Perovskite light absorption layer, perovskite cell and preparation method thereof, and photovoltaic module

By combining perovskite light-absorbing materials and passivation materials with specific structures in perovskite solar cells, the problem of taking into account the photoelectric conversion efficiency and stability of traditional perovskite cells is solved, and efficient photoelectric conversion and long-term stability are achieved.

CN119012735APending Publication Date: 2024-11-22TRINA SOLAR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411183200.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional perovskite solar cells cannot take into account both photoelectric conversion efficiency and stable performance. The existence of defects in light-absorbing materials leads to non-radiative recombination and phase decomposition of carriers, affecting battery performance.

Method used

The perovskite absorbing material is combined with the passivation material of a specific structure, and the energy level between the absorbing layer and the transport layer is adjusted through the passivation material, interface defects are repaired, and perovskite absorbing layer and passivation layer are formed layered. Optimize the concentration and thickness ratio of the passivation material.

Benefits of technology

Effectively improve the photoelectric conversion efficiency and stability of perovskite batteries, and improve the long-term stability and performance of the battery by passivating surface defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119012735A_ABST
    Figure CN119012735A_ABST
Patent Text Reader

Abstract

The invention relates to a perovskite light absorption layer, a perovskite cell, a preparation method of the perovskite cell and a photovoltaic module. The perovskite light absorption layer comprises a perovskite light absorption material and a passivation material, and the structural formula of the passivation material is shown as a formula (I). The passivation material with the specific structure can effectively adjust the energy level between a perovskite light absorption layer and a transmission layer, and effectively passivates surface defects, thereby effectively improving the photoelectric conversion efficiency and the stability of the perovskite cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular to a perovskite light-absorbing layer, a perovskite battery and a preparation method thereof, and a photovoltaic module. Background Art

[0002] Vigorously developing solar cells and improving the utilization rate of solar energy is an important way to solve human energy problems and protect the earth's environment. In recent years, perovskite solar cells (PSCs) have developed rapidly as a new generation of photovoltaic technology, which is expected to solve the problems of high cost and low efficiency of current solar cell technology. However, traditional perovskite solar cells cannot take into account both photoelectric conversion efficiency and stable performance.

[0003] Therefore, it is necessary to improve the traditional technology. Summary of the invention

[0004] Based on this, the present application provides a perovskite light-absorbing layer, a perovskite cell and a preparation method thereof, and a photovoltaic module with high photoelectric conversion efficiency and good stability.

[0005] The technical solution of this application to solve the above technical problems is as follows.

[0006] In a first aspect, the present application provides a perovskite light-absorbing layer, comprising a perovskite light-absorbing material and a passivation material, wherein the passivation material has a structural formula as shown in formula (I):

[0007]

[0008] Among them, R 1 Selected from hydrogen, amino, C 1 ~C 20 alkyl, halogen, nitro, hydroxyl, thiol, carboxyl, cyano, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 6 ~C 20 Aryl, substituted or unsubstituted C 2 ~C 20 Heterocyclic group and substituted or unsubstituted C 2 ~C 20 at least one of heteroaryl groups;

[0009] R 2 Selected from hydrogen, amino, C 1 ~C 20 alkyl, nitro, halogen, cyano, carboxyl, formyl, hydroxymethyl, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 1 ~C20 Alkoxy, substituted or unsubstituted C 3 ~C 20 Cycloalkyl, substituted or unsubstituted C 6 ~C 20 Aryl, substituted or unsubstituted C 2 ~C 20 Heterocyclic group and substituted or unsubstituted C 2 ~C 20 at least one of heteroaryl groups;

[0010] R 3 and R 4 are independently selected from hydrogen, amino, C 1 ~C 20 alkyl, halogen, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 6 ~C 20 Aryl, substituted or unsubstituted C 2 ~C 20 Heterocyclic group and substituted or unsubstituted C 2 ~C 20 at least one of heteroaryl groups;

[0011] R 2 , R 3 and R 4 At least one of them is not hydrogen.

[0012] In some embodiments, in the perovskite light absorbing layer, the formula (I) satisfies at least one of the following characteristics:

[0013] (1) R 1 is selected from hydrogen and substituted or unsubstituted C 1 ~C 10 at least one of the alkyl groups;

[0014] (2) R 2 is selected from hydrogen, formyl, amino, C 1 ~C 10 Amine alkyl and substituted or unsubstituted C 1 ~C 10 at least one of the alkyl groups;

[0015] (3) R 3 and R 4 are independently selected from hydrogen, halogen and substituted or unsubstituted C 1 ~C 10 At least one of the alkyl groups.

[0016] In some embodiments, in the perovskite light absorbing layer, the formula (I) satisfies at least one of the following characteristics:

[0017] (1) R 1 One selected from hydrogen and ethyl;

[0018] (2) R 2 is selected from one of hydrogen, formyl and aminomethyl;

[0019] (3) R 3 and R 4 Each is independently selected from hydrogen and methyl.

[0020] In some embodiments, in the perovskite light absorption layer, the passivation material includes at least one of the compounds represented by formula (I-1) to formula (I-3):

[0021] .

[0022] In some of the embodiments, in the perovskite light absorbing layer, the passivation material and the perovskite light absorbing material are mixed with each other, and the mass ratio of the passivation material to the perovskite light absorbing material is 0.0001~0.01:1.

[0023] In some of the embodiments, in the perovskite light absorbing layer, the perovskite light absorbing layer includes a stacked perovskite material layer and a passivation layer, the perovskite material layer includes the perovskite light absorbing material, and the passivation layer includes the passivation material.

[0024] In some embodiments, in the perovskite light absorbing layer, the perovskite light absorbing layer satisfies at least one of the following characteristics:

[0025] (1) The thickness of the passivation layer is 1 nm to 10 nm;

[0026] (2) The thickness of the perovskite material layer is 10 nm to 100 μm;

[0027] (3) The thickness ratio of the passivation layer to the perovskite material layer is 0.00125~0.025:1.

[0028] The second aspect of the present application provides a method for preparing a perovskite light absorbing layer, comprising the following steps:

[0029] Providing a perovskite precursor, a passivation material and a solvent according to the above perovskite light absorbing layer;

[0030] Mixing the perovskite precursor, the passivation material and the solvent to prepare a perovskite passivation solution;

[0031] The perovskite passivation solution is disposed on the surface of a substrate and subjected to a first annealing treatment to form a perovskite light absorbing layer on the surface of the substrate.

[0032] The present application also provides a method for preparing a perovskite light absorbing layer, comprising the following steps:

[0033] Providing a perovskite precursor, a passivation material and a solvent according to the above perovskite light absorbing layer;

[0034] Mixing the perovskite precursor and a portion of the solvent to prepare a perovskite precursor solution;

[0035] Placing the perovskite precursor solution on the surface of a substrate and performing a second annealing treatment to form a perovskite material layer on the surface of the substrate;

[0036] Mixing the passivation material and the remaining solvent to prepare a passivation solution;

[0037] The passivation solution is disposed on the surface of the perovskite material layer away from the substrate to form a passivation layer on the surface of the perovskite material layer away from the substrate. The perovskite light absorbing layer includes the perovskite material layer and the passivation layer.

[0038] In some of the embodiments, in the method for preparing the perovskite light absorbing layer, the solvent includes a first solvent and a second solvent, the first solvent includes at least one of N,N-dimethylformamide and dimethyl sulfoxide, and the second solvent includes at least one of isopropanol and ethanol.

[0039] In some of the embodiments, in the method for preparing the perovskite light absorbing layer, in the step of preparing the perovskite precursor solution, the perovskite precursor and the first solvent are mixed; in the step of preparing the passivation solution, the passivation material and the second solvent are mixed.

[0040] In some of the embodiments, in the method for preparing the perovskite light absorbing layer, the concentration of the passivation material in the passivation solution is 0.2 mg / mL to 10 mg / mL.

[0041] A third aspect of the present application provides a perovskite cell, comprising a first electrode, the above-mentioned perovskite light-absorbing layer or the perovskite light-absorbing layer prepared by the above-mentioned preparation method, and a second electrode.

[0042] A fourth aspect of the present application provides a method for preparing a perovskite battery, comprising the following steps:

[0043] providing a first electrode;

[0044] Forming the above-mentioned perovskite light-absorbing layer or the perovskite light-absorbing layer prepared by the above-mentioned preparation method on the surface of the first electrode;

[0045] A second electrode is formed on a surface of the perovskite light absorbing layer away from the first electrode.

[0046] A fifth aspect of the present application provides a photovoltaic module, comprising the above-mentioned perovskite cell or the perovskite cell prepared by the above-mentioned preparation method.

[0047] Compared with the prior art, the perovskite light absorbing layer of the present application has the following beneficial effects:

[0048] The perovskite light-absorbing layer of the present application includes a perovskite light-absorbing material and a passivation material. The passivation material with a specific structure can effectively adjust the energy level between the perovskite light-absorbing layer and the transmission layer, effectively passivate surface defects, and thus effectively improve the photoelectric conversion efficiency and stability of the perovskite battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0050] Figure 1 A comparison chart of the stability tests of the perovskite cells provided in Examples 1 to 3, 7 and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0051] References to embodiments of the present invention will now be provided in detail, one or more examples of which are described below. Each example is provided as an explanation rather than a limitation of the present invention. In fact, it will be apparent to those skilled in the art that various modifications and variations may be made to the present invention without departing from the scope or spirit of the present invention. For example, a feature illustrated or described as part of one embodiment may be used in another embodiment to produce a further embodiment.

[0052] Therefore, it is intended that the present invention covers such modifications and variations that fall within the scope of the appended claims and their equivalents. Other objects, features and aspects of the present invention are disclosed in or are obvious from the following detailed description. Those of ordinary skill in the art will appreciate that this discussion is only a description of exemplary embodiments and is not intended to limit the broader aspects of the present invention.

[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0054] The term "comprises", "comprising" or any other variant thereof is intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprising one..." do not exclude the presence of other identical elements in the process, method, article or equipment including the elements. The indefinite articles "a kind of" and "an" before the elements or components of the present invention are not restrictive to the quantity requirements (i.e., the number of occurrences) of the elements or components. Therefore, "a" or "a kind of" should be interpreted as including one or at least one, and the elements or components in the singular form also include the plural form, unless the number clearly refers only to the singular form. The meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0055] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0056] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. For example, therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0057] Defects in perovskites usually cause non-radiative recombination of carriers and aggravate the decomposition of perovskite phases, which has a negative impact on the photoelectric conversion efficiency and stability of perovskite solar cells. Introducing suitable materials for surface passivation at the interface of the perovskite active layer / transport layer can repair deep defects at the interface and effectively improve the performance of perovskite solar cells. Traditional passivation materials have poor passivation stability or cannot effectively improve the photoelectric conversion efficiency of perovskite cells, and cannot take into account both photoelectric conversion efficiency and stability performance.

[0058] An embodiment of the present application provides a perovskite light absorbing layer, comprising a perovskite light absorbing material and a passivation material, wherein the passivation material has a structural formula as shown in formula (I):

[0059]

[0060] Among them, R 1 Selected from hydrogen, amino, C 1 ~C 20 alkyl, halogen, nitro, hydroxyl, thiol, carboxyl, cyano, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 6 ~C 20 Aryl, substituted or unsubstituted C 2 ~C 20 Heterocyclic group and substituted or unsubstituted C 2 ~C 20 at least one of heteroaryl groups;

[0061] R 2 Selected from hydrogen, amino, C 1 ~C 20 alkyl, nitro, halogen, cyano, carboxyl, formyl, hydroxymethyl, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 1 ~C 20 Alkoxy, substituted or unsubstituted C 3 ~C 20 Cycloalkyl, substituted or unsubstituted C 6 ~C 20 Aryl, substituted or unsubstituted C 2 ~C 20 Heterocyclic group and substituted or unsubstituted C 2 ~C 20 at least one of heteroaryl groups;

[0062] R 3 and R 4 are independently selected from hydrogen, amino, C 1 ~C 20 alkyl, halogen, substituted or unsubstituted C 1 ~C 20 Alkyl, substituted or unsubstituted C 6 ~C 20 Aryl, substituted or unsubstituted C 2 ~C 20 Heterocyclic group and substituted or unsubstituted C 2 ~C 20 at least one of heteroaryl groups;

[0063] R2 , R 3 and R 4 At least one of them is not hydrogen.

[0064] The perovskite light-absorbing layer of the present application includes a perovskite light-absorbing material and a passivation material with a specific structure. The passivation material with a specific structure can effectively adjust the energy level between the perovskite light-absorbing layer and the transmission layer, effectively passivate surface defects, and thus effectively improve the photoelectric conversion efficiency and stability of the perovskite battery.

[0065] It is understandable that amino-NH 2 , C 1 ~C 20 The aminoalkyl group refers to -(CH 2 ) n NH 2 , where n is an integer from 1 to 20; for example, C 1 ~C 20 The amine alkyl-CH 2 NH 2 , -C 2 H 4 NH 2 , -C 3 H 6 NH 2 At least one of the following; substituted or unsubstituted C 1 ~C 20 In the alkyl group, C 1 ~C 20 Alkyl refers to an alkyl group with 1 to 20 carbon atoms; substituted or unsubstituted C 2 ~C 20 In heterocyclic groups, C 2 ~C 20 A heterocyclic group refers to a heterocyclic group having 2 to 20 ring carbon atoms, wherein the heteroatoms on the ring include at least one of nitrogen, oxygen, sulfur, etc.; a substituted or unsubstituted C 2 ~C 20 In heteroaryl, C 2 ~C 20 Heteroaryl refers to a heteroaryl group having 2 to 20 ring carbon atoms, wherein the heteroatoms on the ring include at least one of nitrogen, oxygen, sulfur, etc.; substituted or unsubstituted C 6 ~C 20 In aromatic groups, C 6 ~C 20 Aryl refers to an aromatic group having 6 to 20 ring carbon atoms; further, C 1 ~C 20The alkyl group includes, but is not limited to, at least one of methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc., wherein the propyl group includes at least one of n-propyl and isopropyl, and the butyl group includes at least one of n-butyl, isobutyl, tert-butyl, and sec-butyl; the substituted C 1 ~C 20 Alkyl, substituted C 1 ~C 20 Alkoxy, substituted C 3 ~C 20 Cycloalkyl, substituted C 6 ~C 20 Aryl, substituted C 2 ~C 20 Heterocyclic and substituted C 2 ~C 20 The substituents in the heteroaryl group independently include, but are not limited to, at least one of amino, halogen, nitro, hydroxyl, thiol, carboxyl, cyano, etc.; for example, halogen-substituted C 1 ~C 20 Alkoxy, nitro substituted C 1 ~C 20 Alkoxy, etc.

[0066] In some of these examples, in the perovskite absorber, R 1 is selected from hydrogen, hydroxyl and substituted or unsubstituted C 1 ~C 10 At least one of the alkyl groups.

[0067] Furthermore, R 1 is selected from hydrogen, hydroxyl and unsubstituted C 1 ~C 8 At least one of the alkyl groups.

[0068] Optionally, R 1 Selected from hydrogen and C 1 ~C 4 One of the alkyl groups.

[0069] Furthermore, in the perovskite light-absorbing layer, R 1 One selected from hydrogen and ethyl.

[0070] In some of these examples, in the perovskite absorber, R 2 is selected from hydrogen, formyl, amino, C 1 ~C 10 Amine alkyl and substituted or unsubstituted C 1 ~C 10 At least one of the alkyl groups.

[0071] Furthermore, R 2 is selected from hydrogen, formyl, amino, C 1 ~C8 Amine alkyl and substituted or unsubstituted C 1 ~C 8 At least one of the alkyl groups.

[0072] Optionally, R 2 Selected from hydrogen, formyl (-CHO) and aminomethyl (-CH 2 NH 2 )one of the.

[0073] R 2 , R 3 and R 4 When at least one of the amino groups is or contains an amino group, the lone pair of electrons on the amino group can react with the monovalent anions in the perovskite light-absorbing material, anchor the free monovalent anions in the perovskite light-absorbing layer, and form hydrogen bonds between the exposed amino group and the perovskite light-absorbing layer, which can further passivate the defects caused by divalent cations and monovalent anions, thereby further improving the stability of the perovskite battery.

[0074] In some of these examples, in the perovskite absorber, R 3 and R 4 are independently selected from hydrogen, halogen and substituted or unsubstituted C 1 ~C 10 At least one of the alkyl groups.

[0075] It is understood that the halogen includes but is not limited to at least one of F, Cl, Br, I, etc.

[0076] In some of these examples, in the perovskite absorber, R 3 and R 4 are independently selected from hydrogen, halogen and unsubstituted C 1 ~C 8 At least one of the alkyl groups.

[0077] Optionally, R 3 and R 4 are independently selected from hydrogen and unsubstituted C 1 ~C 4 One of the alkyl groups.

[0078] Furthermore, R 3 and R 4 Each is independently selected from hydrogen and methyl.

[0079] In some examples, in the perovskite light absorbing layer, the passivation material includes at least one of the compounds represented by formula (I-1) to formula (I-3):

[0080] .

[0081] It can be understood that the perovskite light absorbing layer includes a perovskite light absorbing material and a passivation material, including the following two schemes:

[0082] Option 1 (the perovskite light-absorbing layer can be only one layer): the passivation material and the perovskite light-absorbing material are mixed with each other.

[0083] In some of these examples, in the perovskite light-absorbing layer, the mass ratio of the passivation material to the perovskite light-absorbing material is 0.0001~0.01:1.

[0084] It can be understood that the mass ratio of the passivation material to the perovskite light absorbing material includes but is not limited to 0.0001:1, 0.001:1, 0.002:1, 0.005:1, 0.008:1, 0.01:1. In some examples, any two of these point values ​​may be used as end values ​​within a range, the same below.

[0085] Optionally, the mass ratio of the passivation material to the perovskite light absorbing material is 0.0001~0.01:1.

[0086] The stability performance can be further improved by controlling the mass ratio of the passivation material to the perovskite light-absorbing material.

[0087] Solution 2 (the perovskite light-absorbing layer is composed of at least two layers): the perovskite light-absorbing layer includes a stacked perovskite material layer and a passivation layer, the perovskite material layer includes a perovskite light-absorbing material, and the passivation layer includes a passivation material.

[0088] In some of these examples, the thickness of the passivation layer in the perovskite light-absorbing layer is 1 nm to 10 nm.

[0089] It can be understood that the thickness of the passivation layer includes but is not limited to 1 nm, 2 nm, 5 nm, 6 nm, 8 nm, and 10 nm.

[0090] In some of these examples, the thickness of the perovskite material layer in the perovskite light-absorbing layer is 10 nm~100 μm.

[0091] It can be understood that the thickness of the perovskite material layer includes but is not limited to 10 nm, 20 nm, 50 nm, 80 nm, and 100 μm.

[0092] In some of these examples, in the perovskite light-absorbing layer, the thickness ratio of the passivation layer to the perovskite material layer is 0.00125~0.025:1.

[0093] It can be understood that the thickness ratio of the passivation layer to the perovskite material layer includes but is not limited to 0.00125:1, 0.005:1, 0.01:1, 0.02:1, and 0.025:1.

[0094] In some of the examples, in the perovskite light absorbing layer, the mass ratio of the passivation material in the passivation layer to the perovskite light absorbing material in the perovskite material layer is 0.0001~0.01:1.

[0095] It can be understood that the mass ratio of the passivation material in the passivation layer to the perovskite light-absorbing material in the perovskite material layer includes but is not limited to 0.0001:1, 0.0005:1, 0.00075:1, 0.001:1, 0.002:1, 0.003:1, 0.005:1, 0.009:1, and 0.01:1.

[0096] In some of the examples, the perovskite light absorbing layer includes ABX 3 , A is a monovalent cation, B is a divalent cation, and X is a monovalent anion.

[0097] The O atoms in the ring of the passivation material can coordinate with the divalent cations in the perovskite light-absorbing material through the lone pair of electrons they contain, and the carboxyl or ester group in the molecule can act as a Lewis base to form a Lewis acid-base adduct defect with the uncoordinated divalent cation. 2 , R 3 and R 4 Specific groups that are not hydrogen can adjust the molecular passivation ability, effectively adjust the energy level between the perovskite light-absorbing layer and the transport layer, and effectively passivate surface defects, thereby effectively improving the photoelectric conversion efficiency and stability of perovskite cells.

[0098] It is understood that this application is for ABX 3 There is no limitation on the types of A monovalent cation, B divalent cation, and X monovalent anion, and any type of light absorbing material in the art can be used.

[0099] Optionally, A includes Cs + , Rb + , CH 3 NH 3 + and CH 2 (NH 2 ) 2 + At least one of .

[0100] Optionally, B includes Pb 2+ , Cu 2+ 、Zn 2+ , Ga 2+ Sn 2+ and Ca 2+ At least one of .

[0101] Optionally, X includes I - Br - , Cl -、F - and SCN - At least one of .

[0102] It can be understood that A, B, and X can each independently be one type, or can each independently be multiple types.

[0103] In some of these examples, the thickness of the perovskite absorber layer ranges from 10 nm to 100 μm.

[0104] It is understood that the thickness of the perovskite light absorbing layer includes but is not limited to 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, and 100 μm.

[0105] An embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising the following steps:

[0106] Step S10: providing a perovskite precursor, a passivation material and a solvent according to the above perovskite light absorbing layer;

[0107] Step S20: mixing a perovskite precursor, a passivation material and a solvent to prepare a perovskite passivation solution;

[0108] Step S30: applying a perovskite passivation solution on the surface of the substrate and performing a first annealing treatment to form a perovskite light absorbing layer on the surface of the substrate.

[0109] It can be understood that in the perovskite light absorbing layer prepared in steps S10 to S30, the passivation material and the titanite light absorbing material are doped and mixed with each other. It can be further understood that the perovskite precursor includes but is not limited to monovalent organic cation halides and divalent organic cation halides.

[0110] In some of the examples, in step S30, the temperature of the first annealing treatment is 100° C. to 150° C., and the time is 10 to 20 minutes.

[0111] It can be understood that the temperature of the first annealing treatment includes but is not limited to 100°C, 110°C, 120°C, 130°C, 140°C, and 150°C, and the time includes but is not limited to 10 min, 12 min, 15 min, 18 min, and 20 min.

[0112] Another embodiment of the present application provides a method for preparing a perovskite light absorbing layer, comprising the following steps:

[0113] Step S40: mixing a perovskite precursor and a portion of a solvent to prepare a perovskite precursor solution;

[0114] Step S50: mixing the passivation material and the remaining solvent to prepare a passivation solution;

[0115] Step S60: placing a perovskite precursor solution on the surface of the substrate and performing a second annealing treatment to form a perovskite material layer on the surface of the substrate;

[0116] Step S70: placing a passivation solution on the surface of the perovskite material layer away from the substrate to form a passivation layer on the surface of the perovskite material layer away from the substrate, wherein the perovskite light absorbing layer includes the perovskite material layer and the passivation layer.

[0117] It can be understood that in the perovskite light absorbing layer prepared in steps S40 to S70, the perovskite light absorbing layer includes a perovskite material layer and a passivation layer, wherein the perovskite material layer includes a perovskite light absorbing material, and the passivation layer includes a passivation material.

[0118] In some of the examples, in the method for preparing the perovskite light-absorbing layer, the solvent includes a first solvent and a second solvent, the first solvent includes at least one of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO), and the second solvent includes at least one of isopropanol and ethanol.

[0119] In some of the examples, in step S40 of preparing a perovskite precursor solution, the perovskite precursor and the first solvent are mixed; in step S50 of preparing a passivation solution, the passivation material and the second solvent are mixed.

[0120] In some of the examples, in step S50, the concentration of the passivation material in the passivation solution is 0.2 mg / mL to 10 mg / mL.

[0121] It is understood that the concentration of the passivation material in the passivation solution includes but is not limited to 0.2 mg / mL, 0.5 mg / mL, 1 mg / mL, 1.5 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL, 5 mg / mL, 8 mg / mL, and 10 mg / mL.

[0122] Optionally, the concentration of the passivation material in the passivation solution is 0.5 mg / mL to 3 mg / mL.

[0123] In some of the examples, in step S60, the temperature of the second annealing treatment is 80° C. to 120° C., and the time is 5 min to 20 min.

[0124] It can be understood that the temperature of the second annealing treatment includes but is not limited to 80° C., 90° C., 100° C., 110° C., and 120° C., and the time includes but is not limited to 5 min, 10 min, 15 min, and 20 min.

[0125] It can be understood that the method of placing the perovskite passivation solution on the substrate surface in step S30, placing the perovskite precursor solution on the substrate surface in step S60, and placing the passivation solution on the surface of the perovskite material layer away from the substrate in step S70 independently includes but is not limited to a solution method. Further, the solution method includes but is not limited to at least one of spin coating, scraper, screen printing, spraying, inkjet printing, dip coating, etc.

[0126] One embodiment of the present application provides a perovskite cell, comprising a first electrode, the above-mentioned perovskite light-absorbing layer or the perovskite light-absorbing layer prepared by the above-mentioned preparation method, and a second electrode.

[0127] In some of the examples, in the perovskite cell, at least one of the first electrode and the second electrode is a transparent conductive electrode.

[0128] In some of the examples, in the perovskite cell, one of the first electrode and the second electrode is a transparent conductive electrode, and the other is one of a transparent conductive electrode and a metal electrode.

[0129] It can be understood that in the perovskite battery, the first electrode and the second electrode may be both transparent conductive electrodes; the first electrode may be a transparent conductive electrode and the second electrode may be a metal electrode; or the first electrode may be a metal electrode and the second electrode may be a transparent conductive electrode. Furthermore, when one of the first electrode and the second electrode is a transparent conductive electrode and the other is a metal electrode, the transparent conductive electrode is a transparent conductive substrate.

[0130] In some of these examples, in the perovskite cell, the metal electrode includes at least one of silver (Ag) and copper (Cu).

[0131] In some of these examples, in the perovskite cell, the transparent conductive electrode includes at least one of indium tin oxide (ITO), indium zinc oxide (IZO), tungsten-doped indium oxide (IWO), and aluminum-doped zinc oxide (AZO).

[0132] In some of the examples, in the perovskite cell, the thickness of the first electrode and the second electrode are independently 20 nm to 200 nm.

[0133] It can be understood that the thickness of the first electrode and the second electrode independently include but are not limited to 20 nm, 50 nm, 80 nm, 100 nm, 120 nm, 150 nm, 180 nm, and 200 nm.

[0134] In some of the examples, the perovskite cell further includes a first transmission layer and a second transmission layer, and the first transmission layer and the second transmission layer are respectively arranged between the first electrode and the perovskite light absorbing layer and between the perovskite light absorbing layer and the second electrode.

[0135] It can be understood that the perovskite cell includes a first electrode, a first transmission layer, the above-mentioned perovskite light-absorbing layer or the perovskite light-absorbing layer prepared by the above-mentioned preparation method, a second transmission layer and a second electrode.

[0136] In some of these examples, in the perovskite cell, one of the first transport layer and the second transport layer is a hole transport layer, and the other is an electron transport layer.

[0137] Furthermore, the perovskite cell includes a first electrode, a hole transport layer, the perovskite light absorbing layer or the perovskite light absorbing layer prepared by the above preparation method, an electron transport layer and a second electrode which are stacked.

[0138] In some of the examples, in the perovskite cell, the perovskite light absorbing layer or the perovskite light absorbing layer prepared by the above preparation method includes a perovskite material layer and a passivation layer, the perovskite material layer is arranged on the surface of the hole transport layer away from the first electrode, and the passivation layer is arranged on the side of the perovskite material layer away from the hole transport layer.

[0139] In some of these examples, in the perovskite cell, the hole transport material in the hole transport layer includes but is not limited to at least one of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), 4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz) and [4-(7H-dibenzocarbazole-7-yl)butyl]phosphonic acid (4PADCB).

[0140] In some of these examples, the thickness of the hole transport layer in perovskite cells is 1 nm to 50 nm.

[0141] In some of these examples, in the perovskite cell, the electron transport material in the electron transport layer includes at least one of fullerene and its derivatives.

[0142] It can be understood that fullerene and its derivatives include but are not limited to at least one of C60, C70 and PCBM.

[0143] In some of these examples, the thickness of the electron transport layer in perovskite cells is 10 nm~50 nm.

[0144] In some of the examples, the perovskite cell further includes a hole blocking layer, which is located between the electron transport layer and the second electrode.

[0145] In some of these examples, the hole-blocking layer in perovskite cells includes bathocuproine (BCP, 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline) and tin dioxide (SnO 2) at least one of the following.

[0146] In some of these examples, the hole-blocking layer in perovskite cells is 3 nm to 10 nm thick.

[0147] It can be understood that the thickness of the hole blocking layer includes but is not limited to 3 nm, 5 nm, 8 nm, and 10 nm.

[0148] An embodiment of the present application provides a method for preparing a perovskite battery, comprising the following steps:

[0149] providing a first electrode;

[0150] Forming the above-mentioned perovskite light-absorbing layer or the perovskite light-absorbing layer prepared by the above-mentioned preparation method on the surface of the first electrode;

[0151] A second electrode is formed on a surface of the perovskite light absorbing layer away from the first electrode.

[0152] In some examples, in the method for preparing a perovskite cell, the step of forming the perovskite light absorbing layer includes:

[0153] A perovskite passivation solution including a perovskite precursor, a passivation material and a solvent is placed on the surface of the first electrode, and is subjected to a first annealing treatment to form a perovskite light absorption layer on the surface of the first electrode.

[0154] In other examples, in the method for preparing a perovskite battery, the step of forming the perovskite light absorbing layer includes:

[0155] Placing a perovskite precursor solution including a perovskite precursor and a first solvent on the surface of the first electrode, and performing a second annealing treatment to form a perovskite material layer on the surface of the first electrode;

[0156] A passivation solution containing a passivation material and a second solvent is placed on a surface of the perovskite material layer away from the first substrate to form a passivation layer on a surface of the perovskite material layer away from the first electrode. The perovskite light absorbing layer includes the perovskite material layer and the passivation layer.

[0157] In some of the examples, the method for preparing the perovskite cell further includes the steps of setting a first transmission layer and a second transmission layer between the first electrode and the perovskite light absorbing layer and between the perovskite light absorbing layer and the second electrode.

[0158] Furthermore, a first transmission layer is arranged between the first electrode and the perovskite light absorbing layer, and a second transmission layer is arranged between the perovskite light absorbing layer and the second electrode.

[0159] In some of the examples, the method for preparing a perovskite cell further includes the step of providing a hole blocking layer between the electron transport layer and the second electrode.

[0160] In some examples, the method for preparing the perovskite cell includes the following steps:

[0161] providing a first electrode;

[0162] forming a hole transport layer on the conductive side surface of the first electrode;

[0163] Forming the above-mentioned perovskite light-absorbing layer or the perovskite light-absorbing layer prepared by the above-mentioned preparation method on the surface of the hole transport layer away from the first electrode;

[0164] An electron transport layer, a hole blocking layer and a second electrode are sequentially formed on a surface of the perovskite light absorbing layer away from the hole transport layer.

[0165] It can be understood that the present application includes but is not limited to the types and thicknesses of the first electrode, the first transmission layer, the perovskite light absorption layer, the second transmission layer and the second electrode as described above; and does not limit the formation method of each layer, for example, including but not limited to one of magnetron sputtering, spin coating, slit coating and evaporation.

[0166] One embodiment of the present application provides a perovskite stack cell, including the above-mentioned perovskite cell or the perovskite cell prepared by the above-mentioned preparation method.

[0167] It can be understood that perovskite tandem cells include but are not limited to crystalline silicon / perovskite tandem cells, full perovskite tandem cells, copper indium gallium selenide and other thin film cells / perovskite tandem cells.

[0168] One embodiment of the present application provides the use of the above-mentioned perovskite solar cell or the above-mentioned perovskite tandem cell in the preparation of a photovoltaic module. Another embodiment of the present application provides a photovoltaic module, including the above-mentioned perovskite solar cell or the above-mentioned perovskite tandem cell,

[0169] It can be understood that photovoltaic modules can be used in photovoltaic power stations, such as ground power stations, rooftop power stations, water power stations, etc., and can also be used in equipment or devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars, solar buildings, etc. It can also be understood that the application scenarios of photovoltaic systems include but are not limited to this, that is, photovoltaic systems can be used in all fields that require solar energy to generate electricity. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array can be an array combination of multiple photovoltaic modules. For example, multiple photovoltaic modules can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to achieve solar power supply.

[0170] The photovoltaic module provided in the present application can be used in, but is not limited to, electrical devices such as vehicles, ships or aircraft. A power supply system comprising the perovskite cell, perovskite stacked cell, photovoltaic module, etc. provided in the present application can be used to form the electrical device, which is conducive to improving stability, thereby effectively extending service life, and effectively improving photoelectric conversion efficiency.

[0171] The embodiments of the present application provide an electric device, which may be, but is not limited to, a mobile phone, a tablet, a laptop, an electric toy, an electric tool, a battery car, an electric car, a ship, a spacecraft, etc. Among them, the electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc., and the spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0172] The present application is further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present application are not limited thereto.

[0173] Example 1

[0174] (1) The ITO conductive glass was ultrasonically cleaned with deionized water, acetone and isopropanol for 15 min respectively, and finally dried in a drying oven at 75°C; the dried ITO glass substrate was treated in a UV ozone machine for 5 min to remove organic impurities on its surface.

[0175] (2) Preparation of hole transport layer

[0176] 1 mg of organic hole transport material MeO-2PACz was dissolved in 2 mL of chlorobenzene and stirred at room temperature until completely dissolved to obtain an organic hole transport material solution; the solution was spin-coated on ITO at a speed of 2000 r / min for 30 s and heated and annealed at 100°C for 10 min.

[0177] (3) Preparation of perovskite material layer

[0178] Weigh 0.4610 g PbI 2 and 0.1589 g CH 3 NH 3 I was dissolved in a mixed solution of DMF and DMSO (volume ratio of 4:1) to prepare a 1.2 mol / L perovskite precursor solution; the perovskite precursor solution was spin-coated on the hole transport layer at a speed of 5000 r / min for 30 s, and 300 μL of ethyl acetate antisolvent was added at the 6th second, and then heated on a heating table at 100°C for 15 min to form a perovskite material layer.

[0179] (4) Preparation of passivation layer

[0180]

[0181] 2.0 mg of the compound of formula I-1 was dissolved in 1 mL of isopropanol and stirred at room temperature to obtain a solution of the passivation material; 75 μL of the solution of the passivation material was added dropwise to the top of the perovskite material layer and spin coated at a speed of 5000 rpm for 30 s to form a passivation layer, that is, a perovskite light-absorbing layer was formed on the hole transport layer, the perovskite light-absorbing layer included a perovskite material layer and a passivation layer, and the mass ratio of the passivation material in the passivation layer to the perovskite light-absorbing material in the perovskite material layer was 0.003:1.

[0182] (5) Preparation of electron transport layer

[0183] Dissolve 20 mg of methanefullerene phenyl-C61-butyric acid methyl ester (PCBM) in 1 mL of chlorobenzene and stir at room temperature to obtain [6,6]-phenyl-C61-butyric acid methyl ester solution; take 30 μL of [6,6]-phenyl-C61-butyric acid methyl ester solution and spin coat it at 3000 rpm for 60 s on the ITO conductive glass with a perovskite light absorption layer to form an electron transport layer.

[0184] (6) Preparation of hole blocking layer

[0185] Dissolve 0.5 mg of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) in 1 mL of isopropanol and stir at room temperature to obtain a hole blocking layer solution; take 40 μL of the hole blocking layer solution and drop it on the top of the electron transport layer, and spin coat at 5000 rpm for 35 s to form a hole blocking layer.

[0186] (7) Preparation of electrode layer

[0187] The TCO conductive glass with hole blocking layer, PCBM electron transport layer, perovskite light absorption layer and hole transport layer is transferred to the vacuum coating instrument and the vacuum degree is drawn to 3*10 -4 A silver electrode was evaporated at 100 Pa to form a silver electrode layer with a thickness of 100 nm.

[0188] Example 2

[0189] The method is basically the same as Example 1, except that in step (4), the compound of formula I-1 is replaced by an equal mass of the compound of formula I-2:

[0190]

[0191] Example 3

[0192] Basically the same as Example 1, except that in step (4), the compound of formula I-1 is replaced by an equal mass of the compound of formula I-3:

[0193]

[0194] Example 4

[0195] The method is basically the same as Example 1, except that in step (4), in the solution of the passivation material, the mass ratio of the I-1 compound to the volume of isopropanol is 1 mg:1 mL, that is, the concentration of the passivation solution is 1 mg / mL. 150 μL of the passivation material solution is added dropwise to the top of the perovskite material layer, and spin-coated at a speed of 5000 rpm for 30 s to form a passivation layer.

[0196] Example 5

[0197] The method is basically the same as Example 1, except that in step (4), in the solution of the passivation material, the mass ratio of the I-1 compound to the volume of isopropanol is 1.5 mg:1 mL, that is, the concentration of the passivation solution is 1.5 mg / mL. 75 μL of the passivation material solution is added dropwise to the top of the perovskite material layer, and spin-coated at a speed of 5000 rpm for 30 s to form a passivation layer.

[0198] Example 6

[0199] The method is basically the same as Example 1, except that in step (4), the mass ratio of compound I-1 to the volume of isopropanol is 0.5 mg:1 mL, that is, the concentration of the passivation solution is 0.5 mg / mL, 75 μL of the passivation material solution is added dropwise to the top of the perovskite material layer, and spin-coated at a speed of 5000 rpm for 30 s to form a passivation layer.

[0200] Example 7

[0201] (1) The ITO conductive glass was ultrasonically cleaned with deionized water, acetone and isopropanol for 15 min respectively, and finally dried in a drying oven at 75°C; the dried ITO glass substrate was treated in a UV ozone machine for 5 min to remove organic impurities on its surface.

[0202] (2) Preparation of hole transport layer

[0203] 1 mg of organic hole transport material MeO-2PACz was dissolved in 2 mL of chlorobenzene and stirred at room temperature until completely dissolved to obtain an organic hole transport material solution; the solution was spin-coated on ITO at a speed of 2000 r / min for 30 s and heated and annealed at 100°C for 10 min.

[0204] (3) Preparation of perovskite light-absorbing layer

[0205] Weigh 0.4610 g PbI 2 and 0.1589 g CH 3 NH 3I was dissolved in a mixed solution of DMF and DMSO (volume ratio of 4:1) to prepare a 1.2 mol / L perovskite precursor solution; then 3 mol% of formula I-1, i.e. 6 mg of the compound of formula I-1, was weighed and added to the perovskite precursor solution, and the mass ratio of the passivation material to the perovskite light-absorbing material was 0.01:1; the perovskite precursor solution was spin-coated on the hole transport layer at a speed of 5000 r / min for 30 s, and 300 μL of ethyl acetate anti-solvent was added dropwise at the 6th s, and then heated on a heating table at 100°C for 15 min to form a perovskite light-absorbing layer.

[0206] (4) Preparation of electron transport layer

[0207] Dissolve 20 mg of methanefullerene phenyl-C61-butyric acid methyl ester (PCBM) in 1 mL of chlorobenzene and stir at room temperature to obtain [6,6]-phenyl-C61-butyric acid methyl ester solution; take 30 μL of [6,6]-phenyl-C61-butyric acid methyl ester solution and spin coat it at 3000 rpm for 60 s on the ITO conductive glass with a perovskite light absorption layer to form an electron transport layer.

[0208] (5) Preparation of hole blocking layer

[0209] Dissolve 0.5 mg of 2,9-dimethyl-4,7-diphenyl-1,10-phenanthroline (BCP) in 1 mL of isopropanol and stir at room temperature to obtain a hole blocking layer solution; take 40 μL of the hole blocking layer solution and drop it on the top of the electron transport layer, and spin coat at 5000 rpm for 35 s to form a hole blocking layer.

[0210] (6) Preparation of electrode layer

[0211] The TCO conductive glass with hole blocking layer, PCBM electron transport layer, perovskite light absorption layer and hole transport layer is transferred to the vacuum coating instrument and the vacuum degree is drawn to 3*10 -4 A silver electrode was evaporated at 100 Pa to form a silver electrode layer with a thickness of 100 nm.

[0212] Comparative Example 1

[0213] The method is basically the same as Example 1, except that step (4) is omitted and an electron transport layer is directly prepared on the surface of the perovskite material layer.

[0214] Comparative Example 2

[0215] The method is basically the same as Example 1, except that the compound of formula I-1 in step (4) of Example 1 is replaced by an equal mass of furoic acid.

[0216] Comparative Example 3

[0217] The method is basically the same as Example 1, except that the compound of formula I-1 in step (4) of Example 1 is replaced by an equal amount of methylpyridine-2-carboxylic acid ethyl ester.

[0218] Some parameters of various embodiments and comparative examples are shown in Table 1.

[0219] Table 1

[0220]

[0221] The perovskite cells prepared in each embodiment and comparative example were subjected to performance tests of open circuit voltage, short circuit current density, fill factor and energy conversion efficiency. The IV curve was used for the test. The test conditions were: AM 1.5G standard solar spectrum, irradiance of 1000W / m 2 The experimental test results are shown in Table 2. PCE represents the energy conversion efficiency in %, Voc represents the open circuit voltage in V, and Jsc represents the short circuit current density in mA / cm 2 , FF stands for fill factor, the unit is %.

[0222] The efficiency of the battery was tested after being placed at 100°C for 200 h. The test results are shown in Table 2. Normalized efficiency = energy conversion efficiency after heating / energy conversion efficiency before heating × 100%. The stability of the solar cell was tested by normalized efficiency. The normalized efficiency of the perovskite battery provided in Example 1 and Comparative Example 1 after being placed at 100°C for different time periods is shown in Table 2. Figure 1 As shown, the horizontal axis is time (unit: h) and the vertical axis is normalized efficiency (unit: %).

[0223] Table 2

[0224]

[0225] Depend on Figure 1 As can be seen from Table 2, compared with the comparative example, the perovskite battery prepared in the embodiment has higher photoelectric conversion efficiency and better stability performance; among them, compared with Example 1, the passivation material in Comparative Example 2 and Comparative Example 3 is replaced with an equal mass of furoic acid or methylpyridine-2-carboxylic acid ethyl ester, and its photoelectric conversion efficiency is obviously not as good as that in Example 1; by introducing different groups to change the interaction between the perovskite surface and the passivation molecule, the difference in passivation ability is achieved.

[0226] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0227] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solution of the present application in detail, but it cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the scope of protection of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the scope of protection of the claims attached to the present application. Therefore, the scope of protection of the patent of this application shall be based on the contents of the attached claims, and the description and drawings can be used to explain the contents of the claims.

Claims

1. A perovskite light absorbing layer, characterized in that: It includes a perovskite light absorbing material and a passivation material, and the structural formula of the passivation material is shown in formula (I): Wherein, R1 is selected from hydrogen, amino, C1~C 20 alkyl, halogen, nitro, hydroxyl, thiol, carboxyl, cyano, substituted or unsubstituted C1~C 20 Alkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C2~C 20 Heterocyclic group and substituted or unsubstituted C2~C 20 at least one of heteroaryl groups; R2 is selected from hydrogen, amino, C1~C 20 alkyl, nitro, halogen, cyano, carboxyl, formyl, hydroxymethyl, substituted or unsubstituted C1~C 20 Alkyl, substituted or unsubstituted C1~C 20 Alkoxy, substituted or unsubstituted C3~C 20 Cycloalkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C2~C 20 Heterocyclic group and substituted or unsubstituted C2~C 20 at least one of heteroaryl groups; R3 and R4 are independently selected from hydrogen, amino, C1~C 20 alkyl, halogen, substituted or unsubstituted C1~C 20 Alkyl, substituted or unsubstituted C6~C 20 Aryl, substituted or unsubstituted C2~C 20 Heterocyclic group and substituted or unsubstituted C2~C 20 at least one of heteroaryl groups; At least one of R2, R3 and R4 is not hydrogen.

2. The perovskite light absorbing layer according to claim 1, characterized in that: The formula (I) satisfies at least one of the following characteristics: (1) R1 is selected from hydrogen and substituted or unsubstituted C1~C 10 at least one of the alkyl groups; (2) R2 is selected from hydrogen, formyl, amino, C1~C 10 Aminoalkyl and substituted or unsubstituted C1~C 10 at least one of the alkyl groups; (3) R3 and R4 are independently selected from hydrogen, halogen and substituted or unsubstituted C1~C 10 At least one of the alkyl groups.

3. The perovskite light absorbing layer according to claim 1, characterized in that: The formula (I) satisfies at least one of the following characteristics: (1) R1 is selected from hydrogen and ethyl; (2) R2 is selected from one of hydrogen, formyl and aminomethyl; (3) R3 and R4 are each independently selected from hydrogen and methyl.

4. The perovskite light absorbing layer according to claim 1, characterized in that: The passivation material includes at least one of the compounds represented by formula (I-1) to formula (I-3): 。 5. The perovskite light absorbing layer according to claim 1, characterized in that: The passivation material and the perovskite light-absorbing material are mixed with each other, and the mass ratio of the passivation material to the perovskite light-absorbing material is 0.0001-0.01:

1.

6. The perovskite light absorbing layer according to claim 1, characterized in that: The perovskite light-absorbing layer comprises a perovskite material layer and a passivation layer which are stacked, the perovskite material layer comprises the perovskite light-absorbing material, and the passivation layer comprises the passivation material.

7. The perovskite light absorbing layer according to claim 6, characterized in that: The perovskite light absorbing layer satisfies at least one of the following characteristics: (1) The thickness of the passivation layer is 1 nm to 10 nm; (2) The thickness of the perovskite material layer is 10 nm to 100 μm; (3) The thickness ratio of the passivation layer to the perovskite material layer is 0.00125~0.025:

1.

8. A method for preparing a perovskite light-absorbing layer, characterized in that: The following steps are involved: Providing a perovskite precursor, a passivation material and a solvent according to the perovskite light absorbing layer according to any one of claims 1 to 7; Mixing the perovskite precursor, the passivation material and the solvent to prepare a perovskite passivation solution; The perovskite passivation solution is disposed on the surface of a substrate and subjected to a first annealing treatment to form a perovskite light absorbing layer on the surface of the substrate.

9. A method for preparing a perovskite light-absorbing layer, characterized in that: The following steps are involved: Providing a perovskite precursor, a passivation material and a solvent according to the perovskite light absorbing layer according to any one of claims 1 to 7; Mixing the perovskite precursor and a portion of the solvent to prepare a perovskite precursor solution; Placing the perovskite precursor solution on the surface of a substrate and performing a second annealing treatment to form a perovskite material layer on the surface of the substrate; Mixing the passivation material and the remaining solvent to prepare a passivation solution; The passivation solution is disposed on the surface of the perovskite material layer away from the substrate to form a passivation layer on the surface of the perovskite material layer away from the substrate. The perovskite light absorbing layer includes the perovskite material layer and the passivation layer.

10. The preparation method according to claim 9, characterized in that: The solvent includes a first solvent and a second solvent, the first solvent includes at least one of N,N-dimethylformamide and dimethyl sulfoxide, and the second solvent includes at least one of isopropanol and ethanol.

11. The preparation method according to claim 10, characterized in that: In the step of preparing the perovskite precursor solution, the perovskite precursor and the first solvent are mixed; in the step of preparing the passivation solution, the passivation material and the second solvent are mixed.

12. The preparation method according to any one of claims 9 to 11, characterized in that: The concentration of the passivation material in the passivation solution is 0.2 mg / mL to 10 mg / mL.

13. A perovskite battery, characterized in that: It comprises a first electrode, a perovskite light absorbing layer as claimed in any one of claims 1 to 7 or a perovskite light absorbing layer prepared by the preparation method as claimed in any one of claims 8 to 11, and a second electrode.

14. A method for preparing a perovskite battery, characterized in that: The following steps are involved: providing a first electrode; Forming a perovskite light-absorbing layer as claimed in any one of claims 1 to 7 or a perovskite light-absorbing layer prepared by the preparation method as claimed in any one of claims 8 to 11 on the surface of the first electrode; A second electrode is formed on a surface of the perovskite light absorbing layer away from the first electrode.

15. A photovoltaic module, characterized in that: Including the perovskite battery as claimed in claim 13 or the perovskite battery prepared by the preparation method as claimed in claim 14.