Preparation method of alicyclic epoxy resin
Through the two-stage etherification of the quaternary ammonium salt catalyst and the hydrogenation reaction of the Rh/L molecular sieve catalyst, combined with the closed-loop reaction of the sodium hydroxide solution, the benzene ring hydrogenation rate of the alicyclic epoxy resin is improved and the total chlorine content is reduced. The problems of low hydrogenation rate of benzene ring and high total chlorine content in the prior art are solved, and are suitable for the preparation of alicyclic epoxy resins with high weather resistance and electrical applications.
Patent Information
- Application Number
- CN202310585445.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
In the existing preparation method of alicyclic 2,2'-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin, the benzene ring hydrogenation rate and high total chlorine content affect its application performance, especially in electrical and are not applicable in areas with high weather resistance requirements.
Quaternary ammonium salt catalyst is used to carry out low-temperature and high-temperature two-stage etherification reaction, combining catalytic hydrogenation reaction and closed-loop reaction, controlling the reaction conditions to increase the benzene ring hydrogenation rate and reduce the total chlorine content, using Rh/L molecular sieve catalyst and sodium hydroxide solution Carry out hydrogenation reaction.
The benzene ring hydrogenation rate has reached more than 97%, the total chlorine content is less than 0.3%, and the epoxy equivalent is between 185 and 192g/eq, which improves the thermal stability and chemical stability of the product. It is suitable for high electrical and weather resistance requirements. use.
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing an alicyclic epoxy resin, in particular to a method for preparing an alicyclic 2,2′-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin, and belongs to the technical field of epoxy resin synthesis. Background Art
[0002] Bisphenol A epoxy resin has excellent adhesion, heat resistance, chemical resistance and electrical properties, and is widely used in coatings, adhesives, fiberglass, laminates, electronic casting, potting, encapsulation and other fields. However, due to the presence of benzene rings in the structure, its weather resistance, yellowing resistance and UV resistance are poor, which limits its application range, especially in outdoor use. In order to improve the weather resistance, yellowing resistance and UV resistance of the resin, hydrogenation of saturated double bonds is often used to improve the antioxidant performance.
[0003] The performance of alicyclic 2,2′-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin cured product is similar to that of bisphenol A epoxy resin, but due to the hydrogenation of the benzene ring into a saturated six-membered ring, its viscosity is greatly reduced compared with ordinary bisphenol A epoxy resin. The thermal stability, chemical stability, corona resistance and weather resistance of the cured product are better. It is widely used in outdoor coatings, outdoor castings, and LED packaging materials, and can replace ordinary bisphenol A epoxy resin in projects with weather resistance and UV resistance requirements.
[0004] There are usually two methods for preparing 2,2′-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. One is to first etherify hydrogenated bisphenol A and epichlorohydrin under the action of a catalyst and then cyclize under the action of an alkali to obtain it. Chinese patents CN102766113A and CN104193961A disclose a method of using hydrogenated bisphenol A and epichlorohydrin as raw materials, first etherifying with Lewis acid as a catalyst, and then adding alkali to close the ring and epoxidize to obtain hydrogenated bisphenol A epoxy resin. When synthesizing hydrogenated bisphenol A epoxy resin by this method, since the etherification of alcohol hydroxyl groups is more difficult than that of phenol hydroxyl groups, the etherification temperature is higher, the β addition is more during etherification, the total chlorine content of the product is high, and the total chlorine content is generally 3-5%, which seriously affects the application performance of the product and is not suitable for electrical use and uses with high weather resistance requirements.
[0005] The other is obtained by direct hydrogenation of bisphenol A epoxy resin. U.S. Patent No. 6060611A discloses that bisphenol A epoxy resin is used as raw material and tetrahydrofuran is used as solvent. Bisphenol A epoxy resin is directly hydrogenated at a temperature of 30-150° C. and a pressure of 2-30 MPa to obtain hydrogenated bisphenol A epoxy resin. This method uses epoxy resin to directly hydrogenate and decompose part of the epoxy groups. The epoxy group decomposition rate is 5-10%. Tetrahydrofuran is used as solvent. Tetrahydrofuran is easily oxidized. Trace peroxides in tetrahydrofuran can reduce the activity of the hydrogenation catalyst, and even deactivate the hydrogenation catalyst, affecting the benzene ring hydrogenation rate of the product. Chinese Patent No. CN100513453A discloses that bisphenol A epoxy resin is directly hydrogenated at a temperature of 30-150° C. and a pressure of 2-15 MPa to obtain hydrogenated bisphenol A epoxy resin. The method uses direct hydrogenation of epoxy resin to decompose part of epoxy groups by hydrogenation, and the decomposition rate of epoxy groups is 7-10%. Ethyl acetate is used as a solvent, and ethyl acetate is easily decomposed by hydrogenation under the action of a hydrogenation catalyst. Summary of the invention
[0006] In view of the defects of the prior art, the object of the present invention is to provide a method for preparing an alicyclic epoxy resin, wherein the alicyclic epoxy resin prepared by the method has the characteristics of high hydrogenation rate of benzene rings, low epoxy equivalent, low total chlorine content, etc.
[0007] In order to achieve the above technical purpose, the present invention provides a method for preparing alicyclic epoxy resin, comprising subjecting bisphenol A and epichlorohydrin to a two-stage etherification reaction at low temperature and high temperature under the action of a quaternary ammonium salt catalyst to obtain chlorohydrin ether; and subjecting the chlorohydrin ether to a catalytic hydrogenation reaction and a ring-closing reaction in sequence to obtain the obtained product.
[0008] The invention firstly adopts quaternary ammonium salt as a catalyst and does not use a catalyst containing sodium ions, so as to reduce the influence of sodium ions on a hydrogenation catalyst and lay a foundation for improving the hydrogenation rate of benzene rings in chlorohydrin ethers. Then, by controlling the two-stage etherification reaction conditions, low-temperature etherification is firstly performed to reduce the etherification side reaction and improve the epoxide value of the product, and then high-temperature etherification is performed to make the bisphenol A react completely. Then, a catalytic hydrogenation reaction is performed, so that the benzene rings on the chlorohydrin ethers can be hydrogenated at a relatively low temperature, the decomposition of the chlorohydrin ethers can be avoided, the hydrogenation rate of the benzene rings can be improved, and the total chlorine content can be reduced. Finally, a closed-ring reaction is performed by controlling the time of adding an alkali solution. The finally prepared alicyclic epoxy resin has high benzene ring hydrogenation rate, low epoxide equivalent and low total chlorine content.
[0009] As a preferred solution, the first stage etherification reaction conditions of the two-stage etherification reaction are: temperature of 60-80°C, time of 3-4h; the second stage etherification reaction conditions of the two-stage etherification reaction are: temperature of 95-105°C, time of 0.5-1h. The present invention adopts a two-stage etherification method and controls the etherification conditions to make bisphenol A react completely. First, low-temperature etherification for a long time can reduce the etherification side reaction and increase the product epoxy value. Most of the substrate can be etherified, and then high-temperature etherification for a short time. High-temperature etherification in a short time can make bisphenol A completely converted, and too long high-temperature etherification leads to side reactions. If the etherification temperature of the first stage is too high, or the etherification reaction time is too long, it will lead to an increase in etherification side reactions and a low product epoxy value. If the etherification temperature of the second stage is too low, or the etherification time is too short, the etherification of bisphenol A will be incomplete, and the product epoxy value will be low. If the two-stage etherification reaction is not adopted, the content of hydrolyzed chlorine and the liquid viscosity of the product will increase significantly, while the hydrogenation rate of the benzene ring will decrease.
[0010] As a preferred solution, the quaternary ammonium salt catalyst is one of n-pentyltriphenylammonium bromide, tetrabutylammonium chloride, tetramethylammonium chloride and benzyltriethylammonium chloride. The present invention adopts quaternary ammonium salt as catalyst to avoid the introduction of sodium ions in the early stage, which is conducive to improving the hydrogenation rate later.
[0011] As a preferred solution, the molar ratio of bisphenol A to epichlorohydrin is 1:5 to 8. The present invention controls the molar ratio of the raw materials bisphenol A and epichlorohydrin to make the bisphenol A react completely and reduce the by-products generated by subsequent operations. If the molar ratio of bisphenol A to epichlorohydrin is too high, bisphenol A cannot react completely, resulting in residual bisphenol A, which ultimately affects the performance of the epoxy resin. If the molar ratio of bisphenol A to epichlorohydrin is too low, the difficulty of subsequent impurity removal is increased, resulting in an increase in the chlorine content of the epoxy resin.
[0012] As a preferred solution, the mass ratio of bisphenol A to quaternary ammonium salt catalyst is 100:1-2.
[0013] As a preferred solution, the conditions of the catalytic hydrogenation reaction are: temperature of 60-120°C, pressure of 4-8MPa, and time of 1.5-4h. In the present invention, if the temperature of the catalytic hydrogenation reaction is too low or the pressure is too low, the activation energy of the reaction cannot be reached and the reaction cannot proceed; and when the reaction temperature is too high or the pressure is too high, the reaction will release a large amount of heat too quickly, which will increase the epoxy decomposition rate of the obtained bisphenol A epoxy resin on the one hand, and on the other hand, there will be safety hazards.
[0014] As a preferred solution, the catalyst used in the catalytic hydrogenation reaction is a Rh / L molecular sieve catalyst.
[0015] As a preferred solution, the mass ratio of the amount of the catalyst to the chlorohydrin ether is 1 to 4:100.
[0016] As a preferred solution, sodium hydroxide aqueous solution and / or potassium hydroxide aqueous solution are used as promoters in the ring-closing reaction, and sodium hydroxide aqueous solution is more preferably used, with a concentration of 20-30%. The role of sodium hydroxide used in the present invention is dechlorination, and sodium hydroxide reacts with chlorine to generate sodium chloride, and the ring is closed to form an epoxy group.
[0017] As a preferred solution, the molar ratio of the sodium hydroxide aqueous solution and / or potassium hydroxide aqueous solution to the hydrogenated chlorohydrin ether is 2.1 to 2.5: 1. If the molar ratio of the alkali solution to the hydrogenated chlorohydrin ether of the present invention is too small, the product ring closure will be incomplete. If the molar ratio of the alkali solution to the hydrogenated chlorohydrin ether is too large, cross-linking will occur between the product molecules, affecting the product quality.
[0018] As a preferred solution, the conditions of the ring-closing reaction are: temperature of 90-100°C, alkali solution addition time of 2-4h, and ring-closing reaction time of 7-14h. Since the ring-closing reaction is an endothermic reaction, a certain temperature must be maintained during the reaction process. However, if the temperature is too high, the epoxy resin after ring-closing will undergo ring-opening polymerization at high temperature, which will affect the product quality.
[0019] As a preferred solution, the solvent used in the ring-closing reaction is at least one of toluene, ethylbenzene, xylene, methyl isobutyl ketone and methyl ethyl ketone.
[0020] As a preferred solution, the mass ratio of the solvent to the hydrogenated chlorohydrin ether used in the ring-closure reaction is 0.5 to 1: 1. If the mass ratio of the solvent to the hydrogenated chlorohydrin ether in the present invention is too large, the organic chlorine content of the final epoxy resin will be high. If the mass ratio of the solvent to the hydrogenated chlorohydrin ether is too small, it will be unfavorable for the ring-closure reaction.
[0021] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:
[0022] 1) In the preparation method of the present invention, the ring-opening etherification reaction adopts a quaternary ammonium salt catalyst, which can effectively reduce the sodium ion content in the chlorohydrin ether and reduce the influence of the sodium ion on the hydrogenation catalyst, thus laying a foundation for improving the hydrogenation rate of the benzene ring in the chlorohydrin ether.
[0023] 2) In the ring-opening etherification reaction of the preparation method of the present invention, low-temperature etherification is first used to reduce the etherification side reaction and increase the epoxy value of the product, and then high-temperature etherification is used to completely convert bisphenol A.
[0024] 3) The Rh / L molecular sieve catalyst used in the hydrogenation reaction of the preparation method of the present invention can achieve a hydrogenation rate of the benzene ring of the prepared chlorohydrin ether of more than 97% at a relatively low hydrogenation temperature.
[0025] 4) The alicyclic 2,2′-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin prepared by the present invention has a benzene ring hydrogenation rate of more than 97%, an epoxy equivalent of 185 to 192 g / eq, and a total chlorine content of no more than 0.3%. DETAILED DESCRIPTION
[0026] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner in conjunction with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0027] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0028] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0029] The preparation method of the Rh / L molecular sieve catalyst used in the present invention is as follows: weigh 100g L molecular sieve (Changling Branch of Sinopec Catalyst Company), add an equal volume of RhCl3·3H2O (Rh≥39%) solution with a concentration of 12.9g / 100mL for impregnation, the impregnation temperature is 30°C, the impregnation time is 8h, the impregnation solution is dried at 120°C for 24h, ground into fine powder, heated to 280°C in a hydrogen atmosphere for reduction for 2h, and a Rh / L molecular sieve catalyst with a mass percentage content of 5% is obtained.
[0030] The concentration of RhCl3·3H2O (Rh≥39%) solution was changed to 8 g / 100 mL and 26 g / 100 mL respectively, and the rest was the same as the above method to prepare 3% Rh / L molecular sieve catalyst and 10% Rh / L molecular sieve catalyst.
[0031] Example 1
[0032] Add 228.3g of bisphenol A and 555g of epichlorohydrin into a reactor, stir under nitrogen protection to make bisphenol A completely dissolved in epichlorohydrin, heat to 70°C, add 2.3g of n-pentyltriphenylammonium bromide, and react at 70°C for etherification for 3h, then heat to 105°C for etherification for 0.5h, wash with water until the pH value of the aqueous phase is 6.5-7, and then remove excess epichlorohydrin to obtain chlorohydrin ether.
[0033] In a 5L magnetic stirring autoclave, 420g of chlorohydrin ether, 12.6g of 5%Rh / L molecular sieve hydrogenation catalyst, and 1680g of isopropanol were added, and nitrogen replacement was performed after sealing, and then hydrogen replacement was performed. Then, hydrogenation reaction was carried out at 80°C and 7MPa pressure for 2h. After the reaction was completed, the catalyst was filtered out, and the filtrate was distilled to recover isopropanol, and the solvent was removed at 180°C and 10kPa pressure to obtain hydrogenated chlorohydrin ether.
[0034] 425g of hydrogenated chlorohydrin ether and 300g of toluene were added to the reactor, stirred under nitrogen protection, heated to 95°C, 440g of 20% sodium hydroxide solution was added dropwise for 2h, and the reaction was continued for 7h after the addition. After the reaction, 400g of toluene was added, stirring was stopped, the mixture was allowed to stand, water was separated, phosphoric acid was added dropwise for neutralization, and the mixture was washed with water until the pH of the aqueous phase was 6.5-7. Toluene was recovered by distillation from the organic phase, and the solvent was removed at 170°C and 10kPa to obtain 345g of 2,2′-di(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. The obtained product was a colorless, transparent, viscous liquid with an epoxy equivalent of 185g / eq, a hydrolyzable chlorine content of 127μg / g, an inorganic chlorine content of 4μg / g, a total chlorine content of 0.23%, a viscosity of 1816mPas (25°C), and a benzene ring hydrogenation rate of 98.2%.
[0035] Example 2
[0036] Add 228.3g of bisphenol A and 740g of epichlorohydrin into a reactor, stir under nitrogen protection to make bisphenol A completely dissolved in epichlorohydrin, heat to 60°C, add 3.5g of tetrabutylammonium chloride, and react at 60°C for etherification for 4h, then heat to 100°C for etherification for 1h, wash with water until the pH value of the aqueous phase is 6.5-7, and then remove excess epichlorohydrin to obtain chlorohydrin ether.
[0037] In a 5L magnetic stirring autoclave, 420g of chlorohydrin ether, 16.8g of 3%Rh / L molecular sieve hydrogenation catalyst, and 1260g of isopropanol were added, and nitrogen replacement was performed after sealing, and then hydrogen replacement was performed. Then, hydrogenation reaction was carried out at 90°C and 6MPa pressure for 3h. After the reaction was completed, the catalyst was filtered out, and the filtrate was distilled to recover isopropanol, and the solvent was removed at 180°C and 10kPa pressure to obtain hydrogenated chlorohydrin ether.
[0038] 425g of hydrogenated chlorohydrin ether and 350g of toluene were added to the reactor, stirred under nitrogen protection, heated to 90°C, 30% sodium hydroxide solution 335g was added dropwise for 1.5h, and the reaction was continued for 6h after the addition. After the reaction, 450g of toluene was added, stirring was stopped, the mixture was allowed to stand, water was separated, phosphoric acid was added dropwise for neutralization, and the mixture was washed with water until the pH of the aqueous phase was 6.5-7. Toluene was recovered by distillation from the organic phase, and the solvent was removed at 170°C and 10kPa to obtain 342g of 2,2′-di(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. The obtained product was a colorless, transparent, viscous liquid with an epoxy equivalent of 188g / eq, a hydrolyzable chlorine content of 135μg / g, an inorganic chlorine content of 4μg / g, a total chlorine content of 0.24%, a viscosity of 2253mPas (25°C), and a benzene ring hydrogenation rate of 97.5%.
[0039] Example 3
[0040] Add 228.3g of bisphenol A and 463g of epichlorohydrin into a reaction kettle, stir under nitrogen protection to make bisphenol A completely dissolved in epichlorohydrin, heat to 65°C, add 4.6g of tetramethylammonium chloride, and etherify at 65-75°C for 4h, then heat to 95°C for etherification for 1h, wash with water until the pH value of the aqueous phase is 6.5-7, and then remove excess epichlorohydrin to obtain chlorohydrin ether.
[0041] In a 5L magnetic stirring autoclave, 420g of chlorohydrin ether, 12.6g of 5%Rh / L molecular sieve hydrogenation catalyst, and 1680g of isopropanol were added, and nitrogen replacement was performed after sealing, and then hydrogen replacement was performed. Then, hydrogenation reaction was carried out at 100°C and 5MPa pressure for 3h. After the reaction was completed, the catalyst was filtered out, and the filtrate was distilled to recover isopropanol, and the solvent was removed at 170°C and 8kPa pressure to obtain hydrogenated chlorohydrin ether.
[0042] Add 425g of hydrogenated chlorohydrin ether and 420g of toluene to the reactor, stir under nitrogen protection, heat to 100℃, add 440g of 20% sodium hydroxide solution, add for 2h, and continue to react for 10h after addition. After the reaction, add 380g of toluene, stop stirring, let stand, separate water, add phosphoric acid to neutralize, wash with water until the pH of the aqueous phase is 6.5-7, distill and recover toluene from the organic phase, remove the solvent at 180℃ and pressure 7kPa, and obtain 343g of 2,2′-di(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. The obtained product is a colorless, transparent, viscous liquid with an epoxy equivalent of 191g / eq, a hydrolyzable chlorine content of 135μg / g, an inorganic chlorine content of 5μg / g, a total chlorine content of 0.25%, a viscosity of 2678mPas (25℃), and a benzene ring hydrogenation rate of 97.7%.
[0043] Example 4
[0044] Add 228.3g of bisphenol A and 555g of epichlorohydrin into a reactor, stir under nitrogen protection to make bisphenol A completely dissolved in epichlorohydrin, heat to 70°C, add 2.3g of benzyltriethylammonium chloride, and then etherify at 80°C for 4h, then heat to 105°C for etherification for 0.5h, wash with water until the pH of the aqueous phase is 6.5-7, and then remove excess epichlorohydrin to obtain chlorohydrin ether.
[0045] In a 5L magnetic stirring autoclave, 420g of chlorohydrin ether, 4.2g of 10%Rh / L molecular sieve hydrogenation catalyst, and 1680g of isopropanol were added, and nitrogen replacement was performed after sealing, and then hydrogen replacement was performed. Then, hydrogenation reaction was carried out at 100°C and 7MPa pressure for 2h. After the reaction was completed, the catalyst was filtered out, and the filtrate was distilled to recover the isopropanol, and the solvent was removed at 180°C and 10kPa pressure to obtain hydrogenated chlorohydrin ether.
[0046] 425g of hydrogenated chlorohydrin ether and 270g of toluene were added to the reactor, stirred under nitrogen protection, heated to 95°C, and 440g of 20% sodium hydroxide solution was added dropwise for 2h. After the addition, the reaction was continued for 8h. After the reaction was completed, 600g of toluene was added, stirring was stopped, the mixture was allowed to stand, water was separated, phosphoric acid was added dropwise for neutralization, and the aqueous phase was washed with water until the pH value of the aqueous phase was 6.5-7. Toluene was recovered by distillation from the organic phase, and the solvent was removed at 170°C and 10kPa to obtain 346g of 2,2′-di(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. The obtained product was a colorless, transparent, viscous liquid with an epoxy equivalent of 190g / eq, a hydrolyzable chlorine content of 128μg / g, an inorganic chlorine content of 5μg / g, a total chlorine content of 0.22%, a viscosity of 2525mPas (25°C), and a benzene ring hydrogenation rate of 98.3%.
[0047] Example 5
[0048] Add 228.3g of bisphenol A and 555g of epichlorohydrin into a reactor, stir under nitrogen protection to make bisphenol A completely dissolved in epichlorohydrin, heat to 65°C, add 3.2g of n-pentyltriphenylammonium bromide, and react at 65°C for etherification for 3h, then heat to 105°C for etherification for 0.5h, wash with water until the pH value of the aqueous phase is 6.5-7, and then remove excess epichlorohydrin to obtain chlorohydrin ether.
[0049] In a 5L magnetic stirring autoclave, 420g of chlorohydrin ether, 12.6g of 5%Rh / L molecular sieve hydrogenation catalyst, and 2380g of isopropanol were added, and nitrogen replacement was performed after sealing, and then hydrogen replacement was performed. Then, hydrogenation reaction was carried out at 80°C and 7MPa pressure for 2h. After the reaction was completed, the catalyst was filtered out, and the filtrate was distilled to recover isopropanol, and the solvent was removed at 170°C and 8kPa pressure to obtain hydrogenated chlorohydrin ether.
[0050] 425g of hydrogenated chlorohydrin ether and 425g of toluene were added to the reactor, stirred under nitrogen protection, heated to 95°C, and 440g of 20% sodium hydroxide solution was added dropwise for 2h. After the addition, the reaction was continued for 9h. After the reaction, 430g of toluene was added, stirring was stopped, the mixture was allowed to stand, water was separated, phosphoric acid was added dropwise for neutralization, and the mixture was washed with water until the pH of the aqueous phase was 6.5-7. Toluene was recovered by distillation from the organic phase, and the solvent was removed at 170°C and 8kPa to obtain 343g of 2,2′-di(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. The obtained product was a colorless, transparent, viscous liquid with an epoxy equivalent of 187g / eq, a hydrolyzable chlorine content of 124μg / g, an inorganic chlorine content of 4μg / g, a total chlorine content of 0.24%, a viscosity of 2285mPas (25°C), and a benzene ring hydrogenation rate of 97.8%.
[0051] Comparative Example 1
[0052] In this comparative implementation, hydrogenated bisphenol A and epichlorohydrin are directly used as raw materials, and alicyclic epoxy resin is prepared by first etherification and then cyclization under the action of a catalyst.
[0053] Add 240.4g hydrogenated bisphenol A and 280g toluene into a reactor and stir to make hydrogenated bisphenol A completely dissolved in toluene. Heat to 113°C and reflux for dehydration. After dehydration for 1h, cool to 100°C and add 0.7g of catalyst boron trifluoride ether solution. Add 207g epichlorohydrin dropwise for 2.5h. After addition, continue the reaction for 0.5h. Maintain the etherification reaction temperature at 98-102°C. After the reaction, distill and recover 140g toluene. Add 270g of pure water to the reactor, add 210g of 49% sodium hydroxide aqueous solution, add 2h of dropping time, reaction temperature 90℃, continue to maintain the reaction for 8h after adding, add 280g of toluene after the reaction, stop stirring, let stand, divide water, add phosphoric acid to neutralize, wash with water to pH 6.5-7 of the aqueous phase, distill and recover toluene from the organic phase, remove the solvent at 170℃ and pressure 8kPa, and obtain 369g of 2,2′-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin. The obtained product is a colorless, transparent, viscous liquid with an epoxy equivalent of 228g / eq, a hydrolyzable chlorine content of 565μg / g, an inorganic chlorine content of 5μg / g, a total chlorine content of 3.27%, and a viscosity of 2785mPas (25℃). It can be seen that the hydrolyzed chlorine content of the obtained product is greatly increased compared with the present invention, and the total chlorine content and epoxy equivalent are much higher than those of the embodiment.
[0054] Comparative Example 2
[0055] In this comparative example, bisphenol A epoxy resin is used as a raw material and alicyclic epoxy resin is prepared by direct hydrogenation.
[0056] 1000g of bisphenol A epoxy resin CYD-128 (Sinopec Baling Petrochemical Company, epoxy equivalent 189g / eq) was dissolved in 3000g of toluene, then washed three times with 900g of deionized water at 60°C, and then the toluene solution was removed. The sodium content of the treated bisphenol A epoxy resin was 0.08μg / g.
[0057] In a 2L magnetic stirring autoclave, add 150g of pretreated bisphenol A epoxy resin, 1.5g of 5% Rh / L molecular sieve hydrogenation catalyst, and 850g of isopropanol, seal it, replace it with nitrogen, and then replace it with hydrogen. Then, carry out hydrogenation reaction at 100°C and 6MPa pressure for 3h. After the reaction is completed, filter to remove the catalyst, distill the filtrate to recover isopropanol, remove the solvent at 180°C and 20kPa pressure, and obtain colorless and transparent hydrogenated bisphenol A epoxy resin with epoxy equivalent of 199g / eq, epoxy group decomposition rate of 4.8%, hydrolyzable chlorine content of 206μg / g, inorganic chlorine content of 5μg / g, total chlorine content of 0.25%, viscosity of 3126mPas (25°C), and benzene ring hydrogenation rate of 97.6%. When bisphenol A epoxy resin is used as a raw material and directly hydrogenated to prepare alicyclic epoxy resin, although the total chlorine content in the product is low, epoxy group decomposition exists and the epoxy equivalent of the product is higher than that in the embodiment.
[0058] Comparative Example 3
[0059] The only difference between this comparative example and Example 1 is that the two-stage etherification reaction is not used, and the etherification at 80°C for 3.5h is directly used, and the other conditions are the same. 332g of 2,2′-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin is obtained. The obtained product is a colorless, transparent, viscous liquid, with an epoxy equivalent of 210g / eq, a hydrolyzable chlorine content of 203μg / g, an inorganic chlorine content of 5μg / g, a total chlorine content of 0.35%, a viscosity of 3629mPas (25°C), and a benzene ring hydrogenation rate of 93.1%. When the two-stage etherification reaction is not used, the content of hydrolyzable chlorine and the liquid viscosity in the obtained product will increase significantly, while the hydrogenation rate of the benzene ring will decrease.
[0060] Comparative Example 4
[0061] The only difference between this comparative example and Example 1 is that the etherification reaction uses sodium hydroxide solution as a catalyst instead of quaternary ammonium salt as a catalyst, 20g of 30% sodium hydroxide solution is added as a catalyst, and the other conditions are the same. 312g of 2,2'-bis(4-hydroxycyclohexyl)propane diglycidyl ether epoxy resin is obtained. The obtained product is a colorless, transparent, viscous liquid, with an epoxy equivalent of 218g / eq, a hydrolyzable chlorine content of 402μg / g, an inorganic chlorine content of 5μg / g, a total chlorine content of 0.38%, a viscosity of 4627mPas (25°C), and a benzene ring hydrogenation rate of 72.6%.
Claims
1. A method for preparing an alicyclic epoxy resin, characterized in that: Bisphenol A and epichlorohydrin are subjected to low-temperature and high-temperature two-stage etherification reactions under the action of a quaternary ammonium salt catalyst to obtain chlorohydrin ether; the chlorohydrin ether is subjected to catalytic hydrogenation reaction and ring-closing reaction in sequence to obtain the product.
2. The method for preparing an alicyclic epoxy resin according to claim 1, characterized in that: The first stage etherification reaction conditions of the two-stage etherification reaction are: temperature of 60-80°C and time of 3-4h; the second stage etherification reaction conditions of the two-stage etherification reaction are: temperature of 95-105°C and time of 0.5-1h.
3. The method for preparing an alicyclic epoxy resin according to claim 1, characterized in that: The quaternary ammonium salt catalyst is one of n-pentyltriphenylammonium bromide, tetrabutylammonium chloride, tetramethylammonium chloride and benzyltriethylammonium chloride.
4. The method for preparing an alicyclic epoxy resin according to claim 1, characterized in that: The molar ratio of bisphenol A to epichlorohydrin is 1:5-8.
5. The method for preparing an alicyclic epoxy resin according to claim 1 or 3, characterized in that: The mass ratio of bisphenol A to quaternary ammonium salt catalyst is 100:1-2.
6. The method for preparing an alicyclic epoxy resin according to claim 1, characterized in that: The conditions of the catalytic hydrogenation reaction are: temperature of 60-120° C., pressure of 4-8 MPa, and time of 1.5-4 h.
7. The method for preparing an alicyclic epoxy resin according to claim 6, characterized in that: The catalyst used in the catalytic hydrogenation reaction is a Rh / L molecular sieve catalyst.
8. The method for preparing an alicyclic epoxy resin according to claim 7, characterized in that: The mass ratio of the amount of the catalyst to the chlorohydrin ether is 1 to 4:
100.
9. The method for preparing an alicyclic epoxy resin according to claim 1, characterized in that: In the ring-closing reaction, sodium hydroxide aqueous solution and / or potassium hydroxide aqueous solution are used as promoters.
10. The method for preparing an alicyclic epoxy resin according to claim 9, characterized in that: The molar ratio of the sodium hydroxide aqueous solution and / or potassium hydroxide aqueous solution to the hydrogenated chlorohydrin ether is 2.1-2.5:
1.
11. The method for preparing an alicyclic epoxy resin according to claim 1, characterized in that: The conditions of the ring-closing reaction are: temperature of 90-100° C. and time of 7-14 h.
12. The method for preparing an alicyclic epoxy resin according to claim 1, 9 or 11, characterized in that: The solvent used in the ring-closing reaction is at least one of toluene, ethylbenzene, xylene, methyl isobutyl ketone and methyl ethyl ketone.
Citation Information
Patent Citations
Method for preparing bisphenol-A liquid epoxy resin
CN101613458A
Preparation method for hydrogenated bisphenol A epoxy resin
CN104193961A
Preparation method of hydrogenated bisphenol A
CN107954832A
Bisphenol A epoxy resin and preparation method thereof
CN115819725A
Alicyclic compound containing glycidyl group, its production method and epoxy resin composition using the same
JP2002097251A