Steel sheet, component, and method for producing same

By forming a surface soft layer on the surface of the steel plate and applying metal plating, its composition and structure are optimized, the problem of insufficient tensile strength and yield stress in impact energy absorbing components in the prior art is solved, and high yield stress and ductility are achieved steel plate, suitable for automotive impact energy absorption components.

CN118974292APending Publication Date: 2024-11-15JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280093939.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2022-11-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art is difficult to simultaneously improve tensile strength, yield stress and press moldability in automotive impact energy absorbing components, resulting in impact absorption energy not meeting expectations, and the components are prone to rupture in simulated collision tests.

Method used

By forming a surface soft layer on the surface of the steel plate and controlling nanohardness and standard deviation during annealing and cooling, combined with the application of metal plating, the composition and structure of the steel plate are optimized to improve yield stress, ductility and bending.

Benefits of technology

The steel plate with tensile strength of more than 590MPa and excellent yield stress and ductility is achieved. It can show good fracture resistance and press moldability during collisions. It is suitable for automotive frames and impact energy absorbing components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005052180070000441
    Figure BDA0005052180070000441
  • Figure BDA0005052180070000451
    Figure BDA0005052180070000451
  • Figure BDA0005052180070000461
    Figure BDA0005052180070000461
Patent Text Reader

Abstract

Provided are: a steel plate which has a TS of 590 MPa or more, a high YS, and excellent press formability (ductility, hole expandability, and bendability) and fracture resistance characteristics during collision (bending fracture characteristics and axial crushing characteristics); a member; and methods for producing the steel plate and the member. The base steel sheet has a prescribed component composition, and when the nano-hardness at 300 points or more is measured in a 50 [mu] m * 50 [mu] m region of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel sheet, the ratio at which the nano-hardness is 7.0 GPa or more is 0.10 or less, and the ratio at which the nano-hardness is 7.0 GPa or more is 0.10 or less. The standard deviation [sigma] of the nano-hardness of the plate surface at a position 1 / 4 of the depth of the surface soft layer in the plate thickness direction from the surface of the base steel plate is 1.8 GPa or less, and the standard deviation [sigma] of the nano-hardness of the plate surface at a position 1 / 2 of the depth of the surface soft layer in the plate thickness direction from the surface of the base steel plate is 2.2 GPa or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a steel plate, a component using the steel plate as a blank, and a method for manufacturing the same. Background Art

[0002] In order to achieve both the improvement of fuel efficiency and the reduction of CO2 emissions and the improvement of collision safety through the thin-wall and lightweight steel plates used in automobile bodies, the high-strength steel plates for automobiles have been promoted. And new laws and regulations have been introduced one after another. Therefore, for the purpose of increasing the strength of the vehicle body, the application of high-strength steel plates to the main structural components and reinforcement components (hereinafter also referred to as the skeleton structural components of the automobile, etc.) assembled in the frame of the automobile cab is increasing. In addition, the high-strength steel plates used in the skeleton structural components of the automobile are required to have high component strength during press forming. For the improvement of component strength, it is effective to increase the yield stress (hereinafter also referred to as YS) of the steel plate. As a result, the impact absorption energy (hereinafter also referred to as impact absorption energy) during a car collision increases. In addition, the skeleton structural components of the automobile, such as energy absorption boxes, have a bending processing part. Therefore, from the perspective of press formability, such components preferably use steel plates with high bendability. In addition, from the perspective of the rust prevention performance of the vehicle body, most steel plates that become blanks for automobile parts are galvanized. Therefore, it is desired to develop a hot-dip galvanized steel sheet having high strength and excellent press formability and impact resistance.

[0003] As a steel plate that becomes a base material for such an automobile part, for example, Patent Document 1 discloses a high-strength steel plate having excellent stretch flange formability and collision resistance, characterized in that it has the following composition: expressed in mass %, it contains 0.04 to 0.22% C, 1.0% or less Si, 3.0% or less Mn, 0.05% or less P, 0.01% or less S, 0.01 to 0.1% Al and 0.001 to 0.005% N, the remainder being Fe and inevitable impurities, and is composed of a ferrite phase as a main phase and a martensite phase as a secondary phase, and the maximum grain size of the martensite phase is less than 2 μm, and its area ratio is more than 5%.

[0004] In addition, Patent Document 2 discloses a high-strength hot-dip galvanized steel sheet with excellent coating adhesion and formability, characterized in that the steel sheet is pre-plated with 0.2 g / m 2 ~2.0g / m 2A hot-dip galvanized steel sheet having a hot-dip galvanized layer on the surface of a cold-rolled steel sheet made of Ni, wherein the surface of the steel sheet contains, by mass%, C: not less than 0.05% and not more than 0.4%, Si: not less than 0.01% and not more than 3.0%, Mn: not less than 0.1% and not more than 3.0%, P: not more than 0.04%, S: not more than 0.05%, N: not more than 0.01%, Al: not less than 0.01% and not more than 2.0%, Si+Al>0.5%, the remainder being Fe and inevitable impurities, and the microstructure having ferrite containing 40% or more of the volume fraction as the main phase, containing 8% or more of retained austenite, containing two or more of the following three martensites [1][2][3] and 1% or more of martensite [3] Bainite and 0-10% pearlite, and the above three types of martensite [1] [2] [3] are respectively calculated by volume fraction as follows: martensite [1]: 0% to 50%, martensite [2]: 0% or more and less than 20%, and martensite [3]: 1% to 30%, the hot-dip galvanized layer contains less than 7% of Fe, and the remainder is composed of Zn, Al and inevitable impurities, as for tensile strength TS (MPa), total elongation EL (%), and hole expansion ratio λ (%), TS×EL is 18000 MPa·% or more, TS×λ is 35000 MPa·% or more, and has a tensile strength of 980 MPa or more (martensite [1]: when the C concentration (CM1) is less than 0.8%, the hardness Hv1 is Hv1 / (-982.1×CM1 2 +1676×CM1+189)≤0.60, martensite [2]: When the C concentration (CM2) is 0.8% or more, the hardness Hv2 is Hv2 / (-982.1×CM2 2 +1676×CM2+189)≤0.60, martensite [3]: When the C concentration (CM3) is 0.8% or more, the hardness Hv3 is Hv3 / (-982.1×CM3 2 +1676×CM3+189)≥0.80.

[0005] In addition, Patent Document 3 discloses a high-strength hot-dip galvanized steel sheet having the following composition and steel sheet structure, wherein the composition contains, by mass%, C: 0.15% to 0.25%, Si: 0.50% to 2.5%, Mn: 2.3% to 4.0%, P: 0.100% or less, S: 0.02% or less, Al: 0.01% to 2.5%, and the remainder is composed of Fe and unavoidable impurities, and the steel sheet structure The steel has, by area ratio, a tempered martensite phase of 30% to 73%, a ferrite phase of 25% to 68%, a retained austenite phase of 2% to 20%, and other phases of 10% or less (including 0%), and as other phases, a martensite phase of 3% or less (including 0%), and a bainitic ferrite phase of less than 5% (including 0%), the average grain size of the tempered martensite phase is less than 8 μm, and the amount of C in the retained austenite phase is less than 0.7% by mass.

[0006] In addition, Patent Document 4 discloses an alloyed hot-dip galvanized steel sheet, which has an alloyed hot-dip galvanized layer on the surface of the steel sheet, and the steel sheet has the following chemical composition and steel structure, wherein the chemical composition contains, by mass%, C: 0.03% to 0.35%, Si: 0.005% to 2.0%, Mn: 1.0% to 4.0%, P: 0.0004% to 0.1%, S: 0.02% or less, sol.Al: 0.0002% to 2.0%, N: 0.01% or less, and the remainder is composed of Fe and impurities, and Mn extending in the rolling direction at a depth of 50 μm from the surface of the steel sheet is 0.03% to 0.35%, Si: 0.005% to 2.0%, Mn: 1.0% to 4.0%, P: 0.0004% to 0.1%, S: 0.02% or less, sol.Al: 0.0002% to 2.0%, N: 0.01% or less, and the remainder is composed of Fe and impurities. The average spacing of concentrated parts in which n and / or Si are concentrated in the rolling right-angle direction, i.e., the average spacing of concentrated parts, is less than 1000 μm, the number density of cracks with a depth of 3 μm to 10 μm on the surface of the steel plate is 3 / mm to 1000 / mm, the steel structure contains, in terms of area%, bainite: more than 60%, retained austenite: more than 1%, martensite: more than 1% and ferrite: more than 2% and less than 20%, and the average value of the closest distance between martensite and retained austenite, i.e., the average spacing of superhard phases, is less than 20 μm, and the above-mentioned alloyed hot-dip galvanized steel sheet has mechanical properties with a tensile strength (TS) of more than 780 MPa.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent No. 3887235

[0010] Patent Document 2: Japanese Patent No. 5953693

[0011] Patent Document 3: Japanese Patent No. 6052472

[0012] Patent Document 4: Japanese Patent No. 5699764 Summary of the invention

[0013] However, the current situation is that although steel plates with a tensile strength TS (hereinafter sometimes abbreviated as TS) exceeding 590 MPa have been used in automobile skeleton parts represented by the center pillar, only steel plates with a TS of 590 MPa can be used in automobile impact energy absorbing parts represented by the front and rear longitudinal beams.

[0014] That is, in order to increase the absorbed energy during a collision (hereinafter also referred to as impact absorbed energy), it is effective to increase the yield stress YS (hereinafter also referred to as YS). However, if the YS of a steel plate is increased, the press formability generally decreases, especially the properties such as ductility, hole expansion, and bendability. Therefore, if such a steel plate with increased TS and YS is used in the above-mentioned automobile impact energy absorbing component, not only will press forming be difficult, but the component will also break in the axial crushing test of the simulated collision test. In other words, the actual impact absorbed energy will not be as high as expected based on the value of YS. As such, the existing technology still has room for improvement.

[0015] In fact, the steel sheets disclosed in Patent Documents 1 to 4 cannot be said to have high YS and YR and excellent press formability (ductility, hole expandability, and bendability) and fracture resistance characteristics during collision (bending fracture characteristics and axial crushing characteristics).

[0016] The present invention has been developed in view of the above-mentioned situation, and its purpose is to provide a steel plate and a method for manufacturing the same having a tensile strength TS of 590 MPa or more, a high yield stress YS, and excellent press formability (ductility, hole expandability and bendability) and fracture resistance during collision (bending fracture characteristics and axial crushing characteristics).

[0017] Another object of the present invention is to provide a component using the above-mentioned steel plate as a base material and a method for manufacturing the component.

[0018] In addition, here, the tensile strength TS is measured based on the tensile test of JIS Z 2241.

[0019] The high yield stress YS means that the yield stress (YS) is measured by a tensile test based on JIS Z 2241, and the TS measured by the tensile test satisfies the following formulas (A) to (F).

[0020] (A) 590MPa≤TS<780MPa, 350MPa≤YS

[0021] (B) 780MPa≤TS<980MPa, 400MPa≤YS

[0022] (C) 980MPa≤TS<1180MPa, 550MPa≤YS

[0023] (D) 1180MPa≤TS<1320MPa, 750MPa≤YS

[0024] (E) 1320MPa≤TS<1470MPa, 900MPa≤YS

[0025] (F) 1470MPa≤TS, 1050MPa≤YS

[0026] In addition, excellent ductility means that the total elongation (El) measured in a tensile test based on JIS Z 2241 satisfies the following formulas (A) to (F) based on TS measured in the tensile test.

[0027] (A) 590MPa≤TS<780MPa, 24.0%≤El

[0028] (B) 780MPa≤TS<980MPa, 18.0%≤El

[0029] (C) 980MPa≤TS<1180MPa, 11.0%≤El

[0030] (D) 1180MPa≤TS<1320MPa, 8.0%≤El

[0031] (E) 1320MPa≤TS<1470MPa, 7.5%≤El

[0032] (F) 1470MPa≤TS, 7.0%≤El

[0033] In addition, excellent hole expansion property means that the limiting hole expansion ratio (λ) measured in the hole expansion test based on JIS Z 2256 is 20% or more.

[0034] Furthermore, excellent bendability means that R (limit bending radius) / t (sheet thickness) measured in a V-bend test based on JIS Z 2248 satisfies the following expressions (A) to (F) from TS.

[0035] (A) 590MPa≤TS<780MPa, 1.0≥R / t

[0036] (B) 780MPa≤TS<980MPa, 2.0≥R / t

[0037] (C) 980MPa≤TS<1180MPa, 2.5≥R / t

[0038] (D) 1180MPa≤TS<1320MPa, 3.0≥R / t

[0039] (E) 1320MPa≤TS<1470MPa, 3.5≥R / t

[0040] (F) 1470MPa≤TS, 4.0≥R / t

[0041] Furthermore, the term "excellent bending fracture characteristics" means that the stroke (SFmax) at the maximum load measured in the V bending + orthogonal VDA bending test satisfies the following expressions (A) to (F) according to TS.

[0042] (A) 590MPa≤TS<780MPa, 29.0mm≤SFmax

[0043] (B) 780MPa≤TS<980MPa, 27.5mm≤SFmax

[0044] (C) 980MPa≤TS<1180MPa, 27.0mm≤SFmax

[0045] (D) 1180MPa≤TS<1320MPa, 26.0mm≤SFmax

[0046] (E) 1320MPa≤TS<1470MPa, 24.5mm≤SFmax

[0047] (F) 1470MPa≤TS, 24.0mm≤SFmax

[0048] Furthermore, the term "excellent axial crush characteristics" means that the sample after the axial crush test has no fracture (appearance crack) in the axial crush test, or the sample after the axial crush test has only one appearance crack.

[0049] The above-mentioned El (ductility), λ (stretch flangeability) and R / t (bendability) are characteristics indicating the ease of forming of the steel sheet during press forming (degree of freedom of forming for press forming without cracking). On the other hand, the V-bend + orthogonal VDA bend test is a test simulating the deformation and fracture behavior of the bending ridge portion in a collision test, and the stroke (SFmax) at the maximum load measured in the V-bend + orthogonal VDA bend test is an indicator indicating the resistance to cracking of the energy absorbing component.

[0050] The present inventors have conducted intensive studies to achieve the above-mentioned objects and have obtained the following findings.

[0051] Under the specified composition, when measuring the nanohardness of more than 300 points in a 50μm×50μm area of ​​the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the steel plate (the surface of the base (base) steel plate) , the ratio of the nanohardness being 7.0GPa or more is 0.10 or less, and the standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction from the surface of the base steel plate is 1.8GPa or less, and the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction from the surface of the base steel plate is measured in the same manner as at the 1 / 4 position. When the nanohardness of the plate surface at a position 1 / 2 of the depth in the plate thickness direction of the soft layer, the standard deviation σ of the nanohardness of the plate surface at a position 1 / 2 of the depth in the plate thickness direction of the surface soft layer is less than 2.2 GPa, thereby achieving an improvement in the index R / t of bendability which is a mode of press formability, and an improvement in the stroke (SFmax) at the maximum load measured in the V-bending + orthogonal VDA bending test which simulates the deformation and fracture behavior of the bending ridge portion in the collision test, which is an indicator of the impact resistance of the steel plates and parts of the automobile body during collision.

[0052] The present disclosure is made in view of the above viewpoints. That is, the gist of the present disclosure is as follows.

[0053] [1] A steel sheet having a base steel sheet, wherein the base steel sheet has the following composition: in terms of mass %, C: 0.030% to 0.500%, Si: 0.01% to 3.00%, Mn: 0.30% or more and less than 10.00%, P: 0.001% to 0.100%, S: 0.0200% or less, Al: 0.005% to 2.000%, N: 0.0100% or less, Ceq represented by the following formula (1) satisfies 0.30% to 0.85%, and the remainder is Fe and unavoidable impurities,

[0054] The surface soft layer is formed in a region 200 μm or less from the surface of the base steel plate in the plate thickness direction, and the Vickers hardness of the surface soft layer is 85% or less relative to the Vickers hardness of the base steel plate at a position 1 / 4 of the plate thickness.

[0055] When the nanohardness of more than 300 points is measured in the 50 μm×50 μm area of ​​the plate surface at the 1 / 4 position and the 1 / 2 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate,

[0056] The ratio of the number of measurements of which the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 7.0 GPa or more is 0.10 or less relative to the total number of measurements,

[0057] Furthermore, the standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 1.8 GPa or less,

[0058] Furthermore, a standard deviation σ of the nanohardness of the plate surface at a position which is 1 / 2 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 2.2 GPa or less.

[0059] Ceq=[%C]+[%Mn] / 6+[%Si] / 24+[%Ni] / 40+[%Cr] / 5+[%Mo] / 4+[%V] / 14···Formula (1)

[0060] Among them, [%C]: C content, [%Mn]: Mn content, [%Si]: Si content, [%Ni]: Ni content, [%Cr]: Cr content, [%Mo]: Mo content, [%V]: V content, and the value is 0 (zero) when not contained.

[0061] [2] The steel sheet according to [1] above, wherein the total area ratio of ferrite and bainite present in the surface soft layer is 20% or more,

[0062] The value obtained by dividing the area ratio of martensite present in the surface soft layer by the total area ratio of martensite and tempered martensite present in the surface soft layer is 0.45 or less.

[0063] [3] The steel sheet according to [1] or [2], wherein the above-mentioned component composition further contains, in terms of mass%, Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less At least one element selected from the group consisting of 0.0200% or less, Zn: 0.0200% or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less.

[0064] [4] The steel sheet according to any one of [1] to [3] above, wherein a metal plating layer is provided as a first plating layer on one or both surfaces of the base steel sheet.

[0065] [5] The steel sheet according to any one of [1] to [4] above, wherein the outermost layer of one or both surfaces of the steel sheet has a metal plating layer as a second plating layer.

[0066] [6] The steel plate according to any one of [1] to [5] above, wherein the surface irregularities of the test piece after 90° V-bending processing where R / t (limit bending radius R divided by plate thickness t) is 4.5 to 5.0 is less than 20.0 μm.

[0067] [7] A component made using the steel plate according to any one of [1] to [6] above.

[0068] [8] A method for manufacturing a steel plate, comprising the following steps:

[0069] The hot rolling step is to hot-roll the steel slab having the component composition described in [1] or [3] above.

[0070] In the annealing step, the obtained steel sheet is annealed under the conditions of annealing temperature: Ac1 point to 950°C, annealing time: 10 seconds or more, and dew point: -30°C or more.

[0071] A first cooling step, after the annealing step, cools the obtained steel sheet in a temperature range from Ac1 point to 450°C in an atmosphere with a dew point of -30°C or less at an average cooling rate of 8°C / s or more; and

[0072] The second cooling step is to cool the obtained steel plate in a temperature range from less than 450° C. to 300° C. at an average cooling rate of less than 8° C. / second after the first cooling step.

[0073] [9] The method for manufacturing a steel sheet according to [8], further comprising a cold rolling step of cold rolling the steel sheet after the hot rolling step and before the annealing step.

[0074]

[10] The method for manufacturing a steel sheet according to [8] or [9], further comprising a first plating step of performing metal plating on one or both surfaces of the steel sheet after the hot rolling step and before the annealing step to form a first plating layer.

[0075]

[11] The method for manufacturing a steel sheet according to any one of [8] to

[10] , further comprising a second plating step of plating the steel sheet after the second cooling step.

[0076]

[12] The method for manufacturing a steel plate according to any one of [8] to

[11] above, comprising a reheating and holding step: after the above second cooling step, the obtained steel plate is cooled to a cooling stop temperature of 250°C or less to room temperature, and then heated to a reheating temperature range of (the above cooling stop temperature + 50°C) to 450°C, and held in the above reheating temperature range for more than 10 seconds.

[0077]

[13] A method for manufacturing a component, comprising the step of subjecting the steel plate according to any one of [1] to [6] above to at least one of forming and joining to form the component.

[0078] According to the present invention, a steel sheet having a tensile strength TS of 590 MPa or more, a high yield stress YS, and excellent press formability (ductility, hole expandability, and bendability) and fracture resistance during collision (axial crushing characteristics) can be obtained.

[0079] Furthermore, since parts made of the steel sheet of the present invention are high-strength and have excellent press formability and impact resistance, they can be very advantageously used in automotive frame parts, impact energy absorbing parts, and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0080] Figure 1 This is a cross-sectional photograph used to illustrate the depth of surface irregularities.

[0081] Figure 2 (a) is a diagram for explaining the V-bending process (primary bending process) in the V-bending + orthogonal VDA bending test of the example. Figure 2 (b) is a diagram for explaining the orthogonal VDA bending process (secondary bending process) in the V-bending + orthogonal VDA bending test of the embodiment.

[0082] Figure 3-1 (a) is a front view of a test member produced in order to conduct an axial crushing test of an example, in which a hat-shaped member and a steel plate are spot-welded. Figure 3-1 (b) is a perspective view of the test component shown in (a).

[0083] Figure 3-2 (c) is a schematic diagram for explaining the axial crushing test of the embodiment. DETAILED DESCRIPTION

[0084] The present invention will be described based on the following embodiments.

[0085] [1.Steel plate]

[0086] The steel sheet of the present invention has a base steel sheet having the following composition: in terms of mass %, it contains C: 0.030% to 0.500%, Si: 0.01% to 3.00%, Mn: 0.30% or more and less than 10.00%, P: 0.001% to 0.100%, S: 0.0200% or less, Al: 0.005% to 2.000%, N: 0.0100% or less, Ceq represented by the following formula (1) satisfies 0.30% to 0.85%, and the remainder is composed of Fe and inevitable impurities,

[0087] A surface soft layer having a Vickers hardness of 85% or less relative to the Vickers hardness at a position 1 / 4 of the plate thickness is formed in an area less than 200 μm from the surface of the base steel plate in the plate thickness direction. When the nanohardness is measured at more than 300 points in an area of ​​50 μm×50 μm on the plate surface at a position 1 / 4 of the depth in the plate thickness direction and a position 1 / 2 of the depth in the plate thickness direction from the base steel plate surface, the ratio of the number of measurements in which the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction from the base steel plate surface of the surface soft layer is 7.0 GPa or more is less than 0.10 relative to the total number of measurements, and the standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction from the base steel plate surface of the surface soft layer is less than 1.8 GPa, and the standard deviation σ of the nanohardness of the plate surface at a position 1 / 2 of the depth in the plate thickness direction from the base steel plate surface of the surface soft layer is less than 2.2 GPa.

[0088] Ceq=[%C]+[%Mn] / 6+[%Si] / 24+[%Ni] / 40+[%Cr] / 5+[%Mo] / 4+[%V] / 14···Formula (1)

[0089] Among them, [%C]: C content, [%Mn]: Mn content, [%Si]: Si content, [%Ni]: Ni content, [%Cr]: Cr content, [%Mo]: Mo content, [%V]: V content, and the value is 0 (zero) when not contained.

[0090] Ingredients

[0091] First, the component composition of the base steel sheet of the steel sheet according to one embodiment of the present invention will be described. It should be noted that the unit in the component composition is "mass %", and hereinafter, it is simply expressed as "%" unless otherwise specified.

[0092] In addition, in the present invention, it is specified that the steel plate has a base steel plate, and the coating (metal coating (first coating), hot-dip galvanized layer, alloyed hot-dip galvanized layer, electrogalvanized layer and other galvanized layers, hot-dip aluminum coating and other coatings (second coating)) on the base steel plate is described below. The coating is a preferred component of the steel plate, and the steel plate does not necessarily have to have the coating.

[0093] C: 0.030%~0.500%

[0094] C is an effective element for generating an appropriate amount of tempered martensite, bainite, etc. to ensure high TS and high YS. Here, when the C content is less than 0.030%, the area ratio of ferrite increases, and the required TS is satisfactorily ensured. In addition, it also leads to a decrease in YS. On the other hand, if the C content exceeds 0.500%, the area ratio of martensite increases, TS becomes too high, and the required El (press formability (ductility)) and R / t (press formability (bendability)) cannot be obtained. In addition, the volume ratio (area ratio) of retained austenite increases, and when the steel plate is punched in the hole expansion test, or when the V-bending process is performed in the V-bending + orthogonal VDA test, hard martensite caused by the processing-induced phase transformation of the retained austenite is generated, and voids are generated in the subsequent test and cracks are promoted, and the required λ (press formability (hole expansion)) and SFmax (fracture resistance during collision (bending fracture characteristics)) cannot be obtained. Therefore, the C content is set to 0.030% to 0.500%. The C content is preferably 0.050% or more. Also, the C content is preferably 0.300% or less.

[0095] Si: 0.01% to 3.00%

[0096] Si promotes ferrite transformation during annealing and in the cooling process after annealing. That is, Si is an element that affects the area ratio of ferrite. Here, when the Si content is less than 0.01%, the area ratio of ferrite decreases and the ductility decreases. On the other hand, when the Si content exceeds 3.00%, the volume ratio of retained austenite increases. When the steel plate is punched in the hole expansion test and when the V-bending process is performed in the V-bending + orthogonal VDA test, hard martensite caused by the processing-induced transformation of the retained austenite is generated, and voids are generated and cracks are promoted in subsequent tests, and the required λ and SFmax cannot be obtained. Therefore, the Si content is set to 0.01% to 3.00%. The Si content is preferably 0.10% or more. In addition, the Si content is preferably 2.0% or less.

[0097] Mn: 0.30% or more and less than 10.00%

[0098] Mn is an element for adjusting the area ratio of tempered martensite, bainite, etc. Here, when the Mn content is less than 0.30%, the area ratio of ferrite increases, and it is difficult to ensure the required TS. In addition, it will also lead to a decrease in YS. On the other hand, if the Mn content is more than 10.00%, the generation of ε martensite as a brittle phase increases, and the required El (pressing formability (ductility)), R / t (pressing formability (bending)) and SFmax (fracture resistance during collision (bending fracture characteristics)) cannot be obtained. Therefore, the Mn content is made to be more than 0.30% and less than 10.00%. The Mn content is preferably more than 1.00%. In addition, the Mn content is preferably less than 3.50%.

[0099] P: 0.001%~0.100%

[0100] P has a solid solution strengthening effect and is an element that increases the TS and YS of the steel plate. In order to obtain such an effect, the P content is set to 0.001% or more. On the other hand, if the P content exceeds 0.100%, P segregates to the original austenite grain boundary and embrittles the grain boundary. Therefore, during the V-bending test, voids are generated along the original austenite grain boundary and cracking is promoted, and the required R / t cannot be obtained. In addition, when the steel plate is punched in the hole expansion test, or when the V-bending is performed in the V-bending + orthogonal VDA test, voids are generated along the original austenite grain boundary and cracking is promoted, and the required λ and SFmax cannot be obtained. Therefore, the P content is set to 0.001% to 0.100%. The P content is preferably 0.030% or less.

[0101] S: 0.0200% or less

[0102] S exists in the form of sulfides in steel. In particular, if the S content exceeds 0.0200%, voids are generated starting from the above sulfides and cracks are accelerated during the V-bending test, and the desired R / t cannot be obtained. In addition, when the steel plate is punched in the hole expansion test, or when the V-bending is performed in the V-bending + orthogonal VDA test, voids are generated starting from the above sulfides and cracks are accelerated, and the desired λ and SFmax cannot be obtained. Therefore, the S content is set to 0.0200% or less. The S content is preferably 0.0080% or less. It should be noted that the lower limit of the S content is not particularly specified, but considering the limitations of production technology, the S content is preferably 0.0001% or more.

[0103] Al: 0.005%~2.000%

[0104] Al promotes ferrite transformation during annealing and in the cooling process after annealing. That is, Al is an element that affects the area ratio of ferrite. Here, when the Al content is less than 0.005%, the area ratio of ferrite decreases and the ductility decreases. On the other hand, if the Al content exceeds 2.000%, the area ratio of ferrite increases excessively, making it difficult to ensure the required TS. In addition, it will also lead to a decrease in YS. Therefore, the Al content is set to 0.005% to 2.000%. The Al content is preferably greater than 0.010%, and more preferably greater than 0.015%. In addition, the Al content is preferably less than 1.000%.

[0105] N: 0.0100% or less

[0106] N exists in the form of nitrides in steel. In particular, if the N content exceeds 0.0100%, voids are generated starting from the above nitrides and cracks are promoted during the V-bending test, and the required R / t cannot be obtained. In addition, when the steel plate is punched in the hole expansion test, or when the V-bending is performed in the V-bending + orthogonal VDA test, voids are generated starting from the above nitrides and cracks are promoted, and the required λ and SFmax cannot be obtained. Therefore, the N content is set to 0.0100% or less. In addition, the N content is preferably 0.0050% or less. It should be noted that the lower limit of the N content is not particularly specified, but considering the limitations of production technology, the N content is preferably 0.0005% or more.

[0107] Ceq: 0.30%~0.85%

[0108] Ceq is an indicator for generating appropriate amounts of martensite, retained austenite, tempered martensite, etc. to ensure high TS and high YS. Here, when Ceq is less than 0.30%, it becomes difficult to generate martensite, retained austenite, and tempered martensite at the 1 / 4 position of the plate thickness, and it is difficult to ensure the required TS and YS. On the other hand, if Ceq exceeds 0.85%, the area ratio of martensite increases, TS becomes too high, and the required El (press formability (ductility)) and R / t (press formability (bending)) cannot be obtained. In addition, the volume ratio of retained austenite increases, and when the steel plate is punched in the hole expansion test, and when the steel plate is V-bending in the V-bending + orthogonal VDA test, hard martensite caused by the processing-induced phase transformation of the retained austenite is generated, and voids are generated and cracks are promoted in subsequent tests, and the required λ (press formability (hole expansion)) and SFmax (fracture resistance during collision (bending fracture characteristics)) cannot be obtained.

[0109] Therefore, Ceq is set to 0.30% to 0.85%. Ceq is preferably 0.35% or more. In addition, Ceq is preferably 0.80% or less.

[0110] In addition, Ceq is calculated by the following formula (1).

[0111] Ceq=[%C]+[%Mn] / 6+[%Si] / 24+[%Ni] / 40+[%Cr] / 5+[%Mo] / 4+[%V] / 14···Formula (1)

[0112] Among them, [%C]: C content, [%Mn]: Mn content, [%Si]: Si content, [%Ni]: Ni content, [%Cr]: Cr content, [%Mo]: Mo content, [%V]: V content, and the value is 0 (zero) when not contained.

[0113] The basic component composition of the base steel sheet of the steel sheet according to one embodiment of the present invention has been described above. The base steel sheet of the hot-dip galvanized steel sheet according to one embodiment of the present invention has a component composition including the above-mentioned basic components and the remainder other than the above-mentioned basic components contains Fe (iron) and inevitable impurities. Here, the base steel sheet of the hot-dip galvanized steel sheet according to one embodiment of the present invention preferably has a component composition including the above-mentioned basic components and the remainder consisting of Fe and inevitable impurities.

[0114] In the base steel sheet of the steel sheet according to one embodiment of the present invention, in addition to the above-mentioned basic components, at least one of the optional components shown below may be contained. It should be noted that the effects of the present invention can be obtained as long as the optional components shown below are contained in an amount below the upper limit shown below, so the lower limit is not particularly specified. It should be noted that when the optional elements shown below are contained in an amount below the preferred lower limit described below, the elements are contained as unavoidable impurities.

[0115] Selected from Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, Co : 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, and REM: 0.0200% or less

[0116] Nb: 0.200% or less

[0117] Nb improves TS, YS and YR by forming fine carbides, nitrides or carbonitrides during hot rolling or annealing. In order to obtain such an effect, it is preferred that the Nb content is 0.001% or more. The Nb content is more preferably 0.005% or more. On the other hand, if the Nb content exceeds 0.200%, a large amount of coarse precipitates or inclusions are sometimes generated. In such a case, the coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bending test and V bending + orthogonal VDA bending test, so the required λ, R / t and SFmax are sometimes not obtained. Therefore, when Nb is contained, the Nb content is preferably 0.200% or less. The Nb content is more preferably 0.060% or less.

[0118] Ti: 0.200% or less

[0119] Ti, like Nb, improves TS and YS by forming fine carbides, nitrides or carbonitrides during hot rolling or annealing. In order to obtain such an effect, it is preferred that the Ti content is 0.001% or more. The Ti content is more preferably 0.005% or more. On the other hand, if the Ti content exceeds 0.200%, a large amount of coarse precipitates or inclusions are sometimes generated. In such a case, the coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bending test and V bending + orthogonal VDA bending test, so the required λ, R / t and SFmax are sometimes not obtained. Therefore, when Ti is contained, the Ti content is preferably 0.200% or less. The Ti content is more preferably 0.060% or less.

[0120] V: 0.200% or less

[0121] V, like Nb and Ti, forms fine carbides, nitrides or carbonitrides during hot rolling or annealing, thereby increasing TS and YS. To achieve such an effect, the V content is preferably 0.001% or more. The V content is more preferably 0.005% or more. The V content is further preferably 0.030% or more.

[0122] On the other hand, if the V content exceeds 0.200%, a large amount of coarse precipitates or inclusions may be generated. In such a case, the coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so the desired λ, R / t, and SFmax may not be obtained. Therefore, when V is contained, the V content is preferably 0.200% or less. The V content is more preferably 0.060% or less.

[0123] B: 0.0100% or less

[0124] B is an element that improves hardenability by segregating at austenite grain boundaries. In addition, B is an element that controls the formation of ferrite and grain growth during cooling after annealing. In order to obtain such an effect, it is preferred that the B content is 0.0001% or more. The B content is more preferably 0.0002% or more. The B content is further preferably 0.0010% or more.

[0125] On the other hand, if the B content exceeds 0.0100%, cracks may be generated inside the steel sheet during hot rolling. In addition, during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, the internal cracks become the starting point of cracking, and the desired λ, R / t, and SFmax may not be obtained. Therefore, when B is contained, the B content is preferably 0.0100% or less. The B content is more preferably 0.0050% or less.

[0126] Cr: 1.000% or less

[0127] Cr is an element that improves hardenability, so by adding Cr, an appropriate amount of tempered martensite can be generated, thereby improving TS and YS. In order to obtain such an effect, the Cr content is preferably 0.0005% or more. In addition, the Cr content is more preferably 0.010% or more. The Cr content is further preferably 0.030% or more, and further preferably 0.200% or more. On the other hand, if the Cr content exceeds 1.000%, the area ratio of martensite increases, the hole expansion and the bendability of the V bending test decrease, and sometimes the required λ and R / t cannot be obtained. Therefore, when Cr is contained, the Cr content is preferably 1.000% or less. In addition, the Cr content is more preferably 0.700% or less, and further preferably 0.600% or less.

[0128] Ni: 1.000% or less

[0129] Ni is an element that improves hardenability, so by adding Ni, a large amount of tempered martensite can be generated, thereby improving TS and YS. In order to obtain such an effect, it is preferred that the Ni content is 0.005% or more. The Ni content is more preferably 0.020% or more. The Ni content is further preferably 0.080% or more, and further more preferably 0.100% or more.

[0130] On the other hand, if the Ni content exceeds 1.000%, the area ratio of martensite increases, the hole expansion property and the bendability of the V bend test decrease, and the desired λ and R / t may not be obtained. Therefore, when Ni is contained, the Ni content is preferably 1.000% or less. The Ni content is more preferably 0.800% or less. The Ni content is further preferably 0.600% or less, and further preferably 0.400% or less.

[0131] Mo: 1.000% or less

[0132] Mo is an element that improves hardenability, so by adding Mo, a large amount of tempered martensite can be generated, thereby improving TS and YS. In order to obtain such an effect, it is preferred that the Mo content is 0.010% or more. The Mo content is more preferably 0.030% or more. On the other hand, if the Mo content exceeds 1.000%, the area ratio of martensite increases, the hole expansion and the bendability of the V bending test decrease, and sometimes the required λ and R / t cannot be obtained. Therefore, when Mo is contained, the Mo content is preferably 1.000% or less. In addition, the Mo content is more preferably 0.500% or less. The Mo content is further preferably 0.450% or less, and further more preferably 0.400% or less.

[0133] Sb: 0.200% or less

[0134] Sb is an effective element for suppressing the diffusion of C near the surface of the steel sheet during annealing to adjust the thickness of the soft layer formed near the surface of the steel sheet. The Sb content is preferably 0.002% or more, more preferably 0.004% or more.

[0135] On the other hand, if the Sb content exceeds 0.200%, a soft layer may not be formed near the surface of the steel sheet, resulting in a decrease in λ, R / t and SFmax. Therefore, when Sb is contained, the Sb content is preferably 0.200% or less. The Sb content is more preferably 0.020% or less.

[0136] Sn: 0.200% or less

[0137] Sn is an effective element for suppressing the diffusion of C near the surface of the steel sheet during annealing to adjust the thickness of the soft layer formed near the surface of the steel sheet. The Sn content is preferably 0.002% or more, more preferably 0.004% or more.

[0138] On the other hand, if the Sn content exceeds 0.200%, a soft layer may not be formed near the surface of the steel sheet, resulting in a decrease in λ, R / t and SFmax. Therefore, when Sn is contained, the Sn content is preferably 0.200% or less. The Sn content is more preferably 0.020% or less.

[0139] Cu: 1.000% or less

[0140] Cu is an element that improves hardenability, so by adding Cu, a large amount of tempered martensite can be generated, thereby improving TS and YS. In order to obtain such an effect, it is preferred that the Cu content is 0.005% or more. The Cu content is more preferably 0.020% or more. The Cu content is further preferably 0.080% or more, and further more preferably 0.150% or more.

[0141] On the other hand, if the Cu content exceeds 1.000%, the area ratio of martensite sometimes increases excessively. In addition, a large amount of coarse precipitates or inclusions are sometimes generated. In such a case, the excessively generated martensite and coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bending test and V bending + orthogonal VDA bending test, so the desired λ, R / t and SFmax are sometimes not obtained. Therefore, when Cu is contained, the Cu content is preferably 1.000% or less. The Cu content is more preferably 0.200% or less.

[0142] Ta: 0.100% or less

[0143] Ta, like Ti, Nb and V, improves TS and YS by forming fine carbides, nitrides or carbonitrides during hot rolling or annealing. In addition, a portion of Ta is dissolved in Nb carbides or Nb carbonitrides to form composite precipitates such as (Nb, Ta)(C, N). As a result, the coarsening of the precipitates is suppressed and the precipitation strengthening is stabilized. As a result, TS and YS are further improved. In order to obtain such an effect, it is preferred that the Ta content is 0.001% or more. On the other hand, if the Ta content exceeds 0.100%, a large amount of coarse precipitates or inclusions are sometimes generated. In such a case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during hole expansion tests, V bending tests and V bending + orthogonal VDA bending tests, so the required λ, R / t and SFmax are sometimes not obtained. Therefore, when Ta is contained, the Ta content is preferably less than 0.100%. The Ta content is further preferably less than 0.080%, and further preferably less than 0.020%.

[0144] W: 0.500% or less

[0145] W is an element that improves hardenability, so by adding W, a large amount of tempered martensite can be generated, thereby improving TS and YS. In order to obtain such an effect, it is preferred that the W content is 0.001% or more. The W content is more preferably 0.030% or more. On the other hand, if the W content exceeds 0.500%, the area ratio of martensite increases, the hole expansion and the bendability of the V bending test decrease, and sometimes the required λ and R / t cannot be obtained. Therefore, when W is contained, the W content is preferably 0.500% or less. The W content is more preferably 0.450% or less, and further preferably 0.400% or less. The W content is further preferably 0.150% or less, and further more preferably 0.080% or less.

[0146] Mg: 0.0200% or less

[0147] Mg is an effective element for spheroidizing the shape of inclusions such as sulfides and oxides to improve the hole expandability and bendability of the steel sheet. In order to obtain such an effect, the Mg content is preferably 0.0001% or more. The Mg content is more preferably 0.0005% or more, and even more preferably 0.0020% or more.

[0148] On the other hand, if the Mg content exceeds 0.0200%, a large amount of coarse precipitates or inclusions may be generated. In such a case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so the desired λ, R / t, and SFmax may not be obtained. Therefore, when Mg is contained, the Mg content is preferably 0.0200% or less. The Mg content is more preferably 0.0150% or less, and even more preferably 0.0100% or less.

[0149] Zn: 0.0200% or less

[0150] Zn is an effective element for spheroidizing the shape of inclusions to improve the hole expandability and bendability of the steel plate. To obtain such an effect, the Zn content is preferably 0.0010% or more. The Zn content is more preferably 0.0005% or more, and even more preferably 0.0020% or more.

[0151] On the other hand, if the Zn content exceeds 0.0200%, a large amount of coarse precipitates or inclusions may be generated. In such a case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so the desired λ, R / t, and SFmax may not be obtained. Therefore, when Zn is contained, the Zn content is preferably 0.0200% or less. The Zn content is more preferably 0.0150% or less, and even more preferably 0.0100% or less.

[0152] Co: 0.0200% or less

[0153] Co, like Zn, is an effective element for spheroidizing the shape of inclusions to improve the hole expandability and bendability of the steel sheet. To obtain such an effect, the Co content is preferably 0.0010% or more. The Co content is more preferably 0.0010% or more, and even more preferably 0.0020% or more.

[0154] On the other hand, if the Co content exceeds 0.0200%, a large amount of coarse precipitates or inclusions may be generated. In such a case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so the desired λ, R / t, and SFmax may not be obtained. Therefore, when Co is contained, the Co content is preferably 0.0200% or less.

[0155] Zr: 0.1000% or less

[0156] Zr is an effective element for spheroidizing the shape of inclusions to improve the hole expandability and bendability of the steel sheet, similarly to Zn and Co. In order to obtain such an effect, the Zr content is preferably 0.0010% or more.

[0157] On the other hand, if the Zr content exceeds 0.1000%, in such a case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so that the desired λ, R / t, and SFmax may not be obtained. Therefore, when Zr is contained, the Zr content is preferably 0.1000% or less. The Zr content is more preferably 0.0150% or less, and even more preferably 0.0100% or less.

[0158] Ca: 0.0200% or less

[0159] Ca exists in the steel as inclusions. Here, if the Ca content exceeds 0.0200%, a large number of coarse inclusions may be generated. In this case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so the desired λ, R / t, and SFmax may not be obtained. Therefore, when Ca is contained, the Ca content is preferably 0.0200% or less. The Ca content is preferably 0.0080% or less.

[0160] It should be noted that the lower limit of the Ca content is not particularly limited, but the Ca content is preferably 0.0005% or more. In addition, from the perspective of production technology limitations, the Ca content is more preferably 0.0010% or more.

[0161] Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, REM: 0.0200% or less

[0162] Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi and REM are all effective elements for improving the hole expandability and bendability of steel plates. In order to obtain such effects, the contents of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi and REM are preferably 0.0001% or more respectively.

[0163] The content of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM is more preferably 0.0020% or more.

[0164] On the other hand, if the content of Se, Te, Ge, Sr, Cs, Hf, Pb, Bi, and REM exceeds 0.0200% respectively, and if the content of As exceeds 0.0500%, a large amount of coarse precipitates or inclusions may be generated. In such a case, excessively coarse precipitates or inclusions become the starting point of voids and cracks during the hole expansion test, V bend test, and V bend + orthogonal VDA bend test, so the required λ, R / t, and SFmax may not be obtained. Therefore, when at least one of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM is contained, the content of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM is preferably 0.0200% or less, and the content of As is preferably 0.0500% or less.

[0165] The content of Se, Te, Ge, As, Sr, Cs, Hf, Pb, Bi, and REM is more preferably 0.0120% or less.

[0166] It should be noted that REM mentioned in the present invention refers to scandium (Sc) with atomic number 21, yttrium (Y) with atomic number 39, and lanthanoids from lanthanum (La) with atomic number 57 to lutetium (Lu) with atomic number 71. The REM concentration in the present invention refers to the total content of one or more elements selected from the above REM.

[0167] REM is not particularly limited, but Sc, Y, Ce, and La are preferred.

[0168] Surface soft layer

[0169] Next, the steel structure of the base steel plate according to one embodiment of the present invention will be described.

[0170] In a steel plate according to one embodiment of the present invention, a surface soft layer is provided on the surface of the base steel plate (in the case of hot-dip galvanized steel plate, alloyed hot-dip galvanized steel plate, electrogalvanized steel plate and other metal-plated steel plates, it is located on the base (base) of the above-mentioned various coating layers.). The above-mentioned surface soft layer helps to suppress the progression of bending cracks during press forming and vehicle body collision, thereby further improving the bending fracture resistance. It should be noted that the surface soft layer refers to a decarburized layer, which is a surface area with a Vickers hardness of less than 85% of the Vickers hardness of the cross section at 1 / 4 of the plate thickness of the base steel plate (a surface parallel to the surface of the steel plate).

[0171] Here, the surface soft layer is formed in a region 200 μm or less from the surface of the base steel plate in the plate thickness direction. The region where the surface soft layer is formed is preferably 150 μm or less, more preferably 120 μm or less from the surface of the base steel plate in the plate thickness direction. The region where the surface soft layer is formed is preferably 30 μm or more, more preferably 40 μm or more from the surface of the base steel plate in the plate thickness direction.

[0172] The 1 / 4 thickness position of the base steel plate for measuring the Vickers hardness is a non-surface soft layer (a layer that does not satisfy the hardness condition of the surface soft layer specified in the present invention).

[0173] The Vickers hardness is measured at a load of 10 gf in accordance with JIS Z 2244-1 (2020).

[0174] Hardness of the soft layer

[0175] When the nanohardness of 300 or more points is measured in the 50μm×50μm area of ​​the plate surface at the position of 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate and the position of 1 / 2 of the depth in the plate thickness direction, the ratio of the number of measurements with a nanohardness of 7.0GPa or more at the position of 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate to the total number of measurements is 0.10 or less

[0176] In the present invention, in order to obtain excellent bendability during press forming and excellent bending fracture characteristics during collision, when measuring the nanohardness of more than 300 points in a 50μm×50μm area of ​​the plate surface at a position of 1 / 4 of the plate thickness direction depth of the surface soft layer from the surface of the base steel plate, the proportion of the plate surface nanohardness of 7.0GPa or more at a position of 1 / 4 of the plate thickness direction depth from the surface of the base steel plate needs to be 0.10 or less relative to the total number of measurements (the total number of measurements at a position of 1 / 4 of the plate thickness direction depth). When the proportion of the nanohardness of 7.0GPa or more is less than 0.10, it means that the proportion of hard structures (martensite, etc.), inclusions, etc. is small, and the generation or connection of voids and the progress of cracks of hard structures (martensite, etc.), inclusions, etc. during press forming and collision can be further suppressed, and excellent R / t and SFmax can be obtained.

[0177] The ratio of the plate surface having a nanohardness of 7.0 GPa or more at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the base steel plate surface is preferably 0.08 or less, more preferably 0.07 or less, relative to the total number of measurements. The lower limit is not particularly limited and may be 0.01 or more.

[0178] The standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth of the surface soft layer in the plate thickness direction from the steel plate surface is less than 1.8 GPa, and the standard deviation σ of the nanohardness of the plate surface at a position 1 / 2 of the depth of the surface soft layer in the plate thickness direction from the steel plate surface is less than 2.2 GPa.

[0179] In the present invention, in order to obtain excellent bendability during press forming and excellent bending fracture characteristics during collision, the standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the steel plate is 1.8 GPa or less, and the standard deviation σ of the nanohardness of the plate surface at a position 1 / 2 of the depth in the plate thickness direction of the surface soft layer from the surface of the steel plate must be 2.2 GPa or less. When the standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the steel plate is 1.8 GPa or less, and the standard deviation σ of the nanohardness of the plate surface at a position 1 / 2 of the depth in the plate thickness direction of the surface soft layer from the surface of the steel plate is 2.2 GPa or less, it means that the difference in structural hardness in the microscopic region is small, and the generation or connection of voids during press forming and collision and the progression of cracks can be further suppressed, and excellent R / t and SFmax can be obtained.

[0180] In addition, the preferred range of the standard deviation σ of the nanohardness of the plate surface at 1 / 4 of the plate thickness direction depth of the surface soft layer from the base steel plate surface is 1.7 GPa or less. The standard deviation σ of the nanohardness of the plate surface at 1 / 4 of the plate thickness direction depth of the surface soft layer from the base steel plate surface is more preferably 1.3 GPa or less. The lower limit is not particularly limited, and the standard deviation σ of the nanohardness of the plate surface at 1 / 4 of the plate thickness direction depth of the surface soft layer from the base steel plate surface can be 0.5 GPa or more.

[0181] The preferred range of the standard deviation σ of the nanohardness of the plate surface at 1 / 2 position of the plate thickness direction depth of the surface soft layer from the base steel plate surface is 2.1GPa or less. The standard deviation σ of the nanohardness of the plate surface at 1 / 2 position of the plate thickness direction depth of the surface soft layer from the base steel plate surface is more preferably 1.7GPa or less. The lower limit is not particularly limited, and the standard deviation σ of the nanohardness of the plate surface at 1 / 2 position of the plate thickness direction depth of the surface soft layer from the base steel plate surface can be 0.6GPa or more.

[0182] Here, the nanohardness of the plate surface at the 1 / 4 position and the 1 / 2 position in the plate thickness direction refers to the hardness measured by the following method.

[0183] First, if a coating is formed, the coating is peeled off. Thereafter, mechanical grinding is performed from the surface of the base steel plate to 1 / 4 position - 5 μm of the depth in the thickness direction of the surface soft layer, polishing grinding is performed from the surface of the base steel plate with diamond and alumina to 1 / 4 position of the depth in the thickness direction of the surface soft layer, and further colloidal silica grinding is performed. Hysitron's tribo-950 is used, and a Berkovich-shaped diamond indenter is used to measure the nanohardness under the conditions of load: 500 μN, measurement area: 50 μm×50 μm, and dot interval: 2 μm.

[0184] In addition, mechanical grinding was performed until the depth of the surface soft layer in the thickness direction was 1 / 2 position, polishing was performed with diamond and alumina, and colloidal silica grinding was further performed. Then, the nanohardness was measured using Hysitron's tribo-950 with a Bosch-shaped diamond indenter under the conditions of load: 500 μN, measurement area: 50 μm×50 μm, and dot interval: 2 μm.

[0185] The nanohardness was measured at 300 or more points at 1 / 4 of the depth in the plate thickness direction, and also at 300 or more points at 1 / 2 of the depth in the plate thickness direction.

[0186] For example, when the thickness of the surface soft layer is 100 μm, the 1 / 4 position is 25 μm from the surface of the surface soft layer, and the 1 / 2 position is 50 μm from the surface of the surface soft layer. More than 300 nanohardness points are measured at the 25 μm position, and more than 300 nanohardness points are also measured at the 50 μm position.

[0187] The surface unevenness depth of the test piece after 90° V bending processing is 20.0μm or less when R / t, which is obtained by dividing the limit bending radius R by the plate thickness t, is 4.5 to 5.0

[0188] In order to further improve the SFmax that is a feature of the present invention, it is effective to control the concavity and convexity of the steel plate surface. That is, the evaluation method of the concavity and convexity of the steel plate surface is as follows. Since the concave part of the concavity and convexity of the steel plate surface is easy to become the starting point of bending cracks, when the surface concavity and convexity depth of the test piece after 90°V bending processing with R / t of 4.5 to 5.0 obtained by dividing the limit bending radius R by the plate thickness t exceeds 20.0μm, the required R / t and SFmax under the specified conditions may not be obtained. Here, the metal plating layer (the first plating layer (the plating layer formed by the plating treatment in the first plating step (metal plating step)) mainly having Fe or Ni contains the internal oxide existing in the outermost layer, and the surface concavity and convexity depth of the test piece after 90°V bending processing with R / t of 4.5 to 5.0 obtained by dividing the limit bending radius R by the plate thickness t is reduced, and better R / t and SFmax can be obtained. The surface concavity and convexity depth is preferably less than 12.0μm, and more preferably less than 9.0μm. In addition, the lower limit is not particularly limited, and may be 0.1 μm or more, or 0.3 μm or more.

[0189] It should be noted that the surface concave-convex depth of the curved cross section is obtained as follows: Figure 1 As shown, 1500 times SEM images of the curved cross section of 5 viewing fields were taken, and reference lines were drawn at the maximum height position of the surface convex part and the maximum depth position of the concave part of the microcrack part in the horizontal direction of the photo within the range of 83μm, and the shortest distance between them was calculated, and the average value of the SEM images of the 5 viewing fields was calculated. The average value of the shortest distance calculated in this way was used as the surface concave-convex depth.

[0190] Here, the above-mentioned evaluation conditions for evaluating the surface irregularity depth are different from the conditions for measurement based on JIS Z2248 when evaluating the bendability, that is, the evaluation criteria for judging the presence or absence of cracks after bending.

[0191] The total area ratio of ferrite and bainite in the surface soft layer: 20% or more, and (the area ratio of martensite in the surface soft layer) / (the total area ratio of martensite and tempered martensite in the surface soft layer): 0.45 or less

[0192] When a surface soft layer exists, the starting point for the generation or connection of voids and the development of cracks during press forming and collision is the boundary between ferrite and bainite as soft phases and martensite and tempered martensite as hard phases in the above-mentioned surface soft layer.

[0193] If the total area ratio of ferrite and bainite present in the surface soft layer is increased, and the value obtained by dividing the area ratio of martensite present in the surface soft layer by the total area ratio of martensite and tempered martensite present in the surface soft layer is made smaller, cracks during press forming and collision can be suppressed, and excellent R / t and SFmax can be obtained.

[0194] When the total area ratio of ferrite and bainite in the surface soft layer is less than 20%, and / or the value obtained by dividing the area ratio of martensite in the surface soft layer by the total area ratio of martensite and tempered martensite in the surface soft layer exceeds 0.45, the generation or connection of voids during the above-mentioned press forming and collision and the progress of cracks may not be suppressed, and the required R / t and SFmax may not be obtained. Therefore, the total area ratio of ferrite and bainite in the surface soft layer is preferably 20% or more, and the value obtained by dividing the area ratio of martensite in the surface soft layer by the total area ratio of martensite and tempered martensite in the surface soft layer is preferably 0.45 or less. More preferably, it is 0.40 or less.

[0195] In addition, the lower limit of the value obtained by dividing the area ratio of martensite present in the surface soft layer by the total area ratio of martensite and tempered martensite present in the surface soft layer is not particularly limited, and may be 0.00. The upper limit of the total area ratio of ferrite and bainite present in the surface soft layer is not particularly limited, and may be 100%.

[0196] Steel structure at 1 / 4 of plate thickness

[0197] The area ratio of martensite is preferably 50.0% or less.

[0198] If the area ratio of martensite increases excessively, it becomes the starting point of void generation during the hole expansion process of the hole expansion test or the bending process of the V bending test, so the required λ and R / t may not be obtained. Therefore, the area ratio of martensite is preferably 50.0% or less. In addition, the area ratio of martensite is more preferably 45.0% or less. It should be noted that the lower limit of the area ratio of martensite is not particularly limited and can be 0.0%. The martensite mentioned here refers to martensite in the quenched state (not tempered).

[0199] The volume fraction of retained austenite is preferably 20.0% or less.

[0200] If the volume fraction of retained austenite increases excessively, hard martensite generated by the work-induced transformation of retained austenite will be generated when the steel sheet is punched in the hole expansion test and when the steel sheet is V-bending in the V-bending + orthogonal VDA test, and voids will be generated and cracks will be accelerated in the subsequent test, and the desired λ and SFmax may not be obtained. Therefore, it is preferable to make the volume fraction of retained austenite 20.0% or less.

[0201] In addition, since tempered martensite is a metal phase that can impart strength and workability to the steel sheet to which the present invention is directed, the area ratio of tempered martensite may be appropriately set to 100% or less.

[0202] The remaining structure other than martensite, retained austenite, and tempered martensite is not particularly limited, and examples thereof include ferrite, unrecrystallized ferrite, pearlite, bainite, and ε martensite.

[0203] In addition, the type of the remaining partial structure can be confirmed by, for example, SEM observation.

[0204] Here, the area ratios of ferrite, bainite, tempered martensite, and hard second phase (martensite+retained austenite) are measured as follows at a position of 1 / 4 of the plate thickness of the base steel plate.

[0205] That is, the sample is cut in such a way that the plate thickness section (L section) parallel to the rolling direction of the steel plate becomes the observation surface. Then, the observation surface of the sample is ground with diamond paste, and then fine grinding is performed using aluminum oxide. Next, the observation surface of the sample is etched with a 3 vol.% nitric acid alcohol solution to make the structure appear. Next, the 1 / 4 position of the plate thickness of the base steel plate is used as the observation position, and 5 fields of view are observed using SEM at a magnification of 3000 times. Based on the obtained organizational image, Adobe Photoshop from Adobe Systems is used to calculate the area ratio of each constituent organization (ferrite, bainite, tempered martensite and hard second phase (martensite + retained austenite)) divided by the measured area for 5 fields of view, and their values ​​are averaged as the area ratio of each organization.

[0206] Ferrite: This is a black area with a massive shape. In addition, it contains almost no carbides. In addition, independent islands of martensite and independent islands of retained austenite in ferrite grains are not included in the area ratio of ferrite.

[0207] Bainite: A black to dark gray area with a blocky or amorphous shape. In addition, it contains relatively few carbides.

[0208] Tempered martensite: It is a gray area with an amorphous shape and contains a large number of carbides.

[0209] Hard second phase (retained austenite + martensite): white to light gray area, amorphous in shape. In addition, it does not contain carbides.

[0210] Carbides: White areas in the form of dots or lines, surrounded by bainite and tempered martensite.

[0211] Remaining structure: In addition to the above-mentioned ferrite and bainite, pearlite, cementite, unrecrystallized ferrite, ε martensite and the like can be mentioned, and their morphologies and the like are well known.

[0212] In addition, the volume ratio of retained austenite was measured as follows.

[0213] That is, after the base steel plate is mechanically ground to 1 / 4 of the plate thickness in the plate thickness direction (depth direction), it is chemically polished with oxalic acid to serve as the observation surface. Next, the observation surface is observed using the X-ray diffraction method. MoKα rays are used as incident X-rays to obtain the ratio of the diffraction intensity of the (200), (220) and (311) surfaces of fcc iron (austenite) to the diffraction intensity of the (200), (211) and (220) surfaces of bcc iron. The volume fraction of retained austenite is calculated from the ratio of the diffraction intensity of each surface. Then, the retained austenite is regarded as homogeneous in three dimensions, and the volume fraction of retained austenite is taken as the area fraction of retained austenite.

[0214] The area ratio of martensite is obtained by subtracting the area ratio of retained austenite from the area ratio of the hard second phase obtained as described above.

[0215] [Area ratio of martensite (%)] = [Area ratio of hard second phase (%)] - [Area ratio of retained austenite (%)]

[0216] The area ratio of the remaining structure is obtained by subtracting the area ratio of ferrite, the area ratio of bainite, the area ratio of tempered martensite, and the area ratio of the hard second phase obtained as described above from 100.0%.

[0217] [Area ratio of the remaining structure (%)] = 100.0 - [Area ratio of ferrite (%)] - [Area ratio of bainite (%)] - [Area ratio of tempered martensite (%)] - [Area ratio of the hard second phase (%)]

[0218] The microstructures (ferrite, bainite, martensite, tempered martensite) present in the surface soft layer are measured in the same manner as the microstructures at the 1 / 4 position of the thickness of the base steel plate, except that the observation position is changed to the 1 / 4 position of the depth in the thickness direction of the surface soft layer instead of the 1 / 4 position of the thickness of the base steel plate.

[0219] Next, the mechanical characteristics of the steel sheet according to one embodiment of the present invention will be described.

[0220] Tensile strength (TS): 590MPa or more

[0221] The tensile strength TS of the steel sheet according to one embodiment of the present invention is 590 MPa or more.

[0222] It should be noted that the yield stress (YS), total elongation (El), limiting hole expansion ratio (λ), limiting bending radius / plate thickness (R / t), stroke (SFmax) at maximum load in V bending + orthogonal VDA bending test, and presence or absence of fracture (appearance crack) in the axial crush test of the steel plate according to one embodiment of the present invention are as described above.

[0223] In addition, the tensile strength (TS), yield stress (YS) and total elongation (El) are measured by a tensile test based on JIS Z 2241 described later in the examples. The limiting hole expansion ratio (λ) is measured by a hole expansion test based on JIS Z 2256 described later in the examples. The limiting bending radius / plate thickness (R / t) is measured by a V-bending test based on JIS Z 2248 described later in the examples. The stroke (SFmax) at the maximum load in the V-bending + orthogonal VDA bending test is measured by the V-bending + orthogonal VDA bending test described later in the examples. The presence or absence of fracture (appearance crack) in the axial crushing test is measured by the axial crushing test described later in the examples.

[0224] First coating

[0225] The steel sheet according to one embodiment of the present invention preferably has a metal coating (first coating, pre-coating) on ​​one or both surfaces of the base steel sheet (it should be noted that the metal coating (first coating) does not include a hot-dip galvanized layer, an alloyed hot-dip galvanized layer, an electrogalvanized layer, or a hot-dip aluminum layer). The metal coating is preferably a metal electroplated layer, and the metal electroplated layer is used as an example for explanation below.

[0226] By forming a metal plating layer on the surface of the steel sheet, the metal plating layer on the outermost surface helps to suppress the occurrence of bending cracks during press forming and vehicle body collision, thereby further improving the bending fracture resistance.

[0227] The metal type of the metal plating layer can be any one of Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, As, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Os, Ir, Rt, Au, Hg, Ti, Pb, and Bi, and more preferably Fe. Hereinafter, the Fe-based plating layer will be described as an example, and other metal types can also adopt the following conditions for Fe.

[0228] The adhesion of Fe-based electroplating layer is greater than 0g / m2 , preferably 2.0g / m 2 The upper limit of the amount of Fe-based electroplating layer deposited on each single side is not particularly limited. From the perspective of cost, the amount of Fe-based electroplating layer deposited on each single side is preferably 60 g / m 2 The Fe-based electroplating layer preferably has a deposition weight of 50 g / m 2 Below, more preferably 40g / m 2 Below, more preferably 30g / m 2 the following.

[0229] The adhesion amount of the Fe-based electroplated layer is measured as follows. A sample of 10×15 mm in size is taken from the Fe-based electroplated steel plate and embedded in resin as a cross-section embedded sample. A scanning electron microscope (SEM) is used for any three locations of the cross section, with an accelerating voltage of 15 kV, and the thickness of the Fe-based plating layer is observed at a magnification of 2000 to 10000 times, and the average value of the thickness of the three fields of view is multiplied by the density of iron, thereby converting it into the adhesion amount of each single side of the Fe-based plating layer.

[0230] As Fe-based electroplating layer, in addition to pure Fe, alloy plating layers such as Fe-B alloy, Fe-C alloy, Fe-P alloy, Fe-N alloy, Fe-O alloy, Fe-Ni alloy, Fe-Mn alloy, Fe-Mo alloy, Fe-W alloy can also be used. The composition of Fe-based electroplating layer is not particularly limited, and preferably the following composition is composed of: the elements selected from 1 or more than 2 of B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co contain less than 10% by mass, and the remainder is made of Fe and inevitable impurities. By making the amount of elements other than Fe total to less than 10% by mass, the decline in electrolysis efficiency can be prevented, and the Fe-based electroplating layer can be formed at low cost. In the case of Fe-C alloy, the content of C is preferably less than 0.08% by mass.

[0231] Second coating

[0232] The steel plate according to one embodiment of the present invention may have a coating (a second coating such as a zinc coating or an aluminum coating) on ​​the outermost surface of one or both sides of the steel plate, and the coating may be a hot-dip galvanized layer, an alloyed hot-dip galvanized layer, an electro-galvanized layer, a hot-dip aluminum coating, etc.

[0233] The coating of the hot-dip galvanized steel sheet with a hot-dip galvanized layer formed on the surface of the steel sheet, the alloyed hot-dip galvanized steel sheet with an alloyed hot-dip galvanized layer formed on the surface of the steel sheet, the electro-galvanized steel sheet with an electro-galvanized layer formed on the surface of the steel sheet, and the plated steel sheet with other metal coatings (aluminum coating, etc.) formed on the surface of the steel sheet can be set only on one surface of the base steel sheet (on the surface of the base steel sheet or on the surface of the metal coating when the metal coating is formed), or on both surfaces.

[0234] That is, the steel sheet of the present invention comprises a base steel sheet on which a second coating (a zinc coating, an aluminum coating, etc.) can be formed, and further comprises a base steel sheet on which a metal coating (a first coating (excluding a second coating such as a zinc coating, an aluminum coating, etc.)) and a second coating (a zinc coating, an aluminum coating, etc.) can be sequentially formed.

[0235] It should be noted that the coating layer of the hot-dip galvanized steel sheet, alloyed hot-dip galvanized steel sheet, and electro-galvanized steel sheet mentioned here refers to a coating layer containing Zn (zinc) as a main component (Zn content is 50.0 mass % or more).

[0236] The plating layer of the aluminum-plated steel sheet refers to a plating layer containing Al (aluminum) as a main component (the Al content is 50.0 mass % or more).

[0237] Here, the hot-dip galvanized layer is preferably composed of Zn, 20.0 mass % or less of Fe, and 0.001 mass % to 1.0 mass % of Al, for example. In addition, the hot-dip galvanized layer may contain 0.0 mass % to 3.5 mass % of one or more elements selected from Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi, and REM. In addition, the Fe content of the hot-dip galvanized layer is more preferably less than 7.0 mass %. It should be noted that the remainder other than the above elements is an inevitable impurity.

[0238] In addition, the alloyed hot-dip galvanized layer is preferably composed of, for example, 20% by mass or less of Fe and 0.001% by mass to 1.0% by mass of Al. In addition, the alloyed hot-dip galvanized layer may arbitrarily contain a total of 0.0% by mass to 3.5% by mass of one or more elements selected from Pb, Sb, Si, Sn, Mg, Mn, Ni, Cr, Co, Ca, Cu, Li, Ti, Be, Bi and REM. The Fe content of the alloyed hot-dip galvanized layer is more preferably 7.0% by mass or more, and further preferably 8.0% by mass or more. In addition, the Fe content of the alloyed hot-dip galvanized layer is more preferably 15.0% by mass or less, and further preferably 12.0% by mass or less. It should be noted that the remainder other than the above-mentioned elements is an unavoidable impurity.

[0239] The coating weight per single side of the zinc plating layer is not particularly limited, but is preferably 20 g / m2 In addition, the coating weight per single side of the zinc plating layer is preferably 80 g / m 2 the following.

[0240] The coating weight of the zinc coating layer of the hot-dip galvanized steel sheet and the alloyed hot-dip galvanized steel sheet was measured as follows.

[0241] That is, a treatment solution is prepared by adding 0.6 g of a corrosion inhibitor for Fe ("Ibit 700BK" (registered trademark) manufactured by Asahi Chemical Industry Co., Ltd.) to 1L of a 10 mass % hydrochloric acid aqueous solution. Next, a hot-dip galvanized steel sheet, which is a test material, is immersed in the treatment solution to dissolve the galvanized layer. Then, the mass reduction of the test material before and after dissolution is measured, and the value is divided by the surface area of ​​the base steel sheet (the surface area of ​​the portion covered by the plating), thereby calculating the plating adhesion amount (g / m 2 ).

[0242] It should be noted that the plate thickness of the steel plate according to one embodiment of the present invention is not particularly limited, but is preferably 0.5 mm or more. In addition, the plate thickness is preferably 3.5 mm or less. More preferably, the plate thickness is 2.3 mm or less.

[0243] The plate thickness is more preferably 0.8 mm or more. The plate thickness is more preferably 1.0 mm or more. The plate thickness is still more preferably 1.2 mm or more.

[0244] [2. Method for manufacturing steel plate]

[0245] Next, a method for producing a steel sheet according to an embodiment of the present invention will be described.

[0246] The method for manufacturing a steel plate of the present invention comprises the following steps: a hot rolling step of hot rolling a steel slab having the above-mentioned component composition; an annealing step of annealing the obtained steel plate under the conditions of an annealing temperature of Ac1 point to 950°C, an annealing time of 10 seconds or more, and an atmosphere with a dew point of -30°C or more; a first cooling step of cooling the obtained steel plate in a temperature range from Ac1 point to 450°C and an atmosphere with a dew point of -30°C or less at an average cooling rate of 8°C / second or more after the annealing step; and a second cooling step of cooling the obtained steel plate in a temperature range from less than 450°C to 300°C at an average cooling rate of less than 8°C / second after the first cooling step.

[0247] In the present invention, the melting method of the steel billet (steel slab) is not particularly limited, and any known melting method such as a converter or an electric furnace is suitable. In addition, in order to prevent macrosegregation, it is preferred to manufacture the steel billet (slab) by a continuous casting method, but it can also be manufactured by an ingot casting method, a thin slab casting method, etc. In addition, in addition to the existing method of temporarily cooling the steel billet to room temperature after manufacturing and then heating it again, it is also possible to use energy-saving processes such as direct rolling or direct rolling without cooling to room temperature, or rolling immediately after a slight heat preservation.

[0248] (Hot rolling process)

[0249] When the slab is heated, the slab heating temperature is preferably 1100°C or higher from the viewpoint of melting of carbides, reduction of rolling load, and improvement of uniformity of formation of the surface soft layer which is a feature of the present invention. In addition, in order to prevent an increase in oxide scale loss, the slab heating temperature is preferably 1300°C or lower. By setting the slab heating temperature to 1300°C or lower, the excessive increase in formation of the surface soft layer which is a feature of the present invention can be suppressed, and the strength which is a feature of the present invention can be stably obtained.

[0250] It should be noted that the slab heating temperature is the temperature of the slab surface. In addition, the slab is made into a thin slab by rough rolling under normal conditions, but when the heating temperature is lowered, it is preferred to heat the thin slab using a strip heater or the like before finish rolling from the viewpoint of preventing failure during hot rolling.

[0251] The rolling load increases, the reduction rate in the non-recrystallized state of austenite increases, and the abnormal structure that elongates in the rolling direction develops, which may result in a decrease in the ductility, hole expansion, and bendability of the final product. Therefore, the finish rolling temperature is preferably 820°C or higher. In addition, since the ductility, hole expansion, and bendability of the final product decrease, the coiling temperature after hot rolling is preferably 300°C or higher. In addition, the coiling temperature is preferably 700°C or lower.

[0252] In addition, when hot-rolling and coiling, from the viewpoint of improving the uniformity of the formation of the surface soft layer which is a feature of the present invention, it is preferred that the coiling temperature is 400°C or more. In addition, the coiling temperature is preferably 650°C or less. When the coiling temperature is lower than 400°C, it is sometimes difficult to stably form the surface soft layer within the range specified in the present invention. In addition, when the coiling temperature exceeds 650°C, the formation of the surface soft layer which is a feature of the present invention increases excessively, and it is sometimes difficult to stably obtain the strength which is a feature of the present invention. Therefore, it is more preferred that the coiling temperature is 400°C or more. In addition, the coiling temperature is preferably 650°C or less.

[0253] It should be noted that during hot rolling, the rough rolled sheets can be joined to each other for continuous finishing rolling. In addition, the rough rolled sheets can be temporarily coiled. In addition, in order to reduce the rolling load during hot rolling, part or all of the finishing rolling can be lubricated rolling. From the perspective of uniformity of the shape of the steel plate and uniformity of the material, lubricated rolling is also effective. It should be noted that the friction coefficient during lubricated rolling is preferably 0.10 or more. In addition, the friction coefficient during lubricated rolling is preferably 0.25 or less.

[0254] (Pickling process)

[0255] The hot-rolled steel sheet thus produced may be pickled. Pickling can remove oxides on the surface of the steel sheet, and thus can be performed to ensure good chemical conversion treatability and plating quality in the high-strength steel sheet of the final product. In addition, pickling can be performed once or in multiple times.

[0256] (Cold rolling process)

[0257] The pickled plate or hot rolled steel sheet obtained after hot rolling as described above is subjected to cold rolling as required. When cold rolling is performed, the pickled plate after hot rolling can be directly subjected to cold rolling, or can be subjected to cold rolling after heat treatment. In addition, the cold rolled steel sheet obtained after cold rolling can be pickled arbitrarily.

[0258] The cold rolling is performed by multi-pass rolling requiring two or more passes, such as tandem multi-stand rolling or reverse rolling.

[0259] Cold rolling reduction rate: 20% to 80%

[0260] When cold rolling is performed, the cold rolling reduction ratio (cumulative reduction ratio) is not particularly limited, but is preferably 20% or more. In addition, the cold rolling reduction ratio is preferably 80% or less. When the cold rolling reduction ratio is less than 20%, the steel structure is likely to become coarse and non-uniform during the annealing process, and the TS or bendability in the final product may decrease. On the other hand, if the cold rolling reduction ratio exceeds 80%, the shape of the steel sheet is likely to be poor, and the amount of coating such as galvanizing may become uneven.

[0261] (Metal plating (metal electroplating, first plating) step)

[0262] One embodiment of the present invention may include a first plating step of plating one or both surfaces of a steel sheet after a hot rolling step (after a cold rolling step in the case of cold rolling) and before an annealing step to form a first plating layer.

[0263] For example, a metal plating treatment such as a metal plating treatment (first plating treatment) can be implemented on the surface of the cold-rolled steel sheet obtained as described above, so as to form a metal-plated steel sheet before annealing having a metal plating layer (first plating layer) before annealing formed on at least one side. It should be noted that the metal plating mentioned here does not include a second plating such as zinc plating or aluminum plating. The metal plating treatment method is not particularly limited. As the metal plating layer formed on the base steel sheet as described above, it is preferably a metal plating layer, so it is preferably implemented. For example, the Fe-based electroplating bath can be a sulfuric acid bath, a hydrochloric acid bath or a mixture of the two. In addition, the adhesion amount of the metal plating layer before annealing can be adjusted by power-on time, etc. It should be noted that the metal-plated steel sheet before annealing refers to a metal plating layer that has not undergone an annealing process, and does not exclude the method of annealing the hot-rolled steel sheet before the metal plating treatment, the pickling plate after hot rolling or the cold-rolled steel sheet in advance.

[0264] Here, the metal type of the electroplating layer can be any one of Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, As, Ru, Rh, Pd, Ag, Cd, In, Sn, Sb, Os, Ir, Rt, Au, Hg, Ti, Pb, and Bi, and Fe is more preferred. Therefore, the manufacturing method of Fe-based electroplating is described below.

[0265] The Fe ion content in the Fe-based electroplating bath before power on is expressed as Fe 2+ If the Fe ion content in the Fe-based electroplating bath is Fe 2+ A sufficient Fe deposition amount can be obtained when the Fe deposition amount is 0.5 mol / L or more. In order to obtain a sufficient Fe deposition amount, the Fe ion content in the Fe-based electroplating bath before the start of energization is preferably 2.0 mol / L or less.

[0266] In addition, the Fe-based electroplating bath may contain Fe ions and at least one element selected from B, C, P, N, O, Ni, Mn, Mo, Zn, W, Pb, Sn, Cr, V and Co. The total content of these elements in the Fe-based electroplating bath is preferably such that the total content of these elements in the Fe-based electroplating layer before annealing is 10% by mass or less. It should be noted that the metal element may be contained in the form of metal ions, and the non-metallic element may be contained in the form of part of boric acid, phosphoric acid, nitric acid, organic acid, etc. In addition, the iron sulfate plating solution may contain conductivity aids such as sodium sulfate and potassium sulfate, chelating agents, and pH buffers.

[0267] Other conditions of the Fe-based electroplating bath are not particularly limited. From the perspective of constant temperature retention, the temperature of the Fe-based electroplating solution is preferably above 30°C and preferably below 85°C. The pH of the Fe-based electroplating bath is also not particularly specified. From the perspective of preventing the decrease in current efficiency caused by hydrogen generation, it is preferably above 1.0. In addition, from the perspective of the conductivity of the Fe-based electroplating bath, it is preferably below 3.0. From the perspective of productivity, the current density is preferably 10A / dm 2 From the viewpoint of easy control of the adhesion amount of the Fe-based electroplating layer, 150 A / dm 2 From the viewpoint of productivity, the sheet passing speed is preferably 5 mpm or more, and from the viewpoint of stably controlling the amount of adhesion, it is preferably 150 mpm or less.

[0268] It should be noted that as a treatment before the Fe-based electroplating treatment, a degreasing treatment and water washing for cleaning the surface of the steel plate, and a pickling treatment and water washing for activating the surface of the steel plate can be implemented. The Fe-based electroplating treatment can be implemented following these pretreatments. The methods of degreasing and water washing are not particularly limited, and the usual methods can be used. In the pickling treatment, various acids such as sulfuric acid, hydrochloric acid, nitric acid and mixtures thereof can be used. Among them, sulfuric acid, hydrochloric acid or a mixture thereof is preferred. The concentration of the acid is not particularly specified, and is preferably 1 to 20 mass% in consideration of the ability to remove the oxide film and prevent the surface roughness (surface defects) caused by over-pickling. In addition, the pickling treatment solution may contain a defoaming agent, a pickling accelerator, a pickling inhibitor, and the like.

[0269] (Annealing process)

[0270] In one embodiment of the present invention, an annealing process is included: after the hot rolling process (after the cold rolling process when cold rolling is performed, after the first plating process when the first plating treatment to form the first plating layer is performed), the steel sheet is annealed under the conditions of an annealing temperature: Ac1 point ~ 950°C, an annealing time: more than 10 seconds, and a dew point: an atmosphere of more than -30°C.

[0271] Annealing temperature: Ac1 point (℃) ~ 950℃

[0272] When the annealing temperature is lower than the Ac1 point (°C), the proportion of austenite generated during annealing is insufficient. Therefore, the area ratio of ferrite at the 1 / 4 position of the plate thickness after annealing increases excessively, and the required TS and YS cannot be obtained. On the other hand, if the annealing temperature exceeds 950°C, it is difficult to form a surface soft layer because it is an austenite single phase region. Therefore, the annealing temperature is set to Ac1 point (°C) to 950°C. The annealing temperature is preferably above Ac1 point + 10°C. In addition, it is preferably below 900°C. More preferably below 840°C. It should be noted that the annealing temperature is the highest temperature reached in the annealing process.

[0273] Annealing time: more than 10 seconds

[0274] If the annealing time is less than 10 seconds, it is difficult to form a soft surface layer. Therefore, the annealing time is set to be more than 10 seconds. It should be noted that the upper limit of the annealing time is not particularly limited, and is preferably less than 900 seconds. It should be noted that the annealing time refers to the holding time in the temperature range of (annealing temperature - 30°C) to annealing temperature. That is, the annealing time includes the residence time in the temperature range of (annealing temperature - 30°C) to annealing temperature during heating and cooling before and after reaching the annealing temperature, in addition to the holding time at the annealing temperature.

[0275] The number of annealing times may be two or more, but is preferably one time from the viewpoint of energy efficiency.

[0276] Dew point of annealing atmosphere (annealing atmosphere): -30°C or above

[0277] The dew point of the atmosphere (annealing atmosphere) in the annealing process must be above -30°C. By making the dew point of the annealing atmosphere in the annealing process above -30°C, the decarbonization reaction can be promoted to form a deeper surface soft layer. Thus, when the nanohardness of more than 300 points is measured in the 50μm×50μm area of ​​the plate surface at a position of 1 / 4 of the depth in the thickness direction of the surface soft layer from the surface of the base steel plate, the proportion of nanohardness of more than 7.0GPa reaches less than 0.10. The annealing atmosphere of the annealing process is preferably above -15°C, more preferably above -5°C. The upper limit of the dew point of the annealing atmosphere of the annealing process is not particularly limited. In order to properly prevent the oxidation of the surface of the Fe-based electroplating layer and make the coating adhesion when the galvanized layer is set good, the dew point of the annealing atmosphere of the annealing process is preferably below 30°C.

[0278] (First Cooling Step)

[0279] In the temperature range from point Ac1 to 450°C, dew point: -30°C or less, and average cooling rate (first average cooling rate): 8°C / sec or more

[0280] In the present invention, by increasing the area ratio of ferrite at the 1 / 4 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate and the 1 / 2 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate, the standard deviation σ of the nanohardness of the plate surface at the 1 / 4 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate becomes less than 1.8 GPa, and the standard deviation σ of the nanohardness of the plate surface at the 1 / 2 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate becomes less than 2.2 GPa.

[0281] In this case, if the average cooling rate in the temperature range from the Ac1 point to 450°C in the first cooling step after the annealing step is lower than 8°C / sec, the nanohardness cannot be adjusted to the above range. Therefore, in the present invention, in the first cooling step after the annealing step, the average cooling rate in the temperature range from the Ac1 point to 450°C is set to 8°C / sec or more.

[0282] In addition, the cooling in the temperature range from the Ac1 point to 450°C must also be performed under the condition of an atmosphere with a dew point of -30°C or less. When the dew point exceeds -30°C, the surface soft layer on the surface of the steel plate is unevenly formed in the steel plate surface, so it is easy to fail to meet the standard deviation σ of the nanohardness of the plate surface at a position of 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate specified in the present invention, which is 1.8 GPa or less, and the standard deviation σ of the nanohardness of the plate surface at a position of 1 / 2 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 2.2 GPa or less. It should be noted that the lower limit of the dew point is not particularly limited, and is preferably above -55°C in consideration of equipment limitations. It should be noted that the cooling in the temperature range from the Ac1 point to 450°C is preferably performed under the condition of an atmosphere with a dew point of -32°C or less.

[0283] In addition, here, the first average cooling rate (° C. / second) can be calculated by cooling start temperature (Ac1 point) in the first cooling step-cooling end temperature (450° C.) / cooling time (seconds).

[0284] In addition, the Ac1 point (°C) can be calculated by the following formula.

[0285] Ac1 point (℃) = 727.0 - 32.7 × [% C] + 14.9 × [% Si] + 2.0 × [% Mn]

[0286] Here, [%C]: C content, [%Si]: Si content, and [%Mn]: Mn content.

[0287] (Second Cooling Step)

[0288] Average cooling rate in the temperature range from less than 450°C to 300°C (second average cooling rate): less than 8°C / sec

[0289] In the present invention, by reducing the area ratio of the hard phase of martensite or retained austenite at the 1 / 4 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate and the 1 / 2 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate, the standard deviation σ of the nanohardness of the plate surface at the 1 / 4 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate becomes less than 1.8 GPa, and the standard deviation σ of the nanohardness of the plate surface at the 1 / 2 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate becomes less than 2.2 GPa.

[0290] In this case, in the second cooling step after the annealing step, if the average cooling rate in the temperature range from less than 450°C to 300°C is 8°C / second or more, the nanohardness cannot be adjusted to the above range. Therefore, in the present invention, in the second cooling step after the annealing step, the average cooling rate in the temperature range from less than 450°C to 300°C is less than 8°C / second.

[0291] In addition, here, the second average cooling rate (° C. / second) can be calculated by cooling start temperature (lower than 450° C.) in the second cooling step - cooling end temperature (300° C.) / cooling time (seconds).

[0292] (Plating step (second plating step))

[0293] One embodiment of the present invention may include a second plating step of plating the steel sheet after the second cooling step to form a second plating layer.

[0294] The plating step (second plating step) is preferably a galvanizing step or a hot-dip aluminum plating treatment. Examples of the galvanizing treatment in the galvanizing step include hot-dip galvanizing treatment, alloy galvanizing treatment, and electrogalvanizing treatment.

[0295] In the case of hot-dip galvanizing, after immersing the steel sheet in a galvanizing bath at 440°C or higher, it is preferred to adjust the coating adhesion by gas wiping or the like. In the above treatment, it is preferred to immerse the steel sheet in a galvanizing bath at 500°C or lower. There is no particular limitation on the hot-dip galvanizing bath as long as the composition of the galvanized layer can be obtained. For example, it is preferred to use a plating bath having an Al content of 0.10% by mass or more and the remainder consisting of Zn and unavoidable impurities. The Al content is preferably 0.23% by mass or less.

[0296] In addition, in the case of alloying galvanizing treatment, after hot-dip galvanizing treatment is carried out according to the above-mentioned essentials, the steel plate (hot-dip galvanized steel plate) having a hot-dip galvanized layer is preferably heated to an alloying temperature of 450°C or more to carry out alloying treatment. The above-mentioned alloying temperature is preferably below 600°C. When the alloying temperature is lower than 450°C, the Zn-Fe alloying rate slows down and alloying sometimes becomes difficult. On the other hand, if the alloying temperature exceeds 600°C, the untransformed austenite transforms to pearlite, and it is difficult to make TS above 590MPa. It should be noted that the alloying temperature is more preferably above 510°C. In addition, the alloying temperature is more preferably below 570°C.

[0297] In addition, the coating weight of the steel sheet with hot-dip galvanizing layer (hot-dip galvanized steel sheet) (GI) and the steel sheet with alloyed hot-dip galvanizing layer (alloyed hot-dip galvanized steel sheet) (GA) is preferably 20 g / m per single side. 2 In addition, the coating weight per single side of the zinc plating layer is preferably 80 g / m 2 It should be noted that the plating deposition amount can be adjusted by gas wiping or the like.

[0298] In addition, when hot-dip aluminum plating, which is a specific example of other metal plating treatment, is performed, the cold-rolled sheet obtained by the cold-rolled sheet annealing is immersed in an aluminum plating bath at 660° C. or higher, and hot-dip aluminum plating is performed, and then the coating adhesion is adjusted by gas wiping, etc. The aluminum plating bath is preferably 730° C. or lower.

[0299] When the electrogalvanizing treatment is performed, the film thickness is not particularly limited, but preferably 2 μm or more and 15 μm or less.

[0300] (Reheating and holding process)

[0301] After the above-mentioned second cooling process (after the second plating process in the case of implementing the second plating treatment), the obtained steel plate can be cooled to a cooling stop temperature from below 250°C to room temperature in the reheating and holding process as needed. As a result, a part of the untransformed austenite in the surface soft layer is transformed into martensite. In addition, in the reheating and holding process, it can be reheated to a reheating temperature range from (cooling stop temperature + 50°C) to 450°C, and maintained in the reheating temperature range for more than 10 seconds. As a result, the martensite in the surface soft layer is tempered, the area ratio of the martensite in the surface soft layer is reduced, and the area ratio of the tempered martensite in the surface soft layer is increased. In addition, the steel structure at the 1 / 4 position of the plate thickness of the base steel plate is also tempered by reheating and holding, and YS and λ increase.

[0302] Here, the room temperature is preferably 1° C. or higher. In addition, the room temperature is preferably 50° C. or lower, and the room temperature is more preferably 29° C. or lower.

[0303] As a cooling method after the above-mentioned second cooling step or after the further reheating and holding step, for example, jet cooling, spray cooling, roll cooling, water cooling, air cooling, etc. can be adopted. It should be noted that from the viewpoint of surface oxidation resistance, it is preferably cooled to 250°C or less. The average cooling rate is preferably 1°C / sec to 50°C / sec, for example.

[0304] In addition, the steel plate obtained as described above can be further subjected to temper rolling. If the reduction rate of temper rolling exceeds 2.00%, the yield stress increases, and the dimensional accuracy when the steel plate is formed into a component may decrease. Therefore, the reduction rate of temper rolling is preferably less than 2.00%. It should be noted that the lower limit of the reduction rate of temper rolling is not particularly limited, and from the perspective of productivity, it is preferably more than 0.05%. In addition, temper rolling is carried out on a device that is continuous with the annealing device used to perform the above-mentioned processes (online), and can also be carried out on a device that is discontinuous with the annealing device used to perform the above-mentioned processes (offline). In addition, the number of temper rolling can be 1 time or more than 2 times. It should be noted that as long as the same elongation as temper rolling can be given, rolling using a straightening machine or the like can be performed.

[0305] The conditions of other manufacturing methods are not particularly limited. From the viewpoint of productivity, the above-mentioned series of treatments such as annealing, hot-dip galvanizing, and galvanized alloying treatment are preferably performed by a hot-dip galvanizing line CGL (Continuous Galvanizing Line). After hot-dip galvanizing, wiping may be performed to adjust the weight per unit area of ​​the coating. It should be noted that the conditions of plating and the like other than the above-mentioned conditions may be in accordance with the conventional method of hot-dip galvanizing.

[0306] [3. Components]

[0307] Next, components according to one embodiment of the present invention will be described.

[0308] The component according to one embodiment of the present invention is a component made of the above-mentioned steel plate (as a blank material). For example, the component is made by subjecting the steel plate as the blank material to at least one of forming processing and joining processing.

[0309] Here, the steel sheet has a TS of 590 MPa or more, and has high YS, excellent press formability (ductility, hole expansion, and bendability), and fracture resistance during collision (axial crushing characteristics). Therefore, the component according to one embodiment of the present invention has high strength, excellent press formability, and excellent impact resistance. Therefore, the component according to one embodiment of the present invention is particularly suitable for use in impact energy absorbing components used in the automotive field.

[0310] [4. Method for manufacturing components]

[0311] Next, a method for manufacturing a component according to one embodiment of the present invention will be described.

[0312] A method for manufacturing a component according to one embodiment of the present invention includes a step of performing at least one of a forming process and a joining process on the above-mentioned steel plate to manufacture the component.

[0313] Here, the molding method is not particularly limited, and for example, general processing methods such as pressing can be used. In addition, the joining method is not particularly limited, and for example, general welding such as spot welding, laser welding, arc welding, riveting, caulking, etc. can be used. It should be noted that the molding conditions and joining conditions are not particularly limited, and conventional methods can be used.

[0314] Example

[0315] Steel billets having the composition shown in Table 1 (the remainder is Fe and inevitable impurities) were melted in a converter and made into steel billets by continuous casting. In Table 1, - indicates the content of the inevitable impurity level.

[0316] The calculated phase transition point Ac1 shown in Table 1 is calculated by the following formula.

[0317] Ac1 point (℃) = 727.0 - 32.7 × [% C] + 14.9 × [% Si] + 2.0 × [% Mn]

[0318] Here, [%C]: C content, [%Si]: Si content, and [%Mn]: Mn content.

[0319] The obtained steel slabs were heated to 1200° C., and after heating, rough rolling and hot rolling were performed on the steel slabs, and the hot rolling coiling temperature was set to 500° C. to produce hot-rolled steel sheets. Next, the obtained hot-rolled steel sheets No. 1 to 96 and No. 107 to 146 were pickled and cold-rolled to produce cold-rolled steel sheets with the thicknesses shown in Tables 2 to 4.

[0320] In addition, the obtained hot-rolled steel sheets No. 97 to 106 were pickled to obtain hot-rolled steel sheets (white skin) having the sheet thickness shown in Table 3. Next, the obtained cold-rolled steel sheets or hot-rolled steel sheets (white skin) were subjected to the treatments in the first plating step (metal plating step), annealing step, first cooling step, second cooling step, and plating step (second plating step) under the conditions shown in Tables 2 to 4 to obtain steel sheets.

[0321] In addition, a part of the steel sheets was not subjected to the treatment in the first plating step (metal plating step) and / or the treatment in the plating step (second plating step).

[0322] In addition, Nos. 107 to 110, 112 to 115, 117 to 120, 122 to 125, and 127 to 142 were subjected to the treatment in the reheating and holding step after the second plating step to obtain steel sheets.

[0323] Here, in the second plating step, a portion of the hot-rolled steel sheet (white skin) or the cold-rolled steel sheet is subjected to hot-dip galvanizing or alloyed galvanizing to obtain a hot-dip galvanized steel sheet (hereinafter also referred to as GI) or an alloyed hot-dip galvanized steel sheet (hereinafter also referred to as GA).

[0324] In addition, a portion of the hot-rolled steel sheet (white skin) or the cold-rolled steel sheet was subjected to electrogalvanizing treatment (bath temperature: room temperature) to obtain a hot-dip electrogalvanized steel sheet (hereinafter, also referred to as EG). In addition, a portion of the hot-rolled steel sheet (white skin) or the cold-rolled steel sheet was subjected to hot-dip aluminum plating treatment (bath temperature: 680° C.) to obtain a hot-dip aluminum-plated steel sheet (hereinafter, also referred to as Al).

[0325] In addition, in Tables 2 to 4, the type of the second plating step is indicated as "GI", "GA", "EG" or "Al". The treated steel sheets that were not subjected to the second plating step are indicated as "CR".

[0326] When manufacturing either GI or GA, the galvanizing bath temperature is 460°C.

[0327] When manufacturing GI, the galvanizing coating weight is 45 to 75 g / m per side. 2 (Double-sided plating), when manufacturing GA, the zinc coating weight is 40 to 65 g / m per side 2 (Both sides plated).

[0328] It should be noted that in the case of GI, the composition of the galvanized layer of the steel sheet finally obtained contains Fe: 0.1-1.0 mass%, Al: 0.20-0.33 mass%, and the remainder is Zn and inevitable impurities. In addition, in the case of GA, the composition of the galvanized layer of the steel sheet finally obtained contains Fe: 7.0-12.0 mass%, Al: 0.10-0.23 mass%, and the remainder is Zn and inevitable impurities.

[0329] In addition, a hot-dip galvanized layer, an alloyed hot-dip galvanized layer, an electro-galvanized layer and other metal coatings (a hot-dip aluminum coating in the embodiment) are formed on both sides of the base steel plate.

[0330] The obtained steel plate was used to identify the steel structure at the 1 / 4 position of the plate thickness (base steel plate) according to the above-mentioned method. The measurement results are shown in Tables 2 to 4. In Tables 2 to 4, F is ferrite, M is martensite, RA is retained austenite, B is bainite, TM is tempered martensite, P is pearlite, θ is carbide, F' is unrecrystallized ferrite, and εM is ε martensite.

[0331] In addition, regarding Nos. 107 to 146 shown in Table 4, the steel structure in the soft surface layer was identified according to the above-mentioned procedure.

[0332] The underlined parts in the table indicate that they are outside the appropriate range of the present invention.

[0333] In addition, tensile tests, hole expansion tests, V-bend tests, V-bend + orthogonal VDA bend tests and axial crush tests were carried out in accordance with the following procedures, and the tensile strength (TS), yield stress (YS), total elongation (El), ultimate hole expansion ratio (λ), R / t in the V-bend test, the stroke at the maximum load measured in the V-bend + orthogonal VDA bend test (SFmax), and the presence or absence of fracture (appearance cracks) in the axial crush test were evaluated according to the following criteria.

[0334] ·TS

[0335] 0(Qualified): 590MPa or above

[0336] ×(Unqualified): less than 590MPa

[0337] ·YS

[0338] 〇(Qualified):

[0339] (A) 590MPa≤TS<780MPa, 350MPa≤YS

[0340] (B) 780MPa≤TS<980MPa, 400MPa≤YS

[0341] (C) 980MPa≤TS<1180MPa, 550MPa≤YS

[0342] (D) 1180MPa≤TS<1320MPa, 750MPa≤YS

[0343] (E) 1320MPa≤TS<1470MPa, 900MPa≤YS

[0344] (F) 1470MPa≤TS, 1050MPa≤YS

[0345] × (unqualified): 590MPa≤TS<780MPa, 350MPa>YS

[0346] 780MPa≤TS<980MPa, 400MPa>YS

[0347] 980MPa≤TS<1180MPa, 550MPa>YS

[0348] 1180MPa≤TS<1320MPa, 750MPa>YS

[0349] 1320MPa≤TS<1470MPa, 900MPa>YS

[0350] When 1470MPa≤TS, 1050MPa>YS

[0351] ·El

[0352] 〇(Qualified):

[0353] (A) 590MPa≤TS<780MPa, 24.0%≤El

[0354] (B) 780MPa≤TS<980MPa, 18.0%≤El

[0355] (C) 980MPa≤TS<1180MPa, 11.0%≤El

[0356] (D) 1180MPa≤TS<1320MPa, 8.0%≤El

[0357] (E) 1320MPa≤TS<1470MPa, 7.5%≤El

[0358] (F) 1470MPa≤TS, 7.0%≤El

[0359] ×(Unqualified):

[0360] 590MPa≤TS<780MPa, 24.0%>El

[0361] 780MPa≤TS<980MPa, 18.0%>El

[0362] 980MPa≤TS<1180MPa, 11.0%>El1180MPa≤TS<1320MPa, 8.0%>El

[0363] 1320MPa≤TS<1470MPa, 7.5%>El

[0364] 1470MPa≤TS, 7.0%>El

[0365] ·λ

[0366] 0(Qualified): 20% or more

[0367] ×(Unqualified): Less than 20%

[0368] ·R / t

[0369] 〇(Qualified):

[0370] (A) 590MPa≤TS<780MPa, 1.0≥R / t

[0371] (B) 780MPa≤TS<980MPa, 2.0≥R / t

[0372] (C) 980MPa≤TS<1180MPa, 2.5≥R / t

[0373] (D) 1180MPa≤TS<1320MPa, 3.0≥R / t

[0374] (E) 1320MPa≤TS<1470MPa, 3.5≥R / t

[0375] (F) 1470MPa≤TS, 4.0≥R / t

[0376] ×(Unqualified):

[0377] 590MPa≤TS<780MPa, 1.0<R / t

[0378] 780MPa≤TS<980MPa, 2.0<R / t

[0379] 980MPa≤TS<1180MPa, 2.5<R / t

[0380] 1180MPa≤TS<1320MPa, 3.0<R / t

[0381] 1320MPa≤TS<1470MPa, 3.5<R / t

[0382] 1470MPa≤TS, 4.0<R / t

[0383] SFmax

[0384] 〇(passed)

[0385] (A) 590MPa≤TS<780MPa, 29.0mm≤SFmax

[0386] (B) 780MPa≤TS<980MPa, 27.5mm≤SFmax

[0387] (C) 980MPa≤TS<1180MPa, 27.0mm≤SFmax

[0388] (D) 1180MPa≤TS<1320MPa, 26.0mm≤SFmax

[0389] (E) 1320MPa≤TS<1470MPa, 24.5mm≤SFmax

[0390] (F) 1470MPa≤TS, 24.0mm≤SFmax

[0391] ×(Unqualified)

[0392] 590MPa≤TS<780MPa, 29.0mm>SFmax

[0393] 780MPa≤TS<980MPa, 27.5mm>SFmax

[0394] 980MPa≤TS<1180MPa, 27.0mm>SFmax

[0395] 1180MPa≤TS<1320MPa, 26.0mm>SFmax

[0396] 1320MPa≤TS<1470MPa, 24.5mm>SFmax

[0397] 1470MPa≤TS, 24.0mm>SFmax

[0398] · Whether there is axial crush fracture (appearance crack)

[0399] ◎ (Pass): No external cracks were observed in the sample after the axial crushing test.

[0400] ○ (Pass): No more than one crack was observed in the sample after the axial crush test.

[0401] × (failed): Two or more cracks were observed in the sample after the axial crush test

[0402] (1) Tensile test

[0403] The tensile test was conducted in accordance with JIS Z 2241. That is, a JIS No. 5 test piece was taken from the obtained steel plate in such a way that the long side direction was perpendicular to the rolling direction of the base steel plate. Using the taken test piece, a tensile test was conducted at a crosshead speed of 10 mm / min to measure TS, YS and El. The results are collectively noted in Tables 2 to 4.

[0404] (2) Hole expansion test

[0405] The hole expansion test is carried out based on JIS Z 2256. That is, a test piece of 100mm×100mm is taken from the obtained steel plate by shearing. A hole with a diameter of 10mm is punched out of the test piece with a gap of 12.5%. Next, a punch with an inner diameter of 75mm is used to apply a blanking force of 9ton (88.26kN) around the hole. In this state, a conical punch with a top angle of 60° is pressed into the hole to measure the diameter of the hole of the test piece at the cracking limit (when cracking occurs). Then, the limiting hole expansion rate is calculated according to the following formula: λ(%). It should be noted that λ is an indicator for evaluating the tensile flangeability. The results are collectively noted in Tables 2 to 4.

[0406] λ(%)={(D f -D0) / D0}×100

[0407] in,

[0408] D f : Diameter of the hole of the test piece when cracks occurred (mm)

[0409] D0: initial diameter of the hole of the test piece (mm).

[0410] (3) V bending test V (90°)

[0411] The bending test was conducted based on JIS Z 2248.

[0412] A test piece of 100 mm×35 mm was collected from the obtained steel plate by shearing and end grinding, wherein the 100 mm side was parallel to the width (C) direction.

[0413] Bending radius R: varies in 0.5mm steps

[0414] Test method: die support, punch press

[0415] Forming load: 10ton

[0416] Test speed: 30mm / min

[0417] Hold time: 5s

[0418] Bending direction: rolling right angle (C) direction

[0419] The evaluation was performed three times, and R / t was calculated by dividing the minimum bending radius (limit bending radius) R without cracks by the plate thickness t. In addition, using a Leica stereo microscope, cracks with a length of 200 μm or more were judged as cracks at a magnification of 25 times. It should be noted that R / t is an index for evaluating the bendability of press formability. The results are collectively annotated in Tables 2 to 4.

[0420] In addition, a 90° V-bending test was performed with a limit bending radius R divided by the plate thickness t, where R / t was 4.5 to 5.0, and images of 5 viewing fields were taken. Figure 1 The 1500 times SEM image of the curved cross section shown in the figure draws a reference line at the maximum height position of the surface convex part and the maximum depth position of the concave part of the microcrack part in the horizontal direction of the photo within the range of 83μm, and finds the shortest distance between them, and finds the average value of the SEM image of 5 viewing fields. The average value of the shortest distance thus found is evaluated as the surface concave-convex depth.

[0421] (4) V-bend + orthogonal VDA bending test

[0422] The V-bend + orthogonal VDA bend test was performed as follows.

[0423] From the obtained steel plate, a 60 mm × 65 mm test piece is obtained by shearing and end grinding. The 60 mm side is parallel to the rolling (L) direction. The test piece is prepared by bending the width (C) direction as the axis in the rolling (L) direction at a curvature radius / plate thickness: 4.2 (primary bending). In the 90° bending (primary bending), if Figure 2 As shown in (a), a punch B1 is pressed into a steel sheet placed on a die A1 having a V-groove to obtain a test piece T1. Figure 2 As shown in (b), the test piece T1 placed on the support roll A2 is subjected to orthogonal bending (secondary bending) by pressing a punch B2 in such a way that the bending direction becomes a direction perpendicular to the rolling direction. Figure 2 (a) and Figure 2 In (b), D1 represents the width (C) direction, and D2 represents the rolling (L) direction.

[0424] The conditions of the V-bend in the V-bend + orthogonal VDA bend test are as follows.

[0425] Test method: die support, punch press

[0426] Forming load: 10ton

[0427] Test speed: 30mm / min

[0428] Hold time: 5s

[0429] Bending direction: rolling (L) direction

[0430] The conditions of VDA bending in the V bending + orthogonal VDA bending test are as follows.

[0431] Test method: Roller support, punch insertion

[0432] Roller diameter: φ30mm

[0433] Punch tip R: 0.4mm

[0434] Distance between rollers: (plate thickness × 2) + 0.5 mm

[0435] Travel speed: 20mm / min

[0436] Test piece size: 60mm×60mm

[0437] Bending direction: rolling right angle (C) direction

[0438] In the stroke-load curve obtained when performing the above VDA bending, find the stroke at the maximum load. The average value of the stroke at the maximum load when performing the above V bending + orthogonal VDA bending test three times is taken as SFmax (mm). It should be noted that SFmax is an indicator for evaluating the fracture resistance during collision (fracture resistance of the bending ridge in the axial crushing test). The results are collectively noted in Tables 2 to 4.

[0439] (5) Axial crush test

[0440] A 150 mm x 100 mm test piece was taken from the obtained steel plate by shearing. Here, the 150 mm side was parallel to the rolling (L) direction. A die with a punch shoulder radius of 5.0 mm and a die shoulder radius of 5.0 mm was used to perform forming (bending) to a depth of 40 mm to produce Figure 3-1 (a) and Figure 3-1 The hat-shaped component 10 shown in (b) is also cut into a size of 80 mm × 100 mm. Next, the cut steel plate 20 is spot welded to the hat-shaped component 10 to produce a hat-shaped component 10 as shown in (b). Figure 3-1 (a) and Figure 3-1 The test component 30 shown in (b). Figure 3-1 (a) is a front view of a test member 30 produced by spot welding a hat-shaped member 10 and a steel plate 20 . Figure 3-1 (b) is a perspective view of the test component 30. The position of the spot welding portion 40 is as shown in FIG. Figure 3-1 As shown in (b), the distance between the end of the steel plate and the welded portion is 10 mm, and the distance between the welded portions is 20 mm. Figure 3-2 As shown in (c), the test component 30 and the bottom plate 50 are joined by TIG welding to produce a sample for the axial crush test. Next, the collision block 60 is made to collide with the produced sample for the axial crush test at a constant collision speed of 10 mm / min, and the sample for the axial crush test is crushed by 70 mm. Figure 3-2 As shown in (c), the crushing direction D3 is a direction parallel to the longitudinal direction of the test member 30. The results are collectively shown in Tables 2 to 4.

[0441] In the V-bend test, V-bend + orthogonal VDA bend test and axial crushing test of steel plates with a thickness greater than 1.2 mm, all the tests were conducted with steel plates with a thickness of 1.2 mm in consideration of the effect of the plate thickness. Steel plates with a thickness greater than 1.2 mm were ground on one side to a thickness of 1.2 mm.

[0442] Since grinding may affect the bendability of the steel plate surface, the ground surface is made to be the inner side of the bend (valley side) in the V-bending test, and the ground surface is made to be the outer side of the bend (mountain side) in the V-bending test + orthogonal VDA bending test, and the ground surface is made to be the inner side of the bend (valley side) in the subsequent VDA bending test.

[0443] <Nanohardness measurement>

[0444] In order to obtain excellent bendability during press forming and excellent bending fracture characteristics during collision, when measuring the nanohardness of more than 300 points in a 50μm×50μm area of ​​the plate surface at a position of 1 / 4 of the plate thickness depth of the surface soft layer from the surface of the base steel plate, the proportion of the plate surface nanohardness of 7.0GPa or more at a position of 1 / 4 of the plate thickness depth of the surface soft layer from the surface of the base steel plate is less than 0.10 relative to the total number of measurements. When the proportion of the above nanohardness of 7.0GPa or more is less than 0.10, it means that the proportion of hard structures (martensite, etc.), inclusions, etc. is small, and the generation or connection of voids and the progress of cracks in the above hard structures (martensite, etc.), inclusions, etc. during press forming and collision can be further suppressed, and excellent R / t and SFmax can be obtained.

[0445] After the plating is peeled off, the surface of the base steel plate is mechanically ground to the position of 1 / 4-5μm in the thickness direction of the surface soft layer, and the surface of the base steel plate is polished and ground to the position of 1 / 4 in the thickness direction of the surface soft layer with diamond and alumina, and then colloidal silica grinding is implemented. Hysitron's tribo-950 is used, and a diamond indenter of the shape of Bosch is used to measure the nanohardness of a total of 512 points under the conditions of load: 500μN, measurement area: 50μm×50μm, and dot interval: 2μm.

[0446] Next, mechanical grinding was performed to 1 / 2 of the depth in the thickness direction of the surface soft layer, and polishing and colloidal silica grinding were performed using diamond and alumina. Hysitron's tribo-950 was used to measure a total of 512 nanohardness points using a Bosch-shaped diamond indenter under the conditions of load: 500 μN, measurement area: 50 μm×50 μm, and dot interval: 2 μm.

[0447] The method for measuring the surface soft layer is as follows. After smoothing the thickness section (L section) parallel to the rolling direction of the steel plate by wet grinding, based on JIS Z 2244-1 (2020), using a Vickers hardness tester, under a load of 10gf, from a position 1μm from the surface of the steel plate in the thickness direction to a position 100μm in the thickness direction at 1μm intervals. Thereafter, the measurement was performed at 20μm intervals until the center of the thickness. The area where the hardness is reduced to less than 85% compared to the hardness at the 1 / 4 position of the plate thickness is defined as a soft layer (surface soft layer), and the thickness in the plate thickness direction of the area is defined as the thickness of the soft layer.

[0448] [Table 1]

[0449]

[0450] [Table 2]

[0451]

[0452] [Table 3]

[0453]

[0454] [Table 4]

[0455]

[0456] As shown in Tables 2 to 4, in all the inventive examples, the tensile strength (TS), yield stress (YS), total elongation (El), ultimate hole expansion ratio (λ), R / t in the V-bend test, and the stroke at the maximum load (SFmax) measured in the V-bend + orthogonal VDA bending test were all qualified, and no fracture (appearance crack) occurred in the axial crush test.

[0457] On the other hand, in the comparative example, at least one of the tensile strength (TS), yield stress (YS), total elongation (El), limiting hole expansion ratio (λ), R / t in the V-bend test, the stroke at the maximum load measured in the V-bend + orthogonal VDA bending test (SFmax), and the presence or absence of fracture (appearance crack) in the axial crush test is insufficient.

[0458] As described above, it is understood that the steel sheet of the present invention has high strength and excellent press formability and impact resistance.

[0459] In addition, it can be seen that the parts obtained by forming the steel plate of the example of the present invention, the parts obtained by joining, and the parts obtained by forming and joining are high-strength and have excellent press formability and impact resistance like the steel plate of the example of the present invention because the steel plate of the example of the present invention is high-strength and has excellent press formability and impact resistance.

[0460] Industrial Applicability

[0461] According to the present invention, it is possible to manufacture steel sheets and parts having TS: 590 MPa or more, high YS, excellent press formability (ductility, hole expansion and bendability) and fracture resistance during collision (bending fracture characteristics and axial crushing characteristics). In addition, by using the steel sheets and parts obtained by the method of the present invention in, for example, automotive structural parts, it is possible to achieve fuel efficiency improvement by reducing the weight of the vehicle body, and the industrial utilization value is extremely high.

Claims

1. A steel plate, comprising a base steel plate, wherein the base steel plate has the following composition: The present invention contains, by mass%, C: 0.030% to 0.500%, Si: 0.01% to 3.00%, Mn: 0.30% or more and less than 10.00%, P: 0.001% to 0.100%, S: 0.0200% or less, Al: 0.005% to 2.000%, N: 0.0100% or less, Ceq represented by the following formula (1) satisfies 0.30% to 0.85%, and the remainder is composed of Fe and unavoidable impurities. Furthermore, the surface soft layer is formed in a region 200 μm or less from the surface of the base steel plate in the plate thickness direction, and the Vickers hardness of the surface soft layer is 85% or less relative to the Vickers hardness of the base steel plate at a position 1 / 4 of the plate thickness, When the nanohardness of 300 points or more is measured in the 50 μm×50 μm area of ​​the plate surface at the 1 / 4 position and the 1 / 2 position of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate, The ratio of the number of measurements of which the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 7.0 GPa or more is 0.10 or less relative to the total number of measurements, Furthermore, the standard deviation σ of the nanohardness of the plate surface at a position 1 / 4 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 1.8 GPa or less, Furthermore, the standard deviation σ of the nanohardness of the plate surface at a position 1 / 2 of the depth in the plate thickness direction of the surface soft layer from the surface of the base steel plate is 2.2 GPa or less, Ceq=[%C]+[%Mn] / 6+[%Si] / 24+[%Ni] / 40+[%Cr] / 5+[%Mo] / 4+[%V] / 14···Formula (1) Among them, [%C]: C content, [%Mn]: Mn content, [%Si]: Si content, [%Ni]: Ni content, [%Cr]: Cr content, [%Mo]: Mo content, [%V]: V content, and the value is 0 when not contained.

2. The steel plate according to claim 1, wherein: The total area ratio of ferrite and bainite present in the surface soft layer is 20% or more. A value obtained by dividing the area ratio of martensite present in the surface soft layer by the total area ratio of martensite and tempered martensite present in the surface soft layer is 0.45 or less.

3. The steel plate according to claim 1 or 2, wherein: The component composition further contains, in mass%, Nb: 0.200% or less, Ti: 0.200% or less, V: 0.200% or less, B: 0.0100% or less, Cr: 1.000% or less, Ni: 1.000% or less, Mo: 1.000% or less, Sb: 0.200% or less, Sn: 0.200% or less, Cu: 1.000% or less, Ta: 0.100% or less, W: 0.500% or less, Mg: 0.0200% or less, Zn: 0.0200% or less, % or less, Co: 0.0200% or less, Zr: 0.1000% or less, Ca: 0.0200% or less, Se: 0.0200% or less, Te: 0.0200% or less, Ge: 0.0200% or less, As: 0.0500% or less, Sr: 0.0200% or less, Cs: 0.0200% or less, Hf: 0.0200% or less, Pb: 0.0200% or less, Bi: 0.0200% or less, REM: 0.0200% or less.

4. The steel plate according to any one of claims 1 to 3, wherein A metal plating layer is provided as a first plating layer on one or both surfaces of the base steel sheet.

5. The steel plate according to any one of claims 1 to 4, wherein The steel sheet has a metal plating layer as a second plating layer on the outermost layer of one or both surfaces.

6. The steel plate according to any one of claims 1 to 5, wherein The surface irregularities of the test piece after 90° V-bending, where R / t, which is obtained by dividing the limiting bending radius R by the plate thickness t, is 4.5 to 5.0, have a depth of 20.0 μm or less.

7. A component formed using the steel plate according to any one of claims 1 to 6.

8. A method for manufacturing a steel plate, comprising the following steps: A hot rolling step of hot rolling the steel slab having the component composition according to claim 1 or 3, In the annealing step, the obtained steel sheet is annealed under the conditions of annealing temperature: Ac1 point to 950°C, annealing time: 10 seconds or more, and dew point: -30°C or more. A first cooling step, after the annealing step, cooling the obtained steel sheet in a temperature range of Ac1 point to 450°C in an atmosphere with a dew point of -30°C or less at an average cooling rate of 8°C / s or more; and The second cooling step is to cool the obtained steel plate in a temperature range of less than 450° C. to 300° C. at an average cooling rate of less than 8° C. / second after the first cooling step.

9. The method for manufacturing a steel plate according to claim 8, wherein: The method comprises a cold rolling step of cold rolling the steel sheet after the hot rolling step and before the annealing step.

10. The method for manufacturing a steel plate according to claim 8 or 9, wherein: The method comprises a first plating step of performing metal plating on one or both surfaces of the steel sheet after the hot rolling step and before the annealing step to form a first plating layer.

11. The method for producing a steel plate according to any one of claims 8 to 10, wherein: The method includes a second plating step of plating the steel sheet after the second cooling step to form a second plating layer.

12. The method for producing a steel plate according to any one of claims 8 to 11, wherein: The method comprises the following steps: after the second cooling step, cooling the obtained steel plate to a cooling stop temperature of 250°C or less to room temperature, reheating the steel plate to a reheating temperature range of (the cooling stop temperature + 50°C) to 450°C, and maintaining the steel plate in the reheating temperature range for more than 10 seconds.

13. A method for manufacturing a component, comprising the step of subjecting the steel sheet according to any one of claims 1 to 6 to at least one of a forming process and a joining process to produce a component.