Treatment method and application of iron oxide

By adding Cu, Cu2O or CuCl as additives to the acid solution for leaching reaction with iron oxide, the problem of difficulty in leaching iron in iron oxide is solved, and rapid and complete iron recycling and low-carbon and energy-saving solid waste treatment are achieved.

CN118993159APending Publication Date: 2024-11-22CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310573179.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to effectively leach iron from iron oxides, resulting in high cost of solid waste treatment and difficult to effectively utilize iron.

Method used

Cu, Cu2O or CuCl is added as additives to hydrochloric acid or sulfuric acid solution, and placed in the acid solution with iron oxide for leaching reaction, the molar ratio and liquid-solid ratio are controlled, and stirring and heating treatment is carried out to improve the leaching efficiency of iron.

Benefits of technology

The rapid and effective leaching of iron in iron oxide is achieved, the reaction time and cost is reduced, the iron element is completely recovered, and the reducing agent used is easy to regenerate, the process is low-carbon and energy-saving, and is suitable for bulk solid waste treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004244394910000151
    Figure BDA0004244394910000151
Patent Text Reader

Abstract

The invention provides a treatment method of iron oxide. The treatment method comprises the following steps: S1, providing an additive and an acid solution; the acid solution comprises one or two of a hydrochloric acid solution and a sulfuric acid solution; the additive is prepared from one or more of Cu, Cu2O and CuCl; and S2, iron oxide and the additive are jointly placed in the acid solution for a leaching reaction, and the iron-containing treating fluid is obtained. According to the method, iron in the iron oxide can be quickly and effectively leached, so that separation and recovery of iron elements can be ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to hydrometallurgy and solid waste treatment, and in particular to a method for treating iron oxide and application thereof. Background Art

[0002] Iron oxides are common components in bulk solid wastes in the metallurgical industry. For example, ZnFe2O4 is commonly found in conventional leaching slag from hydrometallurgical zinc smelting and smoke from arc furnaces in steel smelting; Fe2O3 is commonly found in red mud in the alumina production industry. Taking hydrometallurgical zinc smelting as an example, my country produces about 2 million tons of conventional zinc leaching slag each year, of which ZnFe2O4 accounts for about 60%. Since iron oxides in solid wastes are often difficult to use directly, the treatment of iron oxides is of great significance for solid waste reduction and resource recovery.

[0003] At present, solid waste containing iron oxides is mostly treated by pyrometallurgical processes, which convert iron oxides into iron by carbon thermal reduction, and obtain smoke or slag enriched with valuable metals. However, this process consumes a lot of energy, and the iron produced inevitably contains impurities, which makes it difficult to use effectively. The smoke or slag enriched with valuable metals still needs further treatment, making the cost of solid waste treatment extremely high.

[0004] Compared with the pyrometallurgical process, the hydrometallurgical process has the potential to treat iron oxide-containing solid waste under low-carbon and energy-saving conditions. However, due to the stable chemical properties of iron oxides, even under high temperature, high acid and long-term leaching conditions, iron oxides cannot be completely dissolved, making it impossible to effectively leach iron from iron oxides.

[0005] In view of this, it is necessary to provide a method for treating iron oxides and application thereof to solve or at least alleviate the technical defect that the above-mentioned iron element cannot be effectively leached. Summary of the invention

[0006] The main purpose of the present invention is to provide a method for treating iron oxides and application thereof, aiming to solve the technical problem that the above-mentioned iron element cannot be effectively leached.

[0007] To achieve the above object, the present invention provides a method for treating iron oxides, comprising the steps of:

[0008] S1, providing additives and acid solution;

[0009] The acid solution includes one or both of a hydrochloric acid solution and a sulfuric acid solution; the additive includes one or more of Cu, Cu2O and CuCl;

[0010] S2, placing the iron oxide and the additive together in the acid solution to carry out a leaching reaction to obtain an iron-containing treatment solution.

[0011] Furthermore, the iron oxide includes one or more of ZnFe2O4, Fe2O3 and Fe3O4.

[0012] Further, when the additive is Cu, the molar ratio of the iron oxide to the additive is 1:1.5-4;

[0013] When the additive is Cu2O, the molar ratio of the iron oxide to the additive is 1:1.5-4;

[0014] When the additive is CuCl, the molar ratio of the iron oxide to the additive is 1:3-8.

[0015] Further, when the iron oxide is ZnFe2O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.8-14.4;

[0016] When the iron oxide is Fe2O3, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:3.2-9.6;

[0017] When the iron oxide is Fe3O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.6-13.9.

[0018] Further, the concentration of hydrogen ions in the acid solution is not less than 0.5 mol / L;

[0019] When the additive is Cu, the liquid-to-solid ratio of the acid solution to the iron oxide is 4-50 ml / g;

[0020] When the additive is Cu2O, the liquid-to-solid ratio of the acid solution to the iron oxide is 4 to 66 ml / g;

[0021] When the additive is CuCl, the liquid-to-solid ratio of the acid solution to the iron oxide is 4-66 ml / g.

[0022] Furthermore, when the acid solution includes a sulfuric acid solution, the acid solution is heated during the leaching reaction.

[0023] Furthermore, the heating treatment includes: controlling the temperature of the acid solution to be 50°C-70°C.

[0024] Furthermore, the step S2 further comprises: during the leaching reaction, stirring the acid solution; wherein the stirring speed is 200 r / min to 400 r / min.

[0025] The present invention also provides an application of any one of the above-mentioned treatment methods in iron recovery.

[0026] The present invention also provides a method for recovering iron from solid waste, wherein the solid waste contains iron oxides;

[0027] The method for recovering iron comprises the steps of:

[0028] S10, providing an additive and an acid solution; wherein the acid solution comprises one or both of a hydrochloric acid solution and a sulfuric acid solution; and the additive comprises one or more of Cu, Cu2O and CuCl;

[0029] S20, placing the solid waste and the additive together in the acid solution to perform a leaching reaction to obtain an iron-containing treatment solution;

[0030] S30, performing solid-liquid separation on the treated liquid to obtain an iron-containing recovered liquid.

[0031] Compared with the prior art, the present invention has at least the following advantages:

[0032] The present invention can achieve rapid and effective leaching of iron in iron oxide, thereby ensuring the separation and recovery of iron elements. Through specific exploration, the present invention limits the acid solution to hydrochloric acid solution and sulfuric acid solution, which not only ensures the source of the acid solution, but also actually provides different reaction conditions under hydrochloric acid solution and sulfuric acid solution; the present invention limits the additive to Cu, Cu2O and CuCl, which provides a reaction basis for the effective leaching of iron, and creatively obtains an additive that can effectively leach iron elements from iron oxide; the present invention places the iron oxide and the additive together in the acid solution, avoiding the influence of the addition time on the leaching reaction.

[0033] Specifically, the present invention can achieve a leaching rate of 100% for Fe in ZnFe2O4, Fe2O3, and Fe3O4. Moreover, the complete leaching time of iron in ZnFe2O4 and Fe2O3 can be reduced to at least 20 minutes, and the complete leaching time of iron in Fe3O4 can be reduced to at least 2 minutes. On this basis, the present invention can also reduce the dependence of the reaction on acid concentration and reaction temperature, and can achieve effective leaching of iron at low acid concentration and low reaction temperature.

[0034] In addition, the reducing agent used in the present invention is easy to regenerate and can be recycled and reused through chemical or electrical conversion. The entire process is low-carbon, energy-saving, green and clean. It has the potential to be applied to the treatment of bulk solid waste containing iron oxides, playing a role in solid waste emission reduction and resource recovery. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0037] It should be understood that although Na2SO3, Fe, ZnS, SO2 and other substances can be used for acid leaching of ZnFe2O4, and oxalic acid, ascorbic acid and other substances can be used for dissolving Fe2O3 and Fe3O4, the use of the above substances still cannot avoid the leaching conditions of high temperature, high acidity and long time. In addition, organic reagents are expensive and difficult to regenerate after consumption, and are not suitable for the treatment of bulk iron oxide solid waste.

[0038] Based on this, in order to quickly and completely leach iron from iron oxides, the present invention provides a method for treating iron oxides, comprising the steps of:

[0039] S1, providing an additive and an acid solution; wherein the acid solution includes or is one or both of a hydrochloric acid solution and a sulfuric acid solution; and the additive includes or is one or more of Cu, Cu2O and CuCl.

[0040] It should be noted that not all additives and not all acid solutions can play the same role in the present invention.

[0041] For example: under the same conditions, the effect of hydrochloric acid solution in this application is obviously stronger than that of sulfuric acid solution, and sulfuric acid solution must be under specific conditions to achieve the technical effects in this application.

[0042] For example, under the same conditions, the effects of CuCl and Cu2O are significantly higher than those of Cu; moreover, when Na2SO3 and Fe are used as additives, the leaching efficiency of iron in iron oxides will decrease significantly.

[0043] S2, placing the iron oxide and the additive in the acid solution to perform a leaching reaction to obtain an iron-containing treatment solution. During the leaching reaction, the acid solution may be stirred at a speed of 200 r / min to 400 r / min.

[0044] It should be noted that the iron oxide and the additive must coexist in the acid solution to ensure the leaching reaction, thereby ensuring the dissolution of the iron element; that is, the time interval between the addition of the iron oxide and the additive to the acid solution cannot be too long, and it is best to add them at the same time. In this way, the iron oxide can be separated from the electrons and the generated ions (such as Cu + , Fe 2+ ) to effectively leach iron.

[0045] Preferably, the additive and the iron oxide may both be in powder form (powdered additives and iron oxides are used in subsequent examples and comparative examples).

[0046] It should also be noted that, due to the differences between hydrochloric acid solution and sulfuric acid solution in this application, when the acid solution includes or is a sulfuric acid solution, during the leaching reaction, it is necessary to extend the reaction time or heat the acid solution; the heating treatment may include or be: the temperature of the acid solution may be controlled to 50°C-70°C.

[0047] Normally, temperature and additives have a compensatory effect on each other. In order to completely dissolve iron oxides, the amount of additives needs to be appropriately increased at room temperature, while the amount of additives can be appropriately reduced when the temperature is increased. Acid concentration and liquid-solid ratio have a compensatory effect on each other. In order to completely dissolve iron oxides, high acid concentration can appropriately reduce the liquid-solid ratio, while low acid concentration requires an appropriate increase in the liquid-solid ratio.

[0048] S3, performing solid-liquid separation on the treated liquid to obtain an iron-containing solution.

[0049] It should be noted that the solid-liquid separation method may be filtration. After the solid-liquid separation, a solid separation and the iron-containing solution may be obtained; when there is no solid separation, the iron-containing solution may be equivalent to the iron-containing treatment solution.

[0050] As a further illustration of the above embodiment, the iron oxide may include or be one or more of ZnFe2O4, Fe2O3 and Fe3O4, and the additive mainly acts on the insoluble trivalent iron in the iron oxide (that is, the iron oxide applicable to the present invention contains trivalent iron). By limiting the specific substance of the iron oxide, it is convenient for those skilled in the art to obtain iron elements from the relevant iron oxide in a targeted manner, thereby providing a method for dissolving iron oxides such as zinc ferrite, hematite, and magnetite under normal pressure acidic solution conditions.

[0051] In the present invention, the complete leaching time (leaching reaction time) of iron in ZnFe2O4 and Fe2O3 can be as low as 20 minutes, and the complete leaching time (leaching reaction time) of iron in Fe3O4 can be as low as 2 minutes. Of course, the present invention can further reduce the leaching reaction time by adjusting the acid concentration or the ratio of reactants.

[0052] In order to ensure the leaching reaction, the ratio of the iron oxide to the additive may be further controlled.

[0053] When the additive is Cu, the molar ratio of the iron oxide to the additive is 1:1.5-4;

[0054] When the additive is Cu2O, the molar ratio of the iron oxide to the additive is 1:1.5-4;

[0055] When the additive is CuCl, the molar ratio of the iron oxide to the additive is 1:3-8.

[0056] It should be pointed out that, since the reaction systems of different iron oxides in this application are partially different, when the iron oxides are different, the ratio of the iron oxides to the hydrogen ions in the acid solution can be controlled to ensure effective leaching of the iron element.

[0057] For example, when the iron oxide is ZnFe2O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.8-14.4;

[0058] When the iron oxide is Fe2O3, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:3.2-9.6;

[0059] When the iron oxide is Fe3O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.6-13.9.

[0060] It should also be pointed out that, under the premise of ensuring the amount of hydrogen ions in the acid solution, the concentration and liquid-solid ratio of the acid solution can be further controlled to improve the leaching efficiency of iron.

[0061] Wherein, the concentration of hydrogen ions in the acid solution is not less than 0.5 mol / L; preferably, the concentration of hydrogen ions in the acid solution may be 0.5 mol / L-5 mol / L.

[0062] Since the present invention involves multiple additives, the action conditions and effects of different additives on the iron oxide may be partially different. Therefore, the requirements of different additives on the liquid-to-solid ratio of the acid solution and the iron oxide may also be partially different.

[0063] For example, when the additive is Cu, the liquid-to-solid ratio of the acid solution to the iron oxide is 4 to 50 ml / g;

[0064] When the additive is Cu2O, the liquid-to-solid ratio of the acid solution to the iron oxide is 4 to 66 ml / g;

[0065] When the additive is CuCl, the liquid-to-solid ratio of the acid solution to the iron oxide is 4-66 ml / g.

[0066] It is worth emphasizing that in the present invention, there is a potential difference between Cu, Cu2O, CuCl and iron oxides, forming a circuit in an acidic solution for electron and ion transfer, and spontaneously exchanging electrons and ions. Although substances such as Fe and Na2SO3 also have similar electron transfer modes with iron oxides in acidic solutions, experiments have shown that substances such as Fe and Na2SO3 cannot produce the technical effects of Cu, Cu2O, and CuCl, indicating that there may be incompletely clarified mechanisms and chemical reactions in the present invention.

[0067] In the present invention, the main chemical reactions that have been identified are as follows:

[0068] 1. ZnFe2O4+Cu+8H + =Zn 2+ +2Fe 2+ +Cu 2+ +4H2O

[0069] 2. Fe2O3+Cu+6H + =2Fe 2+ +Cu 2+ +3H2O

[0070] 3. Fe3O4+Cu+8H + =3Fe 2+ +Cu 2+ +4H2O

[0071] 4. ZnFe2O4+2Cu + +8H + =Zn 2+ +2Fe 2+ +2Cu 2+ +4H2O

[0072] 5. Fe2O3+2Cu + +6H + =2Fe 2+ +2Cu 2+ +3H2O

[0073] 6. Fe3O4+2Cu + +8H+ =3Fe 2+ +2Cu 2+ +4H2O

[0074] Note: The above reactions correspond to different iron oxides and additives, among which Cu + Represents Cu2O and CuCl. In addition, the "theoretical amount" involved in the present invention can be calculated based on the above-mentioned chemical reaction that has been clarified.

[0075] The theoretical calculated amount of Na2SO3 and Fe in the present invention can be calculated by the following reaction:

[0076] ZnFe2O4+SO3 2- +6H + =Zn 2+ +2Fe 2+ +SO4 2- +3H2O

[0077] ZnFe2O4+Fe+8H + =Zn 2+ +3Fe 2+ +4H2O

[0078] In view of the fact that the above-mentioned treatment method provided by the present invention can effectively leach iron from iron oxides, the present invention also provides an application of the treatment method described in any of the above-mentioned embodiments in recovering iron.

[0079] For example, the present invention provides a method for recovering iron from solid waste containing iron oxides.

[0080] The method for recovering iron comprises the steps of:

[0081] S10, providing an additive and an acid solution; wherein the acid solution comprises one or both of a hydrochloric acid solution and a sulfuric acid solution; and the additive comprises one or more of Cu, Cu2O and CuCl;

[0082] S20, placing the solid waste and the additive together in the acid solution to perform a leaching reaction to obtain an iron-containing treatment solution;

[0083] S30, performing solid-liquid separation on the treated liquid to obtain an iron-containing recovered liquid.

[0084] It should be noted that the method for recovering iron may include all or part of the methods for treating iron oxides.

[0085] In the method for recovering iron, the iron oxides in the solid waste may include one or more of ZnFe2O4, Fe2O3 and Fe3O4.

[0086] When the additive is Cu, the molar ratio of the iron oxide to the additive is 1:1.5-4; when the additive is Cu2O, the molar ratio of the iron oxide to the additive is 1:1.5-4; when the additive is CuCl, the molar ratio of the iron oxide to the additive is 1:3-8.

[0087] When the iron oxide is ZnFe2O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.8~14.4; when the iron oxide is Fe2O3, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:3.2~9.6; when the iron oxide is Fe3O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.6~13.9.

[0088] The concentration of hydrogen ions in the acid solution is not less than 0.5 mol / L. When the additive is Cu, the liquid-solid ratio of the acid solution to the iron oxide is 4 to 50 ml / g; when the additive is Cu2O, the liquid-solid ratio of the acid solution to the iron oxide is 4 to 66 ml / g; when the additive is CuCl, the liquid-solid ratio of the acid solution to the iron oxide is 4 to 66 ml / g.

[0089] The step S20 further includes: stirring the acid solution during the leaching reaction; wherein the stirring speed is 200 r / min to 400 r / min.

[0090] When the acid solution includes or is a sulfuric acid solution, during the leaching reaction, the acid solution is subjected to a heating treatment; the heating treatment may include or be: controlling the temperature of the acid solution to 50°C-70°C.

[0091] The additive and the iron oxide may both be in powder form, that is, the solid waste may also be in powder form.

[0092] The following are specific examples of the present invention:

[0093] Example 1

[0094] 2 g ZnFe2O4 and 2.11 g Cu (4 times the theoretical amount) were added to the hydrochloric acid solution, and the hydrochloric acid solution was continuously stirred at 25°C to carry out the leaching reaction.

[0095] The volume of hydrochloric acid solution is 24 ml (liquid-to-solid ratio of ZnFe2O4 is 12), and the H + The concentration of the hydrochloric acid solution is 5 mol / L (the total H +The stirring speed is 400r / min.

[0096] Samples were taken for ICP-AES element concentration analysis at 5 min, 10 min, 15 min, 40 min, 60 min and 90 min of reaction, and the leaching rate was calculated based on the obtained element concentrations.

[0097] The test results of this embodiment are shown in the following table:

[0098] Time (min) 5 10 15 40 60 90 Fe leaching rate (%) 39.32 69.26 83.09 88.43 95.32 100

[0099] It can be seen that this embodiment has a better leaching efficiency for iron in ZnFe2O4. Even though ZnFe2O4 is extremely insoluble, the Fe leaching rate can reach 95.32% when the reaction time is 60 minutes, and the leaching rate can reach 100% when the reaction time is 90 minutes; therefore, the leaching time can be 60-90 minutes.

[0100] Comparative Example 1

[0101] Compared with Example 1, this comparative example only changes the hydrochloric acid solution to the sulfuric acid solution.

[0102] The sampling times for this comparative example are 15min, 30min, 50min, 90min, 120min and 150min.

[0103] The test results of this comparative example are shown in the following table:

[0104] Time (min) 15 30 50 90 120 150 Fe leaching rate (%) 13.30 30.82 46.31 70.82 87.55 100

[0105] It can be seen that this comparative example requires a longer reaction time to achieve complete leaching of ZnFe2O4. At 120 min, the leaching rate of iron is only 87.55%, and at 150 min, it reaches 100%.

[0106] Example 2

[0107] 2 g of Fe2O3 and 3.18 g of Cu (4 times the theoretical amount) were added to the hydrochloric acid solution, and the hydrochloric acid solution was continuously stirred at 25°C to carry out the leaching reaction.

[0108] The volume of hydrochloric acid solution is 24 ml (liquid-to-solid ratio of ZnFe2O4 is 12), and the H + The concentration of the hydrochloric acid solution is 5 mol / L (the total H + The stirring speed is 400r / min.

[0109] Samples were taken for ICP-AES element concentration analysis at 1 min, 5 min, 10 min, 15 min and 20 min of reaction time, and the leaching rate was calculated based on the obtained element concentrations.

[0110] The test results of this embodiment are shown in the following table:

[0111] Time (min) 1 5 10 15 20 Fe leaching rate (%) 30.85 73.33 88.29 96.35 100

[0112] It can be seen that this embodiment has a better leaching efficiency for iron in Fe2O3. When the reaction time is 20 minutes, the Fe leaching rate can reach 100%; therefore, the leaching time can be 20 minutes, or 15-25 minutes.

[0113] Comparative Example 2

[0114] Compared with Example 2, this comparative example only changes the hydrochloric acid solution to a sulfuric acid solution.

[0115] The sampling times for this comparative example are 10 min, 20 min, 40 min, 90 min and 120 min.

[0116] The test results of this comparative example are shown in the following table:

[0117] Time (min) 10 20 40 90 120 Fe leaching rate (%) 27.70 54.48 86.66 91.82 100

[0118] It can be seen that this comparative example requires a longer reaction time to achieve complete leaching of Fe2O3. At 90 min, the leaching rate of iron is 91.82%, and at 120 min, it reaches 100%.

[0119] Example 3

[0120] 2 g of Fe3O4 and 2.20 g of Cu (4 times the theoretical calculated amount) were added to the hydrochloric acid solution, and the hydrochloric acid solution was continuously stirred at 25°C to carry out the leaching reaction.

[0121] The volume of hydrochloric acid solution is 24 ml (liquid-to-solid ratio of ZnFe2O4 is 12), and the H + The concentration of the hydrochloric acid solution is 5 mol / L (the total H + The stirring speed is 400r / min.

[0122] Samples were taken at 1 min, 2 min, 4 min and 5 min of reaction time for ICP-AES element concentration analysis, and the leaching rate was calculated based on the obtained element concentrations.

[0123] The test results of this embodiment are shown in the following table:

[0124] Time (min) 1 2 4 5 Fe leaching rate (%) 93.79 100 100 100

[0125] It can be seen that this embodiment has a better leaching efficiency for iron in Fe3O4. When the reaction time is 2 minutes, the Fe leaching rate can reach 100%; therefore, the leaching time can be 2-5 minutes.

[0126] Comparative Example 3

[0127] Compared with Example 3, this comparative example only changes the hydrochloric acid solution to the sulfuric acid solution.

[0128] The sampling times for this comparative example are 5min, 10min, 20min, 30min and 40min.

[0129] The test results of this comparative example are shown in the following table:

[0130] Time (min) 5 10 20 30 40 Fe leaching rate (%) 34.42 55.09 84.17 98.40 100

[0131] It can be seen that this comparative example requires a longer reaction time to achieve complete leaching of Fe3O4. At 30 min, the leaching rate of iron is 98.40%, and at 40 min, it reaches 100%.

[0132] Analysis example 1

[0133] Combine Example 1, Comparative Example 1, Example 2, Comparative Example 2, Example 3 and Comparative Example 3.

[0134] It can be seen that: at 25°C, Fe3O4, Fe2O3 and ZnFe2O4 can be completely dissolved, and different iron oxides have different leaching rates.

[0135] Among them, whether it is sulfuric acid solution or hydrochloric acid solution, the order of reaction rate and reaction efficiency is Fe3O4>Fe2O3>ZnFe2O4.

[0136] And no matter which type of iron oxide, the leaching efficiency of hydrochloric acid solution is significantly better than that of sulfuric acid solution.

[0137] Since sulfuric acid solution is also a kind of conventional acid solution, in order to improve the applicability of the technical solution of the present invention, it is necessary to explore the reaction conditions when the acid solution is sulfuric acid solution, for example, how to quickly and completely dissolve the most stubborn ZnFe2O4 in sulfuric acid solution.

[0138] Example 4

[0139] 0.5 g ZnFe2O4 and 0.20 g Cu (1.5 times the theoretical calculated amount) were added to the sulfuric acid solution, and the sulfuric acid solution was continuously stirred at 60°C to carry out the leaching reaction.

[0140] The volume of sulfuric acid solution is 25 ml (liquid-to-solid ratio with ZnFe2O4 is 50), and the volume of H + The concentration is 0.5 mol / L (the total H + The stirring speed is 400r / min.

[0141] Samples were taken at 5 min, 15 min, 40 min, 60 min and 90 min of reaction time for ICP-AES element concentration analysis, and the leaching rate was calculated based on the obtained element concentrations.

[0142] The test results of this embodiment are shown in the following table:

[0143] Time (min) 5 15 40 60 90 Fe leaching rate (%) 5.99 17.05 52.60 79.30 100

[0144] It can be seen that this embodiment reduces the theoretical calculated amount of Cu and H + After multiples of the theoretical calculated amount, it is still possible to achieve complete leaching of iron in ZnFe2O4 under sulfuric acid conditions, and the leaching time can be 90 minutes, or 85-95 minutes.

[0145] Example 5

[0146] 1 g ZnFe2O4 and 0.40 g Cu (1.5 times the theoretical amount) were added to the sulfuric acid solution, and the sulfuric acid solution was continuously stirred at 60°C to carry out the leaching reaction.

[0147] The volume of sulfuric acid solution is 4 ml (liquid-to-solid ratio with ZnFe2O4 is 4), and the volume of H + The concentration is 5 mol / L (the total H + The stirring speed is 400r / min.

[0148] Samples were taken for ICP-AES element concentration analysis at 5 min, 10 min, 15 min, 20 min and 40 min of reaction, and the leaching rate was calculated based on the obtained element concentrations.

[0149] The test results of this embodiment are shown in the following table:

[0150] Time (min) 5 10 15 20 40 Fe leaching rate (%) 35.53 49.71 66.59 97.37 99.26

[0151] It can be seen that: this embodiment reduces the liquid-to-solid ratio and appropriately reduces H + Under the condition of multiples of the theoretical calculated amount, rapid and effective leaching of iron in ZnFe2O4 is still achieved, and the leaching time can be 20-40min.

[0152] Comparative Example 4

[0153] Compared with Example 4, this comparative example only changes the volume of the sulfuric acid solution to 33 ml (the liquid-to-solid ratio of ZnFe2O4 is 66, and the total H + is 1 times the theoretical calculated amount).

[0154] The sampling times for this comparative example are 10min, 20min, 40min, 60min and 90min.

[0155] The test results of this comparative example are shown in the following table:

[0156] Time (min) 10 20 40 60 90 Fe leaching rate (%) 10.63 22.54 46.53 66.76 88.69

[0157] It can be seen that although this comparative example has a certain leaching efficiency for Fe in ZnFe2O4, compared with Example 4, the leaching efficiency of this comparative example is not high. When the reaction time is 90 minutes, the leaching rate of iron is still only 88.69%.

[0158] Analysis example 2

[0159] Combine Example 4, Example 5 and Comparative Example 4.

[0160] It can be seen that after adjusting the reaction temperature to 60°C, it can be ensured that the present invention can also leach ZnFe2O4 in sulfuric acid solution. + After the theoretical calculated amount, the present invention can still achieve effective leaching of Fe in ZnFe2O4.

[0161] In addition, when H + When the concentration is between 0.5 and 5 mol / L, complete leaching of Fe can be achieved, but the higher the acid concentration, the faster the leaching rate.

[0162] It should be noted that, referring to the test results of Comparative Example 4, although increasing the liquid-solid ratio can increase the total amount of acid, a too high liquid-solid ratio will instead reduce the leaching rate of iron.

[0163] In the present invention, the preferred liquid-to-solid ratio of the acid solution to the iron oxide can be 4 to 50 (ml / g). Within this range, if the liquid-to-solid ratio is small, the concentration of the acid solution can be increased to achieve sufficient reaction; if the liquid-to-solid ratio is large, the concentration of the acid solution can be reduced to save acid.

[0164] Example 6

[0165] Compared with Comparative Example 4, in this embodiment, only 0.20 g of Cu is replaced with 0.45 g of Cu2O (1.5 times the theoretical calculated amount).

[0166] The sampling time in this embodiment is 5min, 10min, 15min, 20min, and 30min.

[0167] The test results of this embodiment are shown in the following table:

[0168] Time (min) 5 10 15 20 30 Fe leaching rate (%) 70.82 82.83 89.15 91.69 100

[0169] It can be seen that after replacing Cu with Cu2O, this embodiment overcomes the defects in Comparative Example 4, and ZnFe2O4 can be completely leached in a shorter time, and the leaching time can be 30 minutes, or 25-35 minutes.

[0170] Example 7

[0171] Compared with Comparative Example 4, in this embodiment, only 0.20 g of Cu is replaced with 0.62 g of CuCl (1.5 times the theoretical calculated amount).

[0172] The sampling time in this embodiment is 5min, 10min, 15min, 20min, and 30min.

[0173] The test results of this embodiment are shown in the following table:

[0174] Time (min) 5 10 15 20 30 Fe leaching rate (%) 67.31 84.62 95.73 100 100

[0175] It can be seen that after replacing Cu with CuCl, this embodiment overcomes the defects in Comparative Example 4 and can completely leach ZnFe2O4 in a shorter time, and the leaching time can be 20-30 minutes.

[0176] Analysis example 3

[0177] Combine Comparative Example 4, Example 6 and Example 7.

[0178] It can be seen that after the additive is changed to Cu2O or CuCl, the technical defects in Comparative Example 4 can be reversed. Even if the liquid-to-solid ratio of the acid solution to the iron oxide reaches 66, Examples 6 and 7 can still achieve complete leaching of Fe in a relatively short time.

[0179] Therefore, combined with the actual data comparison, in terms of reaction rate and reaction effect, CuCl>Cu2O>Cu.

[0180] Comparative Example 5

[0181] Compared with Example 7, in this comparative example, only 0.62 g of CuCl was replaced by 0.39 g of Na2SO3 (1.5 times the theoretical calculated amount).

[0182] The sampling times for this comparative example are 10min, 20min, 40min, 60min and 90min.

[0183] The test results of this comparative example are shown in the following table:

[0184]

[0185]

[0186] It can be seen that after replacing CuCl with Na2SO3 in this comparative example, even after 90 minutes of reaction, the leaching rate of Fe is only 38.51%.

[0187] Comparative Example 6

[0188] Compared with Example 7, this comparative example only replaces 0.62 g CuCl with 0.17 g Fe (1.5 times the theoretical calculated amount).

[0189] The sampling times for this comparative example are 10min, 20min, 40min, 60min and 90min.

[0190] The test results of this comparative example are shown in the following table:

[0191] Time (min) 10 20 40 60 90 Zn leaching rate (%) 5.87 9.30 19.81 27.67 49.94

[0192] It can be seen that after replacing CuCl with Fe in this comparative example, even after 90 minutes of reaction, the leaching rate of Zn is only 49.94%. (Because Fe has an external source, the leaching rate of Zn is used for characterization)

[0193] Analysis example 4

[0194] Combined with Examples 6-7 and Comparative Examples 5-6.

[0195] It can be seen that after adjusting the additive to Na2SO3 or Fe, the leaching rate of Fe in iron oxides cannot be improved.

[0196] Even though the reaction conditions in Comparative Examples 5-6 are the same as those in Examples 6-7, the leaching efficiency of Fe is still low based on the use of Na2SO3 or Fe as additives.

[0197] Comparative Example 7

[0198] 0.25 g ZnFe2O4 and 0.10 g Cu (1.5 times the theoretical calculated amount) were added to the sulfuric acid solution, and the sulfuric acid solution was continuously stirred at 60°C to carry out the leaching reaction.

[0199] The volume of sulfuric acid solution is 27.6 ml (liquid-to-solid ratio with ZnFe2O4 is 1:10), and the volume of H + The concentration of sulfuric acid solution is 0.3 mol / L (the total H + The stirring speed is 400r / min.

[0200] Samples were taken for ICP-AES element concentration analysis at 5 min, 10 min, 20 min, 40 min and 120 min of reaction time, and the leaching rate was calculated based on the obtained element concentrations.

[0201] The test results of this comparative example are shown in the following table:

[0202] Time (min) 5 10 20 40 120 Fe leaching rate (%) 5.03 9.03 18.28 46.54 83.43

[0203] It can be seen that even if the total H + It is 1 times the theoretical calculated amount. However, when the concentration of the acid solution is 0.3 mol / L, the iron in the iron oxide cannot be effectively leached.

[0204] Comparative Example 8

[0205] 1 g ZnFe2O4 and 0.40 g Cu (1.5 times the theoretical amount) were added to the sulfuric acid solution, and the sulfuric acid solution was continuously stirred at 60°C to carry out the leaching reaction.

[0206] The volume of sulfuric acid solution is 33 ml (liquid-to-solid ratio of ZnFe2O4 is 33), and H + The concentration of sulfuric acid solution is 1 mol / L (the total H + The stirring speed is 100r / min.

[0207] Samples were taken at 10 min, 20 min, 40 min and 60 min of reaction for ICP-AES element concentration analysis, and the leaching rate was calculated based on the obtained element concentrations.

[0208] The test results of this comparative example are shown in the following table:

[0209] Time (min) 10 20 40 60 Fe leaching rate (%) 9.96 25.70 53.81 80.37

[0210] It can be seen that after the stirring speed is adjusted to 100 r / min, the leaching efficiency of Fe is not high, and in this comparative example, it can be seen that the copper powder floats on the liquid surface for a long time.

[0211] Analysis example 5

[0212] Combine Comparative Example 7 and Comparative Example 8.

[0213] It can be seen that: even if the acid solution is in H + The amount of acid solution meets the reaction requirements, but the specific parameters of the acid solution will also affect the leaching of Fe. In addition, the stirring speed during the reaction will also have a certain impact on the leaching of iron.

[0214] Therefore, in order to improve the leaching efficiency of iron in iron oxide, the acid solution can be controlled at the same time. + The amount and parameters of the acid solution; the stirring speed during the reaction can also be controlled within a preferred range. The preferred stirring speed of the present invention is 200r / min-400r / min.

[0215] Comparative Example 9

[0216] 1g ZnFe2O4 was added to the sulfuric acid solution; the volume of the sulfuric acid solution was 66ml (the liquid-to-solid ratio of ZnFe2O4 was 66), and the concentration of the sulfuric acid solution was 0.5mol / L (the total H + is 1 times of the theoretical calculation amount),

[0217] The reaction of this comparative example was carried out under an electric field. This comparative example used graphite sheets (2cm*1cm) as electrode sheets (cathode and anode), and the electrode sheets were placed in a sulfuric acid solution. During the reaction, direct current was passed, and the current was 0.01A.

[0218] In this comparative example, the stirring speed of the sulfuric acid solution is 400 r / min and the reaction temperature is 60°C;

[0219] Samples were taken for ICP-AES element analysis at 10 min, 20 min, 40 min, 60 min and 90 min of reaction, and the leaching rate was calculated based on the obtained element concentration.

[0220] The test results of this comparative example are shown in the following table:

[0221] Time (min) 10 20 40 60 90 Fe leaching rate (%) 1.05 1.98 4.25 6.84 11.15

[0222] Comparative Example 10

[0223] Compared with Comparative Example 9, the current in this comparative example is only changed to 0.03A.

[0224] Samples were taken for ICP-AES element analysis at 10 min, 20 min, 40 min, 60 min and 90 min of reaction, and the leaching rate was calculated based on the obtained element concentration.

[0225] The test results of this comparative example are shown in the following table:

[0226] Time (min) 10 20 40 60 90 Fe leaching rate (%) 0.84 2.91 6.35 7.78 15.39

[0227] Analysis example 6

[0228] Combine Comparative Example 9 and Comparative Example 10.

[0229] It can be known that: although the electric field can promote the transfer of electrons, according to the test results of Comparative Examples 9 and 10, the reaction conditions of acid solution plus electric field cannot effectively leach iron from iron oxide.

[0230] Therefore, the present invention is not equivalent to a simple electron transfer process, which illustrates that the present invention has unexpected technical effects in the reaction process.

[0231] Comparative Example 11

[0232] 2 g of Fe3O4 and 0.55 g of Cu (1 times the theoretical calculated amount) were added to the hydrochloric acid solution, and the hydrochloric acid solution was continuously stirred at 60°C to carry out the leaching reaction.

[0233] The volume of hydrochloric acid solution is 24 ml (liquid-to-solid ratio of ZnFe2O4 is 12), and the H + The concentration of the hydrochloric acid solution is 5 mol / L (the total H + The stirring speed is 400r / min.

[0234] Samples were taken at 1 min, 5 min, 20 min and 60 min of reaction for ICP-AES element concentration analysis, and the leaching rate was calculated based on the obtained element concentrations.

[0235] The test results of this comparative example are shown in the following table:

[0236] Time (min) 1 5 20 60 Fe leaching rate (%) 71.04 85.76 87.75 90.01

[0237] It can be seen that: although Fe3O4 is the easiest to dissolve (high efficiency and fast speed, only 2 minutes in hydrochloric acid solution at 25°C).

[0238] However, in this comparative example, even though H + The concentration is 5 mol / L, the reaction temperature is 60℃, and the reaction time is 60min. 1 times the theoretical amount of additive cannot quickly and completely dissolve the Fe in Fe3O4, indicating that the amount of additive added must exceed 1 times the theoretical amount to obtain a better leaching effect.

[0239] The above technical solutions of the present invention are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention specification under the technical concept of the present invention, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for treating iron oxides, characterized in that: Includes steps: S1, providing additives and acid solution; The acid solution includes one or both of a hydrochloric acid solution and a sulfuric acid solution; the additive includes one or more of Cu, Cu2O and CuCl; S2, placing the iron oxide and the additive together in the acid solution to carry out a leaching reaction to obtain an iron-containing treatment solution.

2. The processing method according to claim 1, characterized in that: The iron oxide includes one or more of ZnFe2O4, Fe2O3 and Fe3O4.

3. The processing method according to claim 1, characterized in that: When the additive is Cu, the molar ratio of the iron oxide to the additive is 1:1.5-4; When the additive is Cu2O, the molar ratio of the iron oxide to the additive is 1:1.5-4; When the additive is CuCl, the molar ratio of the iron oxide to the additive is 1:3-8.

4. The processing method according to claim 2, characterized in that: When the iron oxide is ZnFe2O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.8-14.4; When the iron oxide is Fe2O3, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:3.2-9.6; When the iron oxide is Fe3O4, the molar ratio of the iron oxide to the hydrogen ions in the acid solution is 1:4.6-13.

9.

5. The processing method according to claim 1, characterized in that: The concentration of hydrogen ions in the acid solution is not less than 0.5 mol / L; When the additive is Cu, the liquid-to-solid ratio of the acid solution to the iron oxide is 4-50 ml / g; When the additive is Cu2O, the liquid-to-solid ratio of the acid solution to the iron oxide is 4 to 66 ml / g; When the additive is CuCl, the liquid-to-solid ratio of the acid solution to the iron oxide is 4-66 ml / g.

6. The processing method according to claim 1, characterized in that: When the acid solution includes a sulfuric acid solution, the acid solution is heated during the leaching reaction.

7. The processing method according to claim 6, characterized in that: The heating treatment includes: controlling the temperature of the acid solution to be 50° C.-70° C.

8. The processing method according to claim 1, characterized in that: The step S2 further comprises: stirring the acid solution during the leaching reaction; wherein the stirring speed is 200 r / min to 400 r / min.

9. Use of the treatment method according to any one of claims 1 to 8 in recovering iron.

10. A method for recovering iron from solid waste, characterized in that: The solid waste contains iron oxides; The method for recovering iron comprises the steps of: S10, providing an additive and an acid solution; wherein the acid solution comprises one or both of a hydrochloric acid solution and a sulfuric acid solution; and the additive comprises one or more of Cu, Cu2O and CuCl; S20, placing the solid waste and the additive together in the acid solution to perform a leaching reaction to obtain an iron-containing treatment solution; S30, performing solid-liquid separation on the treated liquid to obtain an iron-containing recovered liquid.