negative electrode material can be deposited as a series of stripes, such as described in U.S. Publication 2014 / 0186519, which is hereby incorporated by reference in its entirety. The stripes will form a 3D structure, which is the reason for the expansion of the active negative electrode material during lithiation. For example, silicon may expand by 300% to 400% during lithiation. This expansion has a potential adverse effect on the negative electrode and its performance. By depositing the printable lithium as a thin ribbon in the Y plane as an alternating pattern between the silicon anode stripes, the silicon anode material can expand in the X plane, thereby alleviating electrochemical grinding and loss of electrical contact between particles. Therefore, the printing method can provide a buffer for expansion. In another example, when the printable lithium formulation is used to form the anode, it can be co-extruded in layers with the cathode and separator to obtain a solid-state battery.

[0041] In one embodiment, the printable lithium composition can be used to pre-negatively polarize the negative electrode, as described in U.S. Pat. No. 9,837,659, which is incorporated herein by reference in its entirety. For example, the method includes providing a printable lithium composition layer near the surface of a prefabricated / preformed negative electrode. The prefabricated electrode includes an electroactive material. In certain variations, the printable lithium composition can be applied to a carrier / substrate by a deposition method. The carrier substrate on which the printable lithium composition layer can be provided can be selected from: polymer films (e.g., polystyrene, polyethylene, polyethylene oxide, polyester, polypropylene, polytetrafluoroethylene), ceramic films, copper foil, nickel foil, or metal foam as non-limiting examples. Heat can then be applied to the printable lithium composition layer on the substrate or prefabricated negative electrode. Under applied pressure, the printable lithium composition layer on the substrate or prefabricated negative electrode can be further pressed together. Heating and optionally applying pressure help transfer lithium to the surface of the substrate or negative electrode. In the case of transfer to the prefabricated negative electrode, pressure and heat can cause mechanical lithiation, particularly when the prefabricated negative electrode contains graphite. In this way, lithium is transferred to the electrode and, due to favorable thermodynamics, is incorporated into the active material.

[0042] In additional embodiments, at least a portion of the printable lithium composition may be supplied to the negative electrode active material prior to assembling the battery. In other words, the negative electrode may include a partially lithium-loaded silicon-based active material, wherein the partially loaded active material has a selected level of lithium loading by intercalation / alloying, etc.

[0043] In one embodiment, the printable lithium composition can be incorporated into a three-dimensional electrode structure, as described in U.S. Publication No. 2018 / 0013126, which is incorporated herein by reference in its entirety. For example, the printable lithium composition can be incorporated into a three-dimensional porous negative electrode, a porous current collector, or a porous polymer or ceramic membrane, wherein the printable lithium composition can be deposited therein.

[0044] In certain embodiments, electrodes pre-lithiated using the printable lithium composition can be assembled into a battery, wherein the electrodes are pre-loaded with lithium. A separator can be placed between the respective electrodes. Current can be allowed to flow between the electrodes. For example, a negative electrode pre-lithiated using the printable lithium composition of the present invention can form a secondary battery, such as described in U.S. Patent No. 16,706,447, which is incorporated herein by reference in its entirety.

[0045] The positive electrode is formed by an active material that is usually combined with a carbonaceous material and a binder polymer. The active material used in the positive electrode is preferably a material that can be lithiated. Preferably, non-lithiated materials, such as MnO2, V2O5, MoS2, metal fluorides or mixtures thereof, sulfur and sulfur complexes can be used as active materials. However, lithiated materials that can be further lithiated, such as LiMn2O4 and LiMO2, wherein M is Ni, Co or Mn, can also be used. Non-lithiated active materials are preferred, because in this configuration, they generally have higher specific capacity, lower cost and a wider selection of positive electrode materials, and they can provide improved energy and power compared to conventional secondary batteries including lithiated active materials.

[0046] Example

[0047] Example 1

[0048] 10 g of solution styrene butadiene rubber (S-SBR Europrene Sol R 72613) was dissolved in 90 g of toluene (99% anhydrous, Sigma Aldrich) by stirring at 21°C for 12 hours. 6 g of 10 wt% SBR (polymer binder) in toluene (solvent) was mixed with 0.1 g of carbon black (Timcal Super P) (rheology modifier) ​​and 16 g of toluene and dispersed in a ThinkyARE 250 planetary mixer at 2000 rpm for 6 minutes. 9.3 g of stabilized lithium metal powder ( Livent Corp.) was added to the suspension and dispersed in a Thinky mixer at 1000 rpm for 3 minutes. The printable lithium was then filtered through a 180 μm open stainless steel mesh. The printable lithium suspension was then knife coated onto a copper current collector at a wet thickness of 2 mil (~50 μm). Figure 3 is a graph showing the cycling performance of a pouch cell with a printable lithium-derived thin lithium film as a negative electrode versus a commercial thin lithium foil.

[0049] Example 2

[0050] 10 g of ethylene propylene diene terpolymer (EPDM) (Dow Nordel IP 4725P) with a molecular weight of 135,000 was dissolved in 90 g of p-xylene (99% anhydrous, Sigma Aldrich) by stirring at 21° C. for 12 hours. 6 g of 10 wt % EPDM (polymer binder) in p-xylene (solvent) was mixed with 0.1 g of TiO2 (Evonik Industries) (rheology modifier) ​​and 16 g of toluene and dispersed in a Thinky ARE 250 planetary mixer at 2000 rpm for 6 minutes. 9.3 g of stabilized lithium metal powder ( Livent Corp.) was added to the suspension and dispersed in a Thinky mixer at 1000 rpm for 3 minutes. The printable lithium was then filtered through a 180 μm open stainless steel mesh. The printable lithium composition was then knife coated onto a copper current collector at a wet thickness of 2 mil (~50 μm).

[0051] Shelf life stability

[0052] The printable lithium component must be selected to ensure chemical stability over a long shelf life at room temperature and stability for shorter durations at elevated temperatures, such as during transportation or drying. The stability of the printable lithium composition was determined using calorimetry. 1.5 grams of SLMP was added to a 10 ml volume Hastelloy ARC bomb sample container. 2.4 grams of a 4% SBR binder solution was added to the container. The container was equipped with a 24 ohm resistance heater and a thermocouple to monitor and control the temperature of the sample. The bomb sample assembly was placed in a 350 ml sealed container along with insulation. The Advance Reactive Screening Systems Tool calorimeter from Fauske Industries was used to evaluate the compatibility of the printable lithium solution during a constant rate of heating to 190°C. The heating rate was 2°C / min and the sample temperature was maintained at 190°C for 60 minutes. The test was performed under 200 psi argon pressure to prevent boiling of the solvent. Figure 2 Temperature and pressure profiles for reactivity testing of a SLMP / styrene butadiene / toluene printable lithium composition are shown.

[0053] Printing performance

[0054] The quality of the printable lithium composition with respect to printability is measured by several factors, such as the consistency of flow which directly affects its ability to control the lithium loading on the substrate or electrode surface. An effective way to measure flow is conductivity, which is a statement of the load per square centimeter relative to the factors that control the load, where the factors are the pressure during extrusion and the speed of the print head. It can be simply thought of as the inverse of flow resistance.

[0055] This expression is used to compare prints of varying pressure and speed, and the changes in conductivity can alert one to the non-linear relationship of flow rate with pressure. These are important for varying the loading of printable lithium up or down as needed for the negative or positive electrode. The ideal printable lithium composition exhibits changes in extrusion pressure in a linear manner.

[0056] To test printability, the printable lithium composition was filtered through a 180 μm opening stainless steel mesh and then loaded into a Nordson EFD 10 ml syringe. The syringe was loaded into a Nordson EFD HP4x syringe dispenser and connected to a slot die printhead. The slot die printhead was equipped with a 100 μm–300 μm thick gasket with channel openings designed to provide the required loading of the printable lithium composition. The slot die was mounted on a Loctite 300 series robot. Depending on the gasket and channel design, the printhead speed was set to 200 mm / s and the printing pressure was 20 to 200 psi argon. The print length was 14 cm. In an exemplary printing test, the printable lithium composition was printed 30 times from a single syringe with a dispenser setting of 80 psi to 200 psi. For this printing test, the conductivity averaged 2.33°. The standard deviation is 0.02. Although the printable composition does not behave in a perfectly linear manner, the composition flow rate in response to changes in the pressure in the dispenser is predictable, allowing one skilled in the art to fine-tune the lithium loading to a desired level. Thus, under fixed dispenser pressure conditions, the lithium loading can be controlled very consistently. For example, for For the printing of lithium metal, the CV is about 5%.

[0057] Electrochemical testing

[0058] The pre-lithiation effect of the printable lithium composition can be evaluated by printing the required amount of printable lithium on the surface of the prefabricated electrode. The amount of pre-lithiated lithium is determined by testing the negative electrode material in half-cell form and calculating the lithium required to compensate for the first cycle losses due to SEI formation or other side reactions. In order to calculate the required amount of printable lithium, the capacity of the composition as lithium metal must be known, and is about 3600 mAh / g dry lithium basis weight for the composition used as an example.

[0059] The pre-lithiation effect was tested using a graphite-SiO / NCA pouch cell. The graphite-SiO negative electrode sheet has the following formula: artificial graphite (90.06%) + SiO (4.74%) + carbon black (1.4%) + SBR / CMC (3.8%). The capacity loading of the electrode is 3.59 mAh / cm 2 The first cycle CE (Coulomb efficiency) is 87%. Printable lithium is added at 0.15 mg / cm 2The lithium metal was applied to the graphite-SiO negative electrode. The electrode was dried at 80°C for 100 minutes and then laminated at a roller gap of about 75% of the electrode thickness. A 7 cm × 7 cm electrode was punched out from the negative electrode sheet treated with printable lithium. The positive electrode has the following formula: NCA (96%) + carbon black (2%) + PVdF (2%). The positive electrode is 6.8 cm × 6.8 cm and has a capacity loading of 3.37 mAh / cm 2 . The NCA positive electrode has a first cycle CE of 90%. The capacity ratio of the negative electrode to the positive electrode is 1.06, and the baseline of the first cycle CE of the full battery is 77%. Single-layer pouch cells were assembled, and 1M LiPF6 / EC+DEC (1:1) was used as the electrolyte. The battery was pretreated at 21°C for 12 hours and then subjected to formation cycles at 40°C. The formation conditions were: 0.1C charge to 4.2V, constant voltage to 0.01C, and 0.1C discharge to 2.8V. In the test, the first cycle CE was 89%.

[0060] Although the present method has been described and illustrated with reference to preferred embodiments and specific examples thereof, it will be apparent to one of ordinary skill in the art that other embodiments and examples may perform similar functions and / or achieve similar results. All such equivalent embodiments and examples are within the spirit and scope of the present method.

Claims

1. A solid-state battery comprising a positive electrode, a negative electrode and a solid electrolyte, wherein the negative electrode comprises a printable lithium composition deposited on a current collector, wherein the printable lithium composition comprises: a) stabilized lithium metal powder; b) a polymer binder, wherein the polymer binder is compatible with the lithium metal powder, wherein the polymer binder is selected from the group consisting of polystyrene, polyisobutylene, natural rubber, butadiene rubber, styrene-butadiene rubber, polyisoprene rubber, butyl rubber, hydrogenated nitrile rubber, epichlorohydrin rubber, acrylate rubber, silicone rubber, nitrile rubber, polyacrylic acid, polyvinylidene chloride, polyvinyl acetate, ethylene-propylene diene trimer, ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-propylene terpolymer, and polybutylene; c) a rheology modifier, wherein the rheology modifier is compatible with the lithium metal powder and the polymer binder; and d) a solvent, wherein the solvent is selected from the group consisting of acyclic hydrocarbons and cyclic hydrocarbons, wherein the solvent is compatible with the lithium metal powder and with the polymer binder, The lithium composition comprises a) to d) based on a solution: a) 5 to 50% lithium metal powder; b) 0.1 to 20% polymer binder; c) 0.1 to 30% rheology modifier; d) 50 to 95% solvent.

2. The solid-state battery according to claim 1, wherein the solvent is an aromatic hydrocarbon.

3. A solid-state battery according to claim 1, wherein the negative electrode is formed by printing the printable lithium composition on the current collector.

4. The solid-state battery of claim 1, wherein the negative electrode is formed by coating the current collector with the printable lithium composition.

5. The solid-state battery of claim 1, wherein the negative electrode is formed by depositing the printable lithium composition on the negative electrode using an electric current.

6. The solid-state battery according to claim 1, wherein the rheology modifier is selected from the group consisting of carbon-containing materials, silicon-containing materials, tin-containing materials, Group IIA oxides, Group IIIA oxides, Group IVB oxides, Group VB oxides, and Group VIA oxides.

7. The solid-state battery according to claim 6, wherein the carbon-containing material is selected from the group consisting of carbon black, carbon nanotubes, graphite, hard carbon and graphene.

8. The solid-state battery of claim 6, wherein the silicon-containing material is selected from the group consisting of silicon nanotubes and fumed silicon dioxide. 9 . The solid-state battery according to claim 1 , wherein the molecular weight of the polymer binder is 1,000 to 8,000,000.

10. A solid-state battery comprising a positive electrode, a negative electrode and a solid electrolyte, wherein the positive electrode comprises a printable lithium composition deposited on a lithiated positive electrode active material, wherein the printable lithium composition comprises: a) stabilized lithium metal powder; b) a polymer binder, wherein the polymer binder is compatible with the lithium metal powder, wherein the polymer binder is selected from the group consisting of polystyrene, polyisobutylene, natural rubber, butadiene rubber, styrene-butadiene rubber, polyisoprene rubber, butyl rubber, hydrogenated nitrile rubber, epichlorohydrin rubber, acrylate rubber, silicone rubber, nitrile rubber, polyacrylic acid, polyvinylidene chloride, polyvinyl acetate, ethylene-propylene diene trimer, ethylene-vinyl acetate copolymer, ethylene-propylene copolymer, ethylene-propylene terpolymer, and polybutylene; c) a rheology modifier, wherein the rheology modifier is compatible with the lithium metal powder and the polymer binder; and d) a solvent, wherein the solvent is selected from the group consisting of acyclic hydrocarbons and cyclic hydrocarbons, wherein the solvent is compatible with the lithium metal powder and with the polymer binder, The lithium composition comprises a) to d) based on a solution: a) 5 to 50% lithium metal powder; b) 0.1 to 20% polymer binder; c) 0.1 to 30% rheology modifier; d) 50 to 95% solvent. The solid-state battery according to claim 10 , wherein the solvent is an aromatic hydrocarbon.

12. The solid-state battery of claim 10, wherein the rheology modifier is selected from the group consisting of carbon-containing materials, silicon-containing materials, tin-containing materials, Group IIA oxides, Group IIIA oxides, Group IVB oxides, Group VB oxides, and Group VIA oxides.

13. The solid-state battery according to claim 12, wherein the carbon-containing material is selected from the group consisting of carbon black, carbon nanotubes, graphite, hard carbon and graphene.

14. The solid-state battery of claim 12, wherein the silicon-containing material is selected from the group consisting of silicon nanotubes and fumed silicon dioxide.

15. The solid-state battery according to claim 10, wherein the molecular weight of the polymer binder is 1,000 to 8,000,000.