Transparent substrate with antireflection film, and image display device

CN119013586AInactive Publication Date: 2024-11-22AGC INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032444.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-04-05
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In large μ-LED displays, the anti-reflective film with a diffusion layer causes significant changes in the tone of the diffuse reflected light, resulting in inconsistent appearance and color when extinguished and a decrease in grade.

Method used

By forming a diffusion layer and an anti-reflection film on the transparent substrate, it is ensured that a* and b* of the diffusely reflected light meet specific conditions (-6≤a*≤2, -1≤b*≤12, b*≤-2a*+ 4, b*≥-2a*-5), to control the angle dependence of diffuse reflected light, reduce tone changes, and use a layered dielectric layer, including Si oxide and mixed oxide in the anti-reflection film, optimize Light transmittance and thin layer resistance.

Benefits of technology

It realizes a transparent substrate with not easy to detect color deviation during tiling, improves the taste and black feel of the display, is suitable for the use of large μ-LED displays, and maintains the optical characteristics stable in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013586A_ABST
    Figure CN119013586A_ABST
Patent Text Reader

Abstract

The present invention relates to a transparent substrate with an antireflection film, which is provided with a transparent substrate having two main surfaces, and a diffusion layer and an antireflection film that are provided on one main surface of the transparent substrate in this order from the transparent substrate side, when the reflection of the other main surface of the transparent substrate is removed and the light source is incident on the one main surface side at an incident angle (45) DEG, a * and b * under a D65 light source of diffuse reflection light at each angle of-15 DEG, 15 DEG, 25 DEG, 45 DEG, 75 DEG, and 110 DEG with respect to specular reflection light satisfy the following formulae (1)-(4). (1)-6 < = a * < = 2 (2)-1 < = b * < = 12 (3) b * < =-2a * + 4 (4) b * > =-2a *-5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a transparent substrate with an antireflection film and an image display device having the same. Background Art

[0002] In recent years, from the viewpoint of aesthetics, a method of providing a transparent substrate such as a cover glass in front of an image display device such as a liquid crystal display (LCD) has been adopted. In addition, in order to prevent external light from being reflected into the transparent substrate, a transparent substrate having an anti-reflection film (hereinafter also referred to as a transparent substrate with an anti-reflection film) is known. For example, Patent Document 1 discloses a transparent substrate with an anti-reflection film that has light absorption capability and is insulating.

[0003] In addition, in order to prevent the reflection of external light, it is also known to provide a diffusion layer on a transparent substrate. The diffusion layer suppresses the reflection of external light by diffusing the incident light. However, when the transparent substrate is provided with a diffusion layer, when used in an image display device, the screen when the light is turned off sometimes appears whitish due to the diffused light. Therefore, by further providing an anti-reflection film as described above on the diffusion layer, the reflection of the incident light can be suppressed, thereby suppressing the whitish appearance. As a result, the black texture of the screen when the light is turned off can be improved while appropriately suppressing the reflection.

[0004] However, as an image display device, μ-LED displays using μ-LED elements as light sources have attracted attention in recent years. Among them, large μ-LED displays are manufactured by arranging and connecting (tiling) about 200 small LED panels of A5 size (148mm×210mm) without gaps.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-115105 Summary of the invention

[0008] As disclosed in Patent Document 1, the anti-reflection film utilizes optical interference, so sometimes the light path length changes according to the incident angle and the emission angle of the light, and the reflected color (hue) changes in various ways. In particular, in the case of a structure with an anti-reflection film on the diffusion layer, light is easily diffusely reflected by the diffusion layer, so the change in hue caused by the angle tends to become more significant. Moreover, in the case of manufacturing large μ-LED displays, when tiling multiple LED panels, if the diffuse reflection color (hue of diffusely reflected light) of each panel is different, there is a risk that the appearance will become various colors when it is turned off, and the quality will be greatly reduced.

[0009] Therefore, an object of the present invention is to provide a transparent substrate with an antireflection film in which color deviation is not easily noticed even when tiling is performed, and an image display device including the same.

[0010] The inventors of the present invention have found through experiments that the diffuse reflection light at various angles when light is incident on a transparent substrate with an anti-reflection film at a predetermined angle is * and b * The present invention has been completed by satisfying the prescribed requirements and by being able to obtain a transparent substrate with an antireflection film in which color deviation is not easily noticeable when tiling.

[0011] That is, the present invention relates to the following 1 to 13.

[0012] 1. A transparent substrate with an anti-reflection film, comprising: a transparent substrate having two main surfaces, and a diffusion layer and an anti-reflection film provided on one main surface of the transparent substrate in order from the transparent substrate side,

[0013] When the reflection from the other main surface of the transparent substrate is removed and the light source is incident on the one main surface at an incident angle of 45°, the a value of the diffuse reflected light at angles of -15°, 15°, 25°, 45°, 75° and 110° relative to the specular reflected light under the D65 light source is * and b * The following formulas (1) to (4) are satisfied.

[0014] (1)-6≤a * ≤2

[0015] (2)-1≤b * ≤12

[0016] (3)b * ≤-2a * +4

[0017] (4)b * ≥-2a * -5

[0018] 2. The transparent substrate with an antireflection film according to item 1 above, wherein the haze value is 30% or more.

[0019] 3. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the L value of the diffuse reflected light at -15° under a D65 light source is * The L of the diffuse reflected light at 15° is 30 to 60. * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20.

[0020] 4. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the light transmittance (Y) is 20 to 90%.

[0021] 5. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the sheet resistance of the anti-reflection film is 10 4 Ω / □ or more.

[0022] 6. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the transmission color b under D65 light source is * Is 5 or less.

[0023] 7. A transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the anti-reflection film is a stacked structure formed by stacking at least two dielectric layers with different refractive indices, at least one of the dielectric layers is mainly composed of Si oxide, and at least one other layer of the layers of the stacked structure is mainly composed of a mixed oxide, which is a mixed oxide of at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of Group B contained in the mixed oxide is 65% by mass or less relative to the total of the elements of Group A contained in the mixed oxide and the elements of Group B contained in the mixed oxide.

[0024] 8. The transparent substrate with an antireflection film according to 1 or 2 above, further comprising an antifouling film on the antireflection film.

[0025] 9. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the transparent substrate comprises glass.

[0026] 10. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the transparent substrate comprises at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone and triacetyl cellulose.

[0027] 11. The transparent substrate with an antireflection film according to 1 or 2 above, wherein the transparent substrate is a laminate of glass and at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone and triacetyl cellulose.

[0028] 12. The transparent substrate with an antireflection film according to 11 above, wherein the glass is chemically strengthened.

[0029] 13. An image display device comprising the transparent substrate with an antireflection film according to 1 or 2 above.

[0030] According to one embodiment of the present invention, a transparent substrate with an anti-reflection film and an image display device having the same can be provided, in which color deviation is not easily noticeable when the substrate is laid flat. By making color deviation not easily noticeable when the substrate is laid flat, the quality and appearance of the transparent substrate with an anti-reflection film and the image display device having the same can be improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a cross-sectional view schematically showing a configuration example of a transparent substrate with an antireflection film according to one embodiment of the present invention.

[0032] Figure 2 is an example of diffuse reflection light at each angle. * and b * Schematic diagram of the assay method.

[0033] Figure 3 is a representing the diffuse reflection light at each angle in each example * and b * A graph of the measurement results. DETAILED DESCRIPTION

[0034] The present invention is described in detail below, but the present invention is not limited to the following embodiments and can be arbitrarily deformed and implemented within the scope of the gist of the present invention. In addition, the "to" indicating a numerical range is used to include the numerical values ​​recorded before and after it as the lower limit and upper limit.

[0035] It should be noted that in this specification, the presence of another layer, film, etc. on the main surface of a substrate such as a transparent substrate, on a layer such as a diffusion layer, on a film such as an anti-reflection film is not limited to the form in which the other layer, film, etc. is provided in contact with the above-mentioned main surface, layer or film, as long as the layer, film, etc. is provided in the upper direction thereof. For example, the presence of a diffusion layer on the main surface of a transparent substrate may be provided in a manner that the diffusion layer is provided in contact with the main surface of the transparent substrate, or other arbitrary layers, films, etc. may be provided between the transparent substrate and the diffusion layer.

[0036] A transparent substrate with an antireflection film according to one embodiment of the present invention comprises: a transparent substrate having two main surfaces, and a diffusion layer and an antireflection film provided on one main surface of the transparent substrate in order from the transparent substrate side, wherein when the reflection of the other main surface of the transparent substrate is removed and a light source is incident on the one main surface side at an incident angle of 45°, a diffuse reflection light under a D65 light source at angles of -15°, 15°, 25°, 45°, 75° and 110° relative to the specular reflection light * and b * The following formulas (1) to (4) are satisfied.

[0037] (1)-6≤a * ≤2

[0038] (2)-1≤b * ≤12

[0039] (3)b * ≤-2a * +4

[0040] (4)b * ≥-2a * -5

[0041] (Transparent substrate with anti-reflection film)

[0042] Figure 1 This is a cross-sectional view schematically showing a configuration example of a transparent substrate with an antireflection film according to one embodiment of the present invention. Figure 1 The illustrated transparent substrate 1 with an antireflection film includes a transparent substrate 10 , a diffusion layer 31 , and an antireflection film 30 . Figure 1 In the embodiment, a diffusion layer 31 is formed on one main surface of a transparent substrate 10, and an antireflection film 30 is formed on the diffusion layer 31. The antireflection film is, for example, a multilayer film having a laminated structure in which at least two dielectric layers having different refractive indices are laminated. Figure 1 In the embodiment, the antireflection film 30 is a multilayer film formed by stacking a first dielectric layer 32 and a second dielectric layer 34. Figure 1 In the example, a diffusion layer 31 is further formed on the transparent substrate 10 , but as described later, a diffusion layer may be formed on the surface layer of the transparent substrate itself by a method of surface treating the transparent substrate.

[0043] A transparent substrate with an anti-reflection film according to one embodiment of the present invention has a diffusion layer and an anti-reflection film on one main surface of the transparent substrate in order from the transparent substrate side. Thus, a transparent substrate with an anti-reflection film having an excellent black texture and capable of suppressing reflection of external light and suppressing whitening caused by diffusely reflected light can be obtained.

[0044] In a transparent substrate with an antireflection film according to one embodiment of the present invention, when a light source is incident on one main surface at an incident angle of 45°, excluding reflection from the other main surface of the transparent substrate, the a of diffuse reflected light at angles of -15°, 15°, 25°, 45°, 75° and 110° relative to the specular reflected light under a D65 light source is * and b * The following formulas (1) to (4) are satisfied.

[0045] (1)-6≤a * ≤2

[0046] (2)-1≤b * ≤12

[0047] (3)b * ≤-2a * +4

[0048] (4)b * ≥-2a * -5

[0049] In this specification, the "diffuse reflected light at each angle of -15°, 15°, 25°, 45°, 75° and 110°" obtained by the above method is sometimes referred to as "diffuse reflected light at each angle". In addition, when "diffuse reflected light at -15°" is referred to, the diffuse reflected light at -15° in "diffuse reflected light at each angle" is the same even when the angle is different. In addition, unless otherwise specified, a * 、b * and L * Refers to a under D65 light source * 、b * and L * .

[0050] Figure 2 is an example of diffuse reflection light at each angle. * and b * Schematic diagram of the determination method. Figure 2 In the transparent substrate 1 with an anti-reflection film shown in FIG. 1 , the transparent substrate 10 includes one main surface 11 and another main surface 12. A diffusion layer 31 and an anti-reflection film 30 are formed on the one main surface 11. Figure 2 In the illustrated measurement method, the transparent substrate 1 with an anti-reflection film is provided with a black tape 20 on the other main surface 12 to remove the reflection of the other main surface. Light is incident from a light source 50 at an incident angle of 45° to one main surface 11 side of the transparent substrate 1 with an anti-reflection film. As the incident light source, a light source that emits light in the entire visible light region is used. As the light source, for example, a white light source such as a high color rendering index white LED is appropriately used. With the specular reflection light 61 of the incident light 60 as a reference (0°), the diffuse reflection lights 71, 72, 73, 74, 75 and 76 are diffuse reflection lights of -15°, 15°, 25°, 45°, 75° and 110°, respectively. It should be noted that here, the specular reflection light 61 is set to 0°, the direction in which the angle increases on the side where the incident light 60 is located is set to the + direction, and the direction in which the angle increases on the side opposite to the incident light 60 is set to the - direction. For the diffuse reflected light at each angle, the reflectance of the visible light wavelength is measured and the L under the D65 light source is calculated. * 、a * and b * This measurement can be performed using, for example, CM-M6 manufactured by Konica Minolta. As a method for removing the reflection of the other main surface, Figure 2As exemplified, for example, a method of laminating a black tape on the other main surface can be cited. As a black tape for removing reflection on the other main surface, for example, "Kukiri Miel" manufactured by Tomogawa Paper Co., Ltd. can be cited, and the diffuse reflectivity of the black tape itself is low and the surface of the anti-reflection film with a transparent substrate has little influence on the diffuse reflectivity measurement.

[0051] The inventors conducted in-depth research and found through experiments that the diffuse reflection of light at various angles is * and b * By satisfying the above formulas (1) to (4), a transparent substrate with an antireflection film can be obtained in which color deviation is not easily noticed when tiling, thereby completing the present invention. * and b * Different from each other means that the color tone changes depending on the angle at which the transparent substrate with the anti-reflection film is observed. In this way, the color tone changes depending on the observation angle, which usually becomes a cause of obvious color deviation when tiling. However, the present invention has found that when the a of the diffusely reflected light at each angle * and b * When the above equations (1) to (4) are satisfied, the change in color tone when the angle is changed is not easily noticeable. The reason is presumably as follows. That is, when the a of the diffusely reflected light at each angle is * and b * When the above formulas (1) to (4) are satisfied, the hue changes from colorless to yellowish green depending on the viewing angle. * and b * The difference is not easy to feel due to the angle, so it is estimated that the color deviation is not easy to detect. * and b * The variable region is limited to a limited range, and the magnitude of the change in color tone caused by the angle becomes smaller, so it is believed that the color deviation becomes less noticeable. Furthermore, by satisfying the above formulas (1) to (4), the color difference of transparent substrates with anti-reflection films on both sides adjacent to each other when tiling is limited, and it is also expected that the joints of multiple substrates will be less noticeable.

[0052] a of diffuse reflected light at each angle * is -6≤a * ≤2. From the perspective of improving the black feeling when the display is turned off, a * On the other hand, from the viewpoint of maintaining the reflected color in colorless to yellowish green, a * It is 2 or less, preferably 1.5 or less, and more preferably 1.0 or less.

[0053] b of diffuse reflected light at various angles * For -1≤b *≤12. From the perspective of maintaining the reflected color in the range of colorless to yellowish green, b * On the other hand, from the viewpoint of preventing the yellow-green color of the reflected color from becoming more conspicuous, b * It is 12 or less, preferably 11 or less, and more preferably 10 or less.

[0054] a of diffuse reflected light at each angle * and b * Satisfy b * ≤-2a * +4. This can reduce the red component from the reflected color, so it is preferred. * and b * Preferably satisfy b * ≤-2a * +3.5, preferably satisfying b * ≤-2a * +3.

[0055] a of diffuse reflected light at each angle * and b * Satisfy b * ≥-2a * -5. This is preferred because it can reduce the blue component in the reflected color. * and b * Preferably satisfy b * ≥-2a * -4.5, preferably satisfying b * ≥-2a * -4.

[0056] Among the diffuse reflection lights at various angles, the diffuse reflection lights at angles close to the specular reflection lights of the incident light, for example, the diffuse reflection lights at -15°, 15°, and 25°, have a higher brightness (L) than the diffuse reflection lights at 45°, 75°, and 110°. * ) tends to be large. Moreover, the color of diffuse reflection light with high brightness is more likely to be felt more strongly than the color of diffuse reflection light without such brightness. From this point of view, the a of diffuse reflection light at -15°, 15° and 25° is preferably * and b * is close to zero, or L * This appropriately controls the color tone of light at an angle that is more likely to be felt in the diffusely reflected light, thereby making the color deviation less noticeable.

[0057] -15° diffuse light under D65 light source L * It is preferably 30 to 60, and more preferably 40 to 55. L under D65 light source of diffuse reflected light at -15° *It is preferably 30 or more, and more preferably 70 or more. L under D65 light source of diffuse reflected light at -15° * It is preferably 60 or less, and more preferably 55 or less. L of diffusely reflected light at -15° * In this range, the transparent substrate with an antireflection film has appropriate light diffusivity (antiglare property) or low reflectivity, and can appropriately suppress reflection of external light.

[0058] L under D65 light source with 15° diffuse reflection * The L value under the D65 light source of the diffuse reflected light of 15° is preferably 15 to 35, and more preferably 20 to 30. * It is preferably 15 or more, and more preferably 20 or more. In addition, the L value of the diffuse reflected light at 15° under the D65 light source is * It is preferably 35 or less, and more preferably 30 or less. The L of diffusely reflected light at 15° * In this range, the transparent substrate with an antireflection film has appropriate light diffusivity (antiglare property) or low reflectivity, and can appropriately suppress reflection of external light.

[0059] L under D65 light source with diffuse reflection at 25° * It is preferably 5 to 20, more preferably 7 to 15. The L value of diffuse reflected light at 25° under D65 light source is * It is preferably 5 or more, and more preferably 7 or more. L under D65 light source of diffuse reflected light at 25° * It is preferably 20 or less, and more preferably 15 or less. The L of the diffusely reflected light at 25° * In this range, the transparent substrate with an antireflection film has appropriate light diffusivity (antiglare property) or low reflectivity, and can appropriately suppress reflection of external light.

[0060] In addition, the L under the D65 light source with diffuse reflected light at -15° is preferred. * 30 to 60, the L of the diffuse reflected light at 15° * is 15 to 35, and the L of the diffuse reflected light at 25° * is 5 to 20. As a result, the transparent substrate with an anti-reflection film has more appropriate light diffusion (anti-glare) or low reflectivity, and can suppress the reflection of external light. * By with a * and b * The same method can be used to measure and calculate using, for example, CM-M6 manufactured by Konica Minolta Inc.

[0061] In the transparent substrate with an antireflection film of one embodiment of the present invention, from the viewpoint of appropriately preventing reflection, the haze value is preferably 30% or more, more preferably 40% or more, and further preferably 50% or more. From the viewpoint of improving the clarity of an image when used in an image display device, the haze value is preferably, for example, 90% or less. The haze value may be 30% to 90%.

[0062] A transparent substrate with an anti-reflection film having a high haze value as described above is suitable for use in large μ-LED displays. The reason is that, first, when the display is large, it is easier for lighting and external light to be reflected, so it is required to prevent reflection more appropriately. And, secondly, in a large μ-LED display, the pixel pitch is large, so even if the haze value is high, it is easy to become a high-definition display. However, in such a transparent substrate with an anti-reflection film having a high haze value, the diffuse reflection component becomes more, so the change in color tone caused by the angle of the diffusely reflected light is likely to become particularly significant. In contrast, according to the present invention, even in the case of a high haze value, the color deviation during tiling can be appropriately suppressed.

[0063] It should be noted that in applications such as LCD displays, for example, a transparent substrate with an antireflection film having a haze value of about 0 to 30% is appropriately used. Depending on the application, the haze value may be, for example, 30% or less or less than 30% as long as it is within the range that can achieve the effects of the present invention.

[0064] The haze value can be adjusted by, for example, the surface shape of the diffusion layer. The haze value is measured in accordance with JIS K7136:2000 using a haze meter (HZ-V3 manufactured by Suga Test Instruments Co., Ltd.) or the like.

[0065] (Light transmittance: Y)

[0066] The light transmittance (Y) of the transparent substrate with an anti-reflection film of this embodiment is preferably 20 to 90%. If the light transmittance (Y) is within the above range, it has an appropriate light absorption capacity, so when used as a cover glass of an image display device, it is possible to suppress the reflection of light. As a result, the contrast of the bright area of ​​the image display device is improved. The above light transmittance (Y) is more preferably 50 to 90%, and further preferably 60 to 90%. That is, the light transmittance (Y) is preferably 20% or more, more preferably 50% or more, and further preferably 60% or more. The light transmittance (Y) is preferably 90% or less.

[0067] In addition, the light transmittance (Y) can be measured by the method prescribed|regulated in JIS Z8701 (1999) as described in the Example mentioned later.

[0068] In the transparent substrate with an anti-reflection film of this embodiment, in order to make the light transmittance (Y) 20 to 90%, for example, it is preferred to mainly use a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In as the first dielectric layer of the anti-reflection film and adjust the oxidation amount of the film.

[0069] The light transmittance (Y) in the transparent substrate with an antireflection film of this embodiment can be adjusted by controlling the irradiation time, irradiation output, distance from the substrate, and amount of oxidizing gas of the oxidation source when forming the first dielectric layer as a high refractive index layer in the above-mentioned antireflection film.

[0070] (Sheet resistance)

[0071] In the transparent substrate with an antireflection film of this embodiment, the sheet resistance of the antireflection film is preferably 10 4 Ω / □ or more. Since the sheet resistance of the anti-reflection film is within the above range, the anti-reflection film is insulating, so when used as a cover glass of an image display device, even if a touch panel is provided, the change in electrostatic capacitance caused by finger contact required for an electrostatic capacitive touch sensor can be maintained, and the touch panel can function. The above sheet resistance is more preferably 10 6 Ω / □ or more, more preferably 10 8 Ω / □ or more.

[0072] In addition, the sheet resistance can be measured by the method specified in JIS K 6911 (2006) as described in Examples below.

[0073] In the transparent substrate with an anti-reflection film of this embodiment, in order to make the sheet resistance of the anti-reflection film 10 4 Ω / □ or more, for example, adjusting the metal content in the anti-reflection film.

[0074] (b in the transmitted color under D65 light source * value)

[0075] In the transparent substrate with an anti-reflection film of this embodiment, b in the transmission color under D65 light source is * The value is preferably less than 5. * When the value is within the above range, the transmitted light does not have a yellow tint, so it is suitable for use as a cover glass for image display devices. * The value is more preferably 3 or less, and further preferably 2 or less. * The lower limit of the value is preferably -6 or more, and more preferably -4 or more. * The value is within the above range, because the transmitted light becomes colorless and does not block the transmitted light, so it is preferred.* The value can be from -6 to 5.

[0076] It should be noted that the b in the transmission color under D65 light source * The value can be measured by the method specified in JIS Z 8729 (2004).

[0077] (Transparent substrate)

[0078] The refractive index of the transparent substrate with two main surfaces in this embodiment (hereinafter also referred to as the transparent substrate) is preferably 1.4 to 1.7. If the refractive index of the transparent substrate is in the above range, the reflection of the bonding surface can be fully suppressed when the display, touch panel, etc. are optically bonded. The refractive index is more preferably 1.45 or more, more preferably 1.47 or more, and more preferably 1.65 or less, and more preferably 1.6 or less.

[0079] The transparent substrate preferably includes at least one of glass and resin. More preferably, the transparent substrate includes both glass and resin. By including glass in the transparent substrate, the strength, flatness and durability of the transparent substrate with anti-reflection film can be excellent. In addition, by laminating the laminate formed by the resin substrate-anti-glare layer described later on the glass substrate, it is easy to form a diffusion layer. In the transparent substrate with anti-reflection film formed with a diffusion layer by this method, the transparent substrate includes both glass and resin.

[0080] When the transparent substrate includes glass, the type of glass is not particularly limited, and glasses having various compositions can be used. Among them, the glass preferably contains sodium, and preferably has a composition that can be molded and strengthened by chemical strengthening treatment. As the glass, specifically, for example, aluminosilicate glass, soda-lime glass, borosilicate glass, lead glass, alkali-barium glass, aluminoborosilicate glass, etc. can be cited.

[0081] In addition, in this specification, when a transparent substrate is made of glass, the transparent substrate is also referred to as a glass substrate.

[0082] The thickness of the glass substrate is not particularly limited. When the glass is subjected to chemical strengthening treatment, in order to effectively perform chemical strengthening, it is preferably 5 mm or less, more preferably 3 mm or less, and further preferably 1.5 mm or less. In addition, the thickness is, for example, 0.2 mm or more. The thickness of the glass substrate can be 0.2 mm to 5 mm.

[0083] The glass substrate is preferably a chemically strengthened glass that has been chemically strengthened. Thus, the strength of the transparent substrate with an anti-reflection film is improved. It should be noted that when the glass substrate is subjected to the anti-glare treatment described later, the chemical strengthening is preferably performed after the anti-glare treatment and before the anti-reflection film (multilayer film) is formed.

[0084] When the transparent substrate includes a resin, the type of the resin is not particularly limited, and resins with various compositions can be used. Among them, the above-mentioned resin is preferably a thermoplastic resin or a thermosetting resin, for example, polyvinyl chloride resin, polyethylene resin, polypropylene resin, polystyrene resin, polyvinyl acetate resin, polyester resin, polyurethane resin, cellulose resin, acrylic resin, AS (acrylonitrile-styrene) resin, ABS (acrylonitrile-butadiene-styrene) resin, fluorine resin, thermoplastic elastomer, polyamide resin, polyimide resin, polyacetal resin, polycarbonate resin, modified polyphenylene ether resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polylactic acid resin, cyclic polyolefin resin, polyphenylene sulfide resin, etc. Among these, cellulose resin is preferred, and triacetyl cellulose resin, polycarbonate resin, polyethylene terephthalate resin, etc. can be mentioned. These resins can be used alone or in combination of two or more.

[0085] The resin particularly preferably includes at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic acid, silicone, and triacetyl cellulose, from the viewpoint of excellent visible light transparency and easy availability.

[0086] In addition, in this specification, when a transparent substrate contains a resin, the transparent substrate is also referred to as a resin substrate.

[0087] The shape of the resin substrate is preferably a film. When the resin substrate is in a film shape, that is, a resin film, its thickness is not particularly limited, but is preferably 20 to 300 μm, and more preferably 30 to 130 μm.

[0088] When the transparent substrate includes both glass and resin, for example, a composite substrate is formed by laminating a glass substrate and a resin substrate. More specifically, the transparent substrate may be, for example, a glass substrate having the resin substrate on the glass substrate.

[0089] (Diffusion layer)

[0090] The diffusion layer in this embodiment is provided on one main surface of the transparent substrate. The diffusion layer is a layer having the function of diffusing specularly reflected light to reduce glare and reflection, and an anti-glare layer is provided in which the function of diffusing specularly reflected light (anti-glare property) is imparted to the hard coat layer.

[0091] The anti-glare layer has a concavo-convex shape on one side, and utilizes external scattering or internal scattering to increase the haze value and impart anti-glare properties. The anti-glare layer is formed by an anti-glare layer composition, which is formed by dispersing a particulate substance having at least anti-glare properties in a solution in which a polymer resin serving as a binder is dissolved. The anti-glare layer can be formed by coating the anti-glare layer composition on one main surface of a transparent substrate, for example.

[0092] Examples of the above-mentioned particulate substances having anti-glare properties include inorganic particles such as silica, clay, talc, calcium carbonate, calcium sulfate, barium sulfate, aluminum silicate, titanium oxide, synthetic zeolite, alumina, and montmorillonite, and organic particles containing styrene resins, polyurethane resins, benzoguanamine resins, silicone resins, acrylic resins, and melamine resins.

[0093] In addition, as the polymer resin used as the adhesive for the above-mentioned hard coat layer or the above-mentioned anti-glare layer, for example, a polymer resin containing polyester resin, acrylic resin, acrylic urethane resin, polyester acrylate resin, polyurethane acrylate resin, epoxy acrylate resin, urethane resin, etc. can be used.

[0094] In this method, the diffusion layer can be directly formed on the transparent substrate, or a laminate composed of a resin substrate-anti-glare layer can be prepared in advance and attached to a glass substrate, etc., thereby obtaining a structure with a diffusion layer on a composite substrate of a glass substrate and a resin substrate. The laminate is preferably formed with a diffusion layer on a film-like resin substrate. According to this method, it is easy to form a diffusion layer more simply.

[0095] As a laminate composed of a resin matrix-antiglare layer, specifically, for example, an antiglare PET film and an antiglare TAC film can be cited. As the antiglare PET film, the products manufactured by HIGASHIYAMA FILM Co., Ltd., the product name: BHC-III, EHC-30a, and the products manufactured by Reiko Co., Ltd. can be cited. In addition, as the antiglare TAC film, an antiglare TAC film (manufactured by TOPPAN TOMOEGAWAOPTICALFILM, the product name VZ50), an antiglare TAC film (manufactured by TOPPAN TOMOEGAWAOPTICALFILM, the product name VH66H) and the like can be used.

[0096] Alternatively, the diffusion layer may be formed on the surface of the transparent substrate itself by subjecting the transparent substrate to a surface treatment.

[0097] For example, when a glass substrate is used, a method of performing surface treatment on the main surface of the glass to form desired projections and depressions can be used.

[0098] Specifically, the method of chemically treating the main surface of the glass substrate includes, for example, a method of performing a frosting treatment. The frosting treatment may be performed by immersing the glass substrate as a treatment object in a mixed solution of hydrogen fluoride and ammonium fluoride to perform a chemical surface treatment on the immersed surface.

[0099] In addition, in addition to chemical treatment methods such as frosting, physical treatment methods such as so-called sandblasting, in which crystalline silica powder, silicon carbide powder, etc. are blown onto the surface of the glass substrate with pressurized air, or a brush to which crystalline silica powder, silicon carbide powder, etc. is attached is moistened with water and rubbed.

[0100] The transparent substrate with anti-reflection film having such a diffusion layer has a concavo-convex shape on the surface due to the concavo-convex shape of the diffusion layer. The Sa (arithmetic mean surface roughness) of the transparent substrate with anti-reflection film is preferably 0.05 to 0.6 μm, more preferably 0.05 to 0.55 μm. By Sa being in this range, it is easy to suppress the reflection of the reflected image, so it is preferred. Sa is specified in ISO25178, and can be measured using a laser microscope VK-X3000 manufactured by KEYENCE, for example.

[0101] For the transparent substrate with an antireflection film, the developed area ratio Sdr (hereinafter also referred to as "Sdr") calculated from the surface area obtained by measurement using a laser microscope VK-X3000 manufactured by KEYENCE is preferably 0.001 to 0.4, and more preferably 0.0025 to 0.2. When Sdr is within this range, it is easy to suppress the reflection of the reflected image, so it is preferred.

[0102] Sdr is defined in ISO 25178 and is expressed by the following formula.

[0103] Development area ratio Sdr = {(A-B) / B}

[0104] A: Surface area (developed area) reflecting actual concavity and convexity in the measurement area

[0105] B: The area of ​​the flat surface without unevenness in the measurement area

[0106] The Sdq (root mean square slope) of the transparent substrate with an antireflection film is preferably 0.03 to 0.50, and more preferably 0.07 to 0.49. When Sdq is within this range, it is easy to suppress the reflection of the reflected image, so it is preferred. Sdq is specified in ISO25178 and can be measured, for example, using a laser microscope VK-X3000 manufactured by KEYENCE.

[0107] The Spc (average of the principal curvatures of the surface peaks) of the transparent substrate with an antireflection film is preferably 150 to 6000 (1 / mm). When Spc is within this range, it is easy to suppress the reflection of the reflected image, so it is preferred. Spc is specified in ISO25178 and can be measured using a laser microscope VK-X3000 manufactured by KEYENCE, for example.

[0108] In addition, the above-mentioned Sa, Sdr, Sdq and Spc are values ​​measured on the main surface of the transparent substrate with an antireflection film on the side provided with the diffusion layer and the antireflection film.

[0109] (Barrier layer)

[0110] In the case where the diffusion layer is formed by laminating a laminate composed of a resin substrate and an anti-glare layer to a glass substrate, or in the case where the transparent substrate includes a resin substrate, it is preferred to have a barrier layer between the diffusion layer and the anti-reflection film. By providing the barrier layer between the resin transparent substrate and the anti-reflection film, it is preferred because it has the advantages of being able to suppress the influence of moisture and oxygen that want to penetrate from the resin substrate into the anti-reflection film, and the optical properties become less likely to change. Examples of the barrier layer include metal nitride films, metal oxide films, and more specifically SiN x Film, SiO x However, from the viewpoint of more effectively suppressing the change of optical characteristics, SiN x From the viewpoint of inhibiting the intrusion of water etc. into the anti-reflection film, the thickness of the barrier layer is preferably 2 nm or more, more preferably 4 nm or more, and particularly preferably 8 nm or more. On the other hand, from the viewpoint of inhibiting the increase in the reflectivity of the transparent substrate with the anti-reflection film, the thickness is preferably 50 nm or less. The barrier layer can be formed by a known film-forming method such as sputtering, vacuum evaporation, coating, etc.

[0111] (Anti-reflective film)

[0112] The antireflection film in this embodiment has a function of suppressing reflection of light, and has, for example, a laminated structure in which at least two dielectric layers having mutually different refractive indices are laminated.

[0113] Figure 1 The anti-reflection film (multilayer film) 30 shown is a laminated structure formed by laminating two layers of a first dielectric layer 32 and a second dielectric layer 34 having different refractive indices. By laminating the first dielectric layer 32 and the second dielectric layer 34 having different refractive indices, reflection of light is suppressed. For example, Figure 1 The first dielectric layer 32 is a high refractive index layer, and the second dielectric layer 34 is a low refractive index layer.

[0114] The anti-reflection film has a laminated structure formed by laminating at least two dielectric layers having different refractive indices, at least one of the dielectric layers is mainly composed of Si oxide, and at least one other layer of the layers of the laminated structure is mainly composed of a mixed oxide, the mixed oxide is a mixed oxide of at least one oxide selected from the group A composed of Mo and W and at least one oxide selected from the group B composed of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of the group B contained in the mixed oxide is preferably 65% ​​by mass or less relative to the total of the elements of the group A contained in the mixed oxide and the elements of the group B contained in the mixed oxide. In addition, the layer mainly composed of Si oxide may contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In within a range that does not affect the reflectivity. By having the above-mentioned structure of the anti-reflection film, an anti-reflection film having uniform light absorption ability under visible light and insulating properties can be obtained. The anti-reflection film has light absorption capability. For example, in a structure in which an anti-reflection film is formed on a diffusion layer, light reflected by the surface of the diffusion layer (i.e., closer to the transparent substrate than the anti-reflection film) can be absorbed to a certain extent. As a result, the whitening caused by diffuse reflection in the diffusion layer can be more effectively suppressed, so the black texture when the screen is turned off when used in an image display device can be further improved. In addition, since the anti-reflection film is insulating, the transparent substrate with the anti-reflection film can also be preferably used for touch panels and other purposes. In addition, by setting the content of the dielectric layer to an appropriate range, even in harsh environments such as high temperature environments such as 80°C and 95°C, high temperature and high humidity environments such as 65°C 95%, 85°C 85%, environments irradiated with strong UV light, and environments exposed to rain, an anti-reflection film with little change in optical properties and appearance can be obtained.

[0115] Figure 1 In the anti-reflection film (multilayer film) 30 shown, the first dielectric layer 32 (high refractive index layer) is preferably mainly composed of a mixed oxide, which is a mixed oxide of at least one oxide selected from the A group consisting of Mo and W and at least one oxide selected from the B group consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In. In the mixed oxide, the content of the elements of the B group contained in the mixed oxide (hereinafter referred to as the B group content) is preferably 65% ​​by mass relative to the total of the elements of the A group contained in the mixed oxide and the elements of the B group contained in the mixed oxide. Here, "mainly" means that the first dielectric layer 32 contains the largest component (based on mass), for example, it contains 70% by mass or more of the component.

[0116] If the content of group B in the first dielectric layer (A-B-O) 32 composed of a mixed oxide of at least one oxide selected from group A consisting of Mo and W and at least one oxide selected from group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In is less than 65 mass %, the yellowing of the transmitted light can be suppressed.

[0117] As at least one oxide selected from Group A, Mo or Mo and W are preferred, and as at least one oxide selected from Group B, Nb is preferred. That is, the first dielectric layer is preferably a mixed oxide of Mo and Nb or a mixed oxide of Mo, W and Nb, and more preferably a mixed oxide of Mo, W and Nb.

[0118] As described later, the second dielectric layer can be, for example, an oxygen-deficient silicon oxide layer. Here, in the past, the oxygen-deficient silicon oxide layer was yellowish in visible light, but if the first dielectric layer is a mixed oxide of Mo and Nb or a mixed oxide of Mo, W and Nb, the yellowing of the silicon oxide layer can be suppressed, so it is preferred. In addition, in order to improve reliability, the silicon oxide layer can contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In, and each oxide can also produce oxygen deficiency. In addition, when the second dielectric layer is formed on a diffusion layer having a higher haze, i.e., a larger surface unevenness as described above, high oxidation stability is required during film formation. If the first dielectric layer is a mixed oxide of Mo, W and Nb, the oxidation stability during film formation is easy to be excellent, which is more preferred.

[0119] From the viewpoint of transmittance with the transparent substrate, the refractive index of the first dielectric layer 32 at a wavelength of 550 nm is preferably 1.8 to 2.3.

[0120] The extinction coefficient of the first dielectric layer 32 is preferably 0.005 to 3, and more preferably 0.04 to 0.38. If the extinction coefficient is 0.005 or more, the desired absorptivity can be achieved with an appropriate number of layers. In addition, if the extinction coefficient is 3 or less, it is easier to achieve a balance between reflective tone and transmittance.

[0121] The second dielectric layer 34 (low refractive index layer) is preferably mainly composed of Si oxide (SiO x Here, "mainly" refers to the component with the largest content (based on mass) in the second dielectric layer 34, for example, it contains 70% by mass or more of this component. The second dielectric layer 34 (low refractive index layer) is mainly composed of Si oxide (SiO x ) structure, the refractive index becomes low, and the reflectivity reduction effect becomes high, so it is preferred. It should be noted that SiO xIt can also be fully oxidized silicon oxide (SiO2), but from the viewpoint of improving optical reliability and scratch resistance, oxygen-deficient silicon oxide is preferred. In addition, in order to improve reliability, the silicon oxide layer can also contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In, and each oxide can also produce oxygen deficiency.

[0122] Figure 1 The anti-reflection film (multilayer film) 30 shown is a stacked structure of two layers in total formed by stacking the first dielectric layer 32 and the second dielectric layer 34, but the anti-reflection film (multilayer film) in this mode is not limited to this, and can also be a stacked structure formed by stacking more than three layers of dielectric layers with different refractive indices. In this case, it is not necessary for all dielectric layers to have different refractive indices. That is, the stacked structure can be a stacked structure formed by stacking more than two layers of dielectric layers in a manner where the refractive indices of adjacent layers are different, and the number of stacks can also be more than three layers. For example, in the case of a three-layer stacked structure, it can be a three-layer stacked structure of a low refractive index layer, a high refractive index layer, and a low refractive index layer, and a three-layer stacked structure of a high refractive index layer, a low refractive index layer, and a high refractive index layer. In the former case, there are two layers of low refractive index layers that can have the same refractive index as each other, and in the latter case, there are two layers of high refractive index layers that can have the same refractive index as each other. In the case of a four-layer stacked structure, it can be a four-layer stacked structure of a low refractive index layer, a high refractive index layer, a low refractive index layer, and a high refractive index layer, a four-layer stacked structure of a high refractive index layer, a low refractive index layer, a high refractive index layer, and a low refractive index layer. In this case, at least one of the low refractive index layers and the high refractive index layers that are respectively present in two layers can be the same refractive index.

[0123] In the case of a stacked structure in which three or more layers having different refractive indices are stacked, the first dielectric layer (A—B—O) 32 and the second dielectric layer (SiO x ) 34. In this case, the first dielectric layer (A—B—O) 32 and the second dielectric layer (SiO x )34, a three-layer stacked structure of a low refractive index layer, a high refractive index layer, and a low refractive index layer, or a three-layer stacked structure of a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a four-layer stacked structure of a low refractive index layer, a high refractive index layer, a low refractive index layer, and a high refractive index layer, or a four-layer stacked structure of a high refractive index layer, a low refractive index layer, a high refractive index layer, and a low refractive index layer.

[0124] Among them, the outermost layer is preferably the second dielectric layer (SiO x )34. In order to obtain low reflectivity, if the outermost layer is the second dielectric layer (SiO x), it can be made relatively easily. In addition, the reflectivity may sometimes increase slightly, but in order to improve reliability, the second dielectric layer may also contain at least one oxide selected from Nb, Ti, Zr, Ta, Al, Sn, W, Mo and In. In order to suppress the increase in reflectivity, the content of metals other than Si, excluding oxygen, is preferably 30at% or less, more preferably 20at% or less, and further preferably 15at% or less. In addition, when the anti-reflection film 30 forms the anti-fouling film described later, from the viewpoint of bonding related to the durability of the anti-fouling film, the anti-fouling film is preferably formed on the second dielectric layer (SiO x )superior.

[0125] The first dielectric layer (A—B—O) 32 is preferably amorphous. If it is amorphous, it can be produced at a relatively low temperature, and when the transparent substrate is made of resin, the resin is not damaged by heat, and can be appropriately used.

[0126] It should be noted that as a light-transmitting film having light absorption capability and insulating properties, a half-tone mask used in the field of semiconductor manufacturing is known. As a half-tone mask, Mo—SiO containing a small amount of Mo can be used. x In addition, as a light-transmitting film having light absorption capability and insulating properties, a narrow bandgap film used in the field of semiconductor manufacturing is known.

[0127] However, these light-transmitting films have high absorption capability for short-wavelength light in visible light, so the transmitted light has a yellow tint, and therefore are not suitable for cover glasses of image display devices.

[0128] In a preferred embodiment of the present invention, the first dielectric layer 32 having increased Mo and W contents and the SiO x The second dielectric layer 34 having the structure of the above can obtain a transparent substrate with an antireflection film having light absorbing ability, insulating properties, and excellent adhesion and strength.

[0129] The anti-reflection film 30 in this embodiment can be formed on the main surface of the transparent substrate using a known film forming method such as sputtering, vacuum evaporation, coating, etc. That is, the dielectric layers constituting the anti-reflection film 30 are formed on the main surface of the diffusion layer 31 according to their stacking order using a known film forming method such as sputtering, vacuum evaporation, coating, etc.

[0130] Examples of the sputtering method include magnetron sputtering, pulse sputtering, AC sputtering, and digital sputtering.

[0131] For example, magnetron sputtering is a method in which a magnetic field is generated by setting a magnet on the back side of a dielectric material that serves as a matrix, and gas ion atoms collide with the surface of the dielectric material and escape to form a film by sputtering with a thickness of several nanometers. This method can form a continuous film of a dielectric oxide or nitride that is a dielectric material.

[0132] In addition, for example, the digital sputtering method is different from the usual magnetron sputtering method. It is a method of forming a thin film of metal oxide by first forming a very thin film of metal by sputtering, and then repeatedly performing such a process of oxidation by irradiating oxygen plasma, oxygen ions or oxygen free radicals in the same chamber. In this case, the film-forming molecules are metal when attached to the substrate, so it is presumed that they have ductility compared to the case of film-forming by attachment of metal oxides. Therefore, it is believed that the rearrangement of the film-forming molecules is easy to occur even with the same energy, and as a result, a dense and smooth film can be formed.

[0133] It should be noted that the above is an example of a preferred structure of the anti-reflection film, but the structure of the anti-reflection film is not limited to this. For example, when it is desired to maintain a high brightness of a display, it is sometimes appropriate to use an anti-reflection film that does not have light absorption ability or has a high transmittance and a light transmittance of 90% or more as a transparent substrate with an anti-reflection film. Even in such a transparent substrate with an anti-reflection film including a high transmittance anti-reflection film, if the a of the diffusely reflected light at each angle is * and b * Within the above range, the effect of suppressing color deviation during tiling can be obtained. As the composition of the high-transmittance anti-reflection film, for example, the low-refractive index layer is the same as the second dielectric layer 34, and the high-refractive index layer is a layer that does not have light absorption ability or high transmission. As the high-refractive index layer in this case, for example, a layer mainly composed of Ti oxide (TiO x ) layer, Nb oxide (NbO x ) layer, a layer composed of Ta oxide (TaO x ) is preferably mainly composed of Ti oxide (TiO x In this case, each layer forming the antireflection film can also be formed by a known film-forming method such as sputtering, vacuum evaporation, coating, etc.

[0134] When a highly transmissive antireflection film is provided, the light transmittance (Y) of the transparent substrate with an antireflection film may be, for example, 90 to 96%, and preferably 93 to 96%.

[0135] (Anti-fouling film)

[0136] From the viewpoint of protecting the outermost surface of the anti-reflection film, the transparent substrate with an anti-reflection film of the present embodiment may further have an antifouling film (also referred to as "Anti Finger Print (AFP) film") on the above-mentioned anti-reflection film. The antifouling film may be composed of, for example, a fluorinated organosilicon compound. As a fluorinated organosilicon compound, as long as it can impart antifouling properties, water repellency, and oil repellency, it can be used without particular limitation, for example, a fluorinated organosilicon compound having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group, and a polyfluoroalkylene group. It should be noted that a polyfluoropolyether group refers to a divalent group having a structure in which a polyfluoroalkylene group is alternately bonded to an etheric oxygen atom.

[0137] In addition, as commercially available fluorine-containing silicone compounds having one or more groups selected from a polyfluoropolyether group, a polyfluoroalkylene group and a polyfluoroalkyl group, KP-801 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY178 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-130 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), OPTOOL (registered trademark) DSX and OPTOOL AES (both trade names, manufactured by Daikin Industries, Ltd.) and the like can be preferably used.

[0138] When the transparent substrate with an anti-reflection film of this embodiment has an anti-fouling film, the anti-fouling film is provided on the anti-reflection film. When the anti-reflection films are provided on both sides of the two main surfaces of the transparent substrate, the anti-fouling film can be formed on the anti-reflection films on both sides, but it can also be a structure in which the anti-fouling film is laminated only on one main surface side. This is because the anti-fouling film can be provided at a position that may be touched by a hand or the like, and can be selected according to its use, etc.

[0139] (Method for producing a transparent substrate with an anti-reflection film)

[0140] The method for manufacturing the transparent substrate with an anti-reflection film of the present embodiment is not particularly limited, and can be manufactured by, for example, a method comprising sequentially forming a diffusion layer and an anti-reflection film on a transparent substrate, and further comprising forming a barrier layer, an anti-fouling film, etc. as required.

[0141] The method of forming each layer is as described above, but in order to make the diffuse reflection light at each angle a * and b *In order to satisfy the above formulas (1) to (4), it is preferred to appropriately adjust the film composition of the anti-reflection film, the light transmittance (Y) of the transparent substrate with the anti-reflection film, and other values. In addition, in the case of a transparent substrate with an anti-reflection film of high transmittance, it is difficult to optimize using the transmittance, so it is preferred to more strictly adjust the film thickness of each layer of the anti-reflection film. As a specific adjustment method, it is preferred to make the specular reflectivity of yellow-green light with a wavelength of about 500nm to 600nm higher than that of blue light with a wavelength of 450nm to 500nm and red light with a wavelength of 600nm to 650nm at multiple light incident angles. Thus, the specular reflection color can be maintained as black (colorless) to yellow-green at multiple light incident angles, and as a result, there is a tendency that the diffuse reflection color at multiple incident angles can also be maintained as black (colorless) to yellow-green. The angular dependence of the specular reflection color can be easily predicted by using thin film simulation software. Furthermore, by satisfying (1) to (4), the brightness gradually changes while the reflected color maintains yellow-green, especially in the range of -15° to 45° where the brightness is large, so that a configuration with little discomfort during visual confirmation can be achieved.

[0142] For example, in a case where the high refractive index layer is a mixed oxide layer of Mo, W and Nb and the low refractive index layer is SiO x In the case of the layer, by satisfying the following, it is easy to obtain diffuse reflection light at various angles. * and b * The tendency of the transparent substrate with an antireflection film to satisfy the above-mentioned formulas (1) to (4).

[0143] For example, the total thickness of the antireflection film is preferably 200 nm to 250 nm, more preferably 210 nm to 245 nm. This can suppress the angular dependence of diffuse reflection color, that is, the increase in the change in the color tone of diffuse reflection light caused by angle, and tends to easily satisfy equations (1) to (4).

[0144] The number of layers of the antireflection film is preferably 4 to 8, more preferably 4 to 6. This can ensure mass productivity while suppressing an increase in the angular dependence of diffuse reflection color, and tends to easily satisfy Formulas (1) to (4).

[0145] In addition, the thickness of the first high refractive index layer is the most important for the thickness of each layer, and is preferably 1 to 25 nm, and more preferably 2 to 15 nm. This can suppress the angular dependence of the diffuse reflection color, that is, the increase in the change in the color tone of the diffuse reflection light caused by the angle, and tends to easily satisfy equations (1) to (4).

[0146] (use)

[0147] The transparent substrate with an anti-reflection film of this method can be suitable for use in the cover glass of an image display device, especially the cover glass of a display obtained by tiling multiple displays (such as LED panels, etc.) such as a large μ-LED display. Alternatively, the transparent substrate with an anti-reflection film of this method can also be suitable for use in situations where the haze required for the transparent substrate with an anti-reflection film is high and the change in color tone caused by the angle tends to become more significant. In addition to this, the transparent substrate with an anti-reflection film of this method can also be suitable for use in the cover glass of various image display devices such as liquid crystal displays, organic EL displays, and electronic paper displays.

[0148] (Image display device)

[0149] An image display device in one embodiment of the present invention includes the transparent substrate with the anti-reflection film. As the image display device, there can be cited a form in which the transparent substrate with the anti-reflection film is provided on a small display (such as an LED panel, etc.) used in a flat manner, a large display obtained by flattening it, and preferably a large μ-LED display. In addition, there can be cited a form in which the transparent substrate with the anti-reflection film is provided on various displays such as a liquid crystal display, an organic EL display, and an electronic paper display.

[0150] Example

[0151] The present invention is specifically described below with reference to the following examples, but the present invention is not limited thereto. Examples 1 and 2 are comparative examples, and Examples 3 and 4 are examples.

[0152] (evaluate)

[0153] The following evaluations were performed on the transparent substrate with an antireflection film of each example.

[0154] (a of diffuse reflected light at each angle * b * L * )

[0155] A black tape (Kukiri Miel, manufactured by Tomogawa Paper Co., Ltd.) was attached to the main surface (the other main surface) of the transparent substrate with an anti-reflection film without a diffusion layer and an anti-reflection film. Thus, the reflection of the other main surface was eliminated, and the light source was incident on the main surface (one main surface) with a diffusion layer and an anti-reflection film at an incident angle of 45°. The reflectance of each diffuse reflection light at an angle of -15°, 15°, 25°, 45°, 75°, and 110° relative to the mirror reflection light was measured for the visible light wavelength, and a under the D65 light source was calculated. * 、b * and L * (Diffuse reflection color) The measurement was performed using CM-M6 manufactured by Konica Minolta Inc.

[0156] (Haze)

[0157] The haze value (transmission haze) of the produced transparent substrate with an antireflection film was measured in accordance with JIS K 7136:2000 using a haze meter (HZ-V3 manufactured by Suga Test Instruments Co., Ltd.).

[0158] (Light transmittance: Y)

[0159] In the produced transparent substrate with anti-reflection film, the light transmittance (Y) of the outermost surface of the anti-reflection film is measured by the method specified in JIS Z8701 (1999). It should be noted that in this specification, the light transmittance (Y) of the outermost surface of the anti-reflection film is taken as the light transmittance (Y) of the transparent substrate with anti-reflection film. Specifically, in a state where a black tape is attached to the other main surface of the main surface on the non-anti-reflection film side of the two main surfaces of the transparent substrate and the back reflection is removed, the spectral transmittance is measured using a spectrophotometer (manufactured by Shimadzu Corporation, trade name: SolidSpec-3700), and the light transmittance (stimulation value Y specified in JIS Z 8701 (1999)) is calculated.

[0160] (Transmittance color of transparent substrate with anti-reflection film under D65 light source (b * value))

[0161] The color index (b) specified in JIS Z 8729 (2004) is determined from the transmission spectrum obtained by measuring the above spectral transmittance. * The light source used is D65 light source.

[0162] (Color deviation evaluation)

[0163] For each example, 16 transparent substrates with anti-reflection films made under the same conditions were prepared for testing. For example, in the case of Example 1, 16 transparent substrates with anti-reflection films made under the conditions of Example 1 and slightly changing the film thickness of each layer under the conditions of Example 1 were prepared, and black tape (made by Tomogawa Paper Co., Ltd., Kukiri Miel) was attached to the main surface (the other main surface) without a diffusion layer and an anti-reflection film, and then arranged (tiled) in a vertical 4 × horizontal 4 without gaps. For the transparent substrate with anti-reflection film after tiling, the color deviation was visually evaluated according to the following benchmark. The same test was performed for other examples. The evaluation results are shown in Table 1.

[0164] Good: When white LED lighting is reflected on the main surface (one main surface) of the transparent substrate with an anti-reflection film on one side having a diffusion layer and an anti-reflection film and observed from various angles, only achromatic to yellow-green colors are seen for the white lighting reflected on the transparent substrate with an anti-reflection film, which is a result that the color difference of each substrate is not obvious. In addition, the black sense of the transparent substrate with an anti-reflection film is strong when observed from the front, and a very good quality is obtained as a surface material for a display.

[0165] No: When white LED lighting is reflected onto the main surface (one main surface) of a transparent substrate with an anti-reflection film on one side having a diffusion layer and an anti-reflection film and observed from various angles, the white lighting reflected onto the transparent substrate with the anti-reflection film can be seen in various colors such as achromatic, red, blue, green, etc., resulting in obvious color differences between the substrates.

[0166] (Example 1)

[0167] A transparent substrate with an antireflection film was prepared by sequentially forming a diffusion layer and an antireflection film on one main surface of a transparent substrate by the following method. It should be noted that the transparent substrate is a glass substrate with a resin substrate as described later.

[0168] (Formation of Diffusion Layer)

[0169] An anti-glare PET film (manufactured by Reiko Co., Ltd., Sa: 0.259 μm, Sdr: 0.0620, Sdq: 0.361, Spc: 1703 (1 / mm), haze value: 60%) was bonded to one main surface of a chemically strengthened glass substrate (Dragontrail: registered trademark, manufactured by AGC Co., Ltd.) with an acrylic adhesive (transparent adhesive) as a laminate (resin film + anti-glare layer), thereby providing a diffusion layer on the transparent substrate. It should be noted that Sa, Sdr, Sdq and Spc here are values ​​measured in a state where no anti-reflection film is formed on the diffusion layer, but Sa, Sdr, Sdq and Spc of the transparent substrate with an anti-reflection film after the anti-reflection film is formed are also less different from the above values ​​and are considered to be within the above preferred range.

[0170] (Film formation of barrier layer)

[0171] Next, a barrier layer was formed on the diffusion layer as a SiN layer having a film thickness shown in Table 1. For example, in Example 1, the film thickness of the barrier layer was 15 nm.

[0172] The barrier layer is formed by repeatedly performing the following operations at high speed to form a silicon nitride film, and a silicon nitride (SiN) film having a predetermined film thickness is formed. x ) layer: using a digital sputtering method and a silicon target, while maintaining the pressure at 0.2 Pa with argon gas, at a frequency of 100 kHz and a power density of 10.0 W / cm2 , pulse sputtering is performed under the condition of an inversion pulse width of 3μsec to form a silicon film with a small film thickness, and then nitriding is performed with nitrogen gas. Here, the nitrogen flow rate during nitriding with nitrogen gas is 800sccm, and the input power of the nitriding source is 600W.

[0173] (Formation of anti-reflection film)

[0174] Next, an anti-reflection film having the film composition shown in Table 1 is formed by alternately forming NMWO layers (high refractive index layers) and SiO layers (low refractive index layers) on the barrier layer. It should be noted that the NMWO layer refers to a mixed oxide layer of Nb, Mo and W. For example, the film composition of the anti-reflection film of Example 1 in Table 1 refers to forming a 4nm NMWO layer on the barrier layer, followed by forming a 33nm SiO layer, followed by forming a 110nm NMWO layer, and then forming an 81nm SiO layer, thereby forming an anti-reflection film consisting of a four-layer film. The film forming methods of the SiO layer and the NMWO layer are as follows.

[0175] (Film formation of NMWO layer)

[0176] The oxide film is formed by repeatedly performing the following operation at a high speed, thereby forming a NMWO layer of a predetermined film thickness: using a target obtained by mixing niobium, molybdenum and tungsten in a weight ratio of 45:30:25 and sintering, and maintaining the pressure at 0.2 Pa with argon gas at a frequency of 100 kHz and a power density of 10.0 W / cm 2 , pulse sputtering is performed under the conditions of an inversion pulse width of 3μsec to form a metal film with a small film thickness, and then it is oxidized with oxygen. It should be noted that the composition of the NMWO layer formed by this method was measured by depth composition analysis using X-ray photoelectron spectroscopy (XPS) using argon ion sputtering. The results showed that, except for oxygen, Nb was 51.9at%, Mo was 33.5at%, W was 14.6at%, and the content of group B elements was 45% by weight.

[0177] (SiO layer formation)

[0178] The silicon oxide film is formed by repeatedly performing the following operations at a high speed, and a silicon oxide [silicon dioxide (SiO x )] The layer was formed by digital sputtering using a silicon target, with the pressure of argon gas maintained at 0.2 Pa, at a frequency of 100 kHz and a power density of 10.0 W / cm 2 , pulse sputtering is performed under the condition of an inversion pulse width of 3 μsec to form a silicon film with a very small film thickness, and then it is oxidized with oxygen. Here, the oxygen flow rate during oxidation with oxygen is 500 sccm, and the input power of the oxidation source is 1000W.

[0179] (Formation of antifouling film)

[0180] KY-185 (trade name, manufactured by Shin-Etsu Chemical Co., Ltd.), a fluorine-containing organosilicon compound, was placed in a metal crucible (evaporation source) and heated to evaporate at 230-350°C. The evaporated particles were evaporated and diffused into a vacuum chamber where a substrate was set and adhered to the surface of the substrate. A 4nm thick antifouling film was formed while monitoring the evaporation rate by controlling the crystal oscillator.

[0181] (Example 2)

[0182] A transparent substrate with an antireflection film was obtained in the same manner as in Example 1 except that the film composition of the antireflection film was changed as shown in Table 1 to form an antireflection film having a film composition of 6 layers.

[0183] (Example 3)

[0184] A transparent substrate with an antireflection film was obtained in the same manner as in Example 1 except that the film composition of the antireflection film was changed as shown in Table 1 and the film forming method of the NMWO layer was changed as follows to form an antireflection film consisting of 6 layers.

[0185] (Film formation of NMWO layer)

[0186] The oxide film is formed by repeatedly performing the following operation at a high speed, thereby forming a NMWO layer of a predetermined film thickness: using a target obtained by mixing niobium, molybdenum and tungsten in a weight ratio of 24:30:46 and sintering, and maintaining the pressure at 0.2 Pa with argon gas at a frequency of 100 kHz and a power density of 10.0 W / cm 2 , pulse sputtering is performed under the condition of an inversion pulse width of 3μsec to form a metal film with a very small film thickness, and then it is oxidized with oxygen. The transmittance of the anti-reflection film is adjusted by adjusting the oxidation degree of the NMWO layer. It should be noted that for the NMWO layer formed by this method, the composition was measured by depth composition analysis using X-ray photoelectron spectroscopy (XPS) using argon ion sputtering. The results showed that, except for oxygen, Nb was 31.5at%, Mo was 38.1at%, W was 30.5at%, and the content of group B elements was 24% by weight.

[0187] (Example 4)

[0188] The film composition of the anti-reflection film is changed as shown in Table 1, and the oxidation degree of the high refractive index material is adjusted in such a way that the light transmittance Y of the transparent substrate with the anti-reflection film is 55%, thereby forming an anti-reflection film composed of four layers. Except for this, a transparent substrate with an anti-reflection film is obtained in the same manner as in Example 3.

[0189] The results of the above evaluations of the transparent substrates with antireflection films obtained in each example are shown in Table 1. * and b * Shown in Figure 3 . Figure 3 In the figure, (a) to (d) are the diffuse reflection light at each angle of Examples 1 to 4, respectively. * and b * In each figure, if the curve is within the region indicated by the dotted line, it means that all equations (1) to (4) are satisfied.

[0190]

[0191] The results in Table 1 confirm that in Examples 3 and 4 as embodiments, the a measured by each diffuse reflected light * and b * By satisfying all of the equations (1) to (4), it is possible to suppress color deviation during tiling.

[0192] As described above, this specification discloses the following matters.

[0193] 1. A transparent substrate with an anti-reflection film, comprising: a transparent substrate having two main surfaces, and a diffusion layer and an anti-reflection film provided on one main surface of the transparent substrate in order from the transparent substrate side,

[0194] When the reflection from the other main surface of the transparent substrate is removed and the light source is incident on the one main surface at an incident angle of 45°, the a value of the diffuse reflected light at angles of -15°, 15°, 25°, 45°, 75° and 110° relative to the specular reflected light under the D65 light source is * and b * The following formulas (1) to (4) are satisfied.

[0195] (1)-6≤a * ≤2

[0196] (2)-1≤b * ≤12

[0197] (3)b * ≤-2a * +4

[0198] (4)b * ≥-2a * -5

[0199] 2. The transparent substrate with an antireflection film according to item 1 above, wherein the haze value is 30% or more.

[0200] 3. The transparent substrate with an anti-reflection film according to 1 or 2 above, wherein the L value of the diffuse reflected light at -15° under a D65 light source is * The L of the diffuse reflected light at 15° is 30 to 60. * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20.

[0201] 4. The transparent substrate with an antireflection film according to any one of 1 to 3 above, wherein the light transmittance (Y) is 20 to 90%.

[0202] 5. The transparent substrate with an anti-reflection film according to any one of 1 to 4 above, wherein the anti-reflection film has a sheet resistance of 10 4 Ω / □ or more.

[0203] 6. The transparent substrate with an antireflection film according to any one of 1 to 5 above, wherein the transmission color b under D65 light source is * Is 5 or less.

[0204] 7. A transparent substrate with an anti-reflection film according to any one of 1 to 6 above, wherein the anti-reflection film is a stacked structure formed by stacking at least two dielectric layers with different refractive indices, at least one of the dielectric layers is mainly composed of Si oxide, and at least one other layer of the layers of the stacked structure is mainly composed of a mixed oxide, which is a mixed oxide of at least one oxide selected from Group A consisting of Mo and W and at least one oxide selected from Group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of Group B contained in the mixed oxide is 65% by mass or less relative to the total of the elements of Group A contained in the mixed oxide and the elements of Group B contained in the mixed oxide.

[0205] 8. The transparent substrate with an antireflection film according to any one of 1 to 7 above, further comprising an antifouling film on the antireflection film.

[0206] 9. The transparent substrate with an antireflection film according to any one of 1 to 8 above, wherein the transparent substrate comprises glass.

[0207] 10. The transparent substrate with an antireflection film according to any one of 1 to 9 above, wherein the transparent substrate comprises at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

[0208] 11. The transparent substrate with an antireflection film according to any one of 1 to 10 above, wherein the transparent substrate is a laminate of glass and at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

[0209] 12. The transparent substrate with an antireflection film according to 9 or 11 above, wherein the glass is chemically strengthened.

[0210] 13. An image display device comprising the transparent substrate with an antireflection film according to any one of 1 to 12 above.

[0211] The present invention is described in detail and with reference to specific embodiments, but it is obvious that those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. This application is based on Japanese patent application (Japanese Patent Application No. 2022-064752) filed on April 8, 2022, the contents of which are incorporated herein by reference.

[0212] Explanation of symbols

[0213] 1Transparent substrate with anti-reflection film

[0214] 10 Transparent substrate

[0215] 11 A main surface

[0216] 12 Another main face

[0217] 20 black tape

[0218] 30 Anti-reflective film

[0219] 31 diffusion layer

[0220] 32 first dielectric layer

[0221] 34 Second dielectric layer

[0222] 50 Light Sources

[0223] 60Incident light

[0224] 61 Specular reflection light

[0225] 71, 72, 73, 74, 75, 76 Diffuse reflected light

Claims

1. A transparent substrate with an anti-reflection film, comprising: a transparent substrate having two main surfaces, and a diffusion layer and an anti-reflection film provided on one main surface of the transparent substrate in order from the transparent substrate side, When the reflection from the other main surface of the transparent substrate is removed and the light source is incident on the one main surface at an incident angle of 45°, the a value of the diffuse reflected light under the D65 light source at angles of -15°, 15°, 25°, 45°, 75° and 110° relative to the specular reflected light is * and b * Satisfying the following equations (1) to (4), (1)-6≤a * ≤2 (2)-1≤b * ≤12 (3)b * ≤-2a * +4 (4)b * ≥-2a * -5。 2. The transparent substrate with an anti-reflection film according to claim 1, wherein: The haze value is 30% or more.

3. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The L of the diffuse reflected light at -15° under D65 light source * is 30 to 60, the L of the diffuse reflected light at 15° * is 15 to 35, and the L of the diffuse reflected light at 25° * 5 to 20.

4. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The light transmittance Y is 20 to 90%.

5. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The sheet resistance of the anti-reflection film is 10 4 Ω / □ or more.

6. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: b of the transmitted color under D65 light source * Is 5 or less.

7. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The antireflection film has a stacked structure in which at least two dielectric layers having different refractive indices are stacked, at least one of the dielectric layers is mainly composed of Si oxide, and at least one other layer of the layers of the stacked structure is mainly composed of a mixed oxide, which is a mixed oxide of at least one oxide selected from the group A consisting of Mo and W and at least one oxide selected from the group B consisting of Si, Nb, Ti, Zr, Ta, Al, Sn and In, and the content of the elements of the group B contained in the mixed oxide is 65 mass % or less relative to the total of the elements of the group A contained in the mixed oxide and the elements of the group B contained in the mixed oxide.

8. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: An antifouling film is further provided on the antireflection film.

9. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The transparent substrate comprises glass.

10. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The transparent substrate includes at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic, silicone, and triacetyl cellulose.

11. The transparent substrate with an anti-reflection film according to claim 1 or 2, wherein: The transparent substrate is a laminate of glass and at least one resin selected from the group consisting of polyethylene terephthalate, polycarbonate, acrylic acid, silicone and triacetyl cellulose.

12. The transparent substrate with an anti-reflection film according to claim 11, wherein: The glass is chemically strengthened. 13 . An image display device comprising the transparent substrate with an antireflection film according to claim 1 or 2 .