Electrochemical deposition preparation method and application of silver nanowires
By using niacin solution and silver layer in the preparation of silver nanowires, the complex preparation process and high cost problems caused by cyanide solutions are solved, and the preparation of silver nanowires with low toxicity and low pollution is achieved, and the density of nanowires is improved. and crystallinity.
Patent Information
- Application Number
- CN202411242576.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-22
AI Technical Summary
The use of cyanide solution during the preparation of existing silver nanowires results in complex and costly preparation, and the production of toxic wastewater, requiring strict safety measures.
Using niacin solution as the electrolyte, silver nanowires were prepared in the through holes of the nanometer template by electrochemical deposition. Using a silver layer as the substrate, silver ions formed a complex with ammonia and niacin, and released slowly and controlably. A silver nanowire structure with uniform thickness and high density is formed.
It reduces the complexity and cost of the preparation process, reduces pollution and toxicity, realizes the preparation of low-toxic and low-pollution silver nanowires, and improves the crystallinity and density of the nanowires.
Smart Images

Figure CN118996538A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silver nanowire preparation, and more specifically, to an electrochemical deposition preparation method and application of silver nanowires. Background Art
[0002] With the rapid development of nanotechnology, one-dimensional nanomaterials have shown great application potential in electronics, optics, catalysis, biosensors and other fields due to their unique physical and chemical properties. Among them, silver nanowires (AgNWs), as an important representative of one-dimensional nanomaterials, have become a bridge between traditional electronic devices and emerging flexible electronic technologies due to their excellent conductivity, light transmittance, flexibility and high specific surface area. In particular, their application prospects are particularly broad in the fields of micro-nano robots, flexible displays, touch screens, solar cells, and biosensors.
[0003] As a mature material preparation technology, electrochemical deposition has the advantages of simple equipment, convenient operation, and easy control. It is widely used in the preparation of nanomaterials. Especially in the process of template-assisted electrochemical deposition, by selecting a suitable nano-template and electrolyte system, the morphology and size of nanomaterials can be precisely controlled. The electrolyte used in the existing electrochemical deposition of silver nanowires is mainly cyanide solution. For transition metal ions, cyanide ions (CN - ) is an effective ligand. The cyanide complex ion also has the characteristics of difficult dissociation, slow reduction, and slow movement. This stability helps to control the rate of metal deposition and improve the controllability of the deposition process. However, cyanide is a highly toxic substance. In the process of using cyanide solution to prepare silver nanowires, on the one hand, a large amount of toxic wastewater will be produced. Toxic wastewater needs to be professionally treated to meet environmental emission standards, which is costly; on the other hand, the preparation process of silver nanowires is complicated and requires strict safety measures, including high requirements for the closedness of the equipment. Operators also need to wear professional protective equipment, such as protective clothing, gloves and respirators, to prevent cyanide poisoning. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing silver nanowires by electrochemical deposition and its application, so as to solve the technical problems that in the existing preparation process of silver nanowires, the preparation process is complicated and the cost is high due to the use of cyanide solution as electrolyte.
[0005] In order to achieve the above object, in a first aspect, the present invention provides a method for preparing silver nanowires by electrochemical deposition, comprising: Obtaining a nano template, wherein the nano template has a front side and a back side, a plurality of through holes are disposed between the front side and the back side, and a silver layer is disposed on the back side; Using the nano template as a cathode, a platinum sheet as an anode, and a nicotinic acid solution as an electrolyte, silver nanowires are prepared in the through holes of the nano template by electrochemical deposition; The nicotinic acid solution comprises 30-35 ml / L of ammonia water, 0.5-0.6 mol / L of potassium carbonate, 0.73-0.89 mol / L of nicotinic acid, and 0.25-0.3 mol / L of silver nitrate; the pH value of the nicotinic acid solution is 9-9.5.
[0006] Compared with the prior art, in the electrochemical deposition preparation method of silver nanowires of the present invention, the silver layer disposed on the reverse side of the nano template has good conductivity. In the above electrochemical deposition process, the silver layer can provide a stable substrate for the deposition or growth of silver nanowires. For example, the nano template can be a nanoporous anodic aluminum oxide (AAO) template. In this technical solution, the electrolyte is a nicotinic acid solution, in which potassium carbonate can improve the conductivity of the nicotinic acid solution, silver nitrate is used to provide silver ions, ammonia water and nicotinic acid are both complexing agents, wherein ammonia water is the main complexing agent. In the nicotinic acid solution, the silver ions first form a complex with ammonia water [Ag(NH3)2] + , the remaining free silver ions can be further complexed with nicotinic acid, and the effective concentration of silver ions in the nicotinic acid solution can be increased by forming a complex with ammonia water, nicotinic acid and silver ions. Furthermore, the above complex can slowly and controllably release the silver ions, and then form a silver nanowire structure with uniform thickness and high density in the through-holes of the nanotemplate with the silver layer on the nanotemplate as the substrate. In the above process, nicotinic acid can be used as a stabilizer and a brightener. On the one hand, as a stabilizer, nicotinic acid can form a complex with the remaining silver ions, thereby reducing the concentration of free silver ions and hindering the uneven deposition and particle aggregation of silver ions in the nicotinic acid solution. On the other hand, as a brightener, nicotinic acid can increase the crystallinity of silver nanowires, making the crystal structure of the deposit more perfect. In the above technical scheme of the present invention, compared with the existing cyanide solution, the nicotinic acid solution has the characteristics of low toxicity and low pollution, and the preparation process is simple, which solves the technical problems of the complicated preparation process and high cost in the preparation process of the existing silver nanowires due to the use of cyanide solution as the electrolyte.
[0007] Furthermore, in the electrochemical deposition preparation method of silver nanowires of the present invention, the nicotinic acid solution also includes 0.8-0.98 mol / L potassium hydroxide and 0.9-1.0 mol / L ammonium acetate.
[0008] Furthermore, in the electrochemical deposition preparation method of silver nanowires of the present invention, the thickness of the nano template is 40-60 mm, and the through hole diameter is 40-360 nm.
[0009] Furthermore, in the electrochemical deposition preparation method of silver nanowires of the present invention, the thickness of the silver layer arranged on the reverse side is 60-150 nm.
[0010] Furthermore, in the electrochemical deposition method for preparing silver nanowires of the present invention, the current density during the electrochemical deposition process is 0.2-0.4 mA / cm 2 , the deposition time is 500~1500 seconds.
[0011] Furthermore, in the electrochemical deposition preparation method of the silver nanowires of the present invention, after the silver nanowires are prepared in the through-holes of the nano-template by electrochemical deposition, the method further comprises: After removing the silver layer on the reverse side of the nano template, the nano template is removed by soaking in an alkaline solution; collecting the silver nanowires dispersed in the alkaline solution; Wherein, the alkaline solution is a 1.5-3 mol / L sodium hydroxide solution, and the soaking time is 30-60 minutes.
[0012] Furthermore, in the electrochemical deposition preparation method of silver nanowires of the present invention, the step of collecting the silver nanowires dispersed in the alkaline solution comprises: The silver nanowires dispersed in the alkaline solution were collected by centrifugation; The silver nanowires were cleaned with deionized water and then stored in ultrapure water at room temperature.
[0013] Furthermore, in the electrochemical deposition preparation method of silver nanowires of the present invention, after obtaining a nano template and providing a silver layer on the reverse side of the nano template, the method further comprises: The nano template is ultrasonically treated for 3 to 5 minutes, and the ultrasonic treatment liquid is a nicotinic acid solution.
[0014] In a second aspect, the present invention provides a silver nanowire prepared by the above-mentioned electrochemical deposition preparation method of silver nanowire.
[0015] Compared with the prior art, the beneficial effects of the silver nanowires of the present invention are the same as the beneficial effects of the electrochemical deposition preparation method of the silver nanowires described in the above technical solution, which will not be repeated here.
[0016] In a third aspect, the present invention provides the application of the above-mentioned silver nanowires in flexible micro-nano robots. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings: Figure 1This is a schematic diagram of the SEM surface morphology of the silver nanowires prepared in Example 3 of the present invention; Figure 2 This is a schematic diagram of the SEM surface morphology of the silver nanowires prepared in Example 4 of the present invention; Figure 3 Schematic diagram of the surface structure of the porous anodized aluminum template in the present invention; Figure 4 Schematic diagram of the electrochemical deposition device in the present invention.
[0018] Reference numerals: 1. Platinum electrode; 2. Electrolyte; 3. Reactor plug; 4. Nano template; 5. Copper electrode; 6. Reactor; 7. Ring gasket; 8. DC regulated power supply. DETAILED DESCRIPTION
[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0020] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0021] In addition, in the description of the present invention, "multiple" means two or more, unless otherwise clearly and specifically defined, and "several" means one or more, unless otherwise clearly and specifically defined.
[0022] As a mature material preparation technology, electrochemical deposition has the advantages of simple equipment, convenient operation, and easy control. It is widely used in the preparation of nanomaterials. Especially in the process of template-assisted electrochemical deposition, by selecting a suitable nano-template and electrolyte system, the morphology and size of nanomaterials can be precisely controlled. The electrolyte used in the existing electrochemical deposition of silver nanowires is mainly cyanide solution. For transition metal ions, cyanide ions (CN -) is an effective ligand. The cyanide complex ion also has the characteristics of difficult dissociation, slow reduction, and slow movement. This stability helps to control the rate of metal deposition and improve the controllability of the deposition process. However, cyanide is a highly toxic substance. In the process of using cyanide solution to prepare silver nanowires, on the one hand, a large amount of toxic wastewater will be produced. Toxic wastewater needs to be professionally treated to meet environmental emission standards, which is costly; on the other hand, the preparation process of silver nanowires is complicated and requires strict safety measures, including high requirements for the closedness of the equipment. Operators also need to wear professional protective equipment, such as protective clothing, gloves and respirators, to prevent cyanide poisoning.
[0023] In order to solve the above technical solution, in a first aspect, the present invention provides a method for preparing silver nanowires by electrochemical deposition, comprising: Obtain a nano template, wherein the nano template has a front side and a back side, a plurality of through holes are provided between the front side and the back side, and a silver layer is provided on the back side; Using the nano template as a cathode, a platinum sheet as an anode, and a nicotinic acid solution as an electrolyte, silver nanowires are prepared in the through holes of the nano template by electrochemical deposition; The nicotinic acid solution comprises 30-35 ml / L of ammonia water, 0.5-0.6 mol / L of potassium carbonate, 0.73-0.89 mol / L of nicotinic acid, and 0.25-0.3 mol / L of silver nitrate; the pH value of the nicotinic acid solution is 9-9.5.
[0024] In the case of adopting the above technical solution, in the electrochemical deposition preparation method of silver nanowires of the present invention, the silver layer arranged on the reverse side of the nano template has good conductivity. In the above electrochemical deposition process, the silver layer can provide a stable substrate for the deposition or growth of silver nanowires. For example, the nano template can be a nanoporous anodic aluminum oxide (AAO) template. In this technical solution, the electrolyte is a nicotinic acid solution, in which potassium carbonate can improve the conductivity of the nicotinic acid solution, silver nitrate is used to provide silver ions, ammonia water and nicotinic acid are both complexing agents, wherein ammonia water is the main complexing agent. In the nicotinic acid solution, the silver ions first form a complex with ammonia water [Ag(NH3)2] +, the remaining free silver ions can be further complexed with nicotinic acid, and the effective concentration of silver ions in the nicotinic acid solution can be increased by forming a complex with ammonia water, nicotinic acid and silver ions. Furthermore, the above complex can slowly and controllably release the silver ions, and then form a silver nanowire structure with uniform thickness and high density in the through-holes of the nanotemplate with the silver layer on the nanotemplate as the substrate. In the above process, nicotinic acid can be used as a stabilizer and a brightener. On the one hand, as a stabilizer, nicotinic acid can form a complex with the remaining silver ions, thereby reducing the concentration of free silver ions and hindering the uneven deposition and particle aggregation of silver ions in the nicotinic acid solution. On the other hand, as a brightener, nicotinic acid can increase the crystallinity of silver nanowires, making the crystal structure of the deposit more perfect. In the above technical scheme of the present invention, compared with the existing cyanide solution, the nicotinic acid solution has the characteristics of low toxicity and low pollution, and the preparation process is simple, which solves the technical problems of the complicated preparation process and high cost in the preparation process of the existing silver nanowires due to the use of cyanide solution as the electrolyte.
[0025] Furthermore, the silver layer on the surface of the nano-template can be prepared by a magnetron sputtering machine through a sputtering technique; for example, in the process of preparing the silver layer by the sputtering technique, silver is used as a target material, and the deposition power is 80 W and the background vacuum degree during sputtering is 8×10 -5 Pa, the substrate bias voltage is -80V, and high-purity argon is introduced as an ionizing gas, wherein the flow rate of argon can be 30-60sccm, and the silver plating time can be 2-5 minutes, so that a layer of Ag electrode layer is sputtered on the reverse side of the nano template, and the thickness of the Ag electrode layer can be 60-150nm, so as to form the above-mentioned silver layer on the reverse side of the nano template. In another example, the flow rate of argon is 50sccm, the silver plating time can be 2 minutes, 3 minutes, 4 minutes or 5 minutes, and the cumulative thickness of Ag atoms, that is, the thickness of the silver layer can be 60nm, 90nm, 120nm or 150nm.
[0026] As a possible implementation mode, in the electrochemical deposition preparation method of silver nanowires of the present invention, the nicotinic acid solution also includes 0.8-0.98 mol / L potassium hydroxide and 0.9-1.0 mol / L ammonium acetate. In the case of the above technical solution, by adding potassium hydroxide and ammonium acetate, and controlling the addition amount of potassium hydroxide and ammonium acetate within a reasonable range, the pH value of the nicotinic acid solution can be adjusted to 9-9.5. Furthermore, by controlling the pH value of the nicotinic acid solution to 9-9.5, on the one hand, the stability of silver ions in the nicotinic acid solution can be improved, thereby preparing higher quality silver nanowires. On the other hand, by controlling the pH value of the nicotinic acid solution to 9-9.5, the integrity of the nano template can be protected, and the over-acidic or over-alkaline electrolyte environment can be avoided. Damage to the pore structure or overall structure of the nano template.
[0027] As a possible implementation manner, the preparation process of the nicotinic acid solution in the present invention may be: According to the content of each component, a certain volume of deionized water is measured with a beaker, and then an appropriate amount of potassium hydroxide and potassium carbonate are poured into the beaker to dissolve them, and then an appropriate amount of nicotinic acid and ammonium acetate are added to the solution successively, and then an appropriate amount of silver nitrate is dissolved with a small amount of water, and the dissolved silver nitrate solution is poured into the above beaker, and stirred to completely dissolve the white flocculent; finally, a calculated amount of ammonia water is added, and it is transferred to a volumetric flask and deionized water is added to the required volume. The pH value of the nicotinic acid solution is between 9.0 and 9.5.
[0028] It should be understood that in order to ensure the stability of the above-mentioned electrochemical deposition process, improve the quality of the prepared silver nanowires, and enable the prepared silver nanowires to meet different application requirements, it is also necessary to control the thickness of the nanotemplate and the diameter of the through hole within a reasonable range. For example, the thickness of the nanotemplate can be 40~60mm, and the diameter of the through hole can be 40~360nm; for another example, the thickness of the nanotemplate can be 40mm, 50mm or 60mm, and the diameter of the through hole can be 40nm, 100nm, 200nm or 300nm.
[0029] As a possible manner, in the electrochemical deposition preparation method of silver nanowires of the present invention, the thickness of the silver layer disposed on the reverse side may be 60-150 nm.
[0030] In the case of adopting the above technical solution, the silver layer serves as the starting point of the above electrochemical deposition, and its thickness directly affects the subsequent growth quality of the silver nanowires. If the silver layer is too thin, it may not provide sufficient support for the growth of the silver nanowires, resulting in uneven growth of the nanowires or the formation of defects. On the contrary, if the silver layer is too thick, it may increase resistance, reduce electron transfer efficiency, and reduce the deposition rate. Furthermore, an overly thick silver layer may produce excessive stress on the template, causing deformation or damage to the template during the deposition process. By way of example, the thickness of the silver layer may be 60nm, 100nm, or 150nm.
[0031] It should also be understood that in order to further improve the quality of the prepared silver nanowires, the current density and deposition time during the electrochemical deposition process should be controlled within a reasonable range; for example, during the electrochemical deposition process, the current density is 0.2-0.4 mA / cm 2 , the deposition time is 500-1500 seconds; in another example, during the electrochemical deposition process, the current density can be 0.2 mA / cm 2 , 0.25mA / cm 2 , 0.3mA / cm 2 or 0.4mA / cm 2, the deposition time can be 500 seconds, 700 seconds, 900 seconds, 1100 seconds, 1300 seconds or 1500 seconds.
[0032] As a possible implementation manner, in the electrochemical deposition preparation method of silver nanowires of the present invention, after the silver nanowires are prepared in the through-holes of the nano-template by electrochemical deposition, the method further comprises: After removing the silver layer on the reverse side of the nano template, the nano template is removed by soaking in an alkaline solution; collecting the silver nanowires dispersed in the alkaline solution; Wherein, the alkaline solution is a 1.5-3 mol / L sodium hydroxide solution, and the soaking time is 30-60 minutes.
[0033] In the case of adopting the above technical solution, one end of the silver nanowire is connected to the silver layer in the through hole of the nano template, that is, the silver nanowire is deposited on the surface of the silver layer in the through hole of the nano template, and the purpose of removing the silver layer on the reverse side of the nano template is to separate the silver nanowire from the silver layer, thereby facilitating the collection of the prepared silver nanowire. The nano template can be completely removed by soaking in an alkaline solution and controlling the concentration of the alkaline solution and the soaking time. For example, the concentration of the alkaline solution can be 1.5 mol / L, 2.5 mol / L or 3.0 mol / L, and the soaking time can be 30 minutes, 40 minutes or 60 minutes. For example, the silver layer on the reverse side of the nano template can be removed by polishing or chemical etching; for another example, the silver layer on the reverse side of the nano template can be removed by polishing, which can be: using alumina particle slurry with a diameter of 5 to 6 mm to polish the silver layer on the reverse side of the nano template to remove the silver layer on the reverse side of the template.
[0034] As a possible implementation manner, in the electrochemical deposition preparation method of silver nanowires of the present invention, the step of collecting the silver nanowires dispersed in the alkaline solution comprises: The silver nanowires dispersed in the alkaline solution were collected by centrifugation; The silver nanowires were cleaned with deionized water and then stored in ultrapure water at room temperature.
[0035] In the case of adopting the above technical solution, the silver nanowires dispersed in the alkaline solution can be collected by centrifugation; for example, during the centrifugation process, the high-speed rotating centrifuge will generate a huge centrifugal force, which can separate the nanowires from the solution and then precipitate them to the bottom or wall of the container, thereby realizing the efficient collection of the silver nanowires. For example, the rotation speed during the centrifugation process can be 4000~6000rpm, and the centrifugation time can be 4~6 minutes. For another example, the rotation speed during the centrifugation process can be 4000rpm, 5000rpm or 6000rpm, and the centrifugation time can be 4 minutes, 5 minutes or 6 minutes. In the process of washing the silver nanowires with deionized water, the number of washings can be 3 times, 4 times or 5 times. The cleaned silver nanowires are placed in ultrapure water for storage at room temperature, which can maintain good stability and dispersibility. Ultrapure water has extremely low conductivity and impurity content, and can provide a stable storage environment to prevent the silver nanowires from agglomerating or precipitating. At the same time, room temperature conditions also avoid the influence of extreme temperature on the performance of silver nanowires, ensuring that the prepared silver nanowires can be stored stably for a long time.
[0036] As a possible implementation, in the electrochemical deposition preparation method of silver nanowires of the present invention, after obtaining a nano template and providing a silver layer on the reverse side of the nano template, the method further comprises: The nano template is ultrasonically treated for 3 to 5 minutes, and the ultrasonic treatment liquid is a nicotinic acid solution.
[0037] In the case of the above technical solution, after the silver layer is provided on the reverse side of the nano-template, the air in the through-holes of the nano-template can be removed by ultrasonic treatment, so that the nicotinic acid solution can smoothly enter the through-holes, thereby preparing higher quality silver nanowires; for example, the ultrasonic treatment time can be 3 minutes, 4 minutes or 5 minutes, and the ultrasonic treatment liquid can be the nicotinic acid solution described in the above technical solution.
[0038] In a second aspect, the present invention provides a silver nanowire, which is prepared by the electrochemical deposition preparation method of the silver nanowire described in the above technical solution.
[0039] In the case of adopting the above technical solution, the silver nanowires of the present invention are prepared by the electrochemical deposition preparation method of the silver nanowires described in the above technical solution. In the preparation process of the silver nanowires, the silver layer arranged on the reverse side has good conductivity, and the silver layer can provide a stable substrate for the deposition or growth of the silver nanowires. For example, the nano template can be a nanoporous anodic aluminum oxide (AAO) template. The electrolyte is a nicotinic acid solution, in which potassium carbonate can improve the conductivity of the nicotinic acid solution, silver nitrate is used to provide silver ions, ammonia water and nicotinic acid are both complexing agents, wherein ammonia water is the main complexing agent. In the nicotinic acid solution, the silver ions first form a complex with ammonia water [Ag(NH3)2] + , the remaining free silver ions can be further complexed with nicotinic acid, and the effective concentration of silver ions in the nicotinic acid solution can be increased by forming a complex with ammonia water, nicotinic acid and silver ions. Furthermore, the above complex can slowly and controllably release the silver ions, and then form a silver nanowire structure with uniform thickness and high density in the through-holes of the nanotemplate with the silver layer on the nanotemplate as the substrate. Nicotinic acid can be used as both a stabilizer and a brightener. On the one hand, as a stabilizer, nicotinic acid can form a complex with the remaining silver ions, thereby reducing the concentration of free silver ions and hindering the uneven deposition and particle aggregation of silver ions in the nicotinic acid solution. On the other hand, as a brightener, nicotinic acid can increase the crystallinity of the silver nanowires, making the crystal structure of the deposit more perfect. Thus, the above silver nanowires with uniform thickness, good density and smooth surface are prepared.
[0040] Furthermore, after the silver nanowires are cleaned with deionized water, they are placed in ultrapure water at room temperature and stored, which can also be considered as obtaining a silver nanowire solution; the silver nanowire solution is added to a hydrogen peroxide solution with a concentration of 10-20%, and mixed for 0.5-2 minutes. Through the incomplete corrosion of the hydrogen peroxide solution at the above concentration, a porous structure can be obtained on the surface of the silver nanowires, and silver nanowires with better flexibility or toughness can be obtained. For example, in this process, the volume ratio of the silver nanowire solution to the hydrogen peroxide solution can be 1: (0.5-1.5), and the concentration of the hydrogen peroxide solution can be 10%, 15% or 20%. It should be noted that in the above technical solution, the silver nanowires in the silver nanowire solution are usually difficult to measure, but as long as there are silver nanowires in the silver nanowire solution, incomplete corrosion will be achieved, thereby obtaining a porous structure on the surface of the silver nanowires, further improving the flexibility or toughness of the silver nanowires.
[0041] In a third aspect, the present invention provides the application of the above-mentioned silver nanowires in flexible micro-nano robots.
[0042] When the above technical solution is adopted, the flexible micro-nano robot can have a flexible silver hinge, which is made of the silver nanowires described in the above technical solution.
[0043] In order to better understand the present invention, the content of the present invention is further explained below in conjunction with specific embodiments, but the content of the present invention is not limited to the following embodiments.
[0044] Unless otherwise specified, the raw materials used in the following examples are commercially available. Example 1
[0045] This embodiment provides a method for preparing silver nanowires by electrochemical deposition, comprising the following steps: S100, obtaining a nanoporous anodic aluminum oxide (AAO) template, wherein the nanoporous anodic aluminum oxide template has a front side and a back side, a plurality of through holes are disposed between the front side and the back side, and a silver layer is disposed on the back side; The porous anodized aluminum template has a diameter of 13 mm (the template is circular), a thickness of 40 mm, a through hole diameter of 100 nm, and a silver layer is provided on the reverse side, the thickness of the silver layer is 60 nm; S200, such as Figure 4 As shown, Figure 4 Schematic diagram of the electrochemical deposition device used in this embodiment, the platinum electrode 1 and the copper electrode 5 are connected to a DC regulated power supply 8, a reactor 6 and a nano template 4 are provided at the end of the copper electrode 5, the silver layer of the nano template 4 is in contact with the copper electrode 5 through the limiting effect of the reactor plug 3 and the annular gasket 7, and the platinum electrode 1 and the nano template 4 are arranged in the electrolyte 2; the nanoporous anodized aluminum template is used as the cathode, the platinum sheet is used as the anode, and the nicotinic acid solution is used as the electrolyte, and silver nanowires are prepared in the through holes of the porous anodized aluminum template by electrochemical deposition; The nicotinic acid solution includes 30 ml / L of ammonia water, 0.5 mol / L of potassium carbonate, 0.73 mol / L of nicotinic acid, 0.25 mol / L of silver nitrate, 0.8 mol / L of potassium hydroxide and 0.9 mol / L of ammonium acetate. The pH value of the nicotinic acid solution is 9.4. A DC regulated power supply is used during the electrochemical deposition process, and the current density is 0.2 mA / cm 2 , the deposition time is 1500 seconds. Example 2
[0046] This embodiment provides a method for preparing silver nanowires by electrochemical deposition, comprising the following steps: S100, obtaining a nanoporous anodic aluminum oxide (AAO) template, wherein the nanoporous anodic aluminum oxide template has a front side and a back side, a plurality of through holes are disposed between the front side and the back side, and a silver layer is disposed on the back side; The porous anodized aluminum template has a diameter of 13 mm (the template is circular), a thickness of 60 mm, a through hole diameter of 300 nm, and a silver layer is provided on the reverse side, the thickness of the silver layer is 150 nm; S200, such as Figure 4 As shown, Figure 4 Schematic diagram of the electrochemical deposition device used in this embodiment, with a nanoporous anodic aluminum oxide template as a cathode, a platinum sheet as an anode, and a nicotinic acid solution as an electrolyte, and silver nanowires are prepared in the through holes of the porous anodic aluminum oxide template by electrochemical deposition; The nicotinic acid solution includes 35 ml / L of ammonia water, 0.6 mol / L of potassium carbonate, 0.89 mol / L of nicotinic acid, 0.3 mol / L of silver nitrate, 0.89 mol / L of potassium hydroxide and 0.95 mol / L of ammonium acetate. The pH value of the nicotinic acid solution is 9.3. A DC regulated power supply is used during the electrochemical deposition process, and the current density is 0.4 mA / cm 2 , the deposition time is 500 seconds; S300, polishing the silver layer on the reverse side of the porous anodized aluminum template using an aluminum oxide particle slurry with a diameter of 5-6 μm to remove the silver layer on the reverse side; and then soaking in a 1.5 mol / L sodium hydroxide solution for 60 minutes; S400, collecting the silver nanowires dispersed in the sodium hydroxide solution by centrifugation; washing the silver nanowires with deionized water for 4 times, and storing them in ultrapure water at room temperature; wherein the rotation speed during the centrifugation is 4000 rpm and the centrifugation time is 6 minutes. Example 3
[0047] This embodiment provides a method for preparing silver nanowires by electrochemical deposition, comprising the following steps: S100, obtaining a nanoporous anodic aluminum oxide (AAO) template, wherein the porous anodic aluminum oxide template has a diameter of 13 mm (the template is circular), a thickness of 50 mm, and a through-hole diameter of 200 nm; S200, sputtering a silver layer on the reverse side of the nanoporous anodic aluminum oxide template by using a magnetron sputtering machine, wherein the thickness of the silver layer is 100 nm; ultrasonically treating the nanoporous anodic aluminum oxide template in a nicotinic acid solution for 3 minutes; In the process of preparing the silver layer by the sputtering technology, silver is used as the target material, the deposition power is 80W, the background vacuum degree during sputtering is 8×10 -5 Pa, the substrate bias voltage is -80V, and high-purity argon is introduced as the ionizing gas, wherein the flow rate of the argon is 50sccm, and the silver plating time is 3 minutes and 40 seconds, so that a layer of Ag electrode is sputtered on the first surface of the porous anodized aluminum template, and the thickness of the Ag electrode is 100nm; S300, such as Figure 4 As shown, Figure 4Schematic diagram of the electrochemical deposition device used in this embodiment, with a nanoporous anodic aluminum oxide template as a cathode, a platinum sheet as an anode, and a nicotinic acid solution as an electrolyte, and silver nanowires are prepared in the through holes of the porous anodic aluminum oxide template by electrochemical deposition; The nicotinic acid solution includes 32 ml / L ammonia water, 0.55 mol / L potassium carbonate, 0.8 mol / L nicotinic acid, 0.28 mol / L silver nitrate, 0.85 mol / L potassium hydroxide and 1 mol / L ammonium acetate. The pH value of the nicotinic acid solution is 9.2. A DC regulated power supply is used during the electrochemical deposition process, and the current density is 0.3 mA / cm 2 , deposition time is 1000 seconds; S400, taking the porous anodized aluminum template out of the electrochemical deposition device and rinsing it with deionized water to remove the electrolyte on its surface; S500, polishing the silver layer on the reverse side of the porous anodized aluminum template using an aluminum oxide particle slurry with a diameter of 5 to 6 mm to remove the silver layer on the reverse side; and then soaking in a 3 mol / L sodium hydroxide solution for 30 minutes; S600, collecting the silver nanowires dispersed in the sodium hydroxide solution by centrifugation; washing the silver nanowires with deionized water for 5 times, and storing them in ultrapure water at room temperature to obtain a silver nanowire solution; wherein the rotation speed during the centrifugation is 5000 rpm and the centrifugation time is 5 minutes.
[0048] The surface morphology of the silver nanowires prepared in Examples 1 to 3 is shown in FIG. Figure 1 As shown, specifically, Figure 1 Schematic diagram of the surface morphology of the silver nanowires prepared in Example 3, while the surface morphology of the silver nanowires prepared in Example 1 and Example 2 is similar to Figure 1 Similar. Figure 1 It can be seen that the silver nanowires prepared in Example 3 are uniform in thickness, good in density and smooth in surface. The length of the silver nanowires prepared in Example 3 is 17.5 mm and the deposition rate is 17.5 nm / s. Example 4
[0049] The electrochemical deposition preparation method of the silver nanowires in this embodiment is basically the same as that in Example 3, except that after the silver nanowire solution is prepared in S600, the silver nanowire solution is added to a 15% hydrogen peroxide solution, mixed for 1 minute, and the silver nanowires are collected and washed before being collected; wherein the volume ratio of the silver nanowire solution to the hydrogen peroxide solution is 1:1.
[0050] The silver nanowires prepared in this example are Figure 2 As shown, from Figure 2It can be seen that after being treated with hydrogen peroxide solution, silver nanowires with a porous structure on the surface are obtained. Due to the presence of the porous structure, the silver nanowires prepared in this embodiment have higher flexibility or toughness than the silver nanowires prepared in Examples 1 to 3.
[0051] It should be noted that after the silver nanowires of the above-mentioned embodiments 1 to 4 are prepared respectively, they can be applied to flexible micro-nano robots. The silver nanowires prepared in the above-mentioned embodiments are uniform in thickness, good in density, and have good flexibility or toughness. Micro-nano robots refer to small robots with a scale of micro-nano (several nanometers to hundreds of micrometers), and have broad application prospects in the fields of biosensing, targeted drug delivery, embolization therapy, minimally invasive surgery, cell manipulation, pollutant degradation, micro-nano manufacturing, etc. The silver nanowires prepared by the present invention are applied to micro-nano robots, which helps to improve the flexibility and deformability of the robots and make them better adapt to various complex environments. It should also be noted that in the application of the medical field, the biocompatibility and safety of micro-nano robots are crucial. The silver nanowires of the present invention have good biocompatibility and antibacterial properties, which can reduce the risk of stimulation and infection to biological tissues, so that the micro-nano robots based on the silver nanowires of the present invention have higher safety and reliability in the fields of medical diagnosis, treatment and drug delivery.
[0052] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing silver nanowires by electrochemical deposition, It is characterized in that include: Obtain a nano template, wherein the nano template has a front side and a back side, a plurality of through holes are provided between the front side and the back side, and a silver layer is provided on the back side; Using the nano template as a cathode, a platinum sheet as an anode, and a nicotinic acid solution as an electrolyte, silver nanowires are prepared in the through holes of the nano template by electrochemical deposition; The nicotinic acid solution comprises 30-35 ml / L of ammonia water, 0.5-0.6 mol / L of potassium carbonate, 0.73-0.89 mol / L of nicotinic acid, and 0.25-0.3 mol / L of silver nitrate; the pH value of the nicotinic acid solution is 9-9.
5.
2. The electrochemical deposition method for preparing silver nanowires according to claim 1, It is characterized in that The nicotinic acid solution also includes 0.8-0.98 mol / L potassium hydroxide and 0.9-1.0 mol / L ammonium acetate.
3. The electrochemical deposition method for preparing silver nanowires according to claim 2, It is characterized in that The thickness of the nano template is 40-60 mm, and the diameter of the through hole is 40-360 nm.
4. The electrochemical deposition method for preparing silver nanowires according to claim 3, It is characterized in that The thickness of the silver layer arranged on the reverse side is 60-150 nm.
5. The electrochemical deposition method for preparing silver nanowires according to claim 4, It is characterized in that During the electrochemical deposition process, the current density is 0.2-0.4 mA / cm 2 , the deposition time is 500~1500 seconds.
6. The electrochemical deposition method for preparing silver nanowires according to claim 1, It is characterized in that After preparing the silver nanowires in the through holes of the nano template by electrochemical deposition, the method further comprises: After removing the silver layer on the reverse side of the nano template, the nano template is removed by soaking in an alkaline solution; collecting the silver nanowires dispersed in the alkaline solution; Wherein, the alkaline solution is a 1.5-3 mol / L sodium hydroxide solution, and the soaking time is 30-60 minutes.
7. The method for preparing silver nanowires by electrochemical deposition according to claim 6, It is characterized in that The method of collecting the silver nanowires dispersed in the alkaline solution comprises: The silver nanowires dispersed in the alkaline solution were collected by centrifugation; The silver nanowires were cleaned with deionized water and then stored in ultrapure water at room temperature.
8. The method for preparing silver nanowires by electrochemical deposition according to claim 1, It is characterized in that The method of obtaining a nano template and providing a silver layer on the reverse side of the nano template further comprises: The nano template is ultrasonically treated for 3 to 5 minutes, and the ultrasonic treatment liquid is a nicotinic acid solution.
9. A silver nanowire, It is characterized in that The silver nanowires are prepared by the electrochemical deposition method according to any one of claims 1 to 8.
10. Use of the silver nanowire according to claim 9 in a flexible micro-nano robot.
Citation Information
Cited By
Universal preparation method and device for metal micro-nano structure
CN121571660A
A general method and device for preparing metal micro-nano structures
CN121571660B
Method for preparing silver nanowire through electrolytic silver elementary substance water-phase synthesis and silver nanowire
CN122039160A