Catalytic method for preparing cyclohexanol through hydrodeoxygenation of guaiacol

Pt nanoparticles are prepared by reducing chloroplatinic acid hexahydrate using sodium lignin sulfonate in the aqueous phase. As a catalyst, the problems of high energy consumption for catalyst preparation and harsh reaction conditions are solved, and the efficient and environmentally friendly production of cyclohexanol is achieved. , high catalytic activity and catalyst can be reused.

CN118978424APending Publication Date: 2024-11-19QINGDAO UNIV OF SCI & TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411069117.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, the catalyst preparation consumes high energy, cumbersome process, harsh catalytic reaction conditions, and the use of more chemical reagents, resulting in challenges in the green production of cyclohexanol.

Method used

The aqueous phase dispersed Pt nanoparticles Pt@SLSaq are used to reduce the stable chloroplatinic acid hexahydrate in the aqueous phase, and used as a catalyst to catalyze the hydrodeoxygenation reaction of guaiacin under mild conditions, and prepare Cyclohexanol. This method does not require the addition of reducing agents, stabilizers and organic solvents. The reaction conditions are mild and the catalyst can be reused.

Benefits of technology

It realizes efficient and environmentally friendly production of cyclohexanol, with high catalytic activity and mild reaction conditions, simple and clean catalyst preparation, and the catalyst can be reused, which improves the selectivity and yield of cyclohexanol.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978424A_ABST
    Figure CN118978424A_ABST
Patent Text Reader

Abstract

The invention relates to a green catalysis method for preparing cyclohexanol by hydrodeoxygenation reaction of guaiacol, in particular to a method for preparing cyclohexanol by catalyzing hydrodeoxygenation reaction of guaiacol by adopting one-pot reduction of sodium lignin sulfonate in a water phase and stable Pt nanoparticles, and belongs to the technical field of biomass catalytic conversion. According to the method, the derivatization product sodium lignin sulfonate of the byproduct black liquor in the papermaking industry is used as a reducing agent and a stabilizing agent, chloroplatinic acid is subjected to in-situ reduction in a water phase and generated metal Pt nano particles are stabilized under the condition that no other auxiliary reagents are needed, and a clean water-phase catalytic system is obtained; and the catalyst is directly used for hydrodeoxygenation reaction of guaiacol to prepare cyclohexanol. The method has the characteristics of simple preparation of a catalytic system, high activity, mild reaction conditions and the like, and provides a simple and green new way for preparing cyclohexanol through selective hydrodeoxygenation by taking a lignin platform compound as a raw material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a green catalytic method for preparing cyclohexanol by hydrodeoxygenation of guaiacol, specifically a method for preparing cyclohexanol by catalyzing a selective hydrodeoxygenation reaction of guaiacol using aqueous phase Pt nanoparticles prepared by reduction and stabilization of sodium lignin sulfonate, belonging to the technical field of biomass catalytic conversion. Background Art

[0002] Cyclohexanol is an important precursor of nylon and a key intermediate in organic synthesis. It is widely used in the fields of synthetic compounds, solvents, detergents, analysis and detection, and has received increasing attention in the field of biology. With the development of industry, the demand for cyclohexanol has increased, but the traditional preparation method of fossil resources conflicts with the concept of green chemistry and sustainable development. Therefore, it is of great significance to develop an economical and environmentally friendly biomass-derived catalytic method to replace fossil resources for the preparation of cyclohexanol.

[0003] Guaiacol is one of the major phenolic monomers for lignin depolymerization. Because it contains two types of oxygen-containing functional groups (hydroxyl and methoxy) and three different types of CO bonds (-OH, -OCH3, O-CH3), it is often used as a typical lignin model compound to study the mechanism of hydrodeoxygenation reactions. In recent years, many studies have been devoted to converting guaiacol into important industrial products such as cyclohexane, cyclohexanol, and cyclohexanone. However, these hydrodeoxygenation processes usually have problems such as high temperature, high hydrogen pressure, and low selectivity of target products. Chinese patent [CN114870853B] discloses a method for catalyzing the hydrodeoxygenation of guaiacol to prepare cyclohexanol, using a core-shell catalyst x%-Co@y%-Nb-z%-WOx-MSiO2YSNSs to prepare cyclohexanol in a one-step hydrogenation reaction in decalin, with a maximum yield of 85.72%. However, the preparation steps of the catalyst are complicated, including but not limited to adjusting pH, washing, drying, calcining, high-temperature reduction with hydrogen, etc., and achieving the best yield requires a reaction temperature of 190°C, a reaction time of 150 min, and a hydrogen pressure of 2.0 MPa. Chinese patent [CN115779980A] discloses the application of Ni / CeO2-Rh catalyst in the selective hydrogenation of guaiacol to prepare cyclohexanol. The preparation of the catalyst also involves hydrothermal, washing, drying, calcining, reduction, impregnation, calcination and other steps. At the same time, a reducing agent such as sodium borohydride or high-temperature reduction with hydrogen is used, which is not very environmentally friendly; Chinese patent [CN115254175A] discloses a method for catalyzing the hydrodeoxygenation of guaiacol with a nickel-based bifunctional catalyst. The catalyst needs to be calcined and reduced at high temperature, and the hydrodeoxygenation reaction also needs to be reacted at a high temperature of 160-240°C for 4-8 hours. In general, the preparation process of these precious metal or non-precious transition metal catalysts loaded on various carriers requires chemical reducing agents, stabilizers, or high temperature, hydrogen reduction and other conditions, and the preparation process is complicated and energy-intensive.

[0004] In recent years, people have found that sodium lignin sulfonate (SLS), a water-soluble derivative of lignin, can simultaneously reduce and stabilize some metals in aqueous solution due to its macromolecular stable structure and multiple reducing functional groups. Stable metal nanoparticles can be prepared without adding any other chemical reagents, which not only realizes the reuse of industrial waste, but also provides the possibility for the construction of new environmentally friendly catalytic systems. However, to date, there has been no report in domestic and foreign literature on the method of preparing cyclohexanol by hydrodeoxygenation of guaiacol using a lignin-reduced and stabilized transition metal nanoparticle aqueous system.

[0005] The present invention provides a method for preparing aqueous phase dispersed Pt nanoparticles Pt@SLS by reducing and stabilizing chloroplatinic acid hexahydrate in an aqueous phase using sodium lignin sulfonate. aq The invention discloses a method for preparing cyclohexanol by catalytic hydrodeoxygenation of guaiacol. The method has the characteristics of simple and clean catalyst preparation, high catalytic activity and mild reaction conditions, and has opened up a new and efficient way for the green production of cyclohexanol. Summary of the invention

[0006] The purpose of the present invention is to solve the problems of high energy consumption for catalyst preparation, complicated process, harsh catalytic reaction conditions, and use of a large number of chemical reagents in the prior art of preparing cyclohexanol by using guaiacol as a raw material through a catalytic hydrodeoxygenation process, thereby providing a new environmentally friendly method for efficiently preparing cyclohexanol under mild conditions, which utilizes the structural characteristics of sodium lignin sulfonate, reduces and stabilizes chloroplatinic acid hexahydrate in an aqueous phase in one pot without any external reducing agent, stabilizer and organic solvent, and directly uses the aqueous dispersion system to catalyze the hydrodeoxygenation reaction of guaiacol in a batch reactor.

[0007] The present invention provides the following technical solutions:

[0008] The solution was prepared according to the ratio of 0.6 g sodium lignin sulfonate and 60 mL water per mmol of chloroplatinic acid hexahydrate, and reacted at 80 ° C for 3 h under magnetic stirring at 400 rpm to obtain a stable dark brown translucent aqueous metal Pt nanoparticle catalytic system Pt@SLS. aq .

[0009] A certain amount of guaiacol was added to a stainless steel autoclave lined with polytetrafluoroethylene, and the molar ratio of guaiacol to the Pt substance at the catalyst active center was n. (愈创木酚) / n (Pt) =10~100 ratio is added to the prepared Pt@SLS aqThe aqueous phase catalyst is added with solvent water at a ratio of 6 mL of water per millimole of guaiacol, the kettle is sealed, the air in the kettle is replaced with hydrogen, and the reaction is carried out at 60-100°C for 1-3 hours at an initial H2 pressure of 0.5-1.5 MPa and 400 rpm magnetic stirring. After the reaction is completed, the mixture is extracted with ethyl acetate and the product composition is quantitatively analyzed by gas chromatography. After the aqueous phase catalyst is separated and recovered, it can be directly reused by replenishing it with fresh catalyst of the same concentration to the original catalyst amount.

[0010] Compared with the prior art, the method for preparing cyclohexanol by hydrodeoxygenation of guaiacol catalyzed by aqueous phase reduction of sodium lignin sulfonate and stable metal Pt nanoparticles provided by the present invention has the following characteristics:

[0011] (1) The catalytic method provided by the present invention allows the benzene ring of guaiacol to be preferentially hydrogenated, but cannot completely deoxygenate to produce cyclohexane. Only three products, cyclohexanol, methoxycyclohexane and methoxycyclohexanol, are detected;

[0012] (2) The method provided by the present invention does not require any organic solvents or other chemical reagents during the catalyst preparation stage and the catalytic hydrodeoxygenation reaction stage, and the reaction conditions are mild and environmentally friendly;

[0013] (3) The catalytic guaiacol hydrodeoxygenation method provided by the present invention is a quasi-homogeneous catalysis, which has high catalytic activity and cyclohexanol product selectivity, and its aqueous phase catalyst system can be reused, and the catalytic performance is relatively stable. Specific implementation methods

[0015] The method of the present invention is further described below in conjunction with specific embodiments, but the present invention is not limited thereto.

[0016] [Example 1] Sodium lignin sulfonate reduction-stabilized metal Pt nanoparticle catalyst Pt@SLS aq Preparation

[0017] 0.06 g of sodium lignin sulfonate, 0.1 mmol of chloroplatinic acid hexahydrate and 6 mL of ultrapure water were added to a single-necked flask, and the solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain a sodium lignin sulfonate reduction-stable aqueous metal Pt nanoparticle catalyst Pt@SLS. aq .

[0018] [Example 2]

[0019] 6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aqThe aqueous catalyst and 1 mmol of guaiacol were added, the reactor was sealed, the air was replaced with hydrogen, and the reaction was carried out at 60°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0020] [Example 3]

[0021] 2.4 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 3.6 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0022] [Example 4]

[0023] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0024] [Example 5]

[0025] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 60°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0026] [Example 6]

[0027] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 90°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0028] [Example 7]

[0029] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The reactor was sealed, and the air was replaced with hydrogen. The reaction was carried out at 100 ° C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0030] [Example 8]

[0031] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 0.5 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0032] [Example 9]

[0033] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1.5 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0034] [Example 10]

[0035] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1.5 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0036] [Example 11]

[0037] 0.6 mL of Pt@SLS prepared in Example 1 was added to a stainless steel autoclave lined with polytetrafluoroethylene. aqAqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 3 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0038] [Example 12]

[0039] After the reaction was completed according to the conditions of Example 4, the mixture was extracted with ethyl acetate and the lower aqueous phase was recovered and fresh Pt@SLS of the same concentration was used. aq The catalyst was added to 6 mL and added to a stainless steel autoclave lined with polytetrafluoroethylene, and then 1 mmol of guaiacol was added. After replacing the air with hydrogen, the reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction was completed, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 1.

[0040] Table 1 Pt@SLS aq Catalytic performance of aqueous hydrodeoxygenation of guaiacol

[0041]

[0042] [Comparative Example 1]

[0043] 0.06 g of sodium lignin sulfonate, 0.1 mmol of ruthenium trichloride and 6 mL of ultrapure water were added to a single-necked flask. The resulting solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain an aqueous metal Ru nanoparticle catalyst Ru@SLS. aq .

[0044] 0.6 mL of the Ru@SLS prepared above was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 2.

[0045] [Comparative Example 2]

[0046] 0.06 g of sodium lignin sulfonate, 0.1 mmol of silver nitrate and 6 mL of ultrapure water were added to a single-necked flask. The resulting solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain an aqueous metal Ag nanoparticle catalyst Ag@SLS. aq .

[0047] 0.6 mL of the Ag@SLS prepared above was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 2.

[0048] [Comparative Example 3]

[0049] 0.06 g of sodium lignin sulfonate, 0.1 mmol of sodium chloropalladate and 6 mL of ultrapure water were added to a single-necked flask. The resulting solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain an aqueous metal Pd nanoparticle catalyst Pd@SLS. aq .

[0050] 0.6 mL of the prepared Pd@SLS was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 2.

[0051] [Comparative Example 4]

[0052] 0.06 g of sodium lignin sulfonate, 0.1 mmol of rhodium trichloride hydrate and 6 mL of ultrapure water were added to a single-necked flask. The resulting solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain an aqueous metal Rh nanoparticle catalyst Rh@SLS. aq .

[0053] 0.6 mL of the Rh@SLS prepared above was added to a stainless steel autoclave lined with polytetrafluoroethylene. aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 2.

[0054] [Comparative Example 5]

[0055] 0.06 g of sodium lignin sulfonate, 0.1 mmol of platinum chloride and 6 mL of ultrapure water were added to a single-necked flask. The resulting solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain an aqueous metal Pt nanoparticle catalyst Pt Ⅰ @SLS aq .

[0056] 0.6 mL of the prepared Pt Ⅰ @SLS aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 2.

[0057] [Comparative Example 6]

[0058] 0.06 g of sodium lignin sulfonate, 0.1 mmol of platinum nitrate and 6 mL of ultrapure water were added to a single-necked flask. The resulting solution was heated to 80 °C and stirred at 400 rpm for 3 h to obtain an aqueous metal Pt nanoparticle catalyst Pt Ⅱ @SLS aq .

[0059] 0.6 mL of the prepared Pt Ⅱ @SLS aq Aqueous catalyst and 1 mmol of guaiacol were added, and 5.4 mL of ultrapure water was added. The kettle was sealed, and the air was replaced with hydrogen. The reaction was carried out at 80°C for 1 h under an initial H2 pressure of 1 MPa and magnetic stirring at 400 rpm. After the reaction, the reaction mixture was extracted with ethyl acetate and quantitatively analyzed by gas chromatography. The results are shown in Table 2.

[0060] Table 2 Performance of other aqueous catalysts catalyzing the hydrodeoxygenation of guaiacol in aqueous phase using lignin reduction-stable catalysts

[0061] BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Attached Figure 1 Stable Pt Nanoparticle Catalyst Pt@SLS for the Reduction of Sodium Lignosulfonate aq Typical gas chromatogram of the ethyl acetate extract of the product from the aqueous phase catalytic hydrodeoxygenation of guaiacol.

[0063] Attached Figure 2 Stable Pt Nanoparticle Catalyst Pt@SLS for the Reduction of Sodium Lignosulfonateaq Mass spectrum of methoxycyclohexane, the product of aqueous-catalyzed hydrodeoxygenation of guaiacol.

[0064] Attached Figure 3 Stable Pt Nanoparticle Catalyst Pt@SLS for the Reduction of Sodium Lignosulfonate aq Mass spectrum of cyclohexanol, the target product of aqueous-catalyzed hydrodeoxygenation of guaiacol.

[0065] Attached Figure 4 Stable Pt Nanoparticle Catalyst Pt@SLS for the Reduction of Sodium Lignosulfonate aq Mass spectrum of methoxycyclohexanol, the product of aqueous-catalyzed hydrodeoxygenation of guaiacol.

Claims

1. A method for preparing cyclohexanol by aqueous phase hydrodeoxygenation of guaiacol, characterized in that: The hydrodeoxygenation reaction of guaiacol was directly catalyzed by using a metal Pt catalyst stabilized by aqueous reduction of sodium lignin sulfonate.

2. A method for preparing cyclohexanol by aqueous phase hydrodeoxygenation reaction of guaiacol according to claim 1, characterized in that The catalytic reaction process is as follows: The raw material guaiacol and the metal Pt catalyst stabilized by aqueous reduction of sodium lignin sulfonate were used to n (愈创木酚) / n (Pt) =10 to 100 is added into a stainless steel autoclave, and ultrapure water is added to 6 mL of water per millimole of guaiacol. Under a H2 pressure of 0.5 to 1.5 MPa, the reaction is stirred at 60 to 100°C for 1 to 3 hours. After the reaction is completed, the aqueous phase catalyst can be recovered and recycled.

3. A metal Pt catalyst stabilized by aqueous reduction of sodium lignin sulfonate according to claim 1 or 2, characterized in that: Sodium lignin sulfonate is used as both a reducing agent and a stabilizer, and chloroplatinic acid hexahydrate is used as a metal precursor. No other chemical reagents and organic solvents need to be added, and an aqueous phase dispersed metal Pt catalyst is prepared in an aqueous solution. The specific preparation method is: a solution is prepared in a ratio of 0.6 g sodium lignin sulfonate and 60 mL ultrapure water per millimole of chloroplatinic acid hexahydrate, and the solution is reacted at 80° C. for 3 hours under a magnetic stirring of 400 rpm.

Citation Information