Grain-oriented electrical steel sheet and method for producing same
By forming internal oxidized SiO2 on the base steel plate of the directional electromagnetic steel plate, and using an annealing separator of alumina and bismuth chloride, the problem of insufficient adhesion of the coating is solved, and the iron loss characteristics are significantly improved.
Patent Information
- Application Number
- CN202380034208.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-20
- Publication Date
- 2024-11-22
AI Technical Summary
The prior art is difficult to achieve film adhesion of directional electromagnetic steel sheets without relying on forsterite films, resulting in poor iron loss characteristics.
By forming internal oxidized SiO2 on the base material steel plate and using alumina and bismuth chloride as an annealing separator in the thermal oxidation annealing process, the oxidation conditions are controlled to form excellent film adhesion.
It is realized that the film adhesion of the directional electromagnetic steel plate is improved without relying on the forsterite film, thereby optimizing the iron loss characteristics.
Smart Images

Figure CN119013427A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a grain-oriented electrical steel sheet, and in particular to a grain-oriented electrical steel sheet having excellent film adhesion without relying on a forsterite film, and a method for producing the same.
[0002] This application claims priority based on Japanese Patent Application No. 2022-070071 filed in Japan on April 21, 2022, and the contents of which are incorporated herein by reference. Background Art
[0003] Grain-oriented electrical steel sheets are mainly used in transformers. Transformers are continuously excited over a long period of time from installation to disposal, and energy loss continues to occur. Therefore, the energy loss when the alternating current is magnetized, that is, the iron loss, becomes the main indicator that determines the performance of the transformer.
[0004] To reduce the iron loss of grain-oriented electrical steel sheets, many methods have been proposed. For example, in order to improve the {110} <001> The method of oriented aggregation includes, for steel sheets, a method of increasing the content of solid solution elements such as Si that increase electrical resistance, a method of reducing the thickness of the steel sheet, and the like.
[0005] In addition, it is known that applying tension to a steel sheet is an effective method for reducing iron loss. Therefore, a coating is usually formed on the surface of a directional electromagnetic steel sheet for the purpose of reducing iron loss. The coating reduces the iron loss of a single steel sheet by applying tension to the directional electromagnetic steel sheet. When the directional electromagnetic steel sheets are further stacked for use, the coating reduces the iron loss of the core by ensuring electrical insulation between the steel sheets.
[0006] As a grain-oriented electrical steel sheet with a film formed thereon, there is a grain-oriented electrical steel sheet in which a forsterite film, which is an oxide film containing Mg, is formed on the surface of a base steel sheet, and an insulating film is further formed on the surface of the forsterite film. That is, in this case, the film on the base steel sheet includes a forsterite film and an insulating film. The forsterite film and the insulating film each have two functions of an insulating function and a function of imparting tension to the base steel sheet.
[0007] The forsterite film is formed by a reaction between an annealing separator having magnesium oxide (MgO) as a main component and silicon oxide (SiO2) formed on the base steel sheet during decarburization annealing during a heat treatment at 900 to 1200°C for more than 20 hours in a finish annealing that causes secondary recrystallization in the steel sheet.
[0008] The insulating film is formed by applying a coating solution containing, for example, phosphate and colloidal silica to the steel sheet after the finish annealing, and baking and drying the coating solution at 350° C. to 1150° C. for 5 seconds or more.
[0009] In order for these films to exhibit the functions of insulating and imparting tension to the base steel sheet, high adhesion is required between the films and the base steel sheet.
[0010] In the past, the above-mentioned adhesion was mainly ensured by the anchoring effect generated by the unevenness of the interface between the base steel sheet and the forsterite film. However, in recent years, it has been found that the unevenness of the interface becomes an obstacle to the movement of the magnetic domain wall when the grain-oriented electromagnetic steel sheet is magnetized, which becomes a factor that hinders the reduction of iron loss.
[0011] To further reduce the iron loss, Patent Documents 1 to 3 propose technologies in which a forsterite film is not formed on a base steel sheet and an insulating film is formed on a smooth surface of the base steel sheet.
[0012] In the technology disclosed in Patent Document 1, the formed forsterite film is removed by pickling or the like, and the surface of the base steel plate is smoothed by chemical polishing or electrolytic polishing. In the technology disclosed in Patent Document 2, an annealing separator containing aluminum oxide (Al2O3) is used to suppress the formation of the forsterite film itself, and the surface of the base steel plate is smoothed. In the technology disclosed in Patent Document 3, an annealing separator containing bismuth chloride is used to suppress the formation of the forsterite film itself, and the surface of the base steel plate is smoothed.
[0013] Although these techniques can make the surface of the base steel plate smooth, it is difficult to obtain film adhesion after the insulating film is formed. If film adhesion is not obtained, it is difficult to apply tension to the base steel plate and ensure electrical insulation between the stacked steel plates.
[0014] Therefore, for example, Patent Documents 4 to 6 propose technologies for improving the adhesion of the coating while smoothing the surface of the base steel sheet.
[0015] In the technology disclosed in Patent Document 4, a finish annealing is performed using an annealing separator containing aluminum oxide, and an oxide film forming annealing is performed to control the thermal history and oxygen partial pressure, and then an insulating film is formed. In Patent Document 4, an intermediate oxide film layer of external oxidation type SiO2 is formed on a base steel plate, and an insulating film is formed on the intermediate oxide film layer. In Patent Document 4, an attempt is made to improve the film adhesion by dissolving elements such as Mn in the intermediate oxide film layer.
[0016] In the technology disclosed in Patent Document 5, a finish annealing is performed using an annealing separator containing bismuth chloride, etc., a pickling treatment is performed, and a heat treatment is performed to control the oxygen concentration and dew point, and then an insulating film is formed. In Patent Document 5, an erosion pit is formed on the surface of a base steel plate, an oxide layer containing silicon dioxide and an iron-based oxide layer are formed on the base steel plate, and an insulating film is formed on the iron-based oxide layer. In Patent Document 5, an attempt is made to improve the film adhesion by the erosion pit on the surface of the base steel plate.
[0017] In the technology disclosed in Patent Document 6, an annealing separator containing bismuth chloride or the like is used to perform finish annealing, and then an insulating film containing a metal compound and an insulating film not containing a metal compound are formed. In Patent Document 6, an intermediate layer is formed on a base steel sheet, and an insulating film is formed on the intermediate layer. In Patent Document 6, an attempt is made to improve film adhesion by optimally controlling each manufacturing process.
[0018] Prior art literature
[0019] Patent Literature
[0020] Patent Document 1: Japanese Patent Application Laid-Open No. 49-096920
[0021] Patent Document 2: Japanese Patent Application Laid-Open No. 06-049534
[0022] Patent Document 3: Japanese Patent Application Laid-Open No. 07-054155
[0023] Patent Document 4: International Publication No. 2020 / 012666
[0024] Patent Document 5: International Publication No. 2020 / 149345
[0025] Patent Document 6: International Publication No. 2020 / 149325 Summary of the invention
[0026] Problems to be solved by the invention
[0027] As described above, in order to reduce the iron loss of a grain-oriented electrical steel sheet, it is effective to smooth the surface of the base steel sheet of the grain-oriented electrical steel sheet without a forsterite film. However, this technology has a problem that it is difficult to obtain the film adhesion required for reducing the iron loss.
[0028] The techniques disclosed in Patent Documents 4 to 6 attempt to improve the film adhesion without relying on a forsterite film. Although these techniques also improve the film adhesion to a certain extent, if the film adhesion can be improved by a technique different from Patent Documents 4 to 6, it is preferred because the options in industry increase.
[0029] The present invention has been made in view of the above-mentioned problems. An object of the present invention is to provide a grain-oriented electrical steel sheet having excellent film adhesion without relying on a forsterite film, and a method for producing the same.
[0030] Means for solving problems
[0031] The gist of the present invention is as follows.
[0032] (1) A grain-oriented electrical steel sheet according to one embodiment of the present invention comprises a base steel sheet and an insulating film disposed in contact with the base steel sheet.
[0033] The base steel plate contains, as a chemical composition, in mass %:
[0034] Si: 3.0-4.0%,
[0035] Mn: 0.010~0.50%,
[0036] The rest is Fe and impurities.
[0037] When observed in a cut surface whose cutting direction is parallel to the plate thickness direction and perpendicular to the plate width direction, the base steel plate has internal oxidized SiO2 within a range of 2.0 μm from the interface with the insulating film toward the plate thickness direction.
[0038] (2) The grain-oriented electromagnetic steel sheet according to (1) above, wherein
[0039] The base steel plate may further contain, as the chemical composition, the following in terms of mass %:
[0040] C: 0.010% or less,
[0041] N: 0.010% or less,
[0042] Acid soluble Al: 0.020% or less,
[0043] P: 0.040% or less,
[0044] Total of S and Se: 0.010% or less,
[0045] Sn: 0.50% or less,
[0046] Cu: 0.50% or less,
[0047] Cr: 0.50% or less,
[0048] Sb: 0.50% or less,
[0049] Mo: 0.10% or less,
[0050] Bi: 0.10% or less.
[0051] (3) The grain-oriented electromagnetic steel sheet according to (1) or (2), wherein:
[0052] When observed through the above-mentioned cut surface, the above-mentioned internal oxidized SiO2 may also have a dendrite shape.
[0053] (4) The grain-oriented electromagnetic steel sheet according to any one of (1) to (3), wherein
[0054] When the above-mentioned cut surface is observed at 10 observation locations separated from each other on the plate surface, the above-mentioned internal oxidized SiO2 may be included in 5 or more observation locations.
[0055] (5) The method for producing a grain-oriented electrical steel sheet according to any one of (1) to (4) above comprises a hot rolling step, a hot rolled steel sheet annealing step, a cold rolling step, a decarburization annealing step, a finish annealing step, a thermal oxidation annealing step, and an insulating film forming step,
[0056] In the above-mentioned finish annealing step, an annealing separator containing 20 to 99.5 mass % of aluminum oxide, 0.5 to 20 mass % of bismuth chloride, and the remainder of magnesium oxide and impurities is applied to the steel sheet after the above-mentioned decarburization annealing step in terms of solid content, and then dried, and then the finish annealing is performed.
[0057] In the above-mentioned thermal oxidation annealing process, the steel sheet after the above-mentioned final annealing process is heated from room temperature to a temperature range of 800 to 1100° C. in an atmosphere with an oxygen concentration of less than 1.0 volume % and an oxygen potential PH2O / PH2 of greater than 0.010 and less than 0.50, and is uniformly heated in the temperature range of 800 to 1100° C. for 5 to 200 seconds.
[0058] (6) According to the method for manufacturing a grain-oriented electrical steel sheet described in (5) above, in the thermal oxidation annealing step, as a first surface treatment, the steel sheet after the above-mentioned final annealing step may be immersed in a first treatment liquid containing at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, with a total acid concentration of 1 to 20 mass % and a liquid temperature of 50 to 90° C. for 3 to 60 seconds, and as a heating treatment, the steel sheet after the above-mentioned first surface treatment may be subjected to the above-mentioned heating and the above-mentioned soaking.
[0059] (7) According to the method for manufacturing a grain-oriented electromagnetic steel sheet described in (5) or (6) above, the second surface treatment may be performed by immersing the steel sheet after the heating and the soaking for 3 to 60 seconds in a second treatment liquid containing at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, with a total acid concentration of 1 to 10% by mass and a liquid temperature of 50 to 90°C.
[0060] Effects of the Invention
[0061] According to the above aspect of the present invention, it is possible to provide a grain-oriented electrical steel sheet having excellent film adhesion without relying on a forsterite film and a method for manufacturing the same. In the grain-oriented electrical steel sheet, since there is no forsterite film, the surface of the base steel sheet is smooth, and since internal oxidation is preferably performed near the surface of the base steel sheet, the film adhesion is excellent. Therefore, it becomes possible to preferably improve the iron loss characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 It is a schematic cross-sectional view showing a grain-oriented electrical steel sheet according to one embodiment of the present invention.
[0063] Figure 2 This is a flowchart showing a method for producing a grain-oriented electrical steel sheet according to the present embodiment. DETAILED DESCRIPTION
[0064] Below, the preferred embodiment of the present invention is described in detail. However, the present invention is not limited to the configuration disclosed in the present embodiment, and various changes can be made within the scope of the gist of the present invention. In addition, for the following numerical ranges, the lower limit and the upper limit are included in the range. For the numerical values expressed as "exceeding" or "lower than", the value is not included in the numerical range.
[0065] As described above, if the surface of the base steel sheet of the grain-oriented electromagnetic steel sheet is made smooth without the presence of a forsterite film, the magnetic domain wall movement becomes easier when the grain-oriented electromagnetic steel sheet is magnetized, and the iron loss characteristics are improved. However, this technology has the problem that it is difficult to obtain the film adhesion required for reducing iron loss.
[0066] The inventors of the present invention have conducted intensive studies and, as a result, have found a grain-oriented electrical steel sheet having excellent film adhesion without relying on a forsterite film. Hereinafter, the grain-oriented electrical steel sheet of the present embodiment will be described in detail.
[0067] Figure 1 Schematic diagram showing a cross section of a grain-oriented electromagnetic steel sheet according to the present embodiment. Figure 1As shown in , the grain-oriented electromagnetic steel sheet 1 of the present embodiment, when observed in a cut surface whose cutting direction is parallel to the plate thickness direction and perpendicular to the plate width direction, comprises a base steel sheet 11 and an insulating film 12 disposed in contact with the base steel sheet 11. It should be noted that the layer structure in which the insulating film 12 is disposed in contact with the base steel sheet 11 means that there is no forsterite film, and that the base steel sheet 11 has a smooth surface (smooth surface equivalent to that of a cold-rolled steel sheet). In addition, when the grain-oriented electromagnetic steel sheet 1 of the present embodiment is observed in the above-mentioned cut surface, the base steel sheet 11 has internal oxidized SiO2 11a in the range from the interface with the insulating film 12 to 2.0 μm in the plate thickness direction.
[0068] As described above, in order to improve the iron loss characteristics, it is effective to make the surface of the base steel plate smooth so that the magnetic domain wall can move easily, and it is effective to make the base steel plate and the insulating film close to each other and give tension to the base steel plate to ensure the electrical insulation between the steel plates. In the grain-oriented electromagnetic steel sheet of the present embodiment, the insulating film is arranged in contact with the base steel plate (without the forsterite film), thereby ensuring the surface smoothness of the base steel plate, and further, by the above-mentioned internal oxidation of SiO2, the adhesion between the base steel plate and the insulating film is ensured. Therefore, the grain-oriented electromagnetic steel sheet of the present embodiment is excellent in iron loss characteristics.
[0069] The technical reason why the film adhesion is improved by the internal oxidation SiO2 being contained in the base steel sheet within a range of 2.0 μm from the interface with the insulating film in the sheet thickness direction is not clear at present, but is presumed as follows.
[0070] The above-mentioned internal oxidized SiO2 is mainly composed of SiO2 and is formed by oxidation of Si contained in the base steel plate during annealing. In the grain-oriented electromagnetic steel sheet of the present embodiment, the internal oxidized SiO2 unique to the present embodiment is formed near the surface of the base steel plate by controlling the manufacturing conditions. It is believed that if the above-mentioned internal oxidized SiO2 is formed near the surface in the base steel plate, the Si content in the base material (matrix) around the internal oxidized SiO2 is reduced and becomes close to pure iron. It is believed that the film adhesion is improved by chemical interaction between the matrix in a state close to pure iron and P (phosphorus) contained in the insulating film. Therefore, it is believed that the closer the internal oxidized SiO2 is formed to the surface in the base steel plate, the easier it is to improve the film adhesion. Specifically, if the internal oxidized SiO2 is contained in the base steel plate within a range of 2.0 μm from the interface with the insulating film toward the plate thickness direction, the adhesion between the base steel plate and the insulating film is improved.
[0071] It should be noted that as oxidation forms of Si contained in the base steel plate when oxidized during annealing, external oxidation and internal oxidation are known. For example, external oxidation refers to an oxidation form in which the alloy elements (such as Si) in the base steel plate are diffused to the surface of the base steel plate and then oxidized. It is oxidation produced in a low-oxidizing atmosphere, and an oxide film is formed on the surface of the base steel plate. On the other hand, internal oxidation refers to an oxidation form in which the alloy elements (such as Si) in the base steel plate are oxidized without being diffused in the base steel plate. It is oxidation produced in a high-oxidizing atmosphere, and oxides are formed in the form of precipitates or dendrites near the surface inside the base steel plate.
[0072] Until now, it is generally believed that external oxidation will not be an obstacle to the movement of the magnetic domain wall when the steel sheet is magnetized, but internal oxidation will be an obstacle to the movement of the magnetic domain wall. Therefore, in the prior art, internal oxidation of the base steel sheet is avoided. On the other hand, in the directional electromagnetic steel sheet of the present embodiment, internal oxidation is effectively utilized. The inventors of the present invention have conducted research and found that if the internal oxidation SiO2 unique to the present embodiment is introduced by controlling the manufacturing conditions, the film adhesion can be improved without hindering the movement of the magnetic domain wall. It is believed that in the directional electromagnetic steel sheet of the present embodiment, since the internal oxidation SiO2 is preferentially formed near the surface in the base steel sheet, the movement of the magnetic domain wall is not hindered, and since the matrix around the internal oxidation SiO2 becomes close to pure iron, the film adhesion is improved through chemical interaction with the insulating film.
[0073] The presence of the internal oxidized SiO2 can be confirmed by observing a cut surface whose cutting direction is parallel to the plate thickness direction and perpendicular to the plate width direction. For example, the cut surface can be observed by a transmission electron microscope (TEM). In the grain-oriented electrical steel sheet of the present embodiment, when confirmed by the following method, it is determined that the base steel sheet contains internal oxidized SiO2.
[0074] Specifically, first, a test piece is cut out by FIB (focused ion beam) processing in such a way that the cutting direction becomes parallel to the plate thickness direction and perpendicular to the plate width direction, and the cross-sectional structure of the cut surface is observed by TEM at a magnification at which each layer enters the observation field of view. In the case where each layer does not enter the observation field of view, the cross-sectional structure is observed in a plurality of continuous fields of view. For example, it can be observed in a field of view of 1μm×1μm or more, preferably in a field of view of about 10μm×8μm. In addition, the acceleration voltage can be set to a condition of 200kV. In the case of observation with only one field of view, it is difficult to obtain the average information of the steel plate, so it is sufficient to observe 10 randomly selected places separated from each other to make a judgment.
[0075] In order to identify each layer in the cross-sectional structure, the EDS (Energy Dispersive X-ray Spectroscopy) equipped in the TEM was used to perform line analysis along the thickness direction and quantitative analysis of the chemical composition of each layer. The elements for quantitative analysis were set to five elements: Fe, P, Si, O, and Mg.
[0076] From the quantitative analysis results of the above-mentioned TEM-EDS, the layered region existing at the deepest position in the plate thickness direction and having an Fe content of 80 atomic % or more excluding measurement noise was judged to be the base steel plate, and the region other than the base steel plate was judged to be other films.
[0077] When judging the above-mentioned area as the parent steel plate, the precipitates, inclusions and pores contained in each layer are not included in the object of judgment, but the area that satisfies the above-mentioned quantitative analysis results as the parent phase is judged as the parent steel plate. For example, if the bright field image, dark field image or line analysis result confirms the presence of precipitates, inclusions and pores on the scanning line of the online analysis, the area is not included in the object and is judged by the quantitative analysis result as the parent phase. It should be noted that the precipitates, inclusions and pores can be distinguished from the parent phase by contrast, and can be distinguished from the parent phase by the presence of the constituent elements in the quantitative analysis results. It should be noted that when determining the parent steel plate, it is preferred to determine it at a position on the scanning line of the online analysis that does not contain precipitates, inclusions and pores.
[0078] Regarding the area other than the base steel plate determined above, the area where the Fe content is less than 80 atomic %, the P content is 5 atomic % or more, and the O content is 30 atomic % or more, except for the measurement noise, is judged as an insulating film (phosphate film) based on the quantitative analysis results of TEM-EDS. It should be noted that in addition to the above three elements used to determine the judgment element of the phosphate film, the phosphate film may also contain aluminum, magnesium, nickel, etc. derived from phosphates. In addition, silicon derived from colloidal silica may also be contained.
[0079] When judging the above-mentioned area as a phosphate-based film, the precipitates, inclusions and pores contained in each film are not included in the object of judgment, and the area that satisfies the above-mentioned quantitative analysis results as the parent phase is judged as a phosphate-based film. For example, if the bright field image, dark field image or line analysis result confirms the presence of precipitates, inclusions and pores on the scanning line of the online analysis, the area is not included in the object and is judged by the quantitative analysis result as the parent phase. It should be noted that precipitates, inclusions and pores can be distinguished from the parent phase by contrast, and can be distinguished from the parent phase by the amount of constituent elements in the quantitative analysis results. It should be noted that when determining the phosphate-based film, it is preferably determined at a position on the scanning line of the online analysis that does not contain precipitates, inclusions and pores.
[0080] Since the grain-oriented electrical steel sheet of this embodiment does not have an intermediate ceramic layer such as a forsterite film and an outer oxide film, when the layer structure is determined by the above method, the base steel sheet and the insulating film disposed in contact with the base steel sheet can be confirmed. For example, the base steel sheet has a thickness of 0.17 to 0.29 mm, and the insulating film has a thickness of 0.1 to 10 μm.
[0081] However, in the case where the electromagnetic steel sheet has a forsterite film as an intermediate ceramic layer, a forsterite film can be confirmed between the base steel sheet and the insulating film (phosphate film) determined by the above method. The forsterite film, for example, satisfies the following conditions as an average of the entire film: an Fe content of less than 80 atomic %, an P content of less than 5 atomic %, an Si content of more than 5 atomic %, an O content of more than 30 atomic %, and an Mg content of more than 10 atomic %. It should be noted that the quantitative analysis results of the forsterite film are quantitative analysis results of the parent phase that do not contain the analysis results of precipitates, inclusions, and pores contained in the forsterite film. It should be noted that when determining the forsterite film, it is preferably determined at a position on the scanning line of the online analysis that does not contain precipitates, inclusions, and pores. Generally speaking, the thickness of the forsterite film is 0.1 to 10 μm.
[0082] Similarly, in the case where the electromagnetic steel sheet has an external oxide film as an intermediate ceramic layer, an external oxide film can be confirmed between the base steel sheet and the insulating film (phosphate-based film) determined by the above method. The external oxide film satisfies, for example, the average of the entire oxide film, the Fe content is less than 80 atomic%, the P content is less than 5 atomic%, the Si content is more than 20 atomic%, the O content is more than 30 atomic%, and the Mg content is less than 10 atomic%. It should be noted that the quantitative analysis results of the external oxide film are quantitative analysis results of the parent phase without the analysis results of precipitates, inclusions, and pores contained in the external oxide film. It should be noted that when determining the external oxide film, it is preferably determined at a position on the scanning line of the online analysis that does not contain precipitates, inclusions, and pores. Generally, the thickness of the external oxide film is 2 to 500 nm.
[0083] In the grain-oriented electrical steel sheet of the present embodiment, since the base steel sheet and the insulating coating arranged in contact with the base steel sheet can be confirmed by the above-mentioned method, it is sufficient to confirm whether the base steel sheet contains internal oxidized SiO2 and the area containing internal oxidized SiO2 in the base steel sheet by EDS provided by TEM.
[0084] For example, in the bright field image of TEM, for the precipitates observed in the base steel plate, TEM-EDS is used to perform line analysis along the plate thickness direction in the base steel plate determined by the above method, and quantitative analysis of the chemical composition is performed. The elements for quantitative analysis are set to five elements: Fe, P, Si, Al, and O. From the quantitative analysis results of the above TEM-EDS, the region where the Fe content is less than 80 atomic %, the Si content is 30 atomic % or more, and the O content is 55 atomic % or more, excluding the measurement noise, is judged as internal oxidized SiO2. It should be noted that in the grain-oriented electromagnetic steel sheet of the present embodiment, since the internal oxidized SiO2 contained in the base steel plate is amorphous, no clear diffraction spots are confirmed when electron beam diffraction is performed, and mainly a wide circular electron diffraction pattern is confirmed.
[0085] In the grain-oriented electrical steel sheet of this embodiment, if the internally oxidized SiO2 determined above is contained in the base steel sheet within a range of 2.0 μm from the interface with the insulating film toward the sheet thickness direction, the adhesion between the base steel sheet and the insulating film is improved.
[0086] Furthermore, in the grain-oriented electrical steel sheet of the present embodiment, when observing a cut surface whose cutting direction is parallel to the sheet thickness direction and perpendicular to the sheet width direction, the area ratio of internal oxidized SiO2 is preferably 0.2% or more relative to the area of a region from the interface with the insulating film to 2.0 μm in the sheet thickness direction in the base steel sheet. When the internal oxidized SiO2 satisfies the above-mentioned conditions, the internal oxidized SiO2 preferentially exists near the surface in the base steel sheet, and as a result, the film adhesion is preferably improved.
[0087] The above area ratio is preferably 0.5% or more, more preferably 1.0% or more. The upper limit of the above area ratio is not particularly limited. For example, the above area ratio is preferably 8% or less, preferably 5% or less, preferably less than 2%, and more preferably 1.5% or less.
[0088] It should be noted that the above-mentioned area ratio can be obtained based on the observation and identification in the above-mentioned TEM. For example, it is only necessary to find out the area of the region from the interface with the insulating film to 2.0 μm in the plate thickness direction in the base steel plate, and the total area of the internally oxidized SiO2 contained in the region, and calculate the area ratio. The above-mentioned area and area ratio can also be obtained by image analysis. It should be noted that the binarization of the image used for image analysis can also be based on the identification result of the above-mentioned internally oxidized SiO2, and the image can be binarized by manually coloring the internally oxidized SiO2 on the tissue photograph.
[0089] In addition, in the grain-oriented electrical steel sheet of the present embodiment, when observing a cut surface whose cutting direction is parallel to the sheet thickness direction and perpendicular to the sheet width direction, the internal oxidized SiO2 determined above preferably has a dendrite shape. Specifically, when observing the above cut surface, the isoperimetric constant derived from the area and perimeter of the internal oxidized SiO2 is preferably less than 0.350. When the internal oxidized SiO2 satisfies the above conditions, the film adhesion is preferably improved.
[0090] It should be noted that the dendrite shape (isoperiodic constant) of the internal oxidized SiO 2 may be confirmed by the following method. In the grain-oriented electrical steel sheet of the present embodiment, when confirmed by the following method, it is determined that the internal oxidized SiO 2 has a dendrite shape.
[0091] The above isoperimetric constant is calculated as 4π×(area)÷(perimeter) 2The area can be derived by image analysis or manual operation from the tissue photograph of TEM in the same manner as when calculating the area ratio of the internally oxidized SiO2. The perimeter can also be obtained by image analysis from the tissue photograph of TEM using image analysis software such as imageJ, etc.
[0092] The above isoperimetric constant is preferably less than 0.20, and more preferably less than 0.10. There is no particular restriction on the lower limit of the above isoperimetric constant, and the smaller the lower limit, the better. However, it is not easy to set the isoperimetric constant to 0 in industry, so the above isoperimetric constant may be set to 0.020 or more.
[0093] Furthermore, in the grain-oriented electromagnetic steel sheet of the present embodiment, when the above-mentioned cut surface is observed at 10 observation locations spaced apart from each other on the sheet surface, the above-mentioned internal oxidized SiO2 is preferably included in 5 or more observation locations. When the internal oxidized SiO2 satisfies the above-mentioned conditions, the internal oxidized SiO2 becomes widely distributed with respect to the sheet surface of the grain-oriented electromagnetic steel sheet, and as a result, the film adhesion is preferably improved.
[0094] The number of the above-mentioned observation sites containing internal oxidized SiO2 is preferably 8 or more, and more preferably 9 or more. The upper limit of the above-mentioned observation sites containing internal oxidized SiO2 is not particularly limited, and the larger the number, the better, so it can also be 10. The number of the above-mentioned observation sites containing internal oxidized SiO2 can also be 9 or less.
[0095] In addition, in the grain-oriented electrical steel sheet of the present embodiment, the film remaining area ratio when the grain-oriented electrical steel sheet is wound around a cylinder having a diameter of 20 mm and bent 180° is preferably 80% or more, more preferably 85% or more, more preferably 90% or more, and more preferably 95% or more. The upper limit of the film remaining area ratio is not particularly limited, but may be, for example, 100%.
[0096] The above-mentioned film remaining area ratio can be evaluated by the film remaining ratio when the test piece is wound on a cylinder with a diameter of 20 mm and bent 180°. The area ratio of the remaining surface of the film relative to the area of the steel plate in contact with the cylinder is calculated, and the area of the steel plate in contact with the roller can be obtained by calculation. The area of the remaining surface can be obtained by taking a photo of the steel plate after the test and performing image analysis on the photo image.
[0097] In the grain-oriented electrical steel sheet of the present embodiment, the base steel sheet contains basic elements as a chemical composition, contains optional elements as necessary, and the balance contains Fe and impurities.
[0098] For example, the base steel plate contains, as a chemical composition, in terms of mass %:
[0099] Si: 3.0-4.0%,
[0100] Mn: 0.010~0.50%,
[0101] C: 0~0.010%,
[0102] N: 0~0.010%,
[0103] Acid soluble Al: 0~0.020%
[0104] P: 0~0.040%,
[0105] Total of S and Se: 0 to 0.010%,
[0106] Sn: 0~0.50%,
[0107] Cu: 0-0.50%,
[0108] Cr: 0~0.50%,
[0109] Sb: 0-0.50%,
[0110] Mo: 0~0.10%
[0111] Bi: 0~0.10%,
[0112] The remainder may contain Fe and impurities.
[0113] In addition, the base steel plate may contain, as a chemical composition, at least one selected from the following elements in terms of mass %:
[0114] Sn: 0.0050~0.50%,
[0115] Cu: 0.010~0.50%,
[0116] Cr: 0.010~0.50%,
[0117] Sb: 0.010~0.50%,
[0118] Mo: 0.0050~0.10%,
[0119] Bi: 0.00050~0.10%.
[0120] Si: 3.0-4.0 mass%
[0121] Si (silicon) is a basic element for the base steel plate. If the Si content is less than 3.0%, the eddy current loss cannot be sufficiently reduced, so good magnetic properties cannot be obtained. Therefore, the Si content is set to 3.0% or more. The Si content is preferably 3.10% or more, and more preferably 3.20% or more. On the other hand, if the Si content exceeds 4.0%, the steel plate becomes brittle and the plate passability is significantly deteriorated during manufacturing, so the Si content is set to 4.0% or less. The Si content is preferably 3.70% or less, more preferably 3.60% or less, and more preferably 3.50% or less.
[0122] Mn: 0.010 to 0.50 mass%
[0123] Mn (manganese) is a basic element for the base steel plate. If the Mn content is less than 0.010%, it is difficult to form MnS and MnSe that function as inhibitors, and the secondary recrystallization will not proceed sufficiently, and good magnetic properties cannot be obtained. Therefore, the Mn content is set to 0.010% or more. The Mn content is preferably 0.030% or more, and more preferably 0.050% or more. On the other hand, if the Mn content exceeds 0.50%, the steel undergoes phase transformation during the secondary recrystallization annealing, and the secondary recrystallization will not proceed sufficiently, and good magnetic properties cannot be obtained, so the Mn content is set to less than 0.50%. The Mn content is preferably less than 0.20%, more preferably less than 0.15%, and more preferably less than 0.10%.
[0124] C: 0 to 0.010 mass%
[0125] C (carbon) is an optional element for the base steel plate. C is contained in the steel billet (slab), but if excessive C remains in the base steel plate after the finished annealing, good iron loss characteristics may not be obtained. Therefore, the C content of the base steel plate only needs to be less than 0.010%. The C content is preferably less than 0.0050%, and more preferably less than 0.0030%. On the other hand, the lower limit of the C content of the base steel plate is not particularly limited, as long as it is 0%. However, it is not easy to set the C content to 0% in industry, so the C content can also be set to more than 0%, or it can be set to more than 0.00010%.
[0126] N: 0 to 0.010 mass%
[0127] N (nitrogen) is an optional element for the base steel plate. N is contained in the steel billet (slab), but if an excessive amount of N remains in the base steel plate after the finished annealing, it may have an adverse effect on the magnetic properties. Therefore, the N content of the base steel plate only needs to be 0.010% or less. The N content is preferably 0.0090% or less, and more preferably 0.0080% or less. On the other hand, the lower limit of the N content of the base steel plate is not particularly limited, as long as it is 0%. However, N forms AlN and has the effect of acting as an inhibitor during secondary recrystallization, so the N content can be set to more than 0%, or it can be set to more than 0.00010%.
[0128] Acid soluble Al: 0 to 0.020 mass%
[0129] Acid-soluble Al (aluminum) (sol.Al) is an optional element for the base steel plate. Acid-soluble Al is contained in the steel billet (slab), but if an excessive amount of acid-soluble Al remains in the base steel plate after the finished annealing, it may have an adverse effect on the magnetic properties. Therefore, the acid-soluble Al content of the base steel plate only needs to be 0.020% or less. The acid-soluble Al content is preferably 0.0150% or less, and more preferably 0.010% or less. On the other hand, the lower limit of the acid-soluble Al content of the base steel plate is not particularly limited, as long as it is 0%. However, acid-soluble Al forms AlN and has the effect of acting as an inhibitor during secondary recrystallization, so the acid-soluble Al content can be set to more than 0%, or it can be set to more than 0.00010%.
[0130] P: 0 to 0.040 mass%
[0131] P (phosphorus) is an optional element for the base steel plate. If the P content exceeds 0.040%, the workability of the steel plate may be significantly reduced. Therefore, the P content only needs to be 0.040% or less. The P content is preferably 0.030% or less, and more preferably 0.020% or less. On the other hand, there is no particular restriction on the lower limit of the P content, as long as it is 0%. However, P has the effect of improving the texture and improving the magnetic properties of the steel plate, so the P content can be set to more than 0%, or it can be set to more than 0.0020%.
[0132] Total of S and Se: 0 to 0.010 mass%
[0133] S (sulfur) and Se (selenium) are optional elements for the base steel plate. S and Se are contained in the steel billet (slab), but if excessive amounts of S and Se remain in the base steel plate after finished annealing, it may have an adverse effect on the magnetic properties. Therefore, the total content of S and Se in the base steel plate only needs to be 0.010% or less. On the other hand, there is no particular restriction on the lower limit of the total content of S and Se in the base steel plate, as long as it is 0%. However, S and Se form MnS and MnSe and have the effect of acting as inhibitors during secondary recrystallization, so the total content of S and Se can be set to more than 0%, or can be set to more than 0.0050%.
[0134] Sn: 0-0.50 mass%
[0135] Sn (tin) is an optional element for the base steel plate. If the Sn content exceeds 0.50%, the secondary recrystallization may become unstable, which may have an adverse effect on the magnetic properties. Therefore, the Sn content only needs to be 0.50% or less. The Sn content is preferably 0.30% or less, and more preferably 0.150% or less. On the other hand, the lower limit of the Sn content is not particularly limited, as long as it is 0%. However, Sn has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Sn content can also be set to more than 0%, or it can be set to more than 0.0050%.
[0136] Cu: 0-0.50 mass%
[0137] Cu (copper) is an optional element for the base steel plate. If the Cu content exceeds 0.50%, the steel plate may become brittle during hot rolling. Therefore, the Cu content only needs to be 0.50% or less. The Cu content is preferably 0.30% or less, and more preferably 0.10% or less. On the other hand, there is no particular restriction on the lower limit of the Cu content, as long as it is 0%. However, Cu has the effect of increasing the aggregation of the Goss orientation and improving the magnetic properties, so the Cu content can also be set to more than 0%, or it can be set to more than 0.010%.
[0138] Cr: 0-0.50 mass%
[0139] Cr (chromium) is an optional element for the base steel plate. If the Cr content exceeds 0.50%, Cr oxides may be formed, which may have an adverse effect on the magnetic properties. Therefore, the Cr content only needs to be 0.50% or less. The Cr content is preferably 0.30% or less, and more preferably 0.10% or less. On the other hand, there is no particular restriction on the lower limit of the Cr content, as long as it is 0%. However, Cr has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Cr content can also be set to more than 0%, or it can be set to more than 0.010%.
[0140] Sb: 0-0.50 mass%
[0141] Sb (antimony) is an optional element for the base steel plate. If the Sb content exceeds 0.50%, it may have an adverse effect on the magnetic properties. Therefore, the Sb content only needs to be 0.50% or less. The Sb content is preferably 0.30% or less, and more preferably 0.10% or less. On the other hand, the lower limit of the Sb content is not particularly limited, as long as it is 0%. However, Sb has the effect of stabilizing secondary recrystallization by functioning as an inhibitor, so the Sb content can also be set to more than 0%, or can be set to more than 0.010%.
[0142] Mo: 0-0.10 mass%
[0143] Mo (molybdenum) is an optional element for the base steel plate. If the Mo content exceeds 0.10%, there may be problems with the rolling properties of the steel plate. Therefore, the Mo content only needs to be 0.10% or less. The Mo content is preferably 0.08% or less, and more preferably 0.05% or less. On the other hand, there is no particular restriction on the lower limit of the Mo content, as long as it is 0%. However, Mo has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Mo content can also be set to more than 0%, or it can be set to more than 0.0050%.
[0144] Bi: 0-0.10 mass%
[0145] Bi (bismuth) is an optional element for the base steel plate. If the Bi content exceeds 0.10%, the sheet passability during cold rolling may deteriorate. In addition, if the purification during the finished product annealing is insufficient and Bi remains excessively, it may have an adverse effect on the magnetic properties. Therefore, the Bi content only needs to be 0.10% or less. The Bi content is preferably 0.050% or less, more preferably 0.020% or less, and more preferably 0.0010% or less. On the other hand, the lower limit of the Bi content is not particularly limited, as long as it is 0%. However, Bi has the effect of improving the magnetic properties, so the Bi content can also be set to more than 0%, or it can be set to more than 0.00050%.
[0146] The base steel sheet of the grain-oriented electrical steel sheet of the present embodiment may contain impurities. It should be noted that "impurities" refer to components mixed from ore and scrap as raw materials or from the manufacturing environment when steel is manufactured industrially.
[0147] The chemical composition of the above-mentioned base steel plate can be measured by general analytical methods. For example, it can be measured using ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). It should be noted that acid-soluble Al can be measured by ICP-AES using the filtrate after the sample is heated and decomposed with acid. In addition, C and S can be measured using the combustion-infrared absorption method, N can be measured using the inert gas melting-thermal conductivity method, and O can be measured using the inert gas melting-non-dispersive infrared absorption method.
[0148] In addition, the chemical composition mentioned above is the component of the base steel sheet. When the grain-oriented electrical steel sheet used as the measurement sample has an insulating film etc. on the surface, the film etc. is removed by the following method and then the chemical composition is measured.
[0149] For example, as a method for removing the insulating film, the directional electromagnetic steel sheet having the film can be immersed in a high-temperature alkaline solution. Specifically, the insulating film can be removed from the directional electromagnetic steel sheet by immersing it in a sodium hydroxide aqueous solution of NaOH: 30-50 mass % + H2O: 50-70 mass % at 80-90°C for 5-10 minutes, then washing with water and drying. It should be noted that the immersion time in the sodium hydroxide aqueous solution can be changed according to the thickness of the insulating film.
[0150] In addition, the grain-oriented electrical steel sheet of the present embodiment does not have a forsterite film, but when it is desired to remove the forsterite film, the electrical steel sheet from which the insulating film has been removed by the above method can be immersed in high-temperature hydrochloric acid. Specifically, the concentration of hydrochloric acid preferred for removing the forsterite film to be dissolved is investigated in advance, and the forsterite film can be removed by immersing in hydrochloric acid of this concentration (for example, 30 to 40 mass % hydrochloric acid) at 80 to 90° C. for 1 to 5 minutes, then washing with water and drying. Usually, the treatment liquids are used separately to remove each film, such that an alkaline solution is used for the removal of the insulating film and hydrochloric acid is used for the removal of the forsterite film.
[0151] Next, a method for manufacturing the grain-oriented electrical steel sheet of the present embodiment will be described. It should be noted that the method for manufacturing the grain-oriented electrical steel sheet of the present embodiment is not limited to the method described below. The manufacturing method described below is an example for manufacturing the grain-oriented electrical steel sheet of the present embodiment.
[0152] Figure 2: is a flowchart illustrating a method for manufacturing a grain-oriented electrical steel sheet according to the present embodiment. The method for manufacturing a grain-oriented electrical steel sheet according to the present embodiment mainly includes the following steps: a hot rolling step of hot rolling a slab (steel billet) having a predetermined chemical composition to obtain a hot-rolled steel sheet; a hot-rolled steel sheet annealing step of annealing the hot-rolled steel sheet to obtain a hot-rolled annealed sheet; a cold rolling step of cold rolling the hot-rolled annealed sheet once or multiple cold rollings with annealing inserted to obtain a cold-rolled steel sheet; a decarburization annealing step of decarburizing the cold-rolled steel sheet to obtain a decarburized annealed sheet; a finishing annealing step of applying an annealing separator to the decarburized annealed sheet and then performing finishing annealing to obtain a finished annealed sheet; a thermal oxidation annealing step of thermally oxidizing the finished annealed sheet to obtain a thermal oxidation annealed sheet; and an insulating film forming step of applying an insulating film forming liquid to the thermal oxidation annealed sheet and then performing a heat treatment to form an insulating film on the surface of the thermal oxidation annealed sheet.
[0153] Specifically, the method for manufacturing a grain-oriented electrical steel sheet according to the present embodiment includes a hot rolling step, a hot-rolled steel sheet annealing step, a cold rolling step, a decarburization annealing step, a finish annealing step, a thermal oxidation annealing step, and an insulating film forming step.
[0154] In the above-mentioned finish annealing step, an annealing separator containing 20 to 99.5 mass % of aluminum oxide, 0.5 to 20 mass % of bismuth chloride, and the remainder of magnesium oxide and impurities is applied to the steel sheet after the above-mentioned decarburization annealing step in terms of solid content, and then dried, and then the finish annealing is performed.
[0155] In the above-mentioned thermal oxidation annealing process, the steel sheet after the above-mentioned final annealing process is heated from room temperature to a temperature range of 800 to 1100° C. in an atmosphere with an oxygen concentration of less than 1.0 volume % and an oxygen potential PH2O / PH2 of greater than 0.010 and less than 0.50, and is uniformly heated in the temperature range of 800 to 1100° C. for 5 to 200 seconds.
[0156] Each of the above steps will be described in detail. It should be noted that when the conditions of each step are not described in the following description, known conditions may be appropriately applied.
[0157] Hot rolling process
[0158] In the hot rolling process, a steel slab (for example, a steel ingot such as a slab) having a predetermined chemical composition is hot rolled. For example, the slab (steel slab) provided for the hot rolling process contains, as a chemical composition, in mass %:
[0159] Si: 3.0-4.0%,
[0160] Mn: 0.010~0.50%,
[0161] C: 0.020~0.20%,
[0162] N: 0.0020~0.020%,
[0163] Acid soluble Al: 0.010~0.050%
[0164] P: 0~0.040%,
[0165] Total of S and Se: 0.0010~0.040%,
[0166] Sn: 0~0.50%,
[0167] Cu: 0-0.50%,
[0168] Cr: 0~0.50%,
[0169] Sb: 0-0.50%,
[0170] Mo: 0~0.10%
[0171] Bi: 0~0.10%,
[0172] The remainder may contain Fe and impurities.
[0173] In addition, the above-mentioned slab (steel billet) may contain at least one selected from the following elements in terms of mass % as a chemical composition:
[0174] Sn: 0.0050~0.50%,
[0175] Cu: 0.010~0.50%,
[0176] Cr: 0.010~0.50%,
[0177] Sb: 0.010~0.50%,
[0178] Mo: 0.0050~0.10%,
[0179] Bi: 0.00050~0.10%.
[0180] Si: 3.0-4.0 mass%
[0181] Si (silicon) is a basic element for steel billets (slabs). If the Si content is less than 3.0%, the eddy current loss cannot be sufficiently reduced, so good magnetic properties cannot be obtained. Therefore, the Si content is set to 3.0% or more. The Si content is preferably 3.10% or more, and more preferably 3.20% or more. On the other hand, if the Si content exceeds 4.0%, the steel plate becomes brittle and the plate passability is significantly deteriorated during manufacturing, so the Si content is set to 4.0% or less. The Si content is preferably 3.70% or less, more preferably 3.60% or less, and more preferably 3.50% or less.
[0182] Mn: 0.010 to 0.50 mass%
[0183] Mn (manganese) is a basic element for steel billets (slabs). If the Mn content is less than 0.010%, it is difficult to form MnS and MnSe that function as inhibitors, and secondary recrystallization will not proceed sufficiently, and good magnetic properties cannot be obtained. Therefore, the Mn content is set to 0.010% or more. The Mn content is preferably 0.030% or more, and more preferably 0.050% or more. On the other hand, if the Mn content exceeds 0.50%, the steel undergoes phase transformation during secondary recrystallization annealing, and secondary recrystallization will not proceed sufficiently, and good magnetic properties cannot be obtained, so the Mn content is set to less than 0.50%. The Mn content is preferably less than 0.20%, more preferably less than 0.15%, and more preferably less than 0.10%.
[0184] C: 0.020 to 0.20% by mass
[0185] C (carbon) is a basic element for steel billets (slabs). C is included for the purpose of increasing the aggregation degree of Goss orientation in secondary recrystallization. Regarding the C content required for improving magnetic properties, it is 0.020% or more as a slab, and preferably 0.040% or more. However, if excessive C remains in the final product, it may become a factor that deteriorates iron loss. Therefore, decarburization treatment is required through a decarburization annealing process, but in the case where the slab contains more than 0.20%, decarburization treatment becomes difficult. Regarding the C content, it is less than 0.20% as a slab, preferably less than 0.15%, and more preferably less than 0.10%.
[0186] N: 0.0020 to 0.020 mass%
[0187] N (nitrogen) is an essential element for a steel slab (slab). N is an element necessary for forming AlN as an inhibitor and for increasing the degree of concentration of Goss orientation during secondary recrystallization.
[0188] Regarding the N content required for inhibitor formation, as a slab, it is 0.0020% or more, preferably 0.0040% or more, and more preferably 0.0060% or more. On the other hand, as a slab, if the N content exceeds 0.020%, blisters (voids) will be generated in the steel sheet during cold rolling, and the strength of the steel sheet will increase, and the sheet passability during manufacturing may be deteriorated. Regarding the N content, as a slab, it is 0.020% or less, preferably 0.015% or less, and more preferably 0.010% or less. Like C, if N remains excessively in the final product, it may cause magnetic degradation. Therefore, N needs to be purified during the final product annealing.
[0189] Acid soluble Al: 0.010-0.050 mass%
[0190] Acid-soluble Al (aluminum) (sol.Al) is an essential element for steel billets (slabs). Acid-soluble Al is an element required to form AlN as an inhibitor and to improve magnetic properties. Regarding the content of acid-soluble Al, it is 0.010% or more, preferably 0.015% or more, and more preferably 0.020% or more as a slab. On the other hand, when acid-soluble Al is excessively contained in the slab, embrittlement may become significant. Regarding the content of acid-soluble Al, it is 0.050% or less, preferably 0.040% or less, and more preferably 0.030% or less as a slab. Similar to N, acid-soluble Al needs to be purified from the base steel plate during the finished annealing.
[0191] P: 0 to 0.040 mass%
[0192] P (phosphorus) is an optional element for steel billets (slabs). If the P content exceeds 0.040%, the workability of the steel plate may be significantly reduced. Therefore, the P content only needs to be 0.040% or less. The P content is preferably 0.030% or less, and more preferably 0.020% or less. On the other hand, there is no particular restriction on the lower limit of the P content, as long as it is 0%. However, P has the effect of improving the texture and improving the magnetic properties of the steel plate, so the P content can be set to more than 0%, or it can be set to more than 0.0020%.
[0193] Total of S and Se: 0.0010 to 0.040 mass%
[0194] S (sulfur) and Se (selenium) are basic elements for steel billets (slabs). S and Se are elements that form MnS, which serves as an inhibitor. The total content of S and Se is 0.0010% or more for a slab, preferably 0.010% or more, and more preferably 0.020% or more. On the other hand, if the total content of S and Se exceeds 0.040% for a slab, it may cause hot brittleness and hot rolling becomes difficult. The total content of S and Se is 0.040% or less for a slab, preferably 0.0350% or less, and more preferably 0.030% or less. S and Se may also cause magnetic deterioration if they remain in excess in the final product. Therefore, S and Se also need to be purified from the base steel plate during the finished product annealing.
[0195] Sn: 0-0.50 mass%
[0196] Sn (tin) is an optional element for steel billets (slabs). If the Sn content exceeds 0.50%, the secondary recrystallization may become unstable, which may have an adverse effect on the magnetic properties. Therefore, the Sn content only needs to be 0.50% or less. The Sn content is preferably 0.30% or less, and more preferably 0.150% or less. On the other hand, the lower limit of the Sn content is not particularly limited, as long as it is 0%. However, Sn has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Sn content may be set to more than 0%, or may be set to more than 0.0050%.
[0197] Cu: 0-0.50 mass%
[0198] Cu (copper) is an optional element for steel billets (slabs). If the Cu content exceeds 0.50%, the steel plate may become brittle during hot rolling. Therefore, the Cu content only needs to be 0.50% or less. The Cu content is preferably 0.30% or less, and more preferably 0.10% or less. On the other hand, there is no particular restriction on the lower limit of the Cu content, as long as it is 0%. However, Cu has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Cu content can also be set to more than 0%, or it can be set to more than 0.010%.
[0199] Cr: 0-0.50 mass%
[0200] Cr (chromium) is an optional element for steel billets (slabs). If the Cr content exceeds 0.50%, Cr oxides may be formed, which may have an adverse effect on the magnetic properties. Therefore, the Cr content only needs to be 0.50% or less. The Cr content is preferably 0.30% or less, and more preferably 0.10% or less. On the other hand, there is no particular restriction on the lower limit of the Cr content, as long as it is 0%. However, Cr has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Cr content can also be set to more than 0%, or it can be set to more than 0.010%.
[0201] Sb: 0-0.50 mass%
[0202] Sb (antimony) is an optional element for steel billets (slabs). If the Sb content exceeds 0.50%, it may have an adverse effect on the magnetic properties. Therefore, the Sb content only needs to be 0.50% or less. The Sb content is preferably 0.30% or less, and more preferably 0.10% or less. On the other hand, the lower limit of the Sb content is not particularly limited, as long as it is 0%. However, Sb has the effect of stabilizing secondary recrystallization by functioning as an inhibitor, so the Sb content can also be set to more than 0%, or can be set to more than 0.010%.
[0203] Mo: 0-0.10 mass%
[0204] Mo (molybdenum) is an optional element for steel billets (slabs). If the Mo content exceeds 0.10%, there may be problems with the rolling properties of the steel plate. Therefore, the Mo content only needs to be 0.10% or less. The Mo content is preferably 0.08% or less, and more preferably 0.05% or less. On the other hand, there is no particular restriction on the lower limit of the Mo content, as long as it is 0%. However, Mo has the effect of increasing the aggregation of Goss orientation and improving magnetic properties, so the Mo content can also be set to more than 0%, or it can be set to more than 0.0050%.
[0205] Bi: 0-0.10 mass%
[0206] Bi (bismuth) is an optional element for steel billets (slabs). If the Bi content exceeds 0.10%, the sheet passability during cold rolling may deteriorate. In addition, if the purification during the finished product annealing is insufficient and an excessive amount of Bi remains, it may have an adverse effect on the magnetic properties. Therefore, the Bi content only needs to be 0.10% or less. The Bi content is preferably 0.050% or less, more preferably 0.020% or less, and more preferably 0.0010% or less. On the other hand, the lower limit of the Bi content is not particularly limited, as long as it is 0%. However, Bi has the effect of improving the magnetic properties, so the Bi content can also be set to more than 0%, or it can be set to more than 0.00050%.
[0207] The steel billet (slab) supplied to the hot rolling process may also contain impurities. It should be noted that "impurities" refer to components mixed from ore, scrap, or the manufacturing environment when steel is manufactured industrially. In addition, the chemical composition of the steel billet (slab) supplied to the hot rolling process can be measured by the same method as the chemical composition of the base steel plate described above.
[0208] In the hot rolling process, first, the steel billet is subjected to a heat treatment. The heating temperature may be set to, for example, 1200°C to 1600°C. The lower limit of the heating temperature is preferably 1280°C, and the upper limit of the heating temperature is preferably 1500°C. The heated steel billet is then hot rolled. The thickness of the hot-rolled steel sheet after hot rolling is preferably in the range of 2.0 mm to 3.0 mm, for example.
[0209] Hot rolled steel plate annealing process
[0210] In the hot-rolled steel sheet annealing process, the hot-rolled steel sheet obtained by the hot rolling process is annealed. Through the hot-rolled steel sheet annealing, recrystallization occurs in the steel sheet, and finally good magnetic properties can be achieved. The conditions for the hot-rolled steel sheet annealing are not particularly limited, but for example, the hot-rolled steel sheet can be annealed in a temperature range of 900 to 1200° C. for 10 seconds to 5 minutes. In addition, the surface of the hot-rolled annealed sheet can also be pickled after the hot-rolled steel sheet annealing and before cold rolling.
[0211] Cold rolling process
[0212] In the cold rolling process, the hot-rolled annealed sheet after the hot-rolled steel sheet annealing process is subjected to one cold rolling or multiple cold rollings with intermediate annealing in between. It should be noted that the hot-rolled annealed sheet has a good shape of the steel sheet due to the annealing of the hot-rolled steel sheet, so the possibility of the steel sheet breaking in the first cold rolling can be reduced. In addition, when the intermediate annealing is performed during the cold rolling, the heating method of the intermediate annealing is not particularly limited. In addition, the cold rolling can also be performed in three or more times with the intermediate annealing, but since the manufacturing cost increases, it is preferably set to one or two cold rollings.
[0213] The final cold rolling reduction ratio in cold rolling (the cumulative cold rolling ratio without intermediate annealing or the cumulative cold rolling ratio after intermediate annealing) can be set in the range of 80% to 95%. By setting the final cold rolling reduction ratio in the above range, the final cold rolling reduction ratio to {110} <001> The degree of aggregation of orientation can be reduced, and the instability of secondary recrystallization can be suppressed. It should be noted that the thickness of the cold-rolled steel sheet that has been cold-rolled usually becomes the thickness (final thickness) of the parent steel sheet of the finally manufactured directional electromagnetic steel sheet. The thickness of the cold-rolled steel sheet after cold rolling is preferably in the range of 0.17 mm to 0.29 mm, for example.
[0214] Decarburization annealing process
[0215] In the decarburization annealing process, the cold-rolled steel sheet obtained by the cold rolling process is subjected to decarburization annealing. Through the decarburization annealing, C contained in the cold-rolled steel sheet is removed, and primary recrystallization occurs. In order to remove C contained in the cold-rolled steel sheet, the decarburization annealing is preferably performed in a wet atmosphere, for example, annealing is performed in a wet atmosphere in a temperature range of 700 to 1000° C. for 10 seconds to 10 minutes.
[0216] In addition, nitriding treatment may be performed after decarburization annealing and before applying the annealing separator. In the nitriding treatment, the decarburization annealed steel sheet after decarburization annealing is subjected to nitriding treatment to produce a nitrided steel sheet. For example, annealing may be performed for 10 to 60 seconds in an atmosphere containing a gas having nitriding ability such as hydrogen, nitrogen, and ammonia in a temperature range of 700 to 850°C.
[0217] Finished product annealing process
[0218] In the finish annealing process, an annealing separator is applied to the decarburized annealed sheet obtained in the decarburization annealing process and the finish annealing is performed. The finish annealing can be performed by annealing for a long time in a state where the steel sheet is rolled into a coil. In order to prevent the steel sheet rolled into a coil from sintering during the finish annealing, an annealing separator is applied to the decarburized annealed sheet and dried before the finish annealing.
[0219] The annealing separator contains magnesium oxide (MgO), aluminum oxide (Al2O3) and bismuth chloride. In the annealing separator, aluminum oxide accounts for 20 to 99.5% by mass, bismuth chloride accounts for 0.5 to 20% by mass, and the remainder is magnesium oxide and impurities, calculated on a solid basis. The bismuth chloride may be bismuth oxychloride (BiOCl), bismuth trichloride (BiCl3), or the like.
[0220] The annealing conditions of the final annealing are not particularly limited, and known conditions can be appropriately adopted. For example, in the final annealing, the decarburized annealed sheet coated with an annealing separator and dried is kept in a temperature range of 1000°C to 1300°C for 10 hours to 60 hours. The atmosphere during the final annealing can be set to, for example, a nitrogen atmosphere or a mixed atmosphere of nitrogen and hydrogen. In addition, after the final annealing, the surface of the final annealed sheet can also be washed with water to remove powder.
[0221] Through this finish annealing, secondary recrystallization is induced in the steel sheet, and the crystal orientation is along {110} <001> Orientation is performed. The secondary recrystallization structure is easy to align the magnetization axis in the rolling direction, and the grains are coarse. Due to the secondary recrystallization structure, excellent magnetic properties can be obtained. It should be noted that in this embodiment, since the annealing separator contains bismuth chloride, the formation of forsterite film can be suppressed, and the surface of the finished annealed sheet becomes smooth.
[0222] In addition, the atmosphere during the finish annealing may be changed to a hydrogen atmosphere for purification treatment. By this purification treatment, elements such as Al, N, S, and Se contained in the steel sheet as a steel composition are discharged to the outside of the system, and the steel sheet is purified.
[0223] Thermal oxidation annealing process
[0224] In the thermal oxidation annealing step, the finish annealed sheet obtained in the finish annealing step is subjected to thermal oxidation annealing (heat treatment). In addition, the first surface treatment may be performed before the heat treatment, or the second surface treatment may be performed after the heat treatment.
[0225] First surface treatment
[0226] The finished annealed sheet obtained by the finish annealing step may be subjected to a first surface treatment as required. In the first surface treatment, the pickling conditions are not particularly specified, but for example, the finished annealed sheet may be immersed in an acid (first treatment liquid) of a specific concentration. The first treatment liquid contains at least one of hydrochloric acid, sulfuric acid, nitric acid, and phosphoric acid, and the total acid concentration is 1 to 20% by mass, and the liquid temperature is 50 to 90° C. The finished annealed sheet may be subjected to a surface treatment for 3 to 60 seconds using the first treatment liquid.
[0227] In the first surface treatment, the surface of the finished annealed sheet is made into an active surface state, but on the other hand, it is preferred to perform the surface treatment under the condition that no erosion pits are generated on the surface of the finished annealed sheet. To this end, the above-mentioned conditions can be controlled in a composite and inseparable manner. For example, if the pickling intensity is increased for one of the above-mentioned conditions, the active state of the surface and the smooth state of the surface can be taken into account by changing the other conditions in the above-mentioned conditions in a manner that weakens the pickling intensity. If a person skilled in the art can perform surface control including pickling behavior, then if the influence of the above-mentioned conditions on the pickling intensity is considered, the above-mentioned conditions can be combined to control the surface state.
[0228] It should be noted that if the total acid concentration of the first treatment liquid is less than 1% by mass, it is difficult to set the surface of the finished annealed sheet to an active surface state, and it is difficult to form internally oxidized SiO2 in the subsequent heat treatment. On the other hand, if the total acid concentration of the first treatment liquid exceeds 20% by mass, erosion pits are easily formed on the surface of the finished annealed sheet. Similarly, if the liquid temperature of the first treatment liquid is less than 50°C, an active surface state cannot be obtained, and if the liquid temperature of the first treatment liquid exceeds 90°C, erosion pits are easily formed. Similarly, if the treatment time of the first surface treatment is less than 3 seconds, an active surface state cannot be obtained, and if the treatment time of the first surface treatment exceeds 60 seconds, erosion pits are easily formed.
[0229] Heat treatment
[0230] In the heat treatment, thermal oxidation annealing is performed on the finished annealed sheet after the finish annealing step or the finished annealed sheet after the first surface treatment. In this heat treatment, the steel sheet is heated from room temperature to a temperature range of 800 to 1100° C. in an atmosphere having an oxygen concentration of less than 1.0 volume % and an oxygen potential PH2O / PH2 of 0.010 or more and less than 0.50, and is soaked in the temperature range of 800 to 1100° C. for 5 to 200 seconds. It should be noted that the oxygen potential PH2O / PH2 can be defined by the ratio of the water vapor partial pressure PH2O to the hydrogen partial pressure PH2 in the atmosphere.
[0231] In this embodiment, by including Bi chloride in the annealing separator and setting the atmosphere of the heat treatment to the above-mentioned atmosphere, internal oxidation SiO2 is preferably formed near the surface in the finished annealed sheet. On the other hand, it is preferred that no external oxide film is formed. For this reason, the above-mentioned conditions are controlled in a composite and inseparable manner. For example, if the oxidizability is increased by controlling the conditions within the range of the above-mentioned conditions, internal oxidation is likely to occur, and if the oxidizability is reduced by controlling the conditions within the range of the above-mentioned conditions, external oxidation is likely to occur. If a person skilled in the art is skilled in the art, the above-mentioned conditions can be combined to control the oxidation reaction and form the target oxide.
[0232] For example, if the oxygen concentration is 1.0 volume % or more, internal oxidized SiO2 will not be formed, and the entire surface of the steel sheet is easily excessively oxidized. Therefore, the oxygen concentration is set to less than 1.0 volume %. The oxygen concentration is preferably 0.50 volume % or less, and more preferably 0.10 volume % or less. On the other hand, there is no particular restriction on the lower limit of the oxygen concentration, and the smaller the better. However, it is difficult to set the oxygen concentration to 0 volume % in industry, so the oxygen concentration can also be set to 1.0×10 -20 The oxygen concentration is preferably 1.0×10 -19 Volume % or more, more preferably 1.0×10 -18 Volume % or more.
[0233] Similarly, if the oxygen potential PH2O / PH2 is lower than 0.010, it is difficult to form internal oxidized SiO2. Therefore, the oxygen potential PH2O / PH2 is set to be greater than 0.010. The oxygen potential PH2O / PH2 is preferably greater than 0.020, and more preferably greater than 0.030. On the other hand, if the oxygen potential PH2O / PH2 is greater than 0.50, internal oxidized SiO2 will not be formed, and the entire surface of the steel sheet is easily excessively oxidized. Therefore, the oxygen potential PH2O / PH2 is set to be less than 0.50. The oxygen potential PH2O / PH2 is preferably less than 0.40, and more preferably less than 0.30. The oxygen potential PH2O / PH2 can be derived from the hydrogen concentration and dew point in the annealing atmosphere.
[0234] Similarly, if the soaking temperature is lower than 800°C, it is difficult to form internal oxidized SiO2. Therefore, the soaking temperature is set to 800°C or higher. The soaking temperature is preferably 830°C or higher, and more preferably 860°C or higher. On the other hand, if the soaking temperature exceeds 1100°C, internal oxidized SiO2 will not be formed, and the entire surface of the steel plate is prone to excessive oxidation. Therefore, the soaking temperature is set to 1100°C or lower. The soaking temperature is preferably 1050°C or lower, and more preferably 1000°C or lower.
[0235] Similarly, if the soaking time is less than 5 seconds, it is difficult to form internal oxidized SiO2. Therefore, the soaking time is set to 5 seconds or more. The soaking time is preferably 10 seconds or more, and more preferably 15 seconds or more. On the other hand, if the soaking time exceeds 200 seconds, the entire surface of the steel plate is easily excessively oxidized. Therefore, the soaking time is set to 200 seconds or less. The soaking time is preferably 150 seconds or less, and more preferably 100 seconds or less.
[0236] Second surface treatment
[0237] The thermal oxidation annealed sheet after the heat treatment may also be subjected to a second surface treatment as required. In the second surface treatment, the pickling conditions are not particularly specified, but for example, the thermal oxidation annealed sheet may be immersed in an acid (second treatment liquid) of a specific concentration. The second treatment liquid contains at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, and the total acid concentration is 1 to 10% by mass, and the liquid temperature is 50 to 90° C. The thermal oxidation annealed sheet may be subjected to a surface treatment for 3 to 60 seconds using the second treatment liquid.
[0238] In the second surface treatment, the residual oxides on the surface of the thermal oxidation annealing plate are pickled, but on the other hand, it is preferred to carry out the surface treatment under the condition that no erosion pits are generated on the surface of the thermal oxidation annealing plate. For this reason, the above-mentioned conditions can be controlled in a composite and inseparable manner. For example, if the pickling intensity is increased for one of the above-mentioned conditions, the pickling of the oxide and the smooth state of the surface can be taken into account by changing the other conditions in the above-mentioned conditions in a manner that weakens the pickling intensity. If it is a person skilled in the art, it is possible to perform surface control including pickling behavior, so if the influence of the above-mentioned conditions on the pickling intensity is considered, the above-mentioned conditions can be combined to control the surface state.
[0239] It should be noted that if the total acid concentration of the second treatment liquid is less than 1% by mass, it is difficult to pickle the residual oxide on the surface of the thermal oxidation annealing plate. On the other hand, if the total acid concentration of the second treatment liquid exceeds 10% by mass, erosion pits are easily formed on the surface of the thermal oxidation annealing plate. Similarly, if the liquid temperature of the second treatment liquid is less than 50°C, pickling of the residual oxide is difficult, and if the liquid temperature of the second treatment liquid exceeds 90°C, erosion pits are easily formed. Similarly, if the treatment time of the second surface treatment is less than 3 seconds, pickling of the residual oxide is difficult, and if the treatment time of the second surface treatment exceeds 60 seconds, erosion pits are easily formed.
[0240] Insulation film forming process
[0241] In the insulating film forming step, an insulating film forming liquid is applied to the thermal oxidation annealing plate after the thermal oxidation annealing step to perform heat treatment. By this heat treatment, an insulating film is formed on the surface of the thermal oxidation annealing plate. For example, the insulating film forming liquid only needs to contain colloidal silica and phosphate. The insulating film forming liquid preferably does not contain chromium.
[0242] The insulating film applies tension to the grain-oriented electrical steel sheet to reduce the iron loss of a single steel sheet, and reduces the iron loss of a core by ensuring electrical insulation between the steel sheets when the grain-oriented electrical steel sheets are stacked for use.
[0243] The insulating film is formed by applying an insulating film forming liquid containing at least one of phosphate or colloidal silica as a main component to the surface of the thermal oxidation annealed plate, and performing a heat treatment at 350° C. to 1150° C. for 5 to 300 seconds. When the film is formed, the oxygen potential PH2O / PH2 of the atmosphere can be controlled as needed.
[0244] As the phosphate, phosphates of Ca, Al, Sr, etc. are preferred, among which aluminum phosphate is more preferred. Colloidal silica is not particularly limited to colloidal silica of specific properties. The particle size is also not particularly limited to a specific particle size, but is preferably less than 200 nm (number average particle size). For example, 5 to 30 nm is sufficient. If the particle size exceeds 200 nm, sedimentation may occur in the coating liquid.
[0245] In this embodiment, since internal oxidized SiO2 is preferably formed near the surface in the thermal oxidation annealing sheet in the thermal oxidation annealing step, the insulating film formed in the insulating film forming step is preferably in close contact with the thermal oxidation annealing sheet (base steel sheet).
[0246] After the insulating film is formed, flattening annealing may be performed for shape correction as needed. By performing flattening annealing on the steel sheet, the iron loss can be further reduced.
[0247] Magnetic Domain Control Process
[0248] In the present embodiment, a magnetic domain control treatment may be performed as needed before or after the insulating film forming step. By performing the magnetic domain control treatment, the iron loss of the grain-oriented electrical steel sheet can be further reduced.
[0249] In the case where the magnetic domain control treatment is performed before the insulating film forming step, it is sufficient to form linear or dot-shaped grooves extending in a direction intersecting the rolling direction at a predetermined interval along the rolling direction. In addition, in the case where the magnetic domain control treatment is performed after the insulating film forming step, it is sufficient to form linear or dot-shaped stress strain portions extending in a direction intersecting the rolling direction at a predetermined interval along the rolling direction. Through the magnetic domain control treatment, the width of the 180° magnetic domain is narrowed (the 180° magnetic domain is refined).
[0250] When forming the groove portion, a mechanical groove forming method using a gear or the like, a chemical groove forming method using electrolytic etching to form the groove, a thermal groove forming method using laser irradiation, etc. can be applied. In addition, when forming the stress strain portion, laser beam irradiation, electron beam irradiation, etc. can be applied.
[0251] Example
[0252] Next, the effect of one scheme of the present invention is described in more detail by way of an embodiment, but the conditions in the embodiment are a conditional example adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this conditional example. As long as it does not deviate from the gist of the present invention and achieves the purpose of the present invention, the present invention can adopt various conditions.
[0253] The slab (steel billet) having the chemical composition shown in Table 1 was heated to 1350°C and subjected to hot rolling to produce a hot-rolled steel sheet with a thickness of 2.3 mm. The hot-rolled steel sheet was annealed at 1100°C for 120 seconds and pickled. Thereafter, a single cold rolling or multiple cold rolling with intermediate annealing was performed to produce a cold-rolled steel sheet with a final thickness. The cold-rolled steel sheet was subjected to decarburization annealing at 830°C for 100 seconds in a wet hydrogen atmosphere. It should be noted that after decarburization annealing, nitriding treatment was performed on Test No. 26 and No. 33 shown in the table.
[0254] The annealing separators shown in Tables 3 to 6 are applied to the obtained decarburized annealed plates and dried. It should be noted that in the table, aluminum oxide and bismuth chloride represent the content converted to solid content, and the remainder is represented by magnesium oxide and impurities. After that, a final annealing is performed at 1200°C for 20 hours. The final annealing atmosphere is set to a mixed atmosphere of nitrogen and hydrogen, and then to a hydrogen atmosphere. After the final annealing, the steel plate is washed with water to remove the remaining annealing separator.
[0255] The obtained product annealed sheets were subjected to heat treatment as thermal oxidation annealing under the conditions shown in Tables 7 to 10. If necessary, first surface treatment and second surface treatment were also performed as shown in Tables 3 to 10.
[0256] An insulating film forming liquid containing colloidal silica and phosphate was applied to the surface of the obtained thermal oxidation annealed plate, and heat-treated at 850° C. for 1 minute to form an insulating film having a unit area weight of 2.5 to 4.5 g / m2 per side. 2 The oriented electrical steel sheet is manufactured by forming an insulating film. The obtained oriented electrical steel sheet is subjected to a magnetic domain control treatment by irradiating a laser beam.
[0257] For the obtained grain-oriented electrical steel sheets No. 1 to No. 60, the chemical composition of the base steel sheet, the internal oxidized SiO2 present in the base steel sheet within a range of 2.0 μm from the interface with the insulating film toward the sheet thickness direction, etc. were confirmed based on the above-mentioned method. In addition, for the obtained grain-oriented electrical steel sheets No. 1 to No. 60, the film adhesion and magnetic properties were evaluated.
[0258] Regarding SiO2, a small test piece with a plate width of 10 mm and a rolling direction of 20 mm was used as the starting material, and a cut surface parallel to the plate thickness direction and perpendicular to the plate width direction was cut from 10 places spaced apart from each other on the plate surface. A 10 μm×8 μm evaluation sample was prepared by FIB processing (MI4050, manufactured by Hitachi High-Tech Science Co., Ltd.), and a line analysis was performed along the plate thickness direction under the condition of an acceleration voltage of 200 kV by TEM-EDS (for example, JEM-2100PLUS: manufactured by JEOL Ltd.), and the chemical composition was quantitatively analyzed and identified by the chemical composition ratio. The elements for quantitative analysis were set to the five elements of Fe, P, Si, Al, and O. From the results of TEM-EDS, the region with an Fe content of less than 80 atomic %, a Si content of more than 30 atomic %, and an O content of more than 55 atomic % excluding the measurement noise was identified as internally oxidized SiO2. Next, for SiO2 identified by the above method, a bright field image is taken by TEM at an acceleration voltage of 200 kV and a magnification of 40,000 times, and the brightness value of the bright field image of SiO2 is obtained. The area with the same brightness value is identified as SiO2, and the number of pixels contained in the area of 2.0 μm from the interface with the insulating film to the plate thickness direction in the parent steel plate and the number of pixels of SiO2 are converted from the pixel size to the area, and the area ratio of the internal oxidation SiO2 to the area of the area from the interface with the insulating film to the plate thickness direction to 2.0 μm in the parent steel plate is calculated. For the bright field image, a field of view of 10 μm×8 μm is observed for 10 randomly selected locations. It should be noted that when identifying, the area below the pixel size is removed from the analysis object as noise. In addition, for the identification of each phase and the measurement of the area, general image processing software such as ImageJ can be used, and correction using manual operation can also be included.
[0259] The film adhesion is evaluated by the film remaining area ratio when the test piece is wound on a cylinder with a diameter of 20 mm and bent 180°. Calculate the area ratio of the remaining surface of the film relative to the area of the steel plate in contact with the cylinder. The area of the steel plate in contact with the roller is obtained by calculation. The area of the remaining surface is obtained by taking a photo of the steel plate after the test and performing image analysis on the photo image. The case where the film remaining area ratio is 95% or more is evaluated as excellent (EX), the case where it is 90% or more and less than 95% is evaluated as very good (VG), the case where it is 85% or more and less than 90% is evaluated as good (G), the case where it is 80% or more and less than 85% is evaluated as acceptable (F), and the case where it is less than 80% is evaluated as poor. The case where the film remaining area ratio is 80% or more is judged as qualified.
[0260] Regarding the iron loss characteristics, the test piece was evaluated based on the single sheet magnetic property test method (SST: Single Sheet Tester). Under the conditions of AC frequency: 50Hz, excitation magnetic flux density: 1.7T, the iron loss W17 / 50 (W / kg) defined by the power loss per unit weight (1kg) of the steel plate was measured. The iron loss W17 / 50 below 0.75W / kg was judged to be qualified. It should be noted that the magnetic flux density is the magnetic flux density B8 (T) in the rolling direction measured by applying a magnetic field of 800A / m to the test piece.
[0261] The manufacturing conditions, manufacturing results, and evaluation results are shown in Tables 1 to 14. Note that "-" in the chemical composition in the table means that no alloying element was intentionally added, and "-" other than the chemical composition in the table means that it was not implemented or not applied.
[0262] In addition, in the layer structure in the table, the intermediate ceramic layer is "none", which means that there is no forsterite film or the like as an intermediate ceramic layer, and the insulating film is arranged in contact with the base steel plate, and the base steel plate has a smooth surface. In addition, the intermediate ceramic layer is "yes", which means that there is an intermediate ceramic layer such as a forsterite film that has an adverse effect on the magnetic properties. The intermediate ceramic layer causes magnetic degradation. In addition, the internal oxidized SiO2 in the table is "none", which means that there is not enough internal oxidized SiO2 in the base steel plate within the range of 2.0 μm from the interface with the insulating film to the plate thickness direction. In addition, the "area ratio" of the internal oxidized SiO2 in the table represents the average value of the area ratio of the internal oxidized SiO2 relative to the area of the region from the interface with the insulating film to the plate thickness direction to 2.0 μm in the base steel plate. In addition, the "isoperiodic constant" of the internal oxidized SiO2 in the table represents the average value of the isoperidic constant of the internal oxidized SiO2 present in the base steel plate within the range of 2.0 μm from the interface with the insulating film to the plate thickness direction. In addition, the "existence frequency in 10 viewing fields" of internal oxidized SiO2 in the table indicates the number of locations where internal oxidized SiO2 preferably exists within a range of 2.0 μm from the interface with the insulating coating toward the plate thickness direction in the base steel plate when the cut surface is observed at 10 observation locations separated from each other on the plate surface.
[0263] The examples of the present invention in Test Nos. 1 to 60 were excellent in film adhesion and iron loss characteristics without relying on the forsterite film. On the other hand, the comparative examples in Test Nos. 1 to 60 were not excellent in surface smoothness, film adhesion or iron loss characteristics.
[0264] [Table 1]
[0265]
[0266] [Table 2]
[0267]
[0268] [Table 3]
[0269]
[0270] [Table 4]
[0271]
[0272] [Table 5]
[0273]
[0274] [Table 6]
[0275]
[0276] [Table 7]
[0277]
[0278] [Table 8]
[0279]
[0280] [Table 9]
[0281]
[0282] [Table 10]
[0283]
[0284] [Table 11]
[0285]
[0286] [Table 12]
[0287]
[0288] [Table 13]
[0289]
[0290] [Table 14]
[0291]
[0292] Industrial Applicability
[0293] According to the above-mentioned scheme of the present invention, it is possible to provide a grain-oriented electromagnetic steel sheet having excellent film adhesion without relying on a forsterite film and a method for manufacturing the same. In the grain-oriented electromagnetic steel sheet, since there is no forsterite film, the surface of the base steel sheet is smooth, and since internal oxidation is preferably performed near the surface of the base steel sheet, the film adhesion is excellent. Therefore, it becomes possible to preferably improve the iron loss characteristics. Therefore, the industrial applicability is high.
[0294] Explanation of symbols
[0295] 1. Grain-oriented electrical steel sheet
[0296] 11 Base steel plate
[0297] 11a Internal oxidation SiO2
[0298] 12 Insulation film
Claims
1. A grain-oriented electrical steel sheet comprising a base steel sheet and an insulating film disposed in contact with the base steel sheet, It is characterized in that The base steel plate comprises, as a chemical composition, in terms of mass %: Si: 3.0-4.0%, Mn: 0.010~0.50%, The rest is Fe and impurities. When observed in a cut plane whose cutting direction is parallel to the plate thickness direction and perpendicular to the plate width direction, the base steel plate has internally oxidized SiO in a range of 2.0 μm from the interface with the insulating film toward the plate thickness direction. 2 .
2. The grain-oriented electrical steel sheet according to claim 1, It is characterized in that The base steel plate further comprises, as the chemical composition, in terms of mass %: C: 0.010% or less, N: 0.010% or less, Acid soluble Al: 0.020% or less, P: 0.040% or less, Total of S and Se: 0.010% or less, Sn: 0.50% or less, Cu: 0.50% or less, Cr: 0.50% or less, Sb: 0.50% or less, Mo: 0.10% or less, Bi: 0.10% or less.
3. The grain-oriented electromagnetic steel sheet according to claim 1 or claim 2, It is characterized in that When observing the cut surface, the internal oxidized SiO 2 Has a dendrite shape.
4. The grain-oriented electromagnetic steel sheet according to claim 1 or claim 2, It is characterized in that When the cut surface is observed at 10 observation locations spaced apart from each other on the plate surface, the internally oxidized SiO 2 Included in 5 or more observation sites.
5. A method for manufacturing a directional electromagnetic steel sheet, It is characterized in that The method for manufacturing a grain-oriented electrical steel sheet according to claim 1 or claim 2 comprises a hot rolling step, a hot-rolled steel sheet annealing step, a cold rolling step, a decarburization annealing step, a finish annealing step, a thermal oxidation annealing step and an insulating film forming step. In the finish annealing step, an annealing separator containing 20 to 99.5 mass % of aluminum oxide, 0.5 to 20 mass % of bismuth chloride, and the remainder magnesium oxide and impurities in terms of solid content is applied to the steel sheet after the decarburization annealing step and dried, and then the finish annealing is performed. In the thermal oxidation annealing step, the steel sheet after the final annealing step is subjected to an oxygen concentration of less than 1.0 volume % and an oxygen potential pH of 2 O / PH 2 The temperature is heated from room temperature to a temperature range of 800 to 1100° C. in an atmosphere of 0.010 to less than 0.50, and soaked in the temperature range of 800 to 1100° C. for 5 to 200 seconds.
6. The method for producing a grain-oriented electrical steel sheet according to claim 5, It is characterized in that In the thermal oxidation annealing process, as the first surface treatment, the steel plate after the finished annealing process is immersed in a first treatment liquid containing at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, with a total acid concentration of 1 to 20 mass % and a liquid temperature of 50 to 90° C. for 3 to 60 seconds, and as a heating treatment, the steel plate after the first surface treatment is subjected to the heating and the soaking.
7. The method for producing a grain-oriented electrical steel sheet according to claim 5, It is characterized in that In the thermal oxidation annealing step, as a second surface treatment, the steel sheet after the heating and soaking is immersed in a second treatment liquid containing at least one of hydrochloric acid, sulfuric acid, nitric acid and phosphoric acid, with a total acid concentration of 1 to 10 mass % and a liquid temperature of 50 to 90° C. for 3 to 60 seconds.