Light-proof low-medium low-Tg polyimide film and preparation method thereof
By combining modified black polyimide layers and using specific processing techniques, the problems of insufficient light-shielding effect and dielectric constant of polyimide films were solved, achieving low dielectric constant and low Tg characteristics, making them suitable for 5G frequency electronic products, reducing production energy consumption and broadening the application range.
Patent Information
- Application Number
- CN202410946326.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing polyimide films are inadequate in terms of light-shielding effect, dielectric constant, and high-temperature lamination, and cannot meet the high-frequency performance requirements of 5G and above frequency electronic products. Furthermore, the high-temperature lamination process consumes a lot of energy and causes thermal damage to materials and components.
A modified black polyimide layer is used, comprising soluble polyimide liquid, high-temperature resistant epoxy modified silicone resin, ion scavenger, antioxidant, graphene, aluminum hydroxide, fluorinated resin, acid anhydride polymer material, diphenyl anhydride diamine, matte powder, diluent and silicon dioxide or zirconium oxide, and is processed through a specific process to form an opaque, low dielectric, low Tg polyimide film.
This technology achieves the light-shielding properties, low dielectric constant, and low Tg characteristics of polyimide films, reducing signal attenuation, decreasing production energy consumption, broadening the application range, and making it suitable for more temperature-sensitive scenarios.
Smart Images

Figure SMS_4 
Figure SMS_5 
Figure SMS_6
Abstract
Description
Technical Field
[0001] This invention provides an opaque, low-dielectric, low-Tg polyimide film and its preparation method, relating to the field of special film material preparation technology. Background Technology
[0002] Polyimide film, as a high-performance insulating material, is widely used in electronics, aerospace, automotive, and other fields. However, with continuous technological advancements, the market has placed higher demands on this material. Currently available polyimide films such as YPI (yellow and gold), BPI, WPI (white), and TPI (high-temperature lamination), while performing well in some aspects, still have some significant shortcomings.
[0003] Lack of light-blocking effect: Existing polyimide films generally lack light-blocking properties. When testing mobile phone LED lights attached to the film surface, if light can penetrate the film and form light spots, it indicates that its light-blocking performance is unqualified. This defect may cause performance degradation or even malfunction in electronic products that require strict light control, such as mobile phone screens and photoelectric sensors. Therefore, developing polyimide films with light-blocking properties is particularly important.
[0004] Excessively high dielectric constant: Currently available polyimide films typically have a dielectric constant greater than 3.2. In high-frequency signal transmission, an excessively high dielectric constant leads to faster signal attenuation and reduced transmission efficiency. This is a significant issue for electronic products operating at 5G and higher frequencies. 5G technology places extremely high demands on the high-frequency performance of materials; therefore, reducing the dielectric constant of polyimide films and improving their high-frequency performance is crucial to meeting the needs of next-generation electronic products.
[0005] Limitations of high-temperature lamination: TPI films must be thermally laminated at high temperatures (lamination temperature > 320°C) to fuse their surface T-layer. This not only increases energy consumption during production but can also cause thermal damage to the material itself and other electronic components. Furthermore, high-temperature lamination limits the use of TPI in certain temperature-sensitive applications.
[0006] To address the aforementioned issues, developing a TBPI film with low dielectric constant, low TG (suitable for low-temperature bonding), and light-shielding properties is particularly important. Materials with low dielectric constants exhibit lower signal attenuation in high-frequency signal transmission, which is crucial for 5G and higher frequency electronic products. Simultaneously, low TG means the material can be bonded at lower temperatures, reducing energy consumption during production and broadening its application range to accommodate more temperature-sensitive scenarios.
[0007] Developing TBPI films faces numerous challenges. First, introducing light-blocking properties while maintaining the original excellent properties of polyimide films is a technical challenge. Second, reducing the dielectric constant while ensuring that other properties such as mechanical strength and heat resistance are not affected is also a problem that needs to be overcome. Finally, ensuring the stability and reliability of the film while reducing its dielectric constant (TG) is another challenge that needs to be addressed.
[0008] With the rapid development and widespread adoption of 5G technology, the demand for high-frequency polyimide films will continue to grow. TBPI film, as a novel high-performance material, is expected to find widespread application in electronic products operating at 5G and higher frequencies. Furthermore, its excellent light-shielding properties and low triglyceride (TG) characteristics will also make it a promising candidate for applications in optoelectronic sensors, mobile phone screens, and other fields.
[0009] To address the shortcomings of existing polyimide films in terms of light-shielding effect, dielectric constant, and high-temperature lamination, developing a TBPI film with low dielectric constant, low TG, and light-shielding effect has significant market value and practical implications. This requires not only the continued efforts and innovation of materials scientists but also close cooperation across the entire industry chain to jointly promote the research and application of this new material. Summary of the Invention
[0010] To address the aforementioned problems, the present invention provides a modified black polyimide layer for preparing light-shielding polyimide films. The resulting product exhibits excellent light-shielding properties and simultaneously achieves reduced dielectric constant and low TG. The specific solution is as follows:
[0011] An opaque, low-dielectric-weight, low-Tg polyimide film includes a modified black polyimide layer as a thermoplastic layer, wherein the modified black polyimide layer comprises the following components: soluble polyimide liquid, high-temperature resistant epoxy-modified silicone resin, ion scavenger, antioxidant, curing agent, graphene, aluminum hydroxide, fluorinated resin, acid anhydride polymer material, diphenyl anhydride diamine, matting powder, diluent, and also includes silicon dioxide or zirconium oxide.
[0012] Preferably, the modified black polyimide layer comprises, by mass parts: 30-120 parts soluble polyimide liquid, 10-35 parts high-temperature resistant epoxy modified silicone resin, 0.3-1 parts ion scavenger, 0.1-1 parts antioxidant, 10-15 parts curing agent, 10-15 parts graphene, 15-35 parts aluminum hydroxide, 10-35 parts fluorinated resin, 10-35 parts acid anhydride polymer material, 5-15 parts diphenyl anhydride diamine, 5-15 parts matting powder, and diluent as needed, and further comprises 10-35 parts silicon dioxide or zirconium oxide.
[0013] Preferably, in the modified black polyimide layer, the mass ratio of the high-temperature resistant epoxy-modified silicone resin to the fluorinated resin is 10:10 or 35:15, based on the mass parts of each component.
[0014] Preferably, the opaque, low-dielectric, low-Tg polyimide film further includes a PI film layer.
[0015] The preparation method of the above-mentioned opaque, low-dielectric, low-Tg polyimide film includes the following steps:
[0016] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0017] S2. Disperse the matte powder and aluminum hydroxide in a diluent using ultrasound, and then premix with soluble polyimide solution.
[0018] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, add ion scavenging agent, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silicon dioxide or zirconium oxide, and mix to obtain slurry;
[0019] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0020] Preferably, the concentrations of the solutions of the fluorinated resin and the epoxy-modified silicone resin in S1 are controlled at 10-20 wt%.
[0021] Preferably, the stirring and dissolving process described in S1 involves stirring with a magnetic stirrer at room temperature for 2-3 hours to ensure complete dissolution of the resin.
[0022] Preferably, the mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution of S1 is 10:10 or 35:15.
[0023] Preferably, S1 uses ultrasonic treatment with an ultrasonic power of 100-200W, a frequency of 20-40kHz, and a treatment time of 30-60min.
[0024] Preferably, the mechanical stirring speed in S1 is 300-500 rpm, the stirring is carried out at room temperature, and the stirring time is 4-6 hours.
[0025] Preferably, the ultrasonic dispersion in S2 has an ultrasonic power of 100-200W, a frequency of 20-40kHz, and a duration of 30-45min.
[0026] Preferably, the premixing described in S2 is performed by stirring at room temperature for 2-3 hours using a magnetic stirrer.
[0027] Preferably, the mixing described in S3 is carried out using a mechanical stirrer at a speed of 300-500 rpm at room temperature for 4-5 hours.
[0028] Preferably, in step S4, the coating is applied to the surface of the polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one or both sides of the polyimide film.
[0029] Preferably, the coating method in S4 includes one or more of the following: scraping, dipping, spraying, spin coating, casting, and rolling; the curing process involves standing at room temperature for 12-18 hours, gradually increasing the temperature to 55-60°C and holding for 2-2.5 hours, and further increasing the temperature to 110-120°C and holding for 2-2.5 hours.
[0030] Preferably, in S2, the ratio of aluminum hydroxide to diluent is 1:5 to 1:10 (mass ratio).
[0031] Preferably, the high-temperature resistant epoxy-modified silicone resin includes one or more of high-temperature resistant epoxy-modified silicone resin, siloxane-modified epoxy resin, and silane-modified epoxy resin; the ion scavenger includes one or more of ion exchange resin, chelating agent, ion-selective resin, zeolite, and polymer adsorbent; the antioxidant includes one or more of antioxidant L1010, butylated hydroxytoluene, tetrakis(methylene(3,5-di-tert-butyl-4-hydroxyhydroxycinnamate))methane, phenolic antioxidants, and thioester antioxidants; the curing agent includes curing agent 4,4'-diaminodiphenylmethane, The curing agent comprises one or more of aromatic amine curing agents, acid anhydride curing agents, and epoxy functional curing agents; the fluorinated resin comprises one or more of fluorinated polymers, perfluoropolyethers, fluorosilicone resins, and fluorinated acrylic resins; the acid anhydride polymeric material comprises one or more of acid anhydride modified polymers, maleic anhydride modified resins, phthalic anhydride modified polymers, and nademethyl anhydride modified polymers; the matting powder comprises one or more of matting agents, silica matting agents, wax-based matting agents, and polymer matting agents; the diluent comprises dimethylformamide (DMF) or cyclohexanone (MEK).
[0032] The beneficial effects of this invention are as follows:
[0033] In the polyimide film preparation method provided by the present invention, the transmittance, dielectric constant and TG of the material are first controlled by the innovative formulation; on this basis, the above parameters are further adjusted by optimizing the material treatment method in the preparation process, and an opaque, low dielectric and low Tg polyimide film is obtained. Detailed Implementation
[0034] The technical solutions in the embodiments of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this application.
[0036] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, and the test materials used in the following examples are all commercially available. The soluble polyimide liquid used in the following examples and comparative examples is Ube SP1, the high-temperature resistant epoxy-modified silicone resin is phenolic resin PMC-T383, the ion scavenger is IXE-100, the antioxidant is antioxidant L1010, the curing agent is Ube SP2, and the fluorinated resin is... 500 (Kaina 500), an anhydride-based polymer material is maleic anhydride-modified polyethylene. EMB226D, matte powder is Ropaque, a silica matte agent. TM Ultra E, with dimethylformamide (DMF) as the diluent and silica as the base material. 200, graphene D50 = less than 0.1 μm particle size. The polyimide film used is SKC black matte polyimide film.
[0037] Example 1: Preparation of opaque, low-dielectric, low-Tg polyimide film:
[0038] Formula: 120 parts soluble polyimide liquid, 10 parts high-temperature resistant epoxy modified silicone resin, 0.3 parts ion capture agent, 0.1 parts antioxidant, 10 parts curing agent, 10 parts graphene, 15 parts aluminum hydroxide, 10 parts acid anhydride polymer material, 5 parts diphenyl anhydride diamine, 5 parts matting powder, diluent as needed, and also includes 10 parts silicon dioxide or zirconium oxide.
[0039] Preparation process:
[0040] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0041] S2. Disperse the matte powder and aluminum hydroxide in a diluent using ultrasound, and then premix with soluble polyimide solution.
[0042] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0043] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0044] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 20 wt%.
[0045] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0046] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 10:10.
[0047] S1 describes the use of ultrasonic processing with an ultrasonic power of 200W, a frequency of 40kHz, and a processing time of 30min.
[0048] The mechanical stirring speed of S1 is 500 rpm, and the stirring time is 4 hours at room temperature.
[0049] The ultrasonic dispersion described in S2 has an ultrasonic power of 200W, a frequency of 40kHz, and a duration of 30min.
[0050] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0051] In S2, the ratio of aluminum hydroxide to diluent is 1:5 (mass ratio).
[0052] The mixture described in S3 was stirred at 500 rpm for 4 hours at room temperature using a mechanical stirrer.
[0053] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0054] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0055] Example 2: Preparation of opaque, low-dielectric, low-Tg polyimide films:
[0056] Formula: 120 parts soluble polyimide liquid, 30 parts high-temperature resistant epoxy modified silicone resin, 0.5 parts ion capture agent, 0.5 parts antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 35 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 35 parts silicon dioxide or zirconium oxide.
[0057] Preparation process:
[0058] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0059] S2. Disperse the matte powder and aluminum hydroxide in a diluent using ultrasound, and then premix with soluble polyimide solution.
[0060] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0061] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0062] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 10 wt%.
[0063] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 2 hours to ensure the resin is completely dissolved.
[0064] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 10:10.
[0065] S1 describes the use of ultrasonic processing with an ultrasonic power of 100W, a frequency of 20kHz, and a processing time of 60min.
[0066] The mechanical stirring speed of S1 is 300 rpm, and the stirring time is 6 hours at room temperature.
[0067] The ultrasonic dispersion described in S2 has an ultrasonic power of 100W, a frequency of 20kHz, and a duration of 45min.
[0068] The premix described in S2 is stirred at room temperature for 2 hours using a magnetic stirrer.
[0069] In S2, the ratio of aluminum hydroxide to diluent is 1:10 (mass ratio).
[0070] The mixture described in S3 is stirred at 300 rpm for 5 hours at room temperature using a mechanical stirrer.
[0071] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0072] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0073] Example 3: Preparation of opaque, low-dielectric, low-Tg polyimide films:
[0074] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0075] Preparation process:
[0076] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0077] S2. Disperse the matte powder and aluminum hydroxide in a diluent using ultrasound, and then premix with soluble polyimide solution.
[0078] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0079] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0080] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0081] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0082] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 10:10.
[0083] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0084] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0085] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0086] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0087] In S2, the ratio of aluminum hydroxide to diluent is 1:8 (mass ratio).
[0088] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0089] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0090] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0091] Example 4: Preparation of opaque, low-dielectric, low-Tg polyimide films:
[0092] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0093] Preparation process:
[0094] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0095] S2. Disperse the matte powder and aluminum hydroxide in a diluent using ultrasound, and then premix with soluble polyimide solution.
[0096] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0097] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0098] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0099] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0100] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 35:15.
[0101] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0102] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0103] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0104] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0105] In S2, the ratio of aluminum hydroxide to diluent is 1:8 (mass ratio).
[0106] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0107] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0108] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0109] Preparation of polyimide film in Comparative Example 1 (the difference from Example 4 is that S1 pretreatment and premixing are not performed):
[0110] Preparation of polyimide films:
[0111] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0112] Preparation process:
[0113] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. After ultrasonic treatment of the two resin solutions, transfer them to the reaction vessel and mechanically stir them respectively.
[0114] S2. Disperse the matte powder and aluminum hydroxide in a diluent using ultrasound, and then premix with soluble polyimide solution.
[0115] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0116] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0117] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0118] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0119] The mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 35:15.
[0120] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0121] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0122] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0123] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0124] In S2, the ratio of aluminum hydroxide to diluent is 1:8 (mass ratio).
[0125] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0126] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0127] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0128] Preparation of polyimide film in Comparative Example 2 (the difference from Example 4 is that S2 premixing is not performed):
[0129] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0130] Preparation process:
[0131] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0132] S2. Take the matte powder, aluminum hydroxide, soluble polyimide solution and diluent according to the amounts used in Example 4, wherein the diluent is ultrasonically treated according to the steps in Example 4.
[0133] S3. Add the mixture or raw materials obtained from S1 and S2 to the reaction vessel in the required proportion, add ion scavenging agent, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0134] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0135] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0136] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0137] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 35:15.
[0138] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0139] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0140] The ultrasound described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0141] In S2, the ratio of aluminum hydroxide to diluent is 1:8 (mass ratio).
[0142] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0143] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0144] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0145] Preparation of polyimide film in Comparative Example 3 (the difference from Example 4 is that matte powder is not premixed in S2 premixing):
[0146] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0147] Preparation process:
[0148] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0149] S2. Disperse aluminum hydroxide in a diluent using ultrasound, and then premix it with soluble polyimide solution.
[0150] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add matte powder, ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0151] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0152] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0153] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0154] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 35:15.
[0155] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0156] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0157] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0158] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0159] The amount of diluent used in S2 is the same as in Example 4.
[0160] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0161] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0162] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0163] Preparation of polyimide film in Comparative Example 4 (the difference from Example 4 is that aluminum hydroxide and soluble polyimide solution are not premixed in S2 premixing):
[0164] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0165] Preparation process:
[0166] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0167] S2. The matte powder is ultrasonically dispersed in a diluent and premixed.
[0168] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add aluminum hydroxide, soluble polyimide solution, ion capture agent, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silicon dioxide, and mix to obtain slurry;
[0169] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0170] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0171] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0172] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 35:15.
[0173] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0174] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0175] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0176] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0177] The amount of diluent used in S2 is the same as in Example 4.
[0178] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0179] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0180] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0181] Preparation of polyimide film in Comparative Example 5 (the difference from Example 4 is that in S2 premixing, the matte powder was premixed separately, and the aluminum hydroxide and soluble polyimide solution were premixed separately):
[0182] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0183] Preparation process:
[0184] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. Mix the two resin solutions, treat them with ultrasound, and then transfer them to a reaction vessel for mechanical stirring.
[0185] S2. The matte powder is ultrasonically dispersed in a diluent and premixed; aluminum hydroxide is ultrasonically dispersed in a diluent and premixed with soluble polyimide solution.
[0186] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0187] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0188] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0189] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0190] The mass ratio of fluorinated resin to epoxy-modified silicone resin in the mixed solution described in S1 is 35:15.
[0191] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0192] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0193] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0194] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0195] The total amount of diluent used in S2 is the same as in Example 4, wherein the matte powder premix uses 50% of the diluent used in S2.
[0196] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0197] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0198] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0199] Preparation of polyimide film in Comparative Example 6 (the difference from Example 4 is that S1 premixing and S2 premixing are not performed):
[0200] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0201] Preparation process:
[0202] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. After ultrasonic treatment of the two resin solutions, transfer them to the reaction vessel and mechanically stir them respectively.
[0203] S2. Take aluminum hydroxide, matte powder, soluble polyimide solution and diluent according to the amounts used in Example 4, wherein the diluent is ultrasonically treated according to the steps in Example 4.
[0204] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0205] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0206] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0207] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0208] The mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 35:15.
[0209] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0210] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0211] The ultrasound described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0212] In S2, the ratio of aluminum hydroxide to diluent is 1:8 (mass ratio).
[0213] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0214] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0215] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0216] Preparation of polyimide film in Comparative Example 7 (the difference from Example 4 is that S1 premixing was not performed, and matte powder was not premixed in S2 premixing):
[0217] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0218] Preparation process:
[0219] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. After ultrasonic treatment of the two resin solutions, transfer them to the reaction vessel and mechanically stir them respectively.
[0220] S2. Disperse aluminum hydroxide in a diluent using ultrasound, and then premix it with soluble polyimide solution.
[0221] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add matte powder, ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0222] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0223] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0224] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0225] The mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 35:15.
[0226] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0227] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0228] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0229] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0230] The diluent described in S3 is treated with ultrasound at a power of 150W, a frequency of 30kHz, and a treatment time of 40min.
[0231] The amount of diluent used in S2 is the same as in Example 4.
[0232] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0233] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0234] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0235] Preparation of polyimide film in Comparative Example 8 (the difference from Example 4 is that S1 premixing was not performed, and matte powder was not premixed in S2 premixing):
[0236] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0237] Preparation process:
[0238] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. After ultrasonic treatment of the two resin solutions, transfer them to the reaction vessel and mechanically stir them respectively.
[0239] S2. The matte powder is ultrasonically dispersed in a diluent and premixed.
[0240] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add aluminum hydroxide, soluble polyimide solution, ion capture agent, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silicon dioxide, and mix to obtain slurry;
[0241] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0242] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0243] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0244] The mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 35:15.
[0245] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0246] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0247] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0248] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0249] The amount of diluent used in S2 is the same as in Example 4.
[0250] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0251] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0252] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0253] Preparation of polyimide film in Comparative Example 9 (the difference from Example 4 is that S1 premixing is not performed; in S2 premixing, the matte powder, aluminum hydroxide, and soluble polyimide solution are premixed separately):
[0254] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy modified silicone resin, 1 part ion capture agent, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silicon dioxide or zirconium oxide.
[0255] Preparation process:
[0256] S1. Dissolve the fluorinated resin and epoxy-modified silicone resin separately in a diluent to prepare solutions of fluorinated resin and epoxy-modified silicone resin respectively. Stir and dissolve them separately. After ultrasonic treatment of the two resin solutions, transfer them to the reaction vessel and mechanically stir them respectively.
[0257] S2. The matte powder is ultrasonically dispersed in a diluent and premixed; aluminum hydroxide is ultrasonically dispersed in a diluent and premixed with soluble polyimide solution.
[0258] S3. Add the mixture obtained from S1 and S2 to the reaction vessel in the required proportion, and add ion scavenger, antioxidant, graphene, acid anhydride polymer material, diphenyl anhydride diamine, curing agent and silica, and mix to obtain slurry;
[0259] S4. The obtained slurry is coated on the surface of a polyimide film, and after curing, an opaque, low-medium, low-Tg polyimide film is obtained.
[0260] The concentrations of the solutions containing fluorinated resin and epoxy-modified silicone resin described in S1 are each controlled at 15 wt%.
[0261] S1 describes stirring and dissolving the resin. Use a magnetic stirrer to stir at room temperature for 3 hours to ensure the resin is completely dissolved.
[0262] The mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 35:15.
[0263] S1 describes the use of ultrasonic processing with an ultrasonic power of 150W, a frequency of 30kHz, and a processing time of 40min.
[0264] The mechanical stirring speed of S1 is 400 rpm, and the stirring time is 5 hours at room temperature.
[0265] The ultrasonic dispersion described in S2 has an ultrasonic power of 150W, a frequency of 30kHz, and a duration of 40min.
[0266] The premix described in S2 is stirred at room temperature for 3 hours using a magnetic stirrer.
[0267] In S2, the ratio of aluminum hydroxide to diluent is 1:8 (mass ratio).
[0268] The mixture described in S3 was stirred at 400 rpm for 4 hours at room temperature using a mechanical stirrer.
[0269] S4 refers to coating on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0270] The coating method described in S4 includes spin coating; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0271] Preparation of polyimide film in Comparative Example 10 (the difference from Comparative Example 4 is that all raw materials are directly mixed):
[0272] Formula: 120 parts soluble polyimide liquid, 20 parts high-temperature resistant epoxy-modified silicone resin, 1 part ion scavenger, 1 part antioxidant, 15 parts curing agent, 15 parts graphene, 25 parts aluminum hydroxide, 25 parts acid anhydride polymer material, 15 parts diphenyl anhydride diamine, 15 parts matting powder, diluent as needed, and also includes 25 parts silica or zirconium oxide. The mass ratio of fluorinated resin to epoxy-modified silicone resin is 35:15.
[0273] Preparation process:
[0274] Add the total amount of diluent according to the dosage in Example 4. Mix all the components in the above formula and disperse in a high-speed disperser for 2 hours at a speed of 800 rpm. To avoid excessive temperature during the dispersion process, add a constant temperature water bath to maintain the temperature at 30°C to prepare a slurry. Coat the obtained slurry onto the surface of a polyimide film and cure it to obtain a polyimide film.
[0275] The coating is applied to the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; the coating is applied to one side of the polyimide film.
[0276] The coating is applied using a spin coating method; the curing process involves standing at room temperature for 12 hours, gradually increasing the temperature to 60°C and holding for 2 hours, and then further increasing the temperature to 120°C and holding for 2 hours. The coating thickness is 25 μm.
[0277] Comparative Example 11: Preparation of polyimide film:
[0278] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 40:50.
[0279] Comparative Example 12: Preparation of polyimide film:
[0280] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 45:50.
[0281] Comparative Example 13: Preparation of polyimide film:
[0282] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 65:30.
[0283] Comparative Example 14: Preparation of polyimide film:
[0284] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 60:30.
[0285] Comparative Example 15: Preparation of polyimide film:
[0286] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 50:30.
[0287] Comparative Example 16: Preparation of polyimide film:
[0288] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 40:30.
[0289] Comparative Example 17: Preparation of polyimide film:
[0290] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 35:30.
[0291] Preparation of Comparative Example 18: Polyimide Film
[0292] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 75:30.
[0293] Comparative Example 19: Preparation of polyimide film:
[0294] The difference from Example 4 is that the mass ratio of the fluorinated resin to the epoxy-modified silicone resin in S1 is 80:30.
[0295] Comparative Example 20: Preparation of polyimide film:
[0296] The difference from Comparative Example 10 is that the formulation does not include fluorinated resin.
[0297] Comparative Example 21: Preparation of polyimide film:
[0298] The difference from Comparative Example 10 is that the formulation does not include aluminum hydroxide.
[0299] Preparation of polyimide film in Comparative Example 22:
[0300] The difference from Comparative Example 10 is that the formulation does not include silicon dioxide.
[0301] Preparation of polyimide film in Comparative Example 23:
[0302] The difference from Comparative Example 10 is that the formulation does not include acid anhydride polymers.
[0303] Performance testing:
[0304] The samples obtained in Example 1 (prepared with thicknesses of 25 μm and 38 μm respectively) were tested, and the results are shown in Table 1.
[0305] Table 1. Routine testing of samples from Example 1
[0306]
[0307]
[0308] The transmittance, dielectric constant, and TG of the films obtained from all the above embodiments and comparative examples were tested, and the results are shown in Table 2.
[0309] Table 2 Detection Results
[0310]
[0311]
[0312] As can be seen from the above results, firstly, the formulation provided by the present invention can provide lower transmittance, dielectric constant, and TG; secondly, the blending of fluorinated resin and epoxy resin in step S1 does not significantly contribute to the reduction of the above three parameters; thirdly, when aluminum hydroxide, polyimide, and matte powder are premixed simultaneously, this step makes a very significant contribution to the reduction of the above three parameters, but this phenomenon is not observed when aluminum hydroxide and polyimide are pretreated alone or when matte powder and diluent are pretreated alone. In the work of other researchers, we know that pre-blending fluorinated resins with epoxy-modified silicone resins can control the dielectric constant of the product to some extent, but this effect is not significant in the work of this invention. Furthermore, we know that pre-mixing aluminum hydroxide, polyimide, or matte powder with a diluent may improve the uniformity of mixing, the dispersibility of components, or the compatibility between components. However, in the work of this invention, pre-mixing alone does not seem to have an effect. Therefore, it is clear that the principle behind pre-mixing aluminum hydroxide, polyimide, or matte powder with a diluent in step S2, thereby affecting the dielectric constant and TG of the final film, is not based on affecting dispersibility or compatibility. Simultaneously, given that four components are blended in step S2, the effect of adding components in step S1 on the dielectric constant and GT becomes more significant. When aluminum hydroxide, polyimide, and matting powder are premixed simultaneously, these components form tighter interfacial interactions. Aluminum hydroxide particles create more interfaces within the polyimide matrix, increasing the interfacial density and leading to a decrease in dielectric constant and TG. This enhanced interfacial interaction may not be noticeable with individual premixing. The addition of aluminum hydroxide and matting powder may alter the formation process of the polyimide network structure. Through premixing, these inorganic fillers may form a more uniform distribution within the polyimide matrix, inhibiting the formation of high-density cross-linked structures and thus reducing TG and dielectric constant. Premixing may also alter the surface chemistry of aluminum hydroxide, polyimide, and matting powder, making them more readily involved in chemical reactions during subsequent curing. Functional groups on the surfaces of aluminum hydroxide and matting powder may react with the polyimide matrix to form new chemical bonds, thus affecting the dielectric constant and TG of the film. The film exhibits the lowest dielectric constant and TG when the mass ratio of fluorinated resin to epoxy-modified silicone resin is 35:15 or 1:1. If the mass ratio of the two components is greater than 35:15, less than 1:1, or between 35:15 and 1:1, the dielectric constant of the film increases, while the TG changes little. This may be because at a mass ratio of 35:15 or 1:1, the fluorinated resin and the epoxy-modified silicone resin may form optimal interactions and interfacial compatibility at the molecular level, resulting in a uniform microphase separation structure, or providing optimal freedom of movement for polymer chain segments. When the mass ratio deviates from this range, this optimal balance is disrupted, thus the dielectric constant changes significantly. However, because the overall crosslinking density of the structure does not change significantly, the TG change is not significant.
[0313] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
[0314] The present invention and its embodiments have been described above. This description is not restrictive, and what is shown is only a part of the embodiments of the present invention. The actual application is not limited to this. In conclusion, if those skilled in the art are inspired by this description and design similar methods and embodiments without departing from the spirit of the present invention, they should all fall within the protection scope of the present invention.
Claims
1. A light-proof low-dielectric low-Tg polyimide film, characterized in that: The invention comprises a modified black polyimide layer as a thermoplastic layer, wherein the modified black polyimide layer comprises the following components: soluble polyimide liquid, high temperature resistant epoxy modified silicone resin, ion capture agent, antioxidant, curing agent, graphene, aluminum hydroxide, fluorine-containing resin, acid anhydride polymer material, diphenyl anhydride diamine, matte powder, diluent, and also comprises silicon dioxide or zirconium oxide.
2. The light-proof low-dielectric low-Tg polyimide film according to claim 1, characterized in that: The light-proof low-dielectric low-Tg polyimide film also includes a PI film layer.
3. A method for preparing the light-impermeable low-dielectric low-Tg polyimide film according to claim 1 or 2, characterized in that: The following steps are involved: S1, dissolving the fluorine-containing resin and the epoxy-modified silicone resin in a diluent to prepare solutions of the fluorine-containing resin and the epoxy-modified silicone resin, respectively, stirring and dissolving them, mixing the two resin solutions, and transferring them to a reaction kettle after ultrasonic treatment, and mechanically stirring; S2, subjecting matte powder and aluminum hydroxide to ultrasonic dispersion in a diluent, and adding soluble polyimide liquid to premix; S3, adding the mixture obtained in S1 and S2 into a reaction kettle in a required proportion, adding an ion capture agent, an antioxidant, graphene, anhydride polymer material, diphenyl anhydride diamine, a curing agent and silicon dioxide or zirconium oxide, and mixing to obtain a slurry; S4. The obtained slurry is coated on the surface of the polyimide film, and after curing, an opaque low-dielectric low-Tg polyimide film is obtained.
4. The method for preparing a light-tight low-dielectric low-Tg polyimide film according to claim 3, characterized in that: The concentrations of the solutions of the fluorine-containing resin and the epoxy-modified silicone resin in S1 are controlled at 10-20 wt % respectively; the mass ratio of the fluorine-containing resin to the epoxy-modified silicone resin in the mixed solution in S1 is 10:10 or 35:
15.
5. The method for preparing the light-proof low-dielectric low-Tg polyimide film according to claim 3, characterized in that: The stirring dissolution described in S1 is carried out using a magnetic stirrer to stir at room temperature for 2-3 hours; the ultrasonic treatment described in S1 has an ultrasonic power of 100-200W, a frequency of 20-40kHz, and a treatment time of 30-60min; the mechanical stirring speed described in S1 is 300-500rpm, and the stirring time is 4-6h at room temperature.
6. The method for preparing the light-proof low-dielectric low-Tg polyimide film according to claim 3, characterized in that: The ultrasonic dispersion described in S2 has an ultrasonic power of 100-200 W, a frequency of 20-40 kHz, and a time of 30-45 min. The premixing described in S2 is stirred at room temperature for 2-3 h using a magnetic stirrer.
7. The method for preparing a light-tight low-dielectric low-Tg polyimide film according to claim 3, characterized in that: The mixture as described in S3 was stirred at room temperature for 4-5 hours at a speed of 300-500 rpm using a mechanical stirrer.
8. The method for preparing a light-tight low-dielectric low-Tg polyimide film according to claim 3, characterized in that: S3 is coated on the surface of a polyimide film, wherein the polyimide film is a matte polyimide film or a glossy polyimide film; and the coating is applied on one side or both sides of the polyimide film.
9. The method for preparing a light-tight low-dielectric low-Tg polyimide film according to claim 3, characterized in that: The coating method in S4 includes one or more of blade coating, dip coating, spray coating, spin coating, cast coating and roll coating.
10. The method for preparing a light-tight low-dielectric low-Tg polyimide film according to claim 3, characterized in that: S4 is cured, and the mixture is allowed to stand at room temperature for 12-18 hours, and then gradually heated to 55-60°C and maintained for 2-2.5 hours, and further heated to 110-120°C and maintained for 2-2.5 hours.
Citation Information
Patent Citations
Low-dielectric constant polyimide and preparation method thereof
CN104530703A
Preparation method of black low-gloss polyimide film
CN108047717A
Black polyimide microsphere, preparation method thereof and preparation method of thin film having same
CN109438703A
Black polyimide film with high electrical strength and high shielding property, and preparation process thereof
CN111793360A
Preparation method of black matte polyimide film
CN112920435A
Cited By
High-heat-resistance copper-clad plate and preparation process thereof
CN119317034A
A high heat-resistant copper-clad laminate and its preparation process
CN119317034B