Display device including window and method for manufacturing window
Through multi-layer coating technology and spraying method, the impact resistance coating is formed on the window of the flexible display device, which solves the problem of insufficient impact resistance and flatness in the prior art, and significantly improves the impact resistance and optical of the display device. characteristic.
Patent Information
- Application Number
- CN202410642084.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
The windows of the existing flexible display device are insufficient in impact resistance and flatness when facing external impact, resulting in easy damage to the display panel, and it is difficult for the existing manufacturing method to effectively improve its impact resistance and flatness.
Using a multi-layer coating method, multiple coatings are formed on the substrate by plasma treatment and spraying, and the same or different materials are applied along the zigzag path to form an impact-resistant coating with a uniform top surface. Ensure that the thickness of each layer is within a specific range, reducing or eliminating edge beading phenomena and improving optical flatness.
The impact resistance and flatness of the window of the flexible display device are significantly improved, the risk of damage to the display panel by external impact is reduced, the optical characteristics of the sensor area are improved, and the reliability and service life of the display device are enhanced.
Smart Images

Figure CN119028225A_ABST
Abstract
Description
[0001] This application claims priority to and all benefits derived from Korean Patent Application No. 10-2023-0068687, filed on May 26, 2023, the contents of which are incorporated herein by reference in their entirety. Technical Field
[0002] The disclosed embodiments described herein relate to a display device including a window having improved impact resistance and flatness and a method for manufacturing the window. Background Art
[0003] The display device provides information to the user by displaying various images on the display screen. Generally, the display device displays information within the specified screen. Recently, a flexible display device including a foldable flexible display panel is being developed. The flexible display device may include a flexible window. Unlike a rigid display device, a flexible display device may be folded, curled, or bent. A flexible display device whose shape can be changed variously may be in a size smaller than the screen size in the unfolded state, so that user convenience may be improved. Summary of the invention
[0004] The disclosed embodiments provide a display device including a window having improved impact resistance and flatness, and a method for manufacturing the window.
[0005] According to an embodiment, a method for manufacturing a window includes the following steps: performing plasma treatment on a surface of a substrate; performing a first coating operation by applying a first solution onto the substrate to form a first portion; performing a second coating operation by applying a second solution onto the first portion to form a second portion; performing a third coating operation by applying a third solution onto the second portion to form a third portion; and forming a first coating layer by simultaneously curing the first portion to the third portion.
[0006] In an embodiment, the first solution and the second solution may include the same material as each other.
[0007] In an embodiment, the first portion may have a thickness in a range of about 6.7 micrometers (μm) to about 10 μm, the second portion may have a thickness in a range of about 6.7 μm to about 10 μm, and the third portion may have a thickness in a range of about 6.7 μm to about 10 μm.
[0008] In an embodiment, performing the first coating operation may include coating the first solution along a path in a zigzag shape along the first direction by using a spray coating method.
[0009] In an embodiment, the second coating operation may be performed using a spray coating method, and the second coating operation may include coating the second solution along a path in a zigzag shape in a direction opposite to the first direction by using the spray coating method.
[0010] In an embodiment, the method may further include the following step: after forming the first coating layer, forming a second coating layer on the first coating layer.
[0011] In an embodiment, forming the second coating may include: performing plasma treatment on the surface of the first coating; forming a fourth portion by applying a fourth solution to the first coating; forming a fifth portion by applying a fifth solution to the fourth portion; forming a sixth portion by applying a sixth solution to the fifth portion; and simultaneously curing the fourth to sixth portions.
[0012] In an embodiment, each of the first coating layer and the second coating layer may have a thickness in a range of about 10 μm to about 20 μm.
[0013] In an embodiment, the method may further include the following step: after forming the first coating layer, forming a third coating layer under the substrate.
[0014] According to an embodiment, a method for manufacturing a window includes the following steps: performing plasma treatment on a surface of a substrate; performing a first coating operation by applying a first solution onto the substrate to form a first portion; forming a first layer by curing the first portion; performing plasma treatment on the surface of the first layer; performing a second coating operation by applying a second solution onto the first layer to form a second portion; and curing the second portion to form a second layer, wherein the first layer and the second layer together define a first coating layer.
[0015] In an embodiment, the first layer may have a thickness in a range of about 10 μm to about 15 μm.
[0016] In an embodiment, the second layer may have a thickness in a range of about 10 μm to about 15 μm.
[0017] In an embodiment, the first solution may not include a leveling agent, and the second solution may include a leveling agent.
[0018] In an embodiment, performing the first coating operation may include coating the first solution along a path in a zigzag shape along the first direction by using a spray coating method.
[0019] In an embodiment, performing the second coating operation may include coating the second solution along a path in a zigzag shape along the first direction by using a spray coating method.
[0020] In an embodiment, the method may further include the step of forming a second coating layer under the substrate after forming the first layer and forming the second layer.
[0021] According to an embodiment, a display device includes a display panel and a window disposed on the display panel, wherein the window includes a substrate and a first coating disposed on the substrate, the first coating is a solid layer formed by curing a solution, the solution has a viscosity in a range of approximately 6 centipoise (cp) to 10 cp, and a difference between a maximum value and a minimum value (peak-to-valley (PV) value) of a wavefront aberration of the first coating is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths.
[0022] In an embodiment, the first coating layer may have a thickness in a range of about 20 μm to about 30 μm.
[0023] In an embodiment, the first coating layer may include a first layer and a second layer stacked on each other, and the first layer and the second layer may include the same material as each other.
[0024] In an embodiment, the display device may further include a second coating layer disposed under the substrate and opposite to the first coating layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The above and other features of the disclosed embodiments will become apparent by describing the disclosed embodiments in detail with reference to the attached drawings.
[0026] Figure 1A is a perspective view of an unfolded electronic device according to a disclosed embodiment.
[0027] Figure 1B is a perspective view of a folded electronic device according to a disclosed embodiment.
[0028] Figure 2 is an exploded perspective view of an electronic device according to a disclosed embodiment.
[0029] Figure 3 According to the disclosed embodiment, Figure 2 A cross-sectional view of the display device and the camera module taken along line II' in FIG.
[0030] Figure 4 is a cross-sectional view showing a display panel according to a disclosed embodiment.
[0031] Figure 5 is a flow chart illustrating a method of manufacturing a window according to a disclosed embodiment.
[0032] Fig. 6A is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0033] Figure 6Bis a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0034] Figure 6C According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line.
[0035] Fig.6D is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0036] Fig. 6E According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line.
[0037] Fig. 6F is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0038] Figure 6G According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line.
[0039] Figure 6H is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0040] Fig.6I is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0041] Figure 6J is a perspective view showing a window according to a disclosed embodiment.
[0042] Fig. 7A is a graph showing the thickness of a coating based on the distance from the edge of a substrate according to disclosed embodiments.
[0043] Figure 7B is a graph showing the thickness of a coating based on the distance from the edge of a substrate according to disclosed embodiments.
[0044] Fig. 8A is a box plot showing PV values based on the number of applications according to the disclosed embodiment.
[0045] Figure 8B Shown are captured images of a window based on the number of coatings according to the disclosed embodiment.
[0046] Fig.9A is a box plot showing PV values based on the number of applications according to the disclosed embodiment.
[0047] Fig. 9BA photographed image of a window based on the number of coatings according to the disclosed embodiment may be shown.
[0048] Fig.10 is a flow chart illustrating a method of manufacturing a window according to a disclosed embodiment.
[0049] Fig.11A is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0050] Fig. 11B is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0051] Fig. 11C According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line.
[0052] FIG. 11D to FIG. 11F is a perspective view showing one step of a window manufacturing method according to a disclosed embodiment.
[0053] Fig.11G According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line.
[0054] Fig.11H is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0055] Fig.11I and Fig.11J is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0056] Fig. 12A is a box plot showing PV values based on the number of layers of coating according to disclosed embodiments.
[0057] Fig. 12B Shown are captured images of a window based on the number of layers of coating according to the disclosed embodiment.
[0058] Fig.13 is a box plot showing PV values for windows formed using a multi-stage coating method and a multi-layer coating method according to disclosed embodiments.
[0059] Fig.14 is a flow chart illustrating a method of manufacturing a window according to a disclosed embodiment.
[0060] FIG. 15A to FIG. 15M is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0061] Fig.16Ais a box plot showing PV values for each coating method according to disclosed embodiments.
[0062] Fig. 16B Captured images of the window for each coating method according to the disclosed embodiments are shown.
[0063] FIG. 17A to FIG. 17F A window according to a disclosed embodiment is shown. DETAILED DESCRIPTION
[0064] The invention will now be described more fully hereinafter with reference to the accompanying drawings, in which various embodiments are shown. However, the invention may be implemented in many different forms and should not be construed as limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete and will fully convey the scope of the invention to those skilled in the art.
[0065] Here, when a component (or region, layer, part, etc.) is referred to as being "on" another component, "connected to" or "coupled to" another component, it means that the component can be directly set on the other component / directly connected / directly coupled to the other component, or a third component can be set between the component and the other component.
[0066] The same reference numerals refer to the same components. In addition, in the drawings, for the effective description of the technical contents, the thickness, proportion and size of the components are exaggerated.
[0067] Terms such as first, second, etc. can be used to describe various components, but these components should not be limited by these terms. The above terms are only used to distinguish one component from another component. For example, without departing from the scope of the disclosure, a first component can be named a second component, and similarly, a second component can also be named a first component.
[0068] In addition, terms such as "under", "below", "beneath", "on", and "over" are used to describe the relationship of components shown in the drawings. The above terms are relative concepts and are described with reference to the directions indicated in the drawings.
[0069] The terms used herein are only used to describe the purpose of specific embodiments, and are not intended to be limited. As used herein, unless the context clearly indicates otherwise, "one", "one (kind / person)", "the (described)" and "at least one (kind / person)" do not represent the limitation of quantity, and are intended to include both the singular and the plural. Therefore, in the claims, mentioning "one (kind / person)" element and then mentioning "the (described)" element includes one element and multiple elements. For example, unless the context clearly indicates otherwise, "one (kind / person) element" has the same meaning as "at least one (kind / person) element". "At least one (kind / person)" should not be interpreted as being limited to "one" or "one (kind / person)". "Or" means "and / or". As used herein, the term "and / or" includes any combination and all combinations of one or more of the relevant listed items. It will also be understood that when the terms "include" or "comprising" and / or variations thereof are used in this specification, it indicates the presence of stated features, regions, wholes, steps, operations, elements and / or components, but does not exclude the presence or addition of one or more other features, regions, wholes, steps, operations, elements, components and / or groups thereof.
[0070] As used herein, "about" or "approximately" is inclusive of the stated value and means within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art, taking into account the measurement in question and errors associated with the measurement of the particular quantity (e.g., limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±30%, ±20%, ±10%, or ±5% of the stated value.
[0071] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the present disclosure belongs. It will also be understood that terms (such as those defined in general dictionaries) should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and will not be interpreted in an idealized or overly formal sense unless explicitly so defined herein.
[0072] Embodiments are described herein with reference to schematically illustrated cross-sectional views as idealized embodiments. As such, variations in the shapes of the illustrations due to, for example, manufacturing techniques and / or tolerances are to be expected. Therefore, the embodiments described herein should not be construed as being limited to the specific shapes of the regions as shown herein, but rather include deviations in shape due to, for example, manufacturing. For example, a region shown or described as flat may typically have rough and / or nonlinear features. In addition, the acute angles shown may be rounded. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to illustrate the precise shapes of the regions, and are not intended to limit the scope of the claims given.
[0073] Hereinafter, disclosed embodiments will be described in detail with reference to the accompanying drawings.
[0074] Figure 1A is a perspective view of an unfolded electronic device according to a disclosed embodiment, and Figure 1B is a perspective view of a folded electronic device according to a disclosed embodiment.
[0075] Reference Figure 1A and Figure 1B , an embodiment of the electronic device 1000 may include a display surface DS defined by a first direction DR1 and a second direction DR2 crossing the first direction DR1. The electronic device 1000 may provide an image IM to a user via the display surface DS.
[0076] The display surface DS may include a display area DA and a non-display area NDA around the display area DA. The display area DA may display an image IM, and the non-display area NDA may not display the image IM. The non-display area NDA may surround the display area DA. However, the disclosure may not be limited thereto, and the shape of the display area DA and the shape of the non-display area NDA may be modified variously.
[0077] Hereinafter, a direction substantially perpendicular to a plane defined by the first direction DR1 and the second direction DR2 may be defined as a third direction DR3. The third direction DR3 may be a thickness direction of the electronic device 1000. In addition, herein, "on a plane" or "when viewed in a plan view" may be defined as a state viewed in the third direction DR3.
[0078] The sensor area UA may be defined in the display area DA of the electronic device 1000. Figure 1A 1000 shows an embodiment in which a single sensor area UA is provided as an example, but the number of the sensor area UA is not limited thereto. The sensor area UA may be a part of the display area DA. The electronic device 1000 may display an image IM via the sensor area UA.
[0079] The electronic module may be disposed in an area overlapping the sensor area UA on a plane. The electronic module may receive an external input transmitted via the sensor area UA or provide an output via the sensor area UA. In an embodiment, for example, the electronic module may include a camera module, a sensor for measuring distance (such as a proximity sensor), a sensor for recognizing a body part of a user (e.g., a fingerprint, an iris, or a face), a small lamp for outputting light, etc., but may not be particularly limited.
[0080] In an embodiment of the electronic device 1000, a foldable area FA and a plurality of non-foldable areas NFA1 and NFA2 may be defined. The plurality of non-foldable areas NFA1 and NFA2 may include a first non-foldable area NFA1 and a second non-foldable area NFA2. The foldable area FA may be disposed between the first non-foldable area NFA1 and the second non-foldable area NFA2. The foldable area FA may be referred to as a foldable area, and the first non-foldable area NFA1 and the second non-foldable area NFA2 may be referred to as a first non-foldable area and a second non-foldable area, respectively.
[0081] The foldable area FA may be folded based on a folding axis FX parallel to the second direction DR2. When the electronic device 1000 is folded, the foldable area FA may have a predetermined curvature or a predetermined radius of curvature. The first non-foldable area NFA1 and the second non-foldable area NFA2 may face each other in a folded state, and the electronic device 1000 may be folded inwardly so that the display surface DS is not exposed to the outside.
[0082] The electronic device 1000 according to the disclosed embodiment can be folded outward so that the display surface DS is exposed to the outside. In the disclosed embodiment, the electronic device 1000 can be folded inward or folded outward from the unfolding operation, but may not be limited thereto. In the disclosed embodiment, the electronic device 1000 may be configured to select one of the unfolding operation, the inward folding operation, and the outward folding operation. In the disclosed embodiment, a plurality of folding axes may be defined in the electronic device 1000, and the electronic device 1000 may be folded inward or folded outward from the unfolding operation at each of the plurality of folding axes.
[0083] Figure 2 is an exploded perspective view of an electronic device according to a disclosed embodiment.
[0084] Reference Figure 2 , an embodiment of the electronic device 1000 may include a display device DD, a first electronic module EM1, a second electronic module EM2, a power module PM, and housings EDC1 and EDC2. The electronic device 1000 may further include a mechanical structure for controlling a folding operation of the display device DD.
[0085] The display device DD may include a window WIN and a display module DM. The window WIN may provide a front surface of the electronic device 1000. The display module DM may include at least a display panel DP. The display module DM may generate an image and sense an external input.
[0086] The display module DM may have a stack structure in which a plurality of components including the display panel DP are stacked. The stack structure of the display module DM will be described later.
[0087] In the embodiment of the display panel DP, the display areas DA (see FIG. Figure 1A ) and non-display area NDA (see Figure 1A ) corresponds to the display area DP-DA and the non-display area DP-NDA. Here, "a region / a portion and a region / a portion correspond to each other" means that they overlap each other, but is not limited to the case where they have the same area or size as each other.
[0088] The display area DP-DA may include a first area AA1 and a second area AA2. The first area AA1 may be aligned with the sensor area UA (see FIG. Figure 1A ) are overlapped or corresponded. In the disclosed embodiments, Figure 2 As shown in , the first area AA1 may have a circular shape, but the disclosure is not limited thereto. In an embodiment, for example, the first area AA1 may have various shapes (such as a polygon, an ellipse, a figure with at least one curved edge, or an irregular shape), but the disclosure may not be limited to one embodiment. The first area AA1 may be referred to as a component area, and the second area AA2 may be referred to as a main display area or a general display area.
[0089] The first area AA1 may have a greater transmittance than the second area AA2. In an embodiment, the resolution of the first area AA1 may be less than the resolution of the second area AA2. However, this is merely an example, and the first area AA1 according to the disclosed embodiment may have a greater transmittance than the second area AA2, but the resolution of the first area AA1 may be substantially the same as the resolution of the second area AA2.
[0090] On a plane, the first area AA1 may overlap a camera module CMM to be described later. According to the disclosed embodiment, a portion of the display panel DP corresponding to the first area AA1 may be removed.
[0091] The display module DM may include a driving chip DIC disposed in the non-display area DP-NDA. The display module DM may further include a flexible circuit film FCB coupled to the non-display area DP-NDA.
[0092] The driving chip DIC may include driving elements (eg, data driving circuits) for driving the pixels of the display panel DP. Figure 2 An embodiment having a structure in which the driving chip DIC is mounted on the display panel DP is shown, but the disclosure is not limited thereto. In the embodiment, for example, the driving chip DIC may be mounted on a flexible circuit film FCB.
[0093] The power module PM supplies power for overall operations of the electronic device 1000. The power module PM may include a conventional battery module.
[0094] The first electronic module EM1 and the second electronic module EM2 include various functional modules for operating the electronic device 1000. Each of the first electronic module EM1 and the second electronic module EM2 may be directly mounted on a motherboard electrically connected to the display panel DP, or mounted on a separate board and electrically connected to the motherboard via a connector (not shown). The first electronic module EM1 may include a control module, a wireless communication module, an image input module, an audio input module, a memory, an external interface, etc.
[0095] The second electronic module EM2 may include an audio output module, a light emitting module, a light receiving module, a camera module CMM, and the like.
[0096] The camera module CMM can capture still images and moving images. The camera module CMM may include a plurality of camera modules. Among the plurality of camera modules, some camera modules CMM may overlap with the first area AA1. External input (e.g., light) may be provided to the camera module CMM via the first area AA1. In an embodiment, for example, the camera module CMM may capture an external image by receiving external light via the first area AA1.
[0097] The housings EDC1 and EDC2 accommodate therein a display module DM, first and second electronic modules EM1 and EM2, and a power module PM. The housings EDC1 and EDC2 protect components accommodated therein, such as the display module DM, first and second electronic modules EM1 and EM2, and a power module PM. Figure 2 An embodiment including two housings EDC1 and EDC2 separated from each other is shown as an example, but the disclosure is not limited thereto. Although not shown, the electronic device 1000 may further include a hinge structure for connecting the two housings EDC1 and EDC2 to each other. The housings EDC1 and EDC2 may be coupled to the window WIN.
[0098] Figure 3 According to the disclosed embodiment, Figure 2 A cross-sectional view of the display device and the camera module taken along line II' in FIG. Figure 4is a cross-sectional view showing a display panel according to a disclosed embodiment.
[0099] Reference Figure 3 and Figure 4 , an embodiment of the display device DD may include a window WIN and a display module DM (see Figure 2 ).
[0100] The window WIN may be disposed on the display panel DP. The window WIN may be aligned with the display area DP-DA (see Figure 2 ) is overlapped and provides an optically transparent area. The window WIN may provide a display surface DS (see Figure 1A ). The image IM displayed on the display panel DP (see Figure 1A ) can be viewed by the user via window WIN.
[0101] The window WIN may include thin glass or a synthetic resin film. In an embodiment where the window WIN includes thin glass, the thickness of the window WIN may be equal to or less than about 100 micrometers (μm), and may be, for example, about 60 μm, but the thickness of the window WIN is not limited thereto. In an embodiment where the window WIN includes a synthetic resin film, the window WIN may include a polyimide (PI) film or a polyethylene terephthalate (PET) film.
[0102] The window WIN may comprise or be made of a soft or flexible material. Thus, the window WIN may be folded about a folding axis FX (see Figure 1B That is, when the shape of the display panel DP changes, the shape of the window WIN may also change correspondingly to the shape of the display panel DP.
[0103] The window WIN can transmit the image IM from the display panel DP (see Figure 1A ), while mitigating external impact, thereby effectively preventing the display panel DP from being damaged or malfunctioning due to the external impact. The external impact may be a force from the outside that may be expressed as pressure, stress, etc., and may mean any type of force that may cause defects in the display panel DP.
[0104] Display module DM (see Figure 2 ) may include a display panel DP, an optical layer OPL, a support plate 300, a panel protection film PFL, a lower protection film CPL, a first buffer layer CS1, a second buffer layer CS2, a first plate 400 and a second plate 500, and may also include various other functional layers.
[0105] The display panel DP may be a flexible panel. Figure 4As shown in FIG. 1 , the display panel DP may include a display layer 100 and a sensor layer 200. This will be described later. The display panel DP may have a thickness of about 40 μm.
[0106] The display layer 100 according to the disclosed embodiment may be a light-emitting display layer and may not be particularly limited. In an embodiment, for example, the display layer 100 may include an organic light-emitting display layer, a quantum dot display layer, a micro light-emitting diode (LED) display layer, a nano-LED display layer, etc. The light-emitting layer of the organic light-emitting display layer may include an organic light-emitting material. The light-emitting layer of the quantum dot display layer may include quantum dots, quantum rods, etc. The light-emitting layer of the micro-LED display layer may include micro-LEDs. The light-emitting layer of the nano-LED display layer may include nano-LEDs.
[0107] The display layer 100 may include a base layer 110 , a circuit layer 120 , a light emitting element layer 130 , and an encapsulation layer 140 .
[0108] The base layer 110 may be a member providing a surface on which the circuit layer 120 is disposed. The base layer 110 may be a glass substrate, a metal substrate, or a polymer substrate. However, the embodiment may not be limited thereto, and the base layer 110 may be an inorganic layer, an organic layer, or a composite material layer.
[0109] The base layer 110 may have a multi-layer structure. In an embodiment, for example, the base layer 110 may include a first synthetic resin layer, a silicon oxide (SiO x ) layer, an amorphous silicon (a-Si) layer disposed on the silicon oxide layer, and a second synthetic resin layer disposed on the amorphous silicon layer. The silicon oxide layer and the amorphous silicon layer may be referred to as a substrate barrier layer.
[0110] Each of the first synthetic resin layer and the second synthetic resin layer may include a polyimide resin. In addition, each of the first synthetic resin layer and the second synthetic resin layer may include at least one selected from acrylate resins, methacrylate resins, polyisoprene resins, vinyl resins, epoxy resins, urethane resins, cellulose resins, siloxane resins, polyamide resins, and perylene resins. Here, the "~~" type resin means a functional group containing "~~".
[0111] The circuit layer 120 may be disposed on the base layer 110. The circuit layer 120 may include an insulating layer, a semiconductor pattern, a conductive pattern, a signal line, etc. The insulating layer, the semiconductor layer, and the conductive layer may be formed on the base layer 110 using a method such as coating or deposition, and thereafter, the insulating layer, the semiconductor layer, and the conductive layer may be selectively patterned via a plurality of photolithography processes so that the semiconductor pattern, the conductive pattern, and the signal line included in the circuit layer 120 may be formed.
[0112] The light emitting element layer 130 may be disposed on the circuit layer 120. The light emitting element layer 130 may include a light emitting element. In an embodiment, for example, the light emitting element layer 130 may include an organic light emitting material, a quantum dot, a quantum rod, a micro LED, or a nano LED.
[0113] The encapsulation layer 140 may be disposed on the light emitting element layer 130. The encapsulation layer 140 may protect the light emitting element layer 130 from moisture, oxygen, and foreign substances such as dust particles.
[0114] The sensor layer 200 may be formed on the display layer 100 via a subsequent process. In this case, it may mean that the sensor layer 200 is directly disposed on the display layer 100. Directly disposed may mean that no third component is disposed between the sensor layer 200 and the display layer 100. That is, no separate bonding member may be disposed between the sensor layer 200 and the display layer 100. Alternatively, the sensor layer 200 may be bonded to the display layer 100 via a bonding member. The bonding member may include a conventional adhesive.
[0115] The optical layer OPL may be disposed on the display panel DP. The optical layer OPL may reduce the reflectivity of external light. The optical layer OPL may include a stretchable synthetic resin film. In an embodiment, for example, the optical layer OPL may be provided by dyeing a polyvinyl alcohol (PVA) film with an iodine compound. Alternatively, the optical layer OPL may include a color filter. The optical layer OPL may include various layers as long as they can reduce the reflectivity of external light, and may not be limited to one embodiment.
[0116] The optical layer OPL and the window WIN may be bonded to each other by a predetermined adhesive layer AD1. The adhesive layer AD1 may include an optically clear adhesive (OCA), an optically clear resin (OCR), or a pressure-sensitive adhesive (PSA). The adhesive layer to be described below may include the same material as the adhesive layer AD1, and may include a conventional adhesive. In an embodiment, for example, the adhesive layer AD1 may have a thickness of about 50 μm.
[0117] The support plate 300 may be disposed under the display panel DP. The support plate 300 may support the display panel DP. The support plate 300 may include a first support member 310, a second support member 320, and a foldable portion 330. The first support member 310 and the second support member 320 may be spaced apart from each other in the first direction DR1, and the foldable portion 330 is disposed between the first support member 310 and the second support member 320. The thickness of the support plate 300 may be greater than the thickness of the display panel DP. In an embodiment, for example, the thickness of the support plate 300 may be about 150 μm.
[0118] When viewed in a plan view, the first support 310 may overlap the first non-foldable area NFA1.
[0119] When viewed in a plan view, the second support member 320 may overlap the second non-foldable area NFA2.
[0120] Each of the first support 310 and the second support 320 may have an insulating property. In an embodiment, for example, each of the first support 310 and the second support 320 may include or be made of plastic or glass.
[0121] The foldable portion 330 may overlap the foldable area FA. A plurality of openings HA may be defined through the foldable portion 330. The plurality of openings HA may be spaced apart from each other in the first direction DR1. Therefore, when viewed in a plan view, the foldable portion 330 may have a grid shape. As the size of each of the plurality of openings HA changes, the shape of the support plate 300 in the foldable area FA may be easily changed. In an embodiment, for example, although not shown, a material having high ductility may be filled in the plurality of openings HA.
[0122] When folded, due to the plurality of openings HA, the foldable portion 330 can easily change shape. The foldable portion 330 may include the same material as the first support member 310 and the second support member 320 or be formed of the same material as the first support member 310 and the second support member 320. However, this is an example, and the foldable portion 330 according to the disclosed embodiment may include a material different from that of the first support member 310 and the second support member 320. In an embodiment, for example, the foldable portion 330 may include a single metal or alloy. Therefore, even in a folded state, the foldable portion 330 may stably protect the foldable area FA of the display panel DP.
[0123] The panel protection film PFL and the lower protection film CPL may be disposed between the display panel DP and the support plate 300 .
[0124] The panel protection film PFL may be disposed under the display panel DP. The panel protection film PFL may protect the lower portion of the display panel DP. The panel protection film PFL may include a flexible plastic material. In an embodiment, for example, the panel protection film PFL may include polyethylene terephthalate (PET). The panel protection film PFL may have a thickness greater than that of the display panel DP. In an embodiment, for example, the panel protection film PFL may have a thickness of about 68 μm.
[0125] The lower protective film CPL may be disposed under the panel protective film PFL. The lower protective film CPL may have a predetermined color. The lower protective film CPL may protect the rear surface of the display panel DP and may prevent the problem that the rear surface of the display panel DP is visible through light. The lower protective film CPL may include or be made of a material having a large light absorption rate.
[0126] In an embodiment, for example, a predetermined recess CPL_G overlapping the foldable area FA may be defined in the lower protective film CPL. The recess CPL_G may reduce the folding stress by reducing the thickness of the lower protective film CPL in the foldable area FA. In addition, the bonding force with the support plate 300 may be improved by further adding an adhesive layer to the recess CPL_G.
[0127] The first plate 400 may be disposed under the support plate 300. The first plate 400 may support the display panel DP. When viewed in a plan view, the first plate 400 may overlap the second non-foldable area NFA2.
[0128] The first plate 400 and the second plate 500 may face each other. The first plate 400 and the second plate 500 may be spaced apart from each other in the first direction DR1. When viewed in a plan view, the first plate 400 and the second plate 500 may not overlap each other.
[0129] The first plate 400 may have a greater modulus than the support plate 300. Therefore, the first plate 400 may stably protect the display panel DP from external impact. In an embodiment, for example, the first plate 400 may include aluminum alloy, carbon fiber reinforced plastic, or the like.
[0130] The first buffer layer CS1 and the insulating layer TP may be disposed under the first plate 400. The first buffer layer CS1 may overlap the first plate 400 when viewed in a plan view.
[0131] The first buffer layer CS1 may protect the display panel DP by absorbing external impact. The first buffer layer CS1 may include a foam sheet having predetermined elasticity. The first buffer layer CS1 may include sponge or polyurethane.
[0132] The insulating layer TP may be disposed under the first buffer layer CS1. The insulating layer TP may include an insulating film. The insulating layer TP may effectively prevent the inflow of static electricity.
[0133] The second plate 500 may be disposed under the support plate 300. The second plate 500 may support the display panel DP. When viewed in a plan view, the second plate 500 may overlap the first non-foldable area NFA1.
[0134] The second plate 500 may have a larger modulus than the support plate 300. Therefore, the second plate 500 may stably protect the display panel DP from external impact. In an embodiment, for example, the second plate 500 may include an aluminum alloy, a carbon fiber reinforced plastic, etc. The first plate 400 and the second plate 500 and the support plate 300 may be combined with each other through an adhesive layer AD2. In an embodiment, a predetermined recessed portion AD2_G overlapping the foldable area FA may be defined in the adhesive layer AD2. The recessed portion AD2_G may reduce the folding stress by reducing the thickness of the adhesive layer AD2 in the foldable area FA.
[0135] The second buffer layer CS2 and the insulating layer TP may be disposed under the second plate 500. The second buffer layer CS2 may overlap the second plate 500 when viewed from below.
[0136] The second buffer layer CS2 may protect the display panel DP by absorbing external impact. The second buffer layer CS2 may include a foam sheet having predetermined elasticity. The second buffer layer CS2 may include sponge or polyurethane.
[0137] The insulating layer TP may be disposed under the second buffer layer CS2. The insulating layer TP may include an insulating film. The insulating layer TP may effectively prevent the inflow of static electricity.
[0138] In the sensor area UA, a through hole HAA may be defined to pass through the support plate 300 , the panel protection film PFL, the lower protection film CPL, the first buffer layer CS1 , and the first plate 400 in the third direction DR3 .
[0139] The camera module CMM may be disposed under the through hole HAA. The camera module CMM may capture an external image by receiving natural light through the through hole HAA.
[0140] Figure 5 is a flow chart showing a method of manufacturing a window according to a disclosed embodiment, and Fig. 6A is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0141] Reference Figure 5 , used to make windows WIN (see Figure 3 ) may include: performing plasma treatment on a surface of a substrate (S110); applying a first solution to form a first portion (S210); applying a second solution to form a second portion (S310); applying a third solution to form a third portion (S410); and forming a coating layer (S510). This will be described later.
[0142] Fig. 6A A process ( S110 ) of performing plasma treatment on the surface SF of the substrate 10 is shown.
[0143] The preliminary window WIN-1a may include a substrate 10. The substrate 10 may include thin glass, plastic, or a synthetic resin film. In an embodiment, for example, the substrate 10 may include ultra-thin glass (UTG).
[0144] The substrate 10 may have a thickness GH in the third direction DR3. The thickness GH of the substrate 10 may be equal to or less than about 100 μm. In an embodiment, for example, the thickness GH of the substrate 10 may be about 30 μm. In such an embodiment, because the thickness GH of the substrate 10 is less than 0.5 millimeters (mm) or a thickness of about 500 μm, which is the thickness of an existing or conventional rigid cover glass, when the folding window WIN (see Figure 3 ), the stress generated in the foldable area FA is reduced, so that the window WIN can be flexibly folded.
[0145] Plasma PS may be provided to the preliminary window WIN-1a for plasma treatment. Plasma PS may pre-treat the surface SF of the substrate 10. Plasma PS may modify the surface of the substrate 10 to improve the bonding force between the surface SF of the substrate 10 and the solution to be provided later. Due to the plasma treatment, the surface SF of the substrate 10 may generate a polar surface containing a hydrophilic functional group.
[0146] The plasma PS can clean the substrate 10 .
[0147] According to the disclosed embodiment, the process (S110) of performing plasma treatment on the surface SF of the substrate 10 may be a pretreatment process for easily forming a coating on the substrate 10. The pretreated substrate 10 may easily undergo the next operation of the manufacturing method. Therefore, a method for manufacturing a window with improved reliability may be provided.
[0148] Figure 6B is a perspective view showing a process of a window manufacturing method according to a disclosed embodiment, and Figure 6C According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line. Figure 6B A process of forming a first portion by applying a first solution is shown.
[0149] Reference Figure 5 , Figure 6B and Figure 6C , the first solution SOL1 may be applied to the preliminary window WIN-1b. The first solution SOL1 may be applied to the substrate 10, and the first portion L1 may be formed (S210). The process of forming the first portion L1 (S210) may be referred to as a first coating operation (S210).
[0150] The first solution SOL1 may be applied to improve the impact resistance of the substrate 10 and prevent the substrate 10 from being broken or scattered when the substrate 10 is damaged. The first solution SOL1 may include at least one selected from silicone-based resins, urethane-based resins, epoxy-based resins, polyester-based resins, polyether-based resins, acrylate-based resins, acrylonitrile-butadiene-styrene (ABS) resins, and rubber.
[0151] The first solution SOL1 may have a viscosity in the range of about 6 centipoise (cp) to about 10 cp. If the viscosity of the first solution SOL1 exceeds 10 cp, leveling of the first solution SOL1 disposed on the substrate 10 is difficult, and it may be difficult to use a spray coating method.
[0152] The first solution SOL1 may include an ultraviolet (UV)-curable solvent-free material, a UV-curable solvent material, a thermally curable material, or the like.
[0153] The first solution SOL1 may be applied by spraying. The nozzle SPY may apply the first solution SOL1 to the surface SF of the substrate 10 (see Fig. 6A ). In the first coating operation (S210), the first solution SOL1 applied to the substrate 10 may be provided in a volume of about 2.7 cubic centimeters (cc). However, this is an example, and the volume of the first solution SOL1 according to the disclosed embodiment is not limited thereto. The first solution SOL1 may be provided in a volume based on the first thickness H1 of the first portion L1.
[0154] The first solution SOL1 may be applied along a path in a zigzag shape along (or toward) the first direction DR1. In an embodiment, for example, the first solution SOL1 may be applied along the first direction DR1 in a The first solution SOL1 may be applied onto the substrate 10 along a first path R1.
[0155] The first solution SOL1 applied to the substrate 10 may be formed into a first portion L1. The first portion L1 may be liquid.
[0156] The first portion L1 may be formed to have a first thickness H1. The first thickness H1 may be in the range of about 6.7 μm to about 10 μm.
[0157] A beading phenomenon may occur at the edge of the substrate 10. The beading phenomenon may be caused by interfacial tension between the substrate 10 and a solution applied onto the substrate 10. The beading phenomenon may refer to a phenomenon in which a solution applied onto the substrate 10 gathers. The sensor area UA may refer to an area at a distance of about 2.8 mm to about 6.3 mm away from the edge of the window WIN.
[0158] When the coating CL in the open sensor area UA (see Figure 6J When the peak-to-valley (PV) value of the difference between the maximum value and the minimum value (peak-to-valley) of the wavefront aberration is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as the edge bead phenomenon being reduced or eliminated. When the PV value exceeds 0.92 wavelengths, it can be defined as having occurred.
[0159] Wavefront aberration is a value that indicates the degree of distortion of the wavefront when light passes through an optical system as a measurement object. The PV value can indicate optical flatness. The PV value can be proportional to the difference between the maximum and minimum values (peak to valley) of the physical thickness. The PV value can be used for coating CL (see Figure 6J )’s evaluation.
[0160] In the case where the surface of the sensor area UA may be uneven due to the edge bead phenomenon, this may cause the light received by the camera module CMM to be refracted and the resolution of the camera module CMM to be reduced. According to the disclosed embodiments, due to the small thickness of the first portion L1, the edge bead phenomenon can be reduced or eliminated. The first portion L1 can be coated to have a uniform top surface. The window WIN (see Figure 2 ) may be coated multiple times with a coating CL for improving the impact resistance of the substrate 10 (see Figure 6J ). The first portion L1 having a uniform top surface may be formed in the sensor area UA, so that the optical characteristics of the sensor area UA may be improved. Therefore, a window WIN having improved impact resistance and flatness may be provided (see Figure 2 ) and a method for making a window.
[0161] Fig.6D is a perspective view showing a process of a window manufacturing method according to a disclosed embodiment, and Fig. 6E According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line. Fig.6D A process of forming the second portion by applying the second solution is shown.
[0162] Reference Figure 5 , Fig.6D and Fig. 6E , the second solution SOL2 may be applied to the preliminary window WIN-1c. The second solution SOL2 may be applied to the first portion L1, and the second portion L2 may be formed (S310). The process of forming the second portion L2 (S310) may be referred to as a second coating operation (S310).
[0163] The second solution SOL2 may be substantially the same as the first solution SOL1.
[0164] The second solution SOL2 may be applied by a spray coating method. The nozzle SPY may apply the second solution SOL2 onto the first portion L1. In the second coating operation (S310), the second solution SOL2 applied onto the first portion L1 may be provided in a capacity of about 2.7 cc.
[0165] The second solution SOL2 may be applied along a path in a zigzag shape in a direction opposite to the first direction DR1. The second solution SOL2 can be applied to the first portion L1 along the second path R2. The second path R2 is parallel to the first path R1 (see Figure 6B ) can differ only in direction and can have the same shape.
[0166] The second solution SOL2 applied to the first portion L1 may be formed into the second portion L2. The second portion L2 may be liquid.
[0167] The second portion L2 may be formed to have a second thickness H2. The second thickness H2 may be in the range of about 6.7 μm to about 10 μm. The second thickness H2 may be substantially the same as the first thickness H1.
[0168] According to the disclosed embodiment, because the second portion L2 includes or is made of the same material as the first portion L1, the interfacial tension between the first portion L1 and the second portion L2 can be reduced or eliminated. Therefore, in such an embodiment, the edge bead phenomenon can be reduced or eliminated. The second portion L2 can be coated to have a uniform top surface. In the window WIN according to the disclosed embodiment (see Figure 2 ) in the embodiment, the coating CL for improving the impact resistance of the substrate 10 may be applied multiple times (see Figure 6J ). The second portion L2 having a uniform top surface may be formed in the sensor area UA, so that the optical characteristics of the sensor area UA may be improved. Therefore, a window WIN having improved impact resistance and flatness may be provided (see Figure 2 ).
[0169] Fig. 6F is a perspective view showing a process of a window manufacturing method according to a disclosed embodiment, Figure 6G According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut by the line, and Figure 6H is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0170] Reference Figure 5 as well as FIG. 6F to FIG. 6H, the third solution SOL3 may be applied to the preliminary window WIN-1d. The third solution SOL3 may be applied to the second portion L2, and a third portion L3 may be formed (S410). The process of forming the third portion L3 (S410) may be referred to as a third coating operation (S410).
[0171] The third solution SOL3 may be substantially the same as the first solution SOL1 and the second solution SOL2.
[0172] The third solution SOL3 may be applied by spraying. The nozzle SPY may apply the third solution SOL3 onto the second portion L2. In the third coating operation (S410), the third solution SOL3 applied onto the second portion L2 may be provided in a capacity of 2.7cc.
[0173] The third solution SOL3 may be applied along a path in a zigzag shape along the first direction DR1. The third solution SOL3 may be applied to the second portion L2 along the third path R3. The third path R3 may be aligned with the first path R1 (see Figure 6B ) are basically the same.
[0174] According to the disclosed embodiment, the coating applied to the substrate 10 may be applied multiple times. In odd-numbered applications, the coating may be applied along the first path R1 or the third path R3, and in even-numbered applications, the coating may be applied along the second path R2. The nozzle SPY may perform multiple coating processes with minimal movement. Therefore, a method for manufacturing a window with improved reliability may be provided.
[0175] The third solution SOL3 applied to the second portion L2 may be formed into the third portion L3. The third portion L3 may be liquid.
[0176] The third portion L3 may be formed to have a third thickness H3. The third thickness H3 may be in the range of about 6.7 μm to about 10 μm. The third thickness H3 may be substantially the same as the second thickness H2.
[0177] The beading phenomenon may be proportional to the interfacial tension F between the substrate 10 and the solution applied onto the substrate 10. The interfacial tension F may be calculated based on Mathematical Formula 1 below.
[0178]
Mathematical formula 1
[0179]
[0180] The interfacial tension between the first material and the second material in mathematical formula 1 is given by γ SLThe surface tension of the first material is represented by γ S The surface tension of the polar part of the first material is represented by γ S P The surface tension of the nonpolar portion of the first material is represented by γ S D The surface tension of the second material is represented by γ L The surface tension of the polar part of the second material is represented by γ L P The surface tension of the nonpolar part of the second material is represented by γ L D Surface tension and interfacial tension may have units of millinewtons per meter (mN / m). In this regard, the first material may be a solid and the second material may be a liquid.
[0181]
Table 1
[0182]
[0183] Table 1 shows the surface tension of substrate and existing (conventional) coating solution and the interfacial tension between substrate and existing coating solution calculated using above mathematical formula 1 respectively. In this respect, existing coating solution can be the solution used in the existing process of forming coating with one-time coating. The contact angle between substrate and existing coating solution can be 50.3 °. The smaller the contact angle, the smaller the PV value of coating, and the occurrence of edge bead phenomenon can be reduced or eliminated. The contact angle can be calculated based on the following mathematical formula 2.
[0184]
Mathematical formula 2
[0185]
[0186] In Mathematical Formula 2, the contact angle is represented by θ. The interfacial tension between the first material and the outside (air) is represented by γ SV The interfacial tension between the second material and the outside (air) is represented by γ LV The interfacial tension between the first material and the second material is represented by γ SL express.
[0187] In this regard, γ SV and γ LV It may be a fixed value, and the contact angle may be proportional to the interfacial tension between the first material and the second material.
[0188]
Table 2
[0189]
[0190] Table 2 shows the surface tension of the first part L1 until the surface tension of the third part L3 and the interfacial tension F between the first part L1, the second part L2 and the third part L3 calculated using the above mathematical formula 1. The contact angle between the first part L1 and the second part L2 or the third part L3 may be 10.2°. Referring to Table 1, in the case where the coating is formed once on the substrate 10, the interfacial tension may be relatively large. In this case, an edge bead phenomenon may occur. Due to the edge bead phenomenon, the surface of the sensor area UA may be uneven, and therefore, the light received by the camera module CMM may be refracted and the resolution of the camera module CMM may be reduced. According to the disclosed embodiment, referring to Table 2, the first part L1 may be affected by the polarity of the substrate 10, so that the surface tension of the polar part may increase. The interfacial tension F between the first part L1, the second part L2 and the third part L3 may be relatively small. Therefore, the edge bead phenomenon may be reduced. The third part L3 may be coated to have a uniform top surface. In an embodiment, the coating may be applied multiple times to improve the impact resistance of the substrate 10. The third portion L3 having a uniform top surface may be formed in the sensor area UA, so that the optical characteristics of the sensor area UA may be improved. Therefore, a window WIN having improved impact resistance and flatness may be provided (see FIG. 1 ). Figure 2 ) and a method for making a window.
[0191] The preliminary window WIN-1 e in which the coating process is completed may have a shape in which the first portion L1 , the second portion L2 , and the third portion L3 are sequentially stacked on the substrate 10 .
[0192] The first thickness H1 of the first portion L1 , the second thickness H2 of the second portion L2 , and the third thickness H3 of the third portion L3 may be substantially the same as one another.
[0193] A plurality of portions L1, L2 and L3 are formed to form a coating layer CL (see Figure 6J ) can be limited to three times in the processes S210, S310 and S410. If the number of times the solution is applied is equal to or less than two times, a beading phenomenon may occur, and if the number of times the solution is applied is equal to or greater than four times, the window WIN (see Figure 2 )’s appearance quality may deteriorate and productivity may decrease.
[0194] Fig.6I is a perspective view showing a process of a window manufacturing method according to a disclosed embodiment, and Figure 6J is a perspective view showing a window according to a disclosed embodiment.
[0195] Reference Figure 5 , Fig.6I and Figure 6J, a coating layer CL may be formed in the preliminary window WIN-1f (S510). The process of forming the coating layer CL (S510) may be referred to as forming a coating layer (S510).
[0196] In forming the coating layer (S510), a curing module UVM may be provided on the preliminary window WIN-1f. The curing module UVM may irradiate ultraviolet rays UV to the preliminary window WIN-1f. The curing module UVM may be moved along the second direction DR2. The ultraviolet rays UV may have a wavelength in the range of about 200 nanometers (nm) to about 400 nm.
[0197] In forming the coating layer (S510), the first part L1, the second part L2, and the third part L3 may be simultaneously cured by ultraviolet rays UV irradiated thereto. In this regard, forming the coating layer CL by applying the solution multiple times to form the first part L1, the second part L2, and the third part L3 and then curing them once may be referred to as a multi-stage coating method.
[0198] However, this is an example, and the curing method according to the disclosed embodiment is not limited to ultraviolet curing. In the embodiment, for example, the curing method may include thermal curing, electron beam curing, etc.
[0199] The solidified first portion L1, second portion L2, and third portion L3 may be solid. The solidified first portion L1, second portion L2, and third portion L3 may be referred to as a coating layer CL. That is, the coating layer CL may be a solid layer.
[0200] The window WIN-1 may be manufactured by a window manufacturing method. The window WIN-1 may include a substrate 10 and a coating CL. The coating CL may be disposed on the substrate 10. The coating CL may improve the impact resistance of the substrate 10 and effectively prevent the substrate from being broken or scattered when the substrate 10 is damaged.
[0201] The coating layer CL may have a predetermined thickness CH. In an embodiment, the thickness CH may be in a range of about 20 μm to about 30 μm. If the thickness CH is less than about 20 μm, even when a multi-stage coating method is not used, it may be controlled by one-time solution coating so that the edge bead phenomenon does not occur at the sensor area UA, and if the thickness CH is greater than 30 μm, the edge bead phenomenon may occur even when a multi-stage coating method is used. This will be described later.
[0202] Fig. 7A is a graph showing the thickness of a coating based on the distance from the edge of a substrate according to disclosed embodiments.
[0203] See also Figure 6J and 7A, the first to fourth curves GP1, GP2, GP3 and GP4 show the thickness measured when the thickness of the coating layer is about 20 μm. Fig. 7A , the horizontal axis represents the distance from the edge of the substrate 10 in μm, and the vertical axis represents the thickness in μm.
[0204] The first curve GP1 shows the thickness of the coating formed by a single coating process.
[0205] The second curve GP2 shows the thickness of the coating formed by the two-coating process.
[0206] The third curve GP3 shows the thickness CH of the coating layer CL formed by the three-stage coating process. That is, the third curve GP3 may show the thickness CH of the coating layer CL formed through multi-stage coating according to the disclosed embodiment.
[0207] The fourth curve GP4 shows the thickness of the coating formed by the four-application process.
[0208] The peak value of the interfacial tension at the coating layer CL formed via multi-stage coating may be smaller than the peak value of the interfacial tension at the coating layer formed using a single coating process.
[0209] According to the disclosed embodiment, the difference between the maximum value and the minimum value (peak to valley) of the wavefront aberration of the coating CL in the sensor area UA at the coating CL formed via multi-stage coating can be smaller than the difference between the maximum value and the minimum value (peak to valley) of the wavefront aberration of the coating in the sensor area UA at the coating formed by a single coating process. In such an embodiment, the edge bead phenomenon can be reduced or eliminated in the coating CL, so that the optical characteristics of the sensor area UA can be improved. Therefore, a window WIN-1 with improved impact resistance and flatness can be provided.
[0210] Figure 7B is a graph showing the thickness of a coating based on the distance from the edge of a substrate according to disclosed embodiments.
[0211] Reference Figure 6J and Figure 7B , the first curve GP1-1 and the second curve GP2-1 show the thickness measured when the thickness of the coating layer is about 30 μm. Figure 7B , the horizontal axis represents the distance from the edge of the substrate 10 in μm, and the vertical axis represents the thickness in μm.
[0212] The first curve GP1-1 shows the thickness of the coating formed by a single coating process.
[0213] The second graph GP2-1 shows the thickness CH of the coating layer CL formed by the three-stage coating process. That is, the second graph GP2-1 may show the thickness CH of the coating layer CL formed through multi-stage coating according to the disclosed embodiment.
[0214] The peak value of the interfacial tension at the coating layer CL formed via multi-stage coating may be smaller than the peak value of the interfacial tension at the coating layer formed using a single coating process.
[0215] According to the disclosed embodiment, the difference between the maximum value and the minimum value (peak to valley) of the wavefront aberration of the coating CL in the sensor area UA at the coating CL formed via multi-stage coating can be smaller than the difference between the maximum value and the minimum value (peak to valley) of the wavefront aberration of the coating in the sensor area UA at the coating formed by a single coating process. In such an embodiment, the edge bead phenomenon can be reduced or eliminated in the coating CL, so that the optical characteristics of the sensor area UA can be improved. Therefore, a window WIN-1 with improved impact resistance and flatness can be provided.
[0216] Fig. 8A is a box plot showing PV values based on the number of coatings according to the disclosed embodiment, and Figure 8B Shown are captured images of a window based on the number of coatings according to the disclosed embodiment.
[0217] Reference Figure 6J , 8A 8B, the PV value can be an index representing the optical flatness. Fig. 8A , the horizontal axis shows the number of coatings, and the vertical axis shows the PV value. The PV value shows 0 wavelength to 2.5 wavelength as an example. In this regard, 1 wavelength may be about 632.8 nm. Fig. 8A Each PV value measured for each number of coating times when the thickness of the coating layer is about 20 μm is shown as an example.
[0218] Each of the images IM1 - 1 to IM4 - 2 obtained through the photographing window WIN- 1 shows thickness via a level curve.
[0219] The average value of the PV value in the coating formed by the single coating process S1 may be 1.57 wavelengths, and the maximum value of the PV value may be 2.57 wavelengths. The coating formed by the single coating process S1 may be referred to as an existing (or conventional) coating.
[0220] The first-first image IM1 - 1 and the first-second image IM1 - 2 may be images obtained by photographing a window including a coating layer formed by the single coating process S1 .
[0221] The first-first image IM1-1 may be an image obtained by photographing the top surface of a window having an average value of PV values. For example, the first-first image IM1-1 may be an image obtained by photographing the top surface of a window having a PV value of 1.57 wavelengths.
[0222] The first-second image IM1-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the first-second image IM1-2 may be an image obtained by photographing the top surface of the window having a PV value of 2.57 wavelengths.
[0223] The average value of the PV value in the coating layer formed by the double coating process S2 may be 0.59 wavelengths, and the maximum value of the PV value may be 1.50 wavelengths. In this regard, the difference between the average value of the PV value in the coating layer formed by the double coating process S2 and the average value of the PV value in the coating layer formed by the single coating process S1 may be 0.98 wavelengths.
[0224] The second-first image IM2 - 1 and the second-second image IM2 - 2 may be images obtained by photographing a window including a coating layer formed by the double coating process S2 .
[0225] The second-first image IM2-1 may be an image obtained by photographing the top surface of a window having an average value of PV values. For example, the second-first image IM2-1 may be an image obtained by photographing the top surface of a window having a PV value of 0.59 wavelength.
[0226] The second-second image IM2-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the second-second image IM2-2 may be an image obtained by photographing the top surface of the window having a PV value of 1.5 wavelengths.
[0227] The second-first image IM2-1 may have a greater uniformity of thickness in the sensor area UA than the first-first image IM1-1. The second-second image IM2-2 may have a greater uniformity of thickness in the sensor area UA than the first-second image IM1-2.
[0228] The average value of the PV value in the coating layer CL formed by the three-coating process S3 may be 0.41 wavelengths, and the maximum value of the PV value may be 0.89 wavelengths. In this regard, the difference between the average value of the PV value in the coating layer CL formed by the three-coating process S3 and the average value of the PV value in the coating layer formed by the two-coating process S2 may be 0.18 wavelengths. The reference line RL shows a case where the PV value is 0.92 wavelengths.
[0229] The third-first image IM3 - 1 and the third-second image IM3 - 2 may be images obtained by photographing the window WIN- 1 including the coating layer CL formed by the three-coating process S3 .
[0230] The third-first image IM3-1 may be an image obtained by photographing the top surface of the window WIN-1 having an average value of the PV value. For example, the third-first image IM3-1 may be an image obtained by photographing the top surface of the window WIN-1 having a PV value of 0.41 wavelength.
[0231] The third-second image IM3-2 may be an image obtained by photographing the top surface of the window WIN-1 having the maximum value of the PV value. For example, the third-second image IM3-2 may be an image obtained by photographing the top surface of the window WIN-1 having a PV value of 0.89 wavelength.
[0232] The coating layer CL formed by the three-coating process S3 may have an average PV value having a 1.16 wavelength difference from the average PV value of the existing coating layer, and have a maximum PV value having a 1.68 wavelength difference from the maximum PV value of the existing coating layer.
[0233] The third-first image IM3-1 may have a greater uniformity of thickness in the sensor area UA than the second-first image IM2-1. The third-second image IM3-2 may have a greater uniformity of thickness in the sensor area UA than the second-second image IM2-2.
[0234] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as the edge bead phenomenon is reduced or eliminated. The window WIN-1 may be coated with a coating CL for improving the impact resistance of the substrate 10 multiple times. The coating CL formed by the three-coating process S3 may have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. That is, in an embodiment, the edge bead phenomenon in the sensor area UA may be reduced or eliminated, so that the optical characteristics of the sensor area UA may be improved. Therefore, a window WIN-1 with improved impact resistance and flatness may be provided.
[0235] The average value of the PV value in the coating layer formed by the four-time coating process S4 may be 0.40 wavelengths, and the maximum value of the PV value may be 0.87 wavelengths. In this regard, the difference between the average value of the PV value in the coating layer formed by the four-time coating process S4 and the average value of the PV value in the coating layer CL formed by the three-time coating process S3 may be 0.01 wavelengths.
[0236] The fourth-first image IM4 - 1 and the fourth-second image IM4 - 2 may be images obtained by photographing a window including a coating layer formed by the four-time coating process S4 .
[0237] The fourth-first image IM4-1 may be an image obtained by photographing the top surface of the window having an average value of the PV value. For example, the fourth-first image IM4-1 may be an image obtained by photographing the top surface of the window having a PV value of 0.40 wavelength.
[0238] The fourth-second image IM4-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the fourth-second image IM4-2 may be an image obtained by photographing the top surface of the window having a PV value of 0.87 wavelength.
[0239] There may be no substantial difference in PV value between the coating CL formed by the three-time coating process S3 and the coating formed by the four-time coating process S4. In the window manufacturing method according to the disclosed embodiment, the number of coating processes may be limited to three times. If the number of coating processes is equal to or greater than four times, the appearance quality of the window may deteriorate and productivity may decrease.
[0240] Fig.9A is a box plot showing PV values based on the number of coatings according to the disclosed embodiment, and Fig. 9B A photographed image of a window based on the number of coatings according to the disclosed embodiment may be shown.
[0241] Reference Figure 6J , Fig.9A and Fig. 9B , Fig.9A The vertical axis in represents the PV value. The PV value shows 0 wavelength to 4.0 wavelength as an example. Fig.9A Each PV value measured based on each number of coating times when the thickness of the coating layer is greater than 30 μm is shown as an example.
[0242] Each of the images IM1a-1 to IM3a-2 obtained through the photographing window shows the thickness via a horizontal curve.
[0243] The average value of the PV value in the coating layer formed by the single coating process S1 - 1 may be 2.33 wavelengths, and the maximum value of the PV value may be 2.77 wavelengths.
[0244] The first-first image IM1a-1 and the first-second image IM1a-2 may be images obtained by photographing a window including a coating layer formed by the single coating process S1-1.
[0245] The first-first image IM1a-1 may be an image obtained by photographing the top surface of a window having an average value of PV values. For example, the first-first image IM1a-1 may be an image obtained by photographing the top surface of a window having a PV value of 2.33 wavelengths.
[0246] The first-second image IM1a-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the first-second image IM1a-2 may be an image obtained by photographing the top surface of the window having a PV value of 2.77 wavelengths.
[0247] The average value of the PV value in the coating layer formed by the four-time coating process S2-1 may be 2.10 wavelengths, and the maximum value of the PV value may be 3.07 wavelengths. In this regard, the difference between the average value of the PV value in the coating layer formed by the four-time coating process S2-1 and the average value of the PV value in the coating layer formed by the single coating process S1-1 may be 0.23 wavelengths.
[0248] The second-first image IM2a-1 and the second-second image IM2a-2 may be images obtained by photographing a window including a coating layer formed by the fourth coating process S2-1.
[0249] The second-first image IM2a-1 may be an image obtained by photographing the top surface of a window having an average value of PV value. For example, the second-first image IM2a-1 may be an image obtained by photographing the top surface of a window having a PV value of 2.10 wavelengths.
[0250] The second-second image IM2a-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the second-second image IM2a-2 may be an image obtained by photographing the top surface of the window having a PV value of 3.07 wavelengths.
[0251] The average value of the PV value in the coating layer formed by the five-time coating process S3-1 may be 2.27 wavelengths, and the maximum value of the PV value may be 3.47 wavelengths. In this regard, the difference between the average value of the PV value in the coating layer formed by the five-time coating process S3-1 and the average value of the PV value in the coating layer formed by the four-time coating process S2-1 may be 0.17.
[0252] The third-first image IM3a-1 and the third-second image IM3a-2 may be images obtained by photographing a window including a coating layer formed by the five-time coating process S3-1.
[0253] The third-first image IM3a-1 may be an image obtained by photographing the top surface of the window having an average value of the PV value. For example, the third-first image IM3a-1 may be an image obtained by photographing the top surface of the window having a PV value of 2.27 wavelengths.
[0254] The third-second image IM3a-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the third-second image IM3a-2 may be an image obtained by photographing the top surface of the window having a PV value of 3.47 wavelengths.
[0255] If the thickness CH of the coating CL exceeds 30μm, the effect of multi-stage coating in which the coating is applied multiple times may be small. That is, even when the coating CL is formed via multi-stage coating, the edge bead phenomenon may occur. According to the disclosed embodiment, the thickness CH of the coating CL may be in the range of 20μm to 30μm. In an embodiment, in the case where the coating CL is formed via multi-stage coating, the coating CL may have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the edge bead phenomenon in the sensor area UA can be reduced or eliminated, so that the optical characteristics of the sensor area UA can be improved. Therefore, a window WIN-1 with improved impact resistance and flatness can be provided.
[0256] Fig.10 is a flow chart showing a method of manufacturing a window according to a disclosed embodiment, and Fig.11A is a perspective view showing the process of the window manufacturing method according to the disclosed embodiment. Fig.11A In the above reference Fig. 6A The same or similar components as those described above are marked with the same or similar reference numerals, and any repeated detailed description thereof will be omitted.
[0257] Reference Fig.10 , used to make windows WIN (see Figure 3 ) may include: performing plasma treatment on a surface of a substrate (S120); applying a first solution to form a first portion (S220); curing the first portion to form a first layer (S320); performing plasma treatment on a surface of the first layer (S420); applying a second solution to form a second portion (S520); and curing the second portion to form a second layer and define a coating (S620). This will be described later.
[0258] Fig.11A A process ( S120 ) of performing plasma treatment on the surface SF of the substrate 10 is shown.
[0259] The preliminary window WIN-2a may include a substrate 10. Plasma PS may be provided to the preliminary window WIN-2a for plasma treatment. The plasma PS may pre-treat a surface SF of the substrate 10.
[0260] Fig. 11B is a perspective view showing a process of a window manufacturing method according to a disclosed embodiment, and Fig. 11C According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut along the line. Fig. 11B The process of applying the first solution to form the first part is shown. Fig. 11B In the above reference Figure 6B The same or similar components as those described above are marked with the same or similar reference numerals, and any repeated detailed description thereof will be omitted.
[0261] Reference Fig.10 , Fig. 11B and Fig. 11C , the fourth solution SOL4 may be applied to the preliminary window WIN-2b. The fourth solution SOL4 may be applied to the substrate 10, and the first portion L1a-1 may be formed (S220). The process of forming the first portion L1a-1 (S220) may be referred to as a first coating operation (S220).
[0262] The fourth solution SOL4 can be mixed with the first solution SOL1 (see Figure 6B The fourth solution SOL4 may not include a leveling agent.
[0263] The fourth solution SOL4 may be applied by spraying. The nozzle SPY may apply the fourth solution SOL4 to the surface SF of the substrate 10 (see Fig.11A ). In the first coating operation (S220), the fourth solution SOL4 applied to the substrate 10 may be provided in a volume of about 5.4 cc. However, this is an example, and the volume of the fourth solution SOL4 according to the disclosed embodiment is not limited thereto. The fourth solution SOL4 may be provided in a volume based on the first thickness H1-1 of the first portion L1a-1.
[0264] The fourth solution SOL4 may be applied along a zigzag path along the first direction DR1. The fourth solution SOL4 may be applied onto the substrate 10 along the first path R1.
[0265] The fourth solution SOL4 applied to the substrate 10 may be formed as a first portion L1a-1. The first portion L1a-1 may be liquid.
[0266] The first portion L1a-1 may be formed to have a first thickness H1-1. The first thickness H1-1 may be in the range of about 10 μm to about 15 μm. If the first thickness H1-1 exceeds about 15 μm, when the second layer L2-1 (see Fig.11J ), an edge bead phenomenon occurs in the first portion L1a-1, thereby deteriorating the optical characteristics in the sensor area UA.
[0267] According to the disclosed embodiments, due to the small thickness of the first portion L1a-1, the edge bead phenomenon can be reduced or eliminated. The first portion L1a-1 can be coated to have a uniform top surface. Figure 2 ) may be coated with a coating for improving the impact resistance of the substrate 10 multiple times. In such an embodiment, the first portion L1a-1 having a uniform top surface may be formed in the sensor area UA, so that the optical characteristics of the sensor area UA may be improved. Therefore, a window WIN having improved impact resistance and flatness may be provided (see Figure 2 ).
[0268] Fig.11D and Fig.11E is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0269] Reference Fig.10 , Fig.11D and Fig.11E , a first layer L1 - 1 may be formed in the preliminary window WIN- 2 c ( S320 ).
[0270] A curing module UVM may be provided on the preliminary window WIN-2c. The curing module UVM may irradiate ultraviolet rays UV to the preliminary window WIN-2c. The curing module UVM may be moved along the second direction DR2.
[0271] In forming the first layer L1 - 1 ( S320 ), the first portion L1 a - 1 may be cured using ultraviolet rays UV.
[0272] The solidified first portion L1a-1 may be solid. The solidified first portion L1a-1 may be referred to as a first layer L1-1. That is, the first layer L1-1 may be a solid layer.
[0273] The first layer L1 - 1 may have a first thickness H1 - 1 .
[0274] The preliminary window WIN-2d may include a substrate 10 and a first layer L1-1. Plasma PS may be provided to the preliminary window WIN-2d. The plasma PS may pre-treat a surface of the first layer L1-1.
[0275] Fig.11F is a perspective view showing one step of a window manufacturing method according to a disclosed embodiment, Fig.11G According to the disclosed embodiment, Figure 1A II-II' corresponds to the cross-sectional view of the preliminary window cut by the line, and Fig.11H is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0276] Reference Fig.10 , Fig.11F , Fig.11G and Fig.11H , the fifth solution SOL5 may be applied to the preliminary window WIN-2e. The fifth solution SOL5 may be applied to the first layer L1-1, and the second portion L2a-1 may be formed (S520). The process of forming the second portion L2a-1 (S520) may be referred to as a second coating operation (S520).
[0277] The fifth solution SOL5 may be different from the fourth solution SOL4. The fifth solution SOL5 may include a leveling agent in addition to the fourth solution SOL4.
[0278] The fifth solution SOL5 may be applied by spraying. The nozzle SPY may apply the fifth solution SOL5 onto the first layer L1-1. In the second coating operation (S520), the fifth solution SOL5 applied onto the first layer L1-1 may be provided in a capacity of about 5.4cc.
[0279] The fifth solution SOL5 may be applied along a path in a zigzag shape along the first direction DR1. The fifth solution SOL5 may be applied to the first layer L1-1 along the second path R2-1. The second path R2-1 may be aligned with the first path R1 (see Fig. 11B ) are basically the same.
[0280] The fifth solution SOL5 applied onto the first layer L1-1 may be formed into the second portion L2a-1. The second portion L2a-1 may be liquid.
[0281] The second portion L2a-1 may be formed to have a second thickness H2-1. The second thickness H2-1 may be in the range of about 10 μm to about 15 μm.
[0282]
Table 3
[0283]
[0284] Table 3 above shows the surface tension of the first layer L1-1, the surface tension of the second portion L2a-1, and the interfacial tension Fa between the first layer L1-1 and the second portion L2a-1 calculated using the above mathematical formula 1. The contact angle between the first layer L1-1 and the second portion L2a-1 may be 8.6°. According to the disclosure, referring to Table 3, the first layer L1-1 may be exposed to ultraviolet light UV ( Fig.11D ) is cured, so that the influence of the polarity of the substrate 10 can be reduced or eliminated. The interfacial tension Fa between the first layer L1-1 and the second portion L2a-1 can have a value of 0 or a value close to 0. Therefore, the edge bead phenomenon can be reduced. In an embodiment, the coating layer can be applied multiple times to improve the impact resistance of the substrate 10. In such an embodiment, the second portion L2a-1 having a uniform top surface can be formed in the sensor area UA, so that the optical characteristics of the sensor area UA can be improved. Therefore, a window WIN with improved impact resistance and flatness can be provided (see Figure 2 ).
[0285] The preliminary window WIN-2f in which the coating process is completed may have a shape in which the first layer L1-1 and the second portion L2a-1 are sequentially stacked on the substrate 10.
[0286] The first thickness H1 - 1 of the first layer L1 - 1 and the second thickness H2 - 1 of the second portion L2 a - 1 may be substantially equal to each other.
[0287] Fig.11I and Fig.11J is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0288] Reference Fig.10 , Fig.11I and Fig.11J , a coating layer CL-1 (S620) may be formed in the preliminary window WIN-2g. The process of forming the coating layer CL-1 (S620) may be referred to as an operation of defining the coating layer CL-1 (S620).
[0289] A curing module UVM may be provided on the preliminary window WIN-2g. The curing module UVM may irradiate ultraviolet rays UV to the preliminary window WIN-2g. The curing module UVM may be moved along the second direction DR2.
[0290] In the operation of defining the coating layer CL-1 (S620), the second portion L2a-1 may be cured using ultraviolet rays UV. The conditions for curing the second portion L2a-1 may be substantially the same as the conditions for curing the first portion L1a-1.
[0291] The solidified second portion L2a-1 may be solid. The solidified second portion L2a-1 may be referred to as a second layer L2-1. That is, the second layer L2-1 may be a solid layer. In this regard, defining the coating layer CL-1 (S620) by forming the first layer L1-1 (S320) and forming the second layer L2-1 (S620) may be referred to as a multilayer coating method.
[0292] The first layer L1-1 and the second layer L2-1 may be referred to as a coating layer CL-1. That is, the coating layer CL-1 may include the first layer L1-1 and the second layer L2-1.
[0293] The coating CL-1 according to the disclosed embodiment may include two to three layers. If the coating CL-1 includes four or more layers, the repulsive force between the multiple layers may increase, and the risk of buckling due to reduced interface adhesion may occur. Therefore, the reliability during the folding operation of the electronic device 1000 may be reduced.
[0294] The window WIN-2 may be manufactured by an embodiment of the window manufacturing method. The window WIN-2 may include a substrate 10 and a coating CL-1. The coating CL-1 may be disposed on the substrate 10. The coating CL-1 may improve the impact resistance of the substrate 10 and prevent the substrate 10 from breaking or scattering when the substrate 10 is damaged.
[0295] The coating CL-1 may have a predetermined thickness CH2. In an embodiment, the thickness CH2 may be in a range of about 25 μm to about 35 μm. If the thickness CH2 is less than about 25 μm, it may be controlled without using a multilayer coating method so that an edge bead phenomenon does not occur at the sensor area UA, and if the thickness CH2 is greater than about 35 μm, the repulsive force between the multiple layers L1-1 and L2-1 may increase, and a buckling risk due to reduced interface adhesion may occur. Therefore, reliability may be reduced during the folding operation of the electronic device 1000.
[0296] Fig. 12A is a box plot showing PV values based on the number of layers of coating according to the disclosed embodiment, and Fig. 12B Shown are captured images of a window based on the number of layers of coating according to the disclosed embodiment.
[0297] Reference Fig.11J , Fig. 12A and Fig. 12B ,exist Fig. 12A , the horizontal axis shows coatings classified based on thickness, and the vertical axis shows PV values. The PV values show 0 wavelength to 4.0 wavelength as an example. In this regard, 1 wavelength may be about 632.8 nm.
[0298] Each of the images IM1 b - 1 to IM4 b - 2 obtained through the photographing window WIN- 2 shows the thickness via a horizontal curve.
[0299] The coating layer formed of a single layer may have a first thickness Ha. The first thickness Ha may be 30 μm. In this regard, an average value of the PV value may be 2.33 wavelengths, and a maximum value of the PV value may be 2.77 wavelengths.
[0300] The first-first image IM1b-1 and the first-second image IM1b-2 may be images obtained by photographing a window including a coating layer formed of a single layer and having a first thickness Ha.
[0301] The first-first image IM1b-1 may be an image obtained by photographing the top surface of a window having an average value of PV values. For example, the first-first image IM1b-1 may be an image obtained by photographing the top surface of a window having a PV value of 2.33 wavelengths.
[0302] The first-second image IM1b-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the first-second image IM1b-2 may be an image obtained by photographing the top surface of the window having a PV value of 2.77 wavelengths.
[0303] The coating formed of a single layer may have a second thickness Hb. The second thickness Hb may be 15 μm. In this regard, the average value of the PV value may be 0.35 wavelengths, and the maximum value of the PV value may be 0.60 wavelengths. In this regard, the difference between the average value of the PV value in the coating having the second thickness Hb and the average value of the PV value in the coating having the first thickness Ha may be 1.98 wavelengths. Reference line RL-1 shows a case where the PV value is 0.92 wavelengths.
[0304] The second-first image IM2b-1 and the second-second image IM2b-2 may be images obtained by photographing a window including a coating layer formed of a single layer and having a second thickness Hb.
[0305] The second-first image IM2b-1 may be an image obtained by photographing the top surface of a window having an average value of the PV value. For example, the second-first image IM2b-1 may be an image obtained by photographing the top surface of a window having a PV value of 0.35 wavelength.
[0306] The second-second image IM2b-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the second-second image IM2b-2 may be an image obtained by photographing the top surface of the window having a PV value of 0.60 wavelength.
[0307] The coating CL-1 using the multilayer coating method according to the disclosed embodiment may have a thickness CH2 in the range of 25 μm to 35 μm. When the thickness CH2 is less than 25 μm, even when the coating is formed of a single layer without using the multilayer coating method, the PV value may be equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, like the coating formed of a single layer and having the second thickness Hb.
[0308] The coating CL-1 formed of two layers may have a third thickness Hc. The third thickness Hc may be about 28 μm. In this regard, the average value of the PV value may be 0.54 wavelengths, and the maximum value of the PV value may be 0.86 wavelengths. In this regard, the difference between the average value of the PV value in the coating having the third thickness Hc and the average value of the PV value in the coating having the first thickness Ha may be 1.79 wavelengths.
[0309] The third-first image IM3b-1 and the third-second image IM3b-2 may be images obtained by photographing the window WIN-2 including the coating layer CL-1 formed of two layers and having the third thickness Hc.
[0310] The third-first image IM3b-1 may be an image obtained by photographing the top surface of the window WIN-2 having an average value of the PV value. For example, the third-first image IM3b-1 may be an image obtained by photographing the top surface of the window WIN-2 having a PV value of 0.54 wavelength.
[0311] The third-second image IM3b-2 may be an image obtained by photographing the top surface of the window WIN-2 having the maximum value of the PV value. For example, the third-second image IM3b-2 may be an image obtained by photographing the top surface of the window WIN-2 having a PV value of 0.86 wavelength.
[0312] The third-first image IM3b-1 may have a greater uniformity of thickness in the sensor area UA than the first-first image IM1b-1. The third-second image IM3b-2 may have a greater uniformity of thickness in the sensor area UA than the first-second image IM1b-2.
[0313] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as the edge bead phenomenon is reduced or eliminated. The window WIN-2 can be coated with a coating for improving the impact resistance of the substrate 10 in multiple layers. In this embodiment, the coating CL-1 formed of two layers and having a third thickness Hc can have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In this embodiment, the edge bead phenomenon in the sensor area UA can be reduced or eliminated, so that the optical characteristics of the sensor area UA can be improved. Therefore, a window WIN-2 with improved impact resistance and flatness can be provided.
[0314] The coating formed of three layers may have a fourth thickness Hd. The fourth thickness Hd may be 40 μm. In this regard, the average value of the PV value may be 0.66 wavelengths, and the maximum value of the PV value may be 1.42 wavelengths. In this regard, the difference between the average value of the PV value in the coating having the fourth thickness Hd and the average value of the PV value in the coating having the first thickness Ha may be 1.67 wavelengths.
[0315] The fourth-first image IM4b-1 and the fourth-second image IM4b-2 may be images obtained by photographing a window including a coating layer formed of three layers and having a fourth thickness Hd.
[0316] The fourth-first image IM4b-1 may be an image obtained by photographing the top surface of the window having an average value of the PV value. For example, the fourth-first image IM4b-1 may be an image obtained by photographing the top surface of the window having a PV value of 0.66 wavelength.
[0317] The fourth-second image IM4b-2 may be an image obtained by photographing the top surface of the window having the maximum value of the PV value. For example, the fourth-second image IM4b-2 may be an image obtained by photographing the top surface of the window having a PV value of 1.42 wavelengths.
[0318] The coating CL-1 using the multilayer coating method according to one embodiment of the disclosure may have a thickness CH2 in the range of 25 μm to 35 μm. In the case where the thickness CH2 is greater than 35 μm, the repulsive force between the multiple layers may increase, and the risk of buckling due to the reduction in interfacial adhesion may increase. Therefore, the PV value may deviate from the range of equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths.
[0319] Fig.13 is a box plot showing PV values for windows formed using a multi-stage coating method and a multi-layer coating method according to disclosed embodiments.
[0320] Reference Figure 6J , Fig.11J and Fig.13 In the process 20-1 of forming a single layer with one coating, in a window including a coating having a thickness of 20 μm, an average value of the PV value may be 0.70 wavelengths and a maximum value of the PV value may be 1.14 wavelengths. The coating formed by the process 20-1 may be referred to as a first existing coating.
[0321] In the window WIN-1 including the coating CL having a thickness of 20 μm using the multi-stage coating process 20-2 according to the disclosed embodiment, the average value of the PV value may be 0.49 wavelengths, and the maximum value of the PV value may be 0.63 wavelengths. The coating CL formed by the multi-stage coating process 20-2 may have an average value of the PV value having a difference of 0.21 wavelengths from the average value of the PV value of the first existing coating, and have a maximum value of the PV value having a difference of 0.51 wavelengths from the maximum value of the PV value of the first existing coating.
[0322] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined that the edge bead phenomenon is reduced or eliminated. The window WIN-1 can be coated with a coating for improving the impact resistance of the substrate 10 multiple times. The coating CL formed by the multi-stage coating process 20-2 can have a thickness in the range of 20 μm to 30 μm, and the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the sensor area UA (see Figure 1A ) in the edge bead phenomenon, so that the sensor area UA (see Figure 1A ) optical properties. Therefore, a window WIN-1 having improved impact resistance and flatness can be provided.
[0323] In process 30-1 of forming a single layer with one coating, in a window including a coating having a thickness of 30 μm, an average value of PV value may be 1.77 wavelengths and a maximum value of PV value may be 2.39 wavelengths. The coating formed by process 30-1 may be referred to as a second existing coating.
[0324] In the window WIN-2 including the coating CL-1 having a thickness of 30 μm using the multi-layer coating process 30-2 according to the disclosed embodiment, the average value of the PV value may be 0.53 wavelengths, and the maximum value of the PV value may be 0.77 wavelengths. The coating CL-1 formed by the multi-layer coating process 30-2 may have an average value of the PV value having a difference of 1.24 wavelengths from the average value of the PV value of the second existing coating, and have a maximum value of the PV value having a difference of 1.62 wavelengths from the maximum value of the PV value of the second existing coating.
[0325] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as the edge bead phenomenon is reduced or eliminated. The window WIN-2 can be coated with a coating for improving the impact resistance of the substrate 10 in multiple layers. The coating CL-1 formed by the multi-layer coating process 30-2 can have a thickness in the range of 25 μm to 35 μm, and the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the sensor area UA (see Figure 1A ) in the edge bead phenomenon, so that the sensor area UA (see Figure 1A ) optical properties. Therefore, a window WIN-2 having improved impact resistance and flatness can be provided.
[0326] Fig.14 is a flow chart showing a method of manufacturing a window according to a disclosed embodiment, and Fig.15A is a perspective view showing the process of the window manufacturing method according to the disclosed embodiment. Fig.15A In the above reference Fig. 6A The same or similar components as those described above are marked with the same or similar reference numerals, and any repeated detailed description thereof will be omitted.
[0327] Reference Fig.14 , used to make windows WIN (see Figure 3 ) may include: performing plasma treatment on the surface of the substrate (S130); applying a solution multiple times to form a plurality of portions (S230); curing the plurality of portions to form a first coating layer (S330); performing plasma treatment on the surface of the first coating layer (S430); applying a solution multiple times to form a plurality of portions (S530); and curing the plurality of portions to form a second coating layer (S630). This will be described later.
[0328] Fig.15A A process ( S130 ) of performing plasma treatment on the surface of the substrate 10 is shown.
[0329] In an embodiment, the preliminary window WIN-3a may include a substrate 10. Plasma PS may be provided to the preliminary window WIN-3a for plasma treatment. The plasma PS may pre-treat a surface of the substrate 10.
[0330] FIG. 15B to FIG. 15E is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0331] Reference Fig.14 , Fig. 15B , Fig. 15C , Fig.15D and Fig.15E, a plurality of parts may be formed by applying the solution multiple times (S230).
[0332] The sixth solution SOL6 may be applied to the preliminary window WIN-3b. The sixth solution SOL6 may be applied to the substrate 10 and may form the first portion L1-2. The sixth solution SOL6 may be mixed with the first solution SOL1 (see Figure 6B ) are basically the same.
[0333] The sixth solution SOL6 may be applied by spraying. The nozzle SPY may apply the sixth solution SOL6 to the surface of the substrate 10.
[0334] The sixth solution SOL6 may be applied along a zigzag path along the first direction DR1. Shape-coating the sixth solution SOL6 The sixth solution SOL6 may be coated on the substrate 10 along the first path R1.
[0335] The sixth solution SOL6 applied to the substrate 10 may be formed into a first portion L1-2. The first portion L1-2 may be liquid.
[0336] The first portion L1-2 may be formed to have a first thickness H1-2. The first thickness H1-2 may be in the range of 3.3 μm to 6.7 μm.
[0337] The seventh solution SOL7 may be applied to the preliminary window WIN-3c. The seventh solution SOL7 may be applied to the first portion L1-2, and may form the second portion L2-2. The seventh solution SOL7 may be substantially the same as the sixth solution SOL6.
[0338] The seventh solution SOL7 may be applied by spraying. The nozzle SPY may apply the seventh solution SOL7 onto the first portion L1-2.
[0339] The seventh solution SOL7 may be applied along a path in a zigzag shape in a direction opposite to the first direction DR1. Shape-coating the seventh solution SOL7 The seventh solution SOL7 may be applied onto the first portion L1 - 2 along the second path R2 .
[0340] The seventh solution SOL7 applied to the first portion L1-2 may be formed into the second portion L2-2. The second portion L2-2 may be liquid.
[0341] The second portion L2-2 may be formed to have a second thickness H2-2. The second thickness H2-2 may be in the range of 3.3 μm to 6.7 μm. The second thickness H2-2 may be substantially the same as the first thickness H1-2.
[0342] The eighth solution SOL8 may be applied to the preliminary window WIN-3d. The eighth solution SOL8 may be applied to the second portion L2-2, and may form the third portion L3-2. The eighth solution SOL8 may be substantially the same as the seventh solution SOL7.
[0343] The eighth solution SOL8 may be applied by spraying. The nozzle SPY may apply the eighth solution SOL8 onto the second portion L2-2.
[0344] The eighth solution SOL8 may be applied along a path in a zigzag shape along the first direction DR1. The eighth solution SOL8 may be applied to the second portion L2-2 along the third path R3. The third path R3 may be substantially the same as the first path R1.
[0345] The eighth solution SOL8 applied to the second portion L2-2 may be formed into the third portion L3-2. The third portion L3-2 may be liquid.
[0346] The third portion L3-2 may be formed to have a third thickness H3-2. The third thickness H3-2 may be in the range of 3.3 μm to 6.7 μm. The third thickness H3-2 may be substantially the same as the second thickness H2-2.
[0347] The preliminary window WIN-3 e in which the first coating process is completed may have a shape in which the first portion L1 - 2 , the second portion L2 - 2 , and the third portion L3 - 2 are sequentially stacked on the substrate 10 .
[0348] The first thickness H1-2 of the first portion L1-2, the second thickness H2-2 of the second portion L2-2, and the third thickness H3-2 of the third portion L3-2 may be substantially the same as one another.
[0349] Fig.15F and Figure 15G is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0350] Reference Fig.14 , Fig.15F and Figure 15G , a first coating layer L1a may be formed in the preliminary window WIN-3f ( S330 ).
[0351] A curing module UVM may be provided on the preliminary window WIN-3f. The curing module UVM may irradiate ultraviolet rays UV to the preliminary window WIN-3f. The curing module UVM may be moved along the second direction DR2.
[0352] The first part L1-2, the second part L2-2 and the third part L3-2 may be cured at the same time. The cured first part L1-2, the second part L2-2 and the third part L3-2 may be referred to as a first coating layer L1a. That is, the first coating layer L1a may be formed in a multi-stage coating method. The first coating layer L1a may be a solid layer.
[0353] The first coating layer L1a may have a first thickness LH1. The first thickness LH1 may be in the range of 10 μm to 20 μm.
[0354] Figure 15G A process ( S430 ) of performing plasma treatment on the surface of the first coating layer L1 a is shown.
[0355] Plasma PS may be provided to the preliminary window WIN-3g. Plasma PS may pre-treat the surface of the first coating layer L1a.
[0356] FIG. 15H to FIG. 15K is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0357] Reference Fig.14 , Fig.15H , Fig.15I , Fig.15J and Figure 15K , the solution may be applied multiple times to form a plurality of parts (S530).
[0358] The ninth solution SOL9 may be applied to the preliminary window WIN-3h. The ninth solution SOL9 may be applied to the first coating layer L1a and may form a fourth portion L4-2. The ninth solution SOL9 may be applied to the sixth solution SOL6 (see Fig. 15B ) are basically the same.
[0359] The ninth solution SOL9 may be applied by spraying. The nozzle SPY may apply the ninth solution SOL9 to the surface of the first coating layer L1a.
[0360] The ninth solution SOL9 may be applied along a path in a zigzag shape along the first direction DR1. Shape-coating the ninth solution SOL9 The ninth solution SOL9 may be applied onto the first coating layer L1a along the first path R1.
[0361] The ninth solution SOL9 applied onto the first coating layer L1a may be formed as a fourth portion L4-2. The fourth portion L4-2 may be liquid.
[0362] The fourth portion L4-2 may be formed to have a fourth thickness H4-2. The fourth thickness H4-2 may be in the range of 3.3 μm to 6.7 μm.
[0363] The tenth solution SOL10 may be applied to the preliminary window WIN-3i. The tenth solution SOL10 may be applied to the fourth portion L4-2, and the fifth portion L5-2 may be formed. The tenth solution SOL10 may be substantially the same as the ninth solution SOL9.
[0364] The tenth solution SOL10 may be applied by spraying. The nozzle SPY may apply the tenth solution SOL10 to the surface of the fourth portion L4-2.
[0365] The tenth solution SOL10 may be applied along a path in a zigzag shape in a direction opposite to the first direction DR1. The tenth solution SOL10 may be applied onto the fourth portion L4 - 2 along the second path R2 .
[0366] The tenth solution SOL10 applied to the fourth portion L4-2 may be formed into the fifth portion L5-2. The fifth portion L5-2 may be liquid.
[0367] The fifth portion L5-2 may be formed to have a fifth thickness H5-2. The fifth thickness H5-2 may be in the range of 3.3 μm to 6.7 μm. The fifth thickness H5-2 may be substantially the same as the fourth thickness H4-2.
[0368] The eleventh solution SOL11 may be applied to the preliminary window WIN-3j. The eleventh solution SOL11 may be applied to the fifth portion L5-2, and the sixth portion L6-2 may be formed. The eleventh solution SOL11 may be substantially the same as the tenth solution SOL10.
[0369] The eleventh solution SOL11 may be applied by spraying. The nozzle SPY may apply the eleventh solution SOL11 to the surface of the fifth portion L5-2.
[0370] The eleventh solution SOL11 may be applied along a path in a zigzag shape along the first direction DR1. The eleventh solution SOL11 may be applied to the fifth portion L5-2 along the third path R3. The third path R3 may be substantially the same as the first path R1.
[0371] The eleventh solution SOL11 applied to the fifth portion L5-2 may be formed into the sixth portion L6-2. The sixth portion L6-2 may be liquid.
[0372] The sixth portion L6-2 may be formed to have a sixth thickness H6-2. The sixth thickness H6-2 may be in the range of 3.3 μm to 6.7 μm. The sixth thickness H6-2 may be substantially the same as the fifth thickness H5-2.
[0373] The preliminary window WIN-3k in which the second coating process is completed may have a shape in which the fourth portion L4-2, the fifth portion L5-2, and the sixth portion L6-2 are sequentially stacked on the first coating layer L1a.
[0374] The fourth thickness H4-2 of the fourth portion L4-2, the fifth thickness H5-2 of the fifth portion L5-2, and the sixth thickness H6-2 of the sixth portion L6-2 may be substantially the same as one another.
[0375] Figure 15L and Figure 15M is a perspective view showing the process of a window manufacturing method according to a disclosed embodiment.
[0376] Reference Fig.14 , Figure 15L and Figure 15M , a second coating layer L2a may be formed in the preliminary window WIN-31 (S630).
[0377] A curing module UVM may be provided on the preliminary window WIN-31. The curing module UVM may irradiate ultraviolet rays UV to the preliminary window WIN-31. The curing module UVM may be moved along the second direction DR2.
[0378] The fourth part L4-2, the fifth part L5-2 and the sixth part L6-2 can be cured at the same time. The cured fourth part L4-2, the fifth part L5-2 and the sixth part L6-2 can be referred to as the second coating layer L2a. That is, the second coating layer L2a can be formed by a multi-stage coating method. The second coating layer L2a can be a solid layer.
[0379] The second coating layer L2a may have a second thickness LH2. The second thickness LH2 may be in the range of 10 μm to 20 μm.
[0380] The window WIN-3 may be manufactured by an embodiment of this window manufacturing method. The window WIN-3 may include a substrate 10 and a coating CL-2. The coating CL-2 may be disposed on the substrate 10. The coating CL-2 may improve the impact resistance of the substrate 10 and prevent the substrate 10 from breaking or scattering when the substrate 10 is damaged.
[0381] The coating CL-2 may include a first coating L1a and a second coating L2a. Each of the first coating L1a and the second coating L2a may be formed by a multi-stage coating method, and the coating CL-2 may be formed by a multi-layer coating method. Forming the coating CL-2 using both multi-stage coating and multi-layer coating may be referred to as a hybrid coating method.
[0382] The coating layer CL-2 may have a predetermined thickness CH3. The thickness CH3 may be in the range of 20 μm to 40 μm.
[0383] Fig.16A is a box plot showing PV values for each coating method according to the disclosed embodiments, Fig. 16B Captured images of the window for each coating method according to the disclosed embodiments are shown.
[0384] Reference Figure 6J , Fig.11J , Figure 15M , Fig.16A and Fig. 16B ,exist Fig.16A , the horizontal axis shows the window for each coating method, and the vertical axis shows the PV value. The PV value shows 0 wavelength to 1.2 wavelength as an example. In this regard, 1 wavelength can be about 632.8nm.
[0385] The first window WIN-1 may be formed using a multi-stage coating A1 method, the second window WIN-2 may be formed using a multi-layer coating A2 method, and the third window WIN-3 may be formed using a hybrid coating A3 method.
[0386] That is, the coating CL of the first window WIN-1 may be formed using the multi-stage coating A1 method, the coating CL-1 of the second window WIN-2 may be formed using the multi-layer coating A2 method, and the coating CL-2 of the third window WIN-3 may be formed using the hybrid coating A3 method.
[0387] Each of images IM1c-1 and IM1c-2 obtained by photographing the first window WIN-1, images IM2c-1 and IM2c-2 obtained by photographing the second window WIN-2, and images IM3c-1 and IM3c-2 obtained by photographing the third window WIN-3 shows the thickness of the coating via a horizontal curve.
[0388] The coating layer CL of the first window WIN-1 may have a thickness CH of about 20 μm. In this regard, an average value of the PV value may be 0.41 wavelengths, and a maximum value of the PV value may be 0.89 wavelengths.
[0389] The first-first image IM1c-1 and the first-second image IM1c-2 may be images obtained by photographing the first window WIN-1 including the coating layer CL formed through the multi-stage coating A1 method.
[0390] The first-first image IM1c-1 may be an image obtained by photographing the top surface of the first window WIN-1 having an average value of the PV value. For example, the first-first image IM1c-1 may be an image obtained by photographing the top surface of the first window WIN-1 having a PV value of 0.41 wavelength.
[0391] The first-second image IM1c-2 may be an image obtained by photographing the top surface of the first window WIN-1 having the maximum value of the PV value. For example, the first-second image IM1c-2 may be an image obtained by photographing the top surface of the first window WIN-1 having a PV value of 0.89 wavelength.
[0392] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as that the edge bead phenomenon is reduced or eliminated. The first window WIN-1 can form a coating CL for improving the impact resistance of the substrate 10 by a multi-stage coating A1 method. The coating CL can have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the edge bead phenomenon in the sensor area UA can be reduced or eliminated, so that the optical characteristics of the sensor area UA can be improved. Therefore, a first window WIN-1 with improved impact resistance and flatness can be provided.
[0393] The coating CL-1 of the window WIN-2 may have a thickness CH2 of about 28 μm. In this regard, the average value of the PV value may be 0.54 wavelengths, and the maximum value of the PV value may be 0.86 wavelengths.
[0394] The second-first image IM2c-1 and the second-second image IM2c-2 may be images obtained by photographing the second window WIN-2 including the coating layer CL-1 formed through the multi-layer coating A2 method.
[0395] The second-first image IM2c-1 may be an image obtained by photographing the top surface of the second window WIN-2 having an average value of the PV value. For example, the second-first image IM2c-1 may be an image obtained by photographing the top surface of the second window WIN-2 having a PV value of 0.54 wavelength.
[0396] The second-second image IM2c-2 may be an image obtained by photographing the top surface of the second window WIN-2 having the maximum value of the PV value. For example, the second-second image IM2c-2 may be an image obtained by photographing the top surface of the second window WIN-2 having a PV value of 0.86 wavelength.
[0397] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as the edge bead phenomenon is reduced or eliminated. The second window WIN-2 can form a coating CL-1 for improving the impact resistance of the substrate 10 by a multilayer coating A2 method. The coating CL-1 can have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the edge bead phenomenon in the sensor area UA can be reduced or eliminated, so that the optical characteristics of the sensor area UA can be improved. Therefore, a second window WIN-2 with improved impact resistance and flatness can be provided.
[0398] The coating CL-2 of the window WIN-3 may have a thickness CH3 of about 35 μm. In this regard, the average value of the PV value may be 0.62 wavelengths, and the maximum value of the PV value may have 1.18 wavelengths.
[0399] The third-first image IM3c-1 and the third-second image IM3c-2 may be images obtained by photographing the third window WIN-3 including the coating CL-2 formed by the hybrid coating A3 method. The hybrid coating A3 may be a process of forming the coating CL-2 using both the multi-stage coating A1 method and the multi-layer coating A2 method.
[0400] The third-first image IM3c-1 may be an image obtained by photographing the top surface of the third window WIN-3 having an average value of the PV value. For example, the third-first image IM3c-1 may be an image obtained by photographing the top surface of the third window WIN-3 having a PV value of 0.62 wavelength.
[0401] The third-second image IM3c-2 may be an image obtained by photographing the top surface of the third window WIN-3 having the maximum value of the PV value. For example, the third-second image IM3c-2 may be an image obtained by photographing the top surface of the third window WIN-3 having a PV value of 1.18 wavelengths.
[0402] According to the disclosed embodiment, when the PV value is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as reducing or eliminating the edge bead phenomenon. The third window WIN-3 can form a coating CL-2 for improving the impact resistance of the substrate 10 by a mixed coating A3 method. The coating CL-2 can have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the edge bead phenomenon in the sensor area UA can be reduced or eliminated, so that the optical properties of the sensor area UA can be improved. Therefore, a third window WIN-3 with improved impact resistance and flatness can be provided.
[0403] Figures 17A to 17F A window according to a disclosed embodiment is shown.
[0404] Reference Fig.17A , an embodiment of the window WIN-4 may include a substrate 10 and two coating layers CL. One coating layer CL may be disposed on the substrate 10, and another coating layer CL may be disposed below the substrate 10. Another coating layer CL may be disposed opposite to one coating layer CL. That is, the two coating layers CL may be spaced apart from each other, and the substrate 10 may be placed between the two coating layers CL.
[0405] One coating layer CL may be formed on the substrate 10 , and then another coating layer CL may be formed under the substrate 10 .
[0406] Each of the two coating layers CL may be formed by a multi-stage coating method.
[0407] Reference Fig. 17B , an embodiment of the window WIN-5 may include a substrate 10 and two coatings CL-1. One coating CL-1 may be disposed on the substrate, and the other coating CL-1 may be disposed below the substrate 10. The other coating CL-1 may be disposed opposite to the one coating CL-1. That is, the two coatings CL-1 may be spaced apart from each other, and the substrate 10 is placed between the two coatings CL-1.
[0408] One coating layer CL-1 may be formed on the substrate 10 , and then another coating layer CL-1 may be formed under the substrate 10 .
[0409] Each of the two coating layers CL-1 may be formed by a multilayer coating method.
[0410] Reference Fig. 17C, an embodiment of the window WIN-6 may include a substrate 10 and two coatings CL and CL-1 formed by different methods. One coating CL may be disposed on the substrate, and another coating CL-1 may be disposed below the substrate 10. Another coating CL-1 may be disposed opposite to one coating CL. That is, the two coatings CL and CL-1 may be spaced apart from each other, and the substrate 10 is placed between the two coatings CL and CL-1.
[0411] One coating layer CL may be formed on the substrate 10 , and then another coating layer CL- 1 may be formed under the substrate 10 .
[0412] One coating layer CL may be formed by a multi-stage coating method, and another coating layer CL-1 may be formed by a multi-layer coating method.
[0413] Reference Fig.17D , an embodiment of the window WIN-7 may include a substrate 10 and two coatings CL and CL-2 formed by different methods. One coating CL may be disposed on the substrate, and another coating CL-2 may be disposed below the substrate. Another coating CL-2 may be disposed opposite to one coating CL. That is, the two coatings CL and CL-2 may be spaced apart from each other, and the substrate 10 is placed between the two coatings CL and CL-2.
[0414] One coating layer CL may be formed on the substrate 10 , and then another coating layer CL- 2 may be formed under the substrate 10 .
[0415] One coating layer CL may be formed by a multi-stage coating method, and another coating layer CL-2 may be formed by a hybrid coating method.
[0416] Reference Fig.17E , an embodiment of the window WIN-8 may include a substrate 10 and two coatings CL-1 and CL-2 formed by different methods. One coating CL-1 may be disposed on the substrate, and the other coating CL-2 may be disposed below the substrate 10. The other coating CL-2 may be disposed opposite to the one coating CL-1. That is, the two coatings CL-1 and CL-2 may be spaced apart from each other, and the substrate 10 is placed between the two coatings CL-1 and CL-2.
[0417] One coating layer CL-1 may be formed on the substrate 10 , and then another coating layer CL-2 may be formed under the substrate 10 .
[0418] One coating layer CL-1 may be formed by a multilayer coating method, and the other coating layer CL-2 may be formed by a hybrid coating method.
[0419] Reference Fig.17F, an embodiment of the window WIN-9 may include a substrate 10 and two coatings CL-2. One coating CL-2 may be disposed on the substrate, and the other coating CL-2 may be disposed below the substrate 10. The other coating CL-2 may be disposed opposite to the one coating CL-2. That is, the two coatings CL-2 may be spaced apart from each other, and the substrate 10 is placed between the two coatings CL-2.
[0420] One coating layer CL-2 may be formed on the substrate 10 , and then another coating layer CL-2 may be formed under the substrate 10 .
[0421] Each of the two coating layers CL-2 may be formed by a hybrid coating method.
[0422] In an embodiment of the invention, as described above, when the PV value, which is the difference between the maximum value and the minimum value (peak to valley) of the wavefront aberration, is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths, it can be defined as that the edge bead phenomenon is reduced or eliminated. In an embodiment, the window may be coated with a coating for improving the impact resistance of the substrate multiple times. In such an embodiment, the coating formed by the three-coating process may have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. Therefore, in such an embodiment, the edge bead phenomenon in the sensor area can be reduced or eliminated, so that the optical characteristics of the sensor area can be improved. Therefore, a display device including a window with improved impact resistance and flatness can be provided.
[0423] In addition, according to an embodiment of the invention, the window may be formed with a coating formed of a plurality of layers for improving the impact resistance of the substrate. The coating formed of two layers and having a predetermined thickness may have a PV value equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths. In such an embodiment, the edge bead phenomenon in the sensor region may be reduced or eliminated, so that the optical characteristics of the sensor region may be improved. Therefore, a display device including a window having improved impact resistance and flatness may be provided.
[0424] The invention should not be construed as being limited to the embodiments set forth herein. Rather, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the concept of the invention to those skilled in the art.
[0425] While the invention has been particularly shown and described with reference to embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the spirit or scope of the invention as defined by the claims.
Claims
1. A method for manufacturing a window, the method The following steps are involved: performing a plasma treatment on a surface of a substrate; performing a first coating operation by coating a first solution onto the substrate to form a first portion; performing a second coating operation by applying a second solution onto the first portion to form a second portion; performing a third coating operation by applying a third solution onto the second portion to form a third portion; as well as A first coating layer is formed by simultaneously curing the first to third portions.
2. The method according to claim 1, in, The first solution and the second solution include the same material as each other.
3. The method according to claim 1, in, the first portion has a thickness in the range of 6.7 μm to 10 μm, wherein the second portion has a thickness in the range of 6.7 μm to 10 μm, Wherein, the third portion has a thickness in a range of 6.7 μm to 10 μm.
4. The method according to claim 1, in, Performing the first coating operation includes coating the first solution along a path in a zigzag shape along a first direction by using a spray coating method.
5. The method according to claim 4, in, Performing the second coating operation includes coating the second solution along a path in the zigzag shape in a direction opposite to the first direction by using the spray coating method.
6. The method according to claim 1, further comprising: The following steps are involved: After forming the first coating layer, a second coating layer is formed on the first coating layer.
7. The method according to claim 6, in, Forming the second coating layer comprises: performing the plasma treatment on the surface of the first coating layer; forming a fourth portion by applying a fourth solution onto the first coating; forming a fifth portion by applying a fifth solution to the fourth portion; forming a sixth portion by applying a sixth solution onto the fifth portion; and The fourth to sixth parts are cured at the same time.
8. The method according to claim 6, in, Each of the first coating layer and the second coating layer has a thickness in a range of 10 μm to 20 μm.
9. The method according to claim 1, further comprising: The following steps are involved: After forming the first coating layer, a third coating layer is formed under the substrate.
10. A method for manufacturing a window, the method The following steps are involved: performing a plasma treatment on a surface of a substrate; performing a first coating operation by coating a first solution onto the substrate to form a first portion; forming a first layer by curing the first portion; performing the plasma treatment on a surface of the first layer; performing a second coating operation by coating a second solution onto the first layer to form a second portion; as well as A second layer is formed by curing the second portion, wherein the first layer and the second layer together define a first coating.
11. The method according to claim 10, in, The first layer has a thickness in the range of 10 μm to 15 μm.
12. The method according to claim 11, in, The second layer has a thickness in the range of 10 μm to 15 μm.
13. The method according to claim 10, in, The first solution does not include a leveling agent, Wherein, the second solution includes the leveling agent.
14. The method according to claim 10, in, Performing the first coating operation includes coating the first solution along a path in a zigzag shape along a first direction by using a spray coating method.
15. The method according to claim 14, in, Performing the second coating operation includes coating the second solution along a path in the zigzag shape along the first direction by using the spray coating method.
16. The method according to claim 10, further comprising: The following steps are involved: After forming the first layer and forming the second layer, a second coating layer is formed under the substrate.
17. A display device, the display device include: Display panel; as well as A window is provided on the display panel, Wherein, the window comprises: a substrate; and a first coating disposed on the substrate, wherein the first coating layer is a solid layer formed by solidifying a solution, wherein the solution has a viscosity in the range of 6 cp to 10 cp, Wherein, the difference between the maximum value and the minimum value of the wavefront aberration of the first coating is equal to or greater than 0.2 wavelengths and equal to or less than 0.92 wavelengths.
18. The display device according to claim 17, in, The first coating layer has a thickness in the range of 20 μm to 30 μm.
19. The display device according to claim 17, in, The first coating layer includes a first layer and a second layer stacked on each other, The first layer and the second layer include the same material.
20. The display device according to claim 17, wherein the display device further comprises: include: A second coating is disposed below the substrate and opposite to the first coating.