Secondary battery and electronic device

By controlling the particle size and proportion of silicon-carbon composite particles and optimizing the electrolyte composition, the problem of increasing resistivity of secondary batteries in high temperature and fast charging cycles is solved, and the energy density and electrochemical performance are improved. stability.

CN119029149APending Publication Date: 2024-11-26NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093298.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the high-temperature cycle and fast charging cycle of secondary batteries, the volume expansion and contraction of silicon-carbon composite particles lead to displacement of conductive agent, causing a significant increase in resistivity and affecting electrochemical performance.

Method used

By controlling the average particle size and proportion of silicon element mass of silicon carbon composite particles, optimizing the ratio of electrolyte components, such as propylene carbonate and vinyl carbonate, improving the film-forming quality and conductive agent connection of solid electrolyte interface films, reducing the conductive network Possibility of road breakage.

Benefits of technology

The energy density of secondary batteries is improved under high temperature and fast charging conditions, while reducing the growth rate of high temperature cycle and fast charging resistance, and extending battery life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004987724250000201
    Figure BDA0004987724250000201
  • Figure BDA0004987724250000211
    Figure BDA0004987724250000211
  • Figure BDA0004987724250000221
    Figure BDA0004987724250000221
Patent Text Reader

Abstract

The invention provides a secondary battery and electronic equipment. The secondary battery comprises a negative electrode, a positive electrode and an electrolyte, the negative electrode comprises a negative electrode current collector and a negative electrode mixture layer arranged on at least one surface of the negative electrode current collector, the negative electrode mixture layer contains a conductive agent and silicon-carbon composite particles, the average particle size of the silicon-carbon composite particles is D [mu] m, the silicon-carbon composite particles contain silicon elements and carbon elements, and the average particle size of the silicon-carbon composite particles is D [mu] m. Based on the mass sum of the silicon element and the carbon element, the mass ratio of the silicon element is C%, and C / D2 is greater than or equal to 0.21 and less than or equal to 1.2; the electrolyte comprises propylene carbonate and ethylene carbonate, based on the mass of the electrolyte, the sum of the mass percentage content of propylene carbonate and ethylene carbonate is H%, and H is larger than or equal to 15 and smaller than or equal to 50. According to the secondary battery provided by the invention, relatively high energy density is realized, and meanwhile, the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate are both improved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of a patent application with an application date of May 10, 2024, an application number of 202410574920.8, and an invention name of “Secondary Batteries and Electronic Devices”. Technical Field

[0002] The present application belongs to the field of energy storage technology, and specifically relates to a secondary battery and an electronic device. Background Art

[0003] As a solution for energy storage and supply, secondary batteries are an important choice to meet the needs of sustainable development. With the continuous expansion of its application fields, the requirements for the energy density of secondary batteries are also increasing. Graphite materials are widely used as traditional negative electrode materials, but their theoretical capacity is limited. In contrast, silicon materials have higher theoretical capacity, abundant sources, and low prices, and have the potential to become a new generation of secondary battery materials. However, silicon materials will expand and shrink to a large extent during the insertion and extraction of metal ions, resulting in the degradation of electrochemical performance. Therefore, while improving the energy density, it is necessary to avoid the degradation of other electrochemical properties of secondary batteries to ensure that silicon materials are widely used. Summary of the invention

[0004] The purpose of the present application is to provide a secondary battery and an electronic device, which can achieve a higher energy density while improving the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0005] In the first aspect, the present application provides a secondary battery and an electronic device. The secondary battery includes a negative electrode, a positive electrode and an electrolyte, the negative electrode includes a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, the negative electrode mixture layer contains a conductive agent and silicon-carbon composite particles, the average particle size of the silicon-carbon composite particles is Dμm, the silicon-carbon composite particles contain silicon and carbon, based on the sum of the masses of the silicon and carbon, the mass proportion of the silicon is C%, 0.21≤C / D 2 ≤1.2; the electrolyte includes propylene carbonate and ethylene carbonate, and the sum of the mass percentages of propylene carbonate and ethylene carbonate is H%, based on the mass of the electrolyte, 15≤H≤50. The secondary battery provided in the present application achieves a higher energy density while improving the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0006] The inventors found that the resistivity of secondary batteries containing silicon-carbon composite particles increased significantly after cycling. This type of performance deterioration is particularly evident after high-temperature cycling and fast-charging cycling. By performing the above-mentioned settings on the secondary battery, it is possible to achieve a higher energy density while taking into account the improvement of the high-temperature cycle resistance growth rate and the fast-charging cycle resistance growth rate. The inventors speculate that in the process of embedding and extracting metal ions, the volume of the silicon-carbon composite particles expands and contracts to a large extent, causing the conductive agent to displace with the expansion of the silicon-carbon composite particles, and the displacement of the conductive agent cannot be completely restored with the contraction of the silicon-carbon particles, causing the conductive network inside the negative electrode to be broken. During high-temperature cycling and fast-charging cycles, the volume of the silicon-carbon composite particles expands and contracts to a greater extent and at a faster speed, and the conductive network inside the negative electrode is more likely to be broken, resulting in a significant increase in the resistivity of the secondary battery after high-temperature cycling and fast-charging cycles. The average particle size Dμm of the silicon-carbon composite particles will affect the stacking morphology of the silicon-carbon composite particles inside the negative electrode, and thus affect the distribution state and movable space of the conductive agent inside the negative electrode; the mass percentage C% of the silicon element will affect the degree and speed of volume expansion and contraction of the silicon-carbon composite particles. By controlling the average particle size Dμm of the silicon-carbon composite particles and the mass percentage C% of the silicon element, the following is satisfied: 0.21≤C / D 2 ≤1.2, so that the secondary battery can achieve a higher energy density while improving the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate. On this basis, by adjusting the sum of the mass percentages of propylene carbonate and ethylene carbonate in the electrolyte to meet 15≤H≤50, the film-forming quality of the solid electrolyte interface film on the surface of the silicon-carbon composite particles can be optimized, the connection between the silicon-carbon composite particles and the conductive agent can be strengthened, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery can be further improved.

[0007] In some embodiments, 0.39≤C / D 2 ≤0.96. By adjusting C / D 2 When the value is within the above range, the coordination relationship between the movable space of the conductive agent and the degree and speed of volume expansion and contraction of the silicon-carbon composite particles can be further adjusted, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved.

[0008] In some embodiments, 0.58≤C / D 2 ≤0.88. By adjusting C / D 2 When the value of is within the above range, the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0009] In some embodiments, 7.1≤D≤10.9, 25≤C≤59. By adjusting the value of D and / or C within the above range, the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0010] In some embodiments, the electrolyte includes propyl propionate and ethyl propionate, and the sum of the mass percentages of propyl propionate and ethyl propionate is L%, 12≤L≤39, 18≤H≤44 based on the mass of the electrolyte. By adjusting the value of L and / or H within the above range, the thickness and composition of the solid electrolyte interface film on the surface of the silicon-carbon composite particles can be adjusted, the connection between the silicon-carbon composite particles and the conductive agent can be strengthened, the possibility of a conductive network circuit break inside the negative electrode can be further reduced, and the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be improved.

[0011] In some embodiments, the electrolyte satisfies at least one of the following: (1) 18≤L≤34; (2) 24≤H≤39. By adjusting the value of L and / or H within the above range, the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0012] In some embodiments, the mass percentage of propyl propionate is L1%, the mass percentage of ethyl propionate is L2%, and 1.3≤L1 / L2≤2.8. By adjusting the value of L1 / L2 within the above range, the uniformity of the solid electrolyte interface film can be improved, the connection between the silicon-carbon composite particles and the conductive agent can be strengthened, the possibility of a conductive network break inside the negative electrode can be further reduced, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved. Optionally, 1.7≤L1 / L2≤2.3.

[0013] In some embodiments, the mass percentage of propylene carbonate is H1%, the mass percentage of ethylene carbonate is H2%, and 0.9≤H1 / H2≤2.3. By adjusting the value of H1 / H2 within the above range, the uniformity of the solid electrolyte interface film can be improved, and the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved. Optionally, 1.1≤H1 / H2≤2.0.

[0014] In some embodiments, the electrolyte includes 1,3-propane sultone, and the mass percentage of 1,3-propane sultone is P% based on the mass of the electrolyte, and 2.6≤P≤4.7. By adjusting the value of P within the above range, the elasticity of the solid electrolyte interface film and the ability to connect the conductive agent can be improved, and the possibility of irreversible displacement of the conductive agent during the volume expansion and contraction of the silicon-carbon composite particles can be reduced, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved. Optionally, 3.1≤P≤4.2.

[0015] In some embodiments, the electrolyte includes at least one of fluorobenzene, fluoroethylene carbonate and lithium difluorophosphate, and based on the mass of the electrolyte, the electrolyte satisfies at least one of the following: (1) the mass percentage of fluorobenzene is F1%, 1.1≤F1≤4.3; (2) the mass percentage of fluoroethylene carbonate is F2%, 10.3≤F2≤19.8; (3) the mass percentage of lithium difluorophosphate is F3%, 0.01≤F3≤0.32. By making the electrolyte satisfy at least one of the above conditions, the elasticity of the solid electrolyte interface film and the ability to connect the conductive agent can be improved, the possibility of a conductive network circuit break inside the negative electrode can be further reduced, and the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0016] In some embodiments, the electrolyte includes dimethyl sulfone, and the mass percentage of dimethyl sulfone is S%, based on the mass of the electrolyte, and 1.1≤S≤3.4. By adjusting the value of S within the above range, the elasticity of the solid electrolyte interface film and the ability to adsorb the conductive agent can be improved, and the possibility of irreversible displacement of the conductive agent during the volume expansion and contraction of the silicon-carbon composite particles can be reduced, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved.

[0017] In some embodiments, the electrolyte includes 1,4-dioxane, and the mass percentage of 1,4-dioxane is W%, based on the mass of the electrolyte, and 2.3≤W≤4.6. By adjusting the value of W within the above range, the elasticity of the solid electrolyte interface film and the ability to adsorb the conductive agent can be improved, the connection strength between the silicon-carbon composite particles and the conductive agent can be enhanced, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved.

[0018] In some embodiments, 3.4≤C / F1 2 ≤13.8. By adjusting C / F1 2 When the value is within the above range, the coordination relationship between the elasticity of the solid electrolyte interface film and the degree and speed of volume expansion and contraction of the silicon-carbon composite particles can be further adjusted, the connection strength between the silicon-carbon composite particles and the conductive agent can be enhanced, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved.

[0019] In some embodiments, the silicon-carbon composite particles include a carbon skeleton and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the material of the carbon skeleton includes at least one of artificial graphite, natural graphite, mesophase carbon microbeads, soft carbon or hard carbon.

[0020] In some embodiments, the conductive agent includes carbon nanotubes. The use of a conductive agent including carbon nanotubes can further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0021] The second aspect of the present application provides an electronic device, which includes the secondary battery provided by the first aspect of the present application. The secondary battery provided by the second aspect of the present application achieves a higher energy density while improving the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0022] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. DETAILED DESCRIPTION

[0023] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0024] Unless expressly stated otherwise, the following terms used in this application have the meanings indicated below.

[0025] In the first aspect, the present application provides a secondary battery and an electronic device. The secondary battery includes a negative electrode, a positive electrode and an electrolyte, the negative electrode includes a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, the negative electrode mixture layer contains a conductive agent and silicon-carbon composite particles, the average particle size of the silicon-carbon composite particles is Dμm, the silicon-carbon composite particles contain silicon and carbon, based on the sum of the masses of the silicon and carbon, the mass proportion of the silicon is C%, 0.21≤C / D 2 ≤1.2; the electrolyte includes propylene carbonate and ethylene carbonate, and the sum of the mass percentages of propylene carbonate and ethylene carbonate is H%, based on the mass of the electrolyte, 15≤H≤50. The secondary battery provided in the present application achieves a higher energy density while improving the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0026] negative electrode

[0027] The negative electrode comprises a negative electrode current collector and a negative electrode mixture layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode mixture layer comprises a negative electrode active material. In some embodiments, the chargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material to prevent the active material (e.g., lithium metal) from being accidentally precipitated on the negative electrode during charging.

[0028] The negative electrode active material includes silicon-carbon composite particles. In some embodiments, 0.21≤C / D 2 ≤1.2. In some embodiments, 0.21≤C / D 2 ≤1.17. In some embodiments, 0.39≤C / D 2 ≤1.2. In some embodiments, 0.39≤C / D 2 ≤1.17. In some more preferred embodiments, 0.39≤C / D 2≤0.96. In some more preferred embodiments, 0.39≤C / D 2 ≤0.88. In some more preferred embodiments, 0.58≤C / D 2 ≤0.96. In some more preferred embodiments, 0.58≤C / D 2 ≤0.88. In some embodiments, C / D 2 The values ​​are 0.21, 0.25, 0.28, 0.34, 0.39, 0.43, 0.51, 0.57, 0.58, 0.59, 0.67, 0.73, 0.77, 0.79, 0.88, 0.89, 0.95, 0.96, 0.99, 1.09, 1.13, 1.17, 1.19, 1.2 or a range consisting of any two of these values. By adjusting C / D 2 When the value is within the above range, the coordination relationship between the movable space of the conductive agent and the degree and speed of volume expansion and contraction of the silicon-carbon composite particles can be further adjusted, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved.

[0029] In some embodiments, 7.1≤D≤10.9. In some embodiments, 7.4≤D≤10.9. In some embodiments, 7.1≤D≤9.2. In some embodiments, 7.4≤D≤9.2. In some embodiments, 7.5≤D≤9.2. In some embodiments, 7.4≤D≤8.8. In some embodiments, 7.5≤D≤8.8. In some embodiments, the value of D is 7.1, 7.3, 7.4, 7.5, 7.6, 7.8, 8.2, 8.4, 8.8, 9.0, 9.2, 9.4, 9.5, 9.9, 10.3, 10.5, 10.7, 10.9 or a value within the range of any two of these values. By adjusting the value of D within the above range, the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate can be further improved.

[0030] In some embodiments, 25≤C≤59. In some embodiments, 25≤C≤54. In some embodiments, 33≤C≤59. In some more preferred embodiments, 33≤C≤54. In some more preferred embodiments, 33≤C≤48. In some more preferred embodiments, 45≤C≤54. In some more preferred embodiments, 45≤C≤48. In some embodiments, C is 25, 27, 28, 29, 30, 33, 36, 38, 39, 40, 43, 45, 46, 47, 48, 51, 54, 55, 59 or a value within the range consisting of any two of these values. Adjusting the value of C within the above range can further improve the fast charge cycle resistance growth rate and high temperature cycle resistance growth rate of the secondary battery.

[0031] In some embodiments, the silicon-carbon composite particles include silicon-based materials, silicon-carbon materials (complexes of silicon-based materials and carbon-based materials), or silicon oxide (SiO x , 0<x≤2).

[0032] In some embodiments, the silicon-based material may be silicon particles, silicon alloy particles, etc.

[0033] Exemplarily, the composite of silicon-based substances and carbon-based substances may be an active material obtained by dispersing silicon nanoparticles having an average particle size of 200nm or less on carbon-based substance particles, and then coating with carbon, an active material in which silicon (Si) particles are present on and inside graphite, etc. The average particle size of the secondary particles of the composite of silicon-based substances and carbon-based substances may be 5μm to 20μm. The secondary particles of the composite of silicon-based substances and carbon-based substances in this application refer to silicon-based substance particles and / or carbon-based substance particles in the composite of silicon-based substances and carbon-based substances, such as silicon nanoparticles. The average particle size of silicon nanoparticles may be 5nm or more, for example, 10nm or more, for example, 20nm or more, for example, 50nm or more, for example, 70nm or more. The average particle size of silicon nanoparticles may be 200nm or less, 150nm or less, 100nm or less, 50nm or less, 20nm or less or 10nm or less. For example, the average particle size of silicon nanoparticles may be 100nm to 150nm. The secondary particles of the composite of the silicon-based substance and the carbon-based substance may have an average particle size of 5 μm to 20 μm, for example, 7 μm to 15 μm, for example, 10 μm to 13 μm.

[0034] In some preferred embodiments, the silicon-carbon composite particles include a carbon skeleton and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the material of the carbon skeleton includes at least one of artificial graphite, natural graphite, mesophase carbon microspheres, soft carbon or hard carbon. The use of this type of silicon-carbon composite particles can further improve the fast charge cycle resistance growth rate and high temperature cycle resistance growth rate of the secondary battery.

[0035] In some embodiments, based on the total number of particles in the negative electrode mixture layer, the number of silicon-carbon composite particles accounts for 1% to 25%, for example, the number of silicon-carbon composite particles accounts for 1%, 3%, 6%, 7%, 9%, 11%, 12%, 15%, 17%, 19%, 20%, 21%, 24%, 25% or a value within the range composed of any two of these values. Adjusting the number of silicon-carbon composite particles in the negative electrode mixture layer within the above range can further improve the fast charge cycle resistance growth rate and high temperature cycle resistance growth rate of the secondary battery.

[0036] Optionally, the negative electrode active material may further include an amorphous carbon material, and the amorphous carbon may be soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide or calcined coke, etc.

[0037] In some embodiments, the negative electrode mixture layer includes a conductive agent; the type of the conductive agent is not limited, and any known conductive material can be used. Examples of the conductive agent may include, but are not limited to, carbon black such as acetylene black and Super-P; amorphous carbon materials such as needle coke; carbon nanotubes; graphene, etc. The above conductive agents can be used alone or in any combination.

[0038] In some more preferred embodiments, the conductive agent includes carbon nanotubes. Using the conductive agent including carbon nanotubes can further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0039] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, aluminum foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or a polymer substrate covered with a conductive metal, etc. Among them, the conductive metal includes but is not limited to copper, nickel or titanium, and the material of the polymer substrate includes but is not limited to at least one of polyethylene, polypropylene, ethylene propylene copolymer, polyethylene terephthalate, polyethylene naphthalate or poly(p-phenylene terephthalamide). In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode mixture layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 12μm, and the thickness of the single-sided negative electrode mixture layer is 30μm to 160μm. In the present application, the negative electrode mixture layer can be arranged on one surface in the thickness direction of the negative electrode current collector, or on two surfaces in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector or a partial area of ​​the negative electrode current collector. This application has no special restrictions as long as the purpose of this application can be achieved.

[0040] The negative electrode mixture layer may further include a negative electrode binder. The negative electrode binder can improve the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. The type of negative electrode binder is not particularly limited, as long as it is a material that is stable to the electrolyte or the solvent used in the manufacture of the electrode. In some embodiments, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic resins, polyolefin resins, and the like. When an aqueous solvent is used to prepare the negative electrode mixture slurry, the negative electrode binder includes, but is not limited to, hydroxyethylcarboxymethylcellulose (HECMC) or its salt, carboxymethylcellulose (CMC) or its salt, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salt, polyacrylate, polyvinyl alcohol, and the like.

[0041] Exemplarily, the negative electrode can be prepared by the following method: a negative electrode mixture slurry containing a negative electrode binder, silicon-carbon composite particles, a conductive agent, etc. is coated on a negative electrode current collector, and after drying, the negative electrode mixture slurry is rolled to form a negative electrode mixture layer on both sides of the negative electrode current collector, thereby obtaining a negative electrode.

[0042] The present application has no particular restrictions on the compaction density of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the compaction density of the negative electrode sheet can be 1.0 g / cm 3 Up to 1.85g / cm 3 The present application has no particular limitation on the cold pressing pressure of the negative electrode sheet, as long as the purpose of the present application can be achieved. For example, the cold pressing pressure of the negative electrode sheet can be 3 tons to 30 tons.

[0043] Electrolyte

[0044] The electrolyte used in the secondary battery of the present application includes an electrolyte and a solvent for dissolving the electrolyte. In some embodiments, the electrolyte includes propylene carbonate and ethylene carbonate, and the sum of the mass percentages of propylene carbonate and ethylene carbonate based on the mass of the electrolyte is H%, 15≤H≤50. In some embodiments, 18≤H≤44. In some embodiments, 18≤H≤39. In some embodiments, 24≤H≤44. In some embodiments, 24≤H≤39. In some embodiments, 18≤H≤24. In some embodiments, 39≤H≤44. In some embodiments, H is 15, 18, 19, 22, 23, 25, 28, 30, 32, 33, 36, 37, 39, 40, 43, 44, 50 or a value within the range of any two of these values. By adjusting the value of H within the above range, the thickness and composition of the SEI film can be adjusted to reduce the possibility of conductive network disconnection inside the negative electrode, and further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0045] In some embodiments, the electrolyte includes propyl propionate and ethyl propionate, and the sum of the mass percentages of propyl propionate and ethyl propionate is L%, based on the mass of the electrolyte, and 12≤L≤39. In some embodiments, 12≤L≤34. In some embodiments, 18≤L≤39. In some embodiments, 18≤L≤34. In some embodiments, 12≤L≤18. In some embodiments, 34≤L≤39. In some embodiments, L is 12, 13, 16, 18, 19, 21, 24, 26, 27, 30, 32, 34, 36, 38, 39 or a value within the range of any two of these values. By adjusting the value of L within the above range, the composition and thickness of the SEI film can be improved, the connection between the silicon-carbon composite particles and the conductive agent can be strengthened, and the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further improved.

[0046] In some embodiments, the mass percentage of propyl propionate is L1%, the mass percentage of ethyl propionate is L2%, and 1.3≤L1 / L2≤2.8. In some embodiments, 1.3≤L1 / L2≤2.3. In some embodiments, 1.7≤L1 / L2≤2.8. In some embodiments, 1.7≤L1 / L2≤2.3. In some embodiments, 1.3≤L1 / L2≤1.7. In some embodiments, 2.3≤L1 / L2≤2.8. In some embodiments, the value of L1 / L2 is 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8 or a value in the range composed of any two of these values. Regulating the value of L1 / L2 within the above range can improve the uniformity of the SEI film, thereby further improving the high temperature cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery.

[0047] In some embodiments, 4≤L1≤24. In some embodiments, 8≤L1≤15. In some embodiments, 10≤L1≤19. In some embodiments, 13≤L1≤23. Exemplarily, the value of L1 is 4, 5, 7, 8, 10, 11, 13, 15, 16, 18, 19, 20, 21, 23, 24 or a value in the range of any two of these values. The present application regulates the value of L1 in the above range, which can further improve the high temperature cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery.

[0048] In some embodiments, 5≤L2≤22. In some embodiments, 7≤L2≤15. In some embodiments, 11≤L2≤18. In some embodiments, 16≤L2≤21. Exemplarily, the value of L2 is 4, 5, 7, 9, 10, 11, 12, 13, 15, 16, 18, 19, 20, 21, 22 or a value in the range of any two of these values. The present application regulates the above range of the value of L2, which can further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0049] In some embodiments, the mass percentage of propylene carbonate is H1%, the mass percentage of ethylene carbonate is H2%, and 0.9≤H1 / H2≤2.3. In some embodiments, 0.9≤H1 / H2≤2.0. In some embodiments, 1.1≤H1 / H2≤2.3. In some embodiments, 1.1≤H1 / H2≤2.0. In some embodiments, the value of H1 / H2 is 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.1, 2.2, 2.2, 2.3 or a value in the range composed of any two of these values. By adjusting the value of H1 / H2 within the above range, the uniformity of the SEI film can be further improved, so that the secondary battery exhibits a lower high temperature cycle resistance growth rate and a fast charge cycle resistance growth rate.

[0050] In some embodiments, 6≤H1≤30. In some embodiments, 8≤H1≤19. In some embodiments, 15≤H1≤23. In some embodiments, 20≤H1≤29. Exemplarily, the value of H1 is 6, 7, 8, 10, 11, 13, 15, 16, 18, 19, 20, 21, 23, 24, 25, 26, 27, 28, 29, 30 or a value in the range of any two of these values. The present application regulates the above range of the value of H1, which can further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0051] In some embodiments, 5≤H2≤29. In some embodiments, 11≤H2≤19. In some embodiments, 15≤H2≤23. In some embodiments, 18≤H2≤27. Exemplarily, the value of H2 is 5, 7, 9, 10, 11, 12, 13, 15, 16, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29 or a value in the range composed of any two of these values. The present application regulates the above range of the value of H2, which can further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery.

[0052] In some embodiments, the electrolyte includes 1,3-propane sultone, and the mass percentage of 1,3-propane sultone is P%, based on the mass of the electrolyte, and 2.6≤P≤4.7. In some embodiments, 2.6≤P≤4.2. In some embodiments, 3.1≤P≤4.7. In some embodiments, 3.1≤P≤4.2. In some embodiments, 2.6≤P≤3.1. In some embodiments, 4.2≤P≤4.7. In some embodiments, P is 2.6, 2.7, 2.8, 3.0, 3.2, 3.4, 3.5, 3.7, 3.8, 4.0, 4.2, 4.3, 4.4, 4.6, 4.7 or a value within the range of any two of these values. Regulating the value of P within the above range can improve the elasticity of the solid electrolyte interface film and the ability to connect the conductive agent, and further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0053] In some embodiments, the electrolyte includes at least one of fluorobenzene, fluoroethylene carbonate and lithium difluorophosphate, and the mass percentage of fluorobenzene is F1%, 1.1≤F1≤4.3 based on the mass of the electrolyte. In some embodiments, 1.1≤F1≤3.7. In some embodiments, 2.3≤F1≤4.3. In some embodiments, 2.3≤F1≤3.7. In some embodiments, 1.1≤F1≤2.3. In some embodiments, 3.7≤F1≤4.3. In some embodiments, the value of F1 is 1.1, 1.3, 1.4, 1.8, 2.1, 2.2, 2.4, 2.6, 2.9, 3.2, 3.4, 3.6, 4.0, 4.2, 4.3 or a value within the range of any two of these values. The present application regulates the value of F1 within the above range, which can further reduce the possibility of conductive network disconnection inside the negative electrode, so that the secondary battery exhibits a lower high temperature cycle resistance growth rate and fast charge cycle resistance growth rate.

[0054] In some embodiments, 3.4≤C / F1 2 ≤13.8. In some embodiments, 3.4≤C / F1 2 ≤12.8. In some embodiments, 5.5≤C / F1 2 ≤13.8. In some embodiments, 5.5≤C / F1 2 ≤12.8. In some embodiments, 7.0≤C / F1 2 ≤12.8. In some embodiments, 3.4≤C / F1 2 ≤5.5. In some embodiments, C / F1 2The value of C / F1 is 3.4, 4.2, 4.8, 5.6, 6.0, 7.1, 7.9, 8.3, 9.5, 10.5, 11.2, 11.6, 12.8, 13.5, 13.8 or a value within the range of any two of these values. 2 The value of is within the above range, which can further improve the high temperature cycle resistance growth rate and fast charge cycle resistance growth rate of the secondary battery.

[0055] In some embodiments, based on the mass of the electrolyte, the mass percentage of fluoroethylene carbonate is F2%, 10.3≤F2≤19.8. In some embodiments, 10.3≤F2≤18.7. In some embodiments, 14.4≤F2≤19.8. In some embodiments, 14.4≤F2≤18.7. In some embodiments, the value of F2 is 10.3, 12.8, 13.0, 13.8, 14.4, 14.7, 15.4, 16.1, 16.5, 17.1, 17.8, 18.5, 19.0, 19.4, 19.8 or a value within the range composed of any two of these values. The present application regulates the value of F2 within the above range, which can further reduce the possibility of conductive network short circuit inside the negative electrode, so that the secondary battery exhibits a lower high temperature cycle resistance growth rate and fast charge cycle resistance growth rate.

[0056] In some embodiments, based on the mass of the electrolyte, the mass percentage of lithium difluorophosphate is F3%, 0.01≤F3≤0.32. In some embodiments, 0.01≤F3≤0.22. In some embodiments, 0.12≤F3≤0.32. In some embodiments, 0.12≤F3≤0.22. In some embodiments, 0.01≤F3≤0.12. In some embodiments, 0.22≤F3≤0.32. In some embodiments, the value of F3 is 0.01, 0.02, 0.05, 0.07, 0.08, 0.12, 0.15, 0.16, 0.20, 0.22, 0.23, 0.25, 0.29, 0.31, 0.32 or a value within the range of any two of these values. The present application regulates the value of F3 within the above range, which can further reduce the possibility of conductive network disconnection inside the negative electrode, so that the secondary battery exhibits a lower high temperature cycle resistance growth rate and fast charge cycle resistance growth rate.

[0057] In some embodiments, the electrolyte includes dimethyl sulfone, and the mass percentage of dimethyl sulfone is S% based on the mass of the electrolyte, and 1.1≤S≤3.4. In some embodiments, 1.1≤S≤2.7. In some embodiments, 2.7≤S≤3.4. In some embodiments, S is 1.1, 1.2, 1.4, 1.5, 1.7, 1.8, 1.9, 2.2, 2.5, 2.6, 2.7, 2.9, 3.1, 3.4 or a value within the range of any two of these values. By regulating S within the above range, the possibility of irreversible displacement of the conductive agent during the volume expansion and contraction of the silicon-carbon composite particles can be reduced, further improving the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0058] In some embodiments, the electrolyte includes 1,4-dioxane, and the mass percentage of 1,4-dioxane is W%, based on the mass of the electrolyte, and 2.3≤W≤4.6. In some embodiments, 2.3≤W≤3.2. In some embodiments, 3.2≤W≤4.6. In some embodiments, W is 2.3, 2.6, 2.7, 2.9, 3.0, 3.3, 3.4, 3.6, 3.7, 3.9, 4.2, 4.3, 4.5, 4.6 or a value within the range of any two of these values. The present application regulates the value of W within the above range, which can enhance the connection strength between the silicon-carbon composite particles and the conductive agent, and further improve the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate.

[0059] The type of non-aqueous solvent of the present application is not particularly limited, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of chain carbonate compounds or cyclic carbonate compounds. The above-mentioned chain carbonate compounds may include but are not limited to at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or methyl ethyl carbonate. The above-mentioned cyclic carbonate compounds may include but are not limited to at least one of ethylene carbonate, propylene carbonate, butylene carbonate or ethylene ethylene carbonate. The above-mentioned carboxylate compounds may include but are not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of ethylene glycol dimethyl ether, dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0060] In some embodiments, the electrolyte is not particularly limited, and any substance known as an electrolyte can be used. The weight of the electrolyte is not particularly limited as long as the effects of the present application are not impaired.

[0061] positive electrode

[0062] The positive electrode includes a positive electrode current collector and a positive electrode mixture layer disposed on the surface of the positive electrode current collector.

[0063] The positive electrode mixture layer contains positive electrode active material, and the positive electrode mixture layer can be one layer or multiple layers. Each layer of the multiple layers of positive electrode active material can contain the same or different positive electrode active materials. The positive electrode active material is any material that can reversibly embed and de-embed alkali metal ions.

[0064] The positive electrode active material includes a lithium transition metal oxide containing nickel and other transition metals. In the lithium transition metal oxide including nickel and other transition metals, the amount of nickel relative to the total molar number of the transition metal may be 60 mol% or more, for example, 75 mol% or more, for example, 80 mol% or more, for example, 85 mol% or more, or for example, 90 mol% or more.

[0065] For example, the lithium transition metal oxide may be a compound represented by the following formula α:

[0066] Formula α: Li a Ni x Co y M z O 2-b A b ,

[0067] Wherein, in formula α, 0.9≤a≤1.2, 0≤b≤0.2, 0.6≤x<1, 0<y≤0.3, 0<z≤0.3, and x+y+z=1, M is at least one selected from manganese (Mn), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al) or boron (B), and A is F, S, Cl, Br or a combination thereof. For example, the above subscripts may be 0.7≤x<1, 0<y≤0.3, and 0<z≤0.3; 0.8≤x<1, 0<y≤0.3, and 0<z≤0.3; 0.8≤x<1, 0<y≤0.2, and 0<z≤0.2; 0.83≤x<0.97, 0<y≤0.15, and 0<z≤0.15; or 0.85≤x<0.95, 0<y≤0.1, and 0<z≤0.1.

[0068] For example, the lithium transition metal oxide may be at least one compound represented by the following formula β or formula γ:

[0069] Formula β: LiNi x Co y Mn z O2,

[0070] Wherein, in formula β, 0.6≤x≤0.95, 0<y≤0.2, and 0<z≤0.1, for example, 0.7≤x≤0.95, 0<y≤0.3, and 0<z≤0.3.

[0071] Formula γ: LiNi x Co y Al z O2,

[0072] Wherein, in formula γ, 0.6≤x≤0.95, 0<y≤0.2, and 0<z≤0.1, for example, 0.7≤x≤0.95, 0<y≤0.3, and 0<z≤0.3, for example, 0.8≤x≤0.95, 0<y≤0.3, and 0<z≤0.3, for example, 0.82≤x≤0.95, 0<y≤0.15, and 0<z≤0.15, for example, 0.85≤x≤0.95, 0<y≤0.1, and 0<z≤0.1.

[0073] For example, the lithium transition metal oxide may be LiNi0.6 Co 0.2 Mn 0.2 O2、LiNi 0.88 Co 0.08 Mn 0.04 O2、LiNi 0.8 Co 0.15 Mn 0.05 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.88 Co 0.1 Mn 0.02 O2、LiNi 0.8 Co 0.15 Al 0.05 O2 or LiNi 0.88 Co 0.1 Al 0.02 O2.

[0074] According to another embodiment, the positive electrode active material includes at least one active material selected from the group consisting of Li-Ni-Co-Al (NCA), Li-Ni-Co-Mn (NCM), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMnO2), lithium nickel oxide (LiNiO2) and lithium iron phosphate (LiFePO4).

[0075] In some embodiments, the positive electrode mixture layer includes a positive electrode conductive material; the type of the positive electrode conductive material is not limited, and any known conductive material can be used. Examples of positive electrode conductive materials may include, but are not limited to, carbon black such as acetylene black and Super-P; amorphous carbon materials such as needle coke; carbon nanotubes; graphene, etc. The above positive electrode conductive materials may be used alone or in any combination.

[0076] There is no particular restriction on the type of positive electrode binder used in the manufacture of the positive electrode mixture layer. In the case of a coating method, any material that can be dissolved or dispersed in the liquid medium used in the manufacture of the electrode can be used. Examples of positive electrode binders may include, but are not limited to, one or more of the following: resin polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and nitrocellulose; rubber polymers such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, polybutadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymers or their hydrogenates, ethylene-propylene-diene terpolymers (EPDM), Thermoplastic elastomer polymers such as styrene·ethylene·butadiene·ethylene copolymers, styrene·isoprene·styrene block copolymers or their hydrogenated products; soft resin polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene·vinyl acetate copolymers, propylene·α-olefin copolymers; fluorine-based polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, polytetrafluoroethylene·ethylene copolymers; polymer compositions having ion conductivity of alkali metal ions (especially lithium ions), etc. The above positive electrode binders can be used alone or in any combination.

[0077] There is no limitation on the type of solvent used to form the positive electrode slurry, as long as it is a solvent that can dissolve or disperse the positive electrode active material, the conductive material, the positive electrode binder, and the thickener used as needed. Examples of solvents used to form the positive electrode slurry may include any of aqueous solvents and organic solvents. Examples of aqueous media may include, but are not limited to, a mixed medium of alcohol and water or water, etc. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; aprotic polar solvents such as hexamethylphosphoramide and dimethyl sulfoxide, etc.

[0078] Thickeners are generally used to adjust the viscosity of the slurry. In the case of using an aqueous medium, a thickener and a styrene-butadiene rubber (SBR) emulsion can be used for slurrying. The type of thickener is not particularly limited, and examples thereof may include, but are not limited to, carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The above thickeners may be used alone or in any combination.

[0079] The type of positive electrode current collector is not particularly limited, and it can be any material known to be suitable for use as a positive electrode current collector. Examples of positive electrode current collectors may include, but are not limited to, metal materials such as aluminum, stainless steel, nickel plating, titanium, tantalum, and materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metal material. In some embodiments, the positive electrode current collector is aluminum.

[0080] In order to reduce the electronic contact resistance between the positive electrode current collector and the positive electrode mixture layer, the surface of the positive electrode current collector may include a conductive additive or a conductive coating. Examples of conductive additives may include, but are not limited to, carbon and precious metals such as gold, platinum, and silver. Examples of conductive coatings may include a mixture layer containing an inorganic oxide, a conductive agent, and a binder.

[0081] The positive electrode can be made by forming a positive electrode mixture layer containing a positive electrode active material and a binder on a current collector. The manufacture of a positive electrode using a positive electrode active material can be carried out by a conventional method, that is, the positive electrode active material and the binder, as well as a conductive material and a thickener as required, are dry-mixed to form a sheet, and the obtained sheet is pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, and the slurry is applied to the positive electrode current collector and dried to form a positive electrode mixture layer on the current collector, thereby obtaining a positive electrode.

[0082] Isolation film

[0083] In order to prevent short circuit, a separator is usually provided between the positive electrode and the negative electrode. In this case, the electrolyte of the present application is usually used by infiltrating the separator.

[0084] There is no particular restriction on the material and shape of the isolation membrane, as long as the effect of the present application is not significantly impaired. The isolation membrane may be a resin, glass fiber, inorganic substance, etc. formed of a material that is stable to the electrolyte of the present application. In some embodiments, the isolation membrane includes a porous sheet or a non-woven fabric-like material with excellent liquid retention. Examples of materials for resin or glass fiber isolation membranes may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, polyether sulfone, etc. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the above isolation membranes may be used alone or in any combination.

[0085] The separator may also be a material formed by laminating the above materials, examples of which include, but are not limited to, a three-layer separator formed by laminating polypropylene, polyethylene, and polypropylene in this order.

[0086] Examples of inorganic materials may include, but are not limited to, oxides such as aluminum oxide and silicon dioxide, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.) The form of the inorganic material may include, but is not limited to, granular or fibrous.

[0087] The separator may be in the form of a thin film, examples of which include, but are not limited to, nonwoven fabrics, woven fabrics, microporous films, etc. In the thin film form, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the above-mentioned independent thin film separators, the following separators can also be used: a separator formed by forming a composite porous layer containing the above-mentioned inorganic particles on the surface of the positive electrode and / or the negative electrode using a resin-based adhesive, for example, a separator formed by using a fluororesin as an adhesive to form a porous layer on both sides of the positive electrode with aluminum oxide particles having a particle size of 90% less than 1 μm.

[0088] The thickness of the separator is arbitrary. In some embodiments, the thickness of the separator is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the separator is less than 50 μm, less than 40 μm, or less than 30 μm. When the thickness of the separator is within the above range, insulation and mechanical strength can be ensured, and the rate characteristics and energy density of the secondary battery can be ensured.

[0089] The present application further provides an electronic device, which includes the secondary battery according to the present application.

[0090] The purpose of the secondary battery of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the secondary battery of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium ion capacitors, etc.

[0091] Example

[0092] Hereinafter, taking lithium-ion batteries as an example, examples and comparative examples are given to more specifically describe the implementation of the secondary battery of the present application. Those skilled in the art will understand that the preparation method described in the present application is only an example, and any other suitable preparation method is within the scope of the present application. Various tests and evaluations are carried out according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0093] Test Method

[0094] Resistance growth rate after high temperature (45℃) cycling

[0095] (1) Test the initial resistance: After placing the lithium-ion battery in a charge and discharge device at room temperature (25°C), perform constant current charging at 0.33C to 4.45V, and then perform constant voltage charging to 0.05C to cut off the charge. Discharge at a constant current of 0.33C to 3.0V. Then, after charging and discharging 3 times according to the above charge and discharge process, the battery is set to SOC 50% based on the last discharge capacity. Then, the DC internal resistance is measured by the voltage drop displayed when a discharge pulse is applied at 5A (2.5C) for 10 seconds (PNE-0506 charge and discharge device), and the resistance at this time is defined as the initial resistance.

[0096] (2) High temperature cycle: After the lithium ion battery whose initial resistance was measured was moved to a high temperature (45° C.), the above-mentioned charging and discharging process was set as one cycle, and a total of 200 cycles of charging and discharging were performed.

[0097] (3) Resistance after high-temperature cycling: After the lithium-ion battery was placed in a charge-discharge device at room temperature, the SOC was set to 50%. The resistance after 200 cycles was then measured by the voltage drop displayed when a discharge pulse was applied at 5A (2.5C) for 10 seconds using a PNE-0506 charge-discharge device.

[0098] (4) Calculate the resistance increase rate R1 after high temperature (45°C) cycling:

[0099] Resistance increase rate after high temperature (45°C) cycle R1 (%) = {(resistance after 200 cycles - initial resistance) / initial resistance} × 100 fast charge (5C) cycle resistance growth rate

[0100] (1) Test the initial resistance: After moving the lithium-ion battery to a charge and discharge device at room temperature (25°C), perform constant current charging at 0.33C to 4.45V, and then perform constant voltage charging to 0.05C with charge cutoff. Discharge at a constant current of 0.33C to 3.0V. Then, after charging and discharging three times, the battery is set to SOC 50% based on the last discharge capacity. The DC internal resistance is then measured by the voltage drop displayed when a discharge pulse is applied at 5A (2.5C) for 10 seconds (PNE-0506 charge and discharge device), and the resistance at this time is defined as the initial resistance.

[0101] (2) Fast charge cycle: The lithium-ion battery was charged at a constant current of 5C to a voltage of 4.45V, then charged at a constant voltage of 4.45V to a current of 0.05C. After standing for 10 minutes, it was discharged at a constant current of 1C to a cut-off voltage of 3.0V. The above charging and discharging process was set as 1 cycle, and a total of 200 cycles of charging and discharging were performed.

[0102] (3) Resistance after fast charge cycle: The SOC was set to 50%. Then, the resistance after 200 cycles was measured by the voltage drop shown when a discharge pulse was applied at 5 A (2.5 C) for 10 seconds using a PNE-0506 charge-discharge device.

[0103] (4) Calculate the fast charge (5C) cycle resistance increase rate R2:

[0104] Fast charge (5C) cycle resistance increase rate R2 (%) = {(resistance after 200 cycles - initial resistance) / initial resistance} × 100

[0105] Energy density (ED)

[0106] The lithium ion batteries of each embodiment and comparative example were placed in a constant temperature box at 25°C ± 1°C for 30 minutes, charged to 4.25V at a constant current of 0.5C, then charged to 0.025C at a constant voltage of 4.25V, placed for 5 minutes, and then discharged to 3.0V at 0.5C. The discharge energy E mAh of the lithium ion battery was recorded, and the length, width and height of the battery at a 50% charge state (the lithium ion battery was charged to 3.95V at a constant current of 0.5C) were measured to obtain the volume V cm of the battery. 3 , energy density ED = E / V.

[0107] Mass proportion of silicon element (C)

[0108] The negative electrode sheet was cut into a size of 1 cm×1 cm, and then the cut surface of the negative electrode sheet was polished using argon plasma polishing technology (CP) to obtain a CP sample.

[0109] Silicon-carbon composite particles in the CP sample were selected and cut into slices using a focused ion beam (FIB) to obtain FIB samples.

[0110] The cut surface of the FIB sample was subjected to energy spectrum analysis, specifically: a 1μm×1μm area was randomly selected in the center of the silicon-carbon composite particle for surface scanning, and the mass percentage (wt%) of silicon and carbon was tested, and the mass percentage of silicon was calculated. Among them, the center of the silicon-carbon composite particle is an area greater than 1μm away from the surface of the silicon-carbon composite particle.

[0111] Average particle size of silicon-carbon composite particles (D)

[0112] The negative electrode sheet was cut into a size of 1 cm×1 cm, and then the cut surface of the negative electrode sheet was polished using argon plasma polishing (CP) technology to prepare a CP sample.

[0113] Select silicon-carbon composite particles in the CP sample, count the cross-sectional area of ​​the silicon-carbon composite particles and record it as S, according to S = π × R 2The formula is used to calculate R. The particle size of the silicon-carbon composite particles is 2R.

[0114] A total of 20 silicon-carbon composite particles are randomly selected, and the arithmetic mean of the particle sizes of the 20 silicon-carbon composite particles is calculated, which is recorded as the average particle size D of the silicon-carbon composite particles.

[0115] Example 1-1

[0116] <Preparation of negative electrode>

[0117] Preparation of silicon-carbon composite particles:

[0118] The carbon precursor resin carbon is placed in a rotary kiln, and a mixed gas of silane and argon is introduced, and vapor deposition is performed at a deposition temperature of 550°C for 6.5 hours to obtain silicon-carbon composite particles, wherein the volume ratio of silane to argon is 3:7.

[0119] Preparation of negative electrode sheet:

[0120] Silicon-carbon composite particles and artificial graphite are mixed evenly in a mass ratio of 12:88 as negative electrode active materials. The above-mentioned negative electrode active materials, styrene-butadiene rubber (SBR), polyacrylic acid (PAA), carbon nanotubes (CNT), and carboxymethyl cellulose (CMC) are mixed in a mass ratio of 95.8:2.4:0.5:0.5:0.8, and then deionized water is added as a solvent and stirred evenly to prepare a negative electrode slurry with a solid content of 45wt%. The negative electrode slurry is evenly coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried to obtain a negative electrode sheet coated with a negative electrode mixture layer on one side. Repeat the above steps on the other surface of the negative electrode current collector copper foil to obtain a negative electrode sheet coated with a negative electrode mixture layer on both sides. After cold pressing, cutting, slitting and drying, a negative electrode sheet with a specification of 76.6mm×875mm is obtained.

[0121] <Preparation of positive electrode>

[0122] The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black, and polyvinylidene fluoride (PVDF) are mixed in a mass ratio of 95:2:3, N-methylpyrrolidone (NMP) is added, and the mixture is stirred evenly under the action of a vacuum mixer to obtain a positive electrode slurry with a solid content of 70wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 9μm, and dried to obtain a positive electrode sheet coated with a positive electrode mixture layer on one side. Repeat the above steps on the other surface of the positive electrode current collector aluminum foil to obtain a positive electrode sheet coated with a positive electrode mixture layer on both sides. After cold pressing, cutting, slitting and drying, a positive electrode sheet with a specification of 74mm×867mm is obtained.

[0123] <Preparation of Electrolyte>

[0124] In a dry argon atmosphere glove box, lithium hexafluorophosphate (LiPF6) is dissolved in a mixed solution containing propyl propionate, ethyl propionate, ethylene carbonate, propylene carbonate and diethyl carbonate (DEC). Based on the mass of the electrolyte, the mass percentage of LiPF6 is 12.5%, and the mass percentages of other substances are shown in Table 1, wherein the mass percentage of propyl propionate is L1%, the mass percentage of ethyl propionate is L2%, the mass percentage of propylene carbonate is H1%, the mass percentage of ethylene carbonate is H2%, and the remainder is DEC.

[0125] <Diaphragm>

[0126] A porous polyethylene film with a thickness of 15 μm (provided by Celgard Company) was used as a separator.

[0127] <Preparation of lithium-ion batteries>

[0128] The positive electrode and negative electrode prepared as above are connected to the pole ears respectively. They are stacked via a separator to obtain a laminate. Then, the laminate is housed in an aluminum laminate housing together with an electrolyte. The opening of the housing is heat-sealed, and a lithium-ion battery is prepared through steps such as formation and degassing.

[0129] Examples 1-2 to 1-31, Comparative Examples 1 to 3

[0130] Except for adjusting the parameters according to Table 1, the rest is the same as Example 1-1. By adjusting the duration of vapor deposition when preparing silicon-carbon composite particles, the mass proportion C% of silicon element is as shown in Table 1. By crushing and ball milling the silicon-based particles, the average particle size Dμm of the silicon-based particles is as shown in Table 1. Among them, the negative electrode mixture layer of Comparative Example 3 does not contain silicon-carbon composite particles, and the negative electrode active material is artificial graphite particles.

[0131] Table 1

[0132]

[0133]

[0134] As shown in Table 1, the average particle size Dμm of the silicon-carbon composite particles and the mass proportion C% of the silicon element in the secondary battery of the present application satisfy 0.21≤C / D 2 ≤1.2, it is possible to adjust the coordination between the movable space of the conductive agent and the degree and speed of volume expansion and contraction of the silicon-carbon composite particles, so as to achieve a higher energy density for the secondary battery while improving the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate. 2 The value satisfies 0.39≤C / D 2≤0.96, the high temperature cycle resistance growth rate and fast charge cycle resistance growth rate can be further improved. In particular, when adjusting C / D 2 The value satisfies 0.58≤C / D 2 ≤0.88, the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further significantly improved. In particular, by adjusting the values ​​of D and / or C to satisfy 7.1≤D≤10.9 and / or 25≤C≤59, the high temperature cycle resistance growth rate and the fast charge cycle resistance growth rate of the secondary battery can be further improved.

[0135] In particular, the H value in the sum of the mass percentage of propylene carbonate and ethylene carbonate in the electrolyte is regulated to meet 15≤H≤50, and the average particle size of the silicon-carbon composite particles in the negative electrode and the mass percentage of the silicon element are matched, which can show a significant improvement effect on the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery. In particular, when the L value in the sum of the mass percentage of propyl propionate and ethyl propionate in the electrolyte is regulated to meet 12≤L≤39, and / or, the H value in the sum of the mass percentage of propylene carbonate and ethylene carbonate in the electrolyte is regulated to meet 18≤H≤44, the thickness and composition of the SEI film can be adjusted, and after being matched with silicon-based composite particles and conductive agents, the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved. In particular, when the value of L is regulated to be within the range of 18≤L≤34, and / or, the value of H is regulated to meet 24≤H≤39, the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery can be further significantly improved.

[0136] In particular, by adjusting the mass percentage of propyl propionate L1% and the mass percentage of ethyl propionate L2% in the electrolyte, the value of L1 / L2 satisfies 1.3≤L1 / L2≤2.8, and the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate can be further improved. Furthermore, by adjusting the mass percentage of propylene carbonate H1% and the mass percentage of ethylene carbonate H2% in the electrolyte, the value of H1 / H2 satisfies 0.9≤H1 / H2≤2.3, the secondary battery can exhibit a lower high-temperature cycle resistance growth rate and fast-charge cycle resistance growth rate.

[0137] Example 2-1 to Example 2-32

[0138] The same as in Example 1-27 except that the content P% of 1,3-propane sultone, the content F1% of fluorobenzene, the content F2% of fluoroethylene carbonate, the content F3% of lithium difluorophosphate and / or the content S% of dimethyl sulfone are adjusted according to the parameters in Table 2. The content of DEC is adjusted accordingly according to the contents of the above components.

[0139] Table 2

[0140]

[0141] As can be seen from Table 2, the present application further regulates the mass percentage content P% of 1,3-propane sultone in the electrolyte to satisfy 2.6≤P≤4.7, which can further improve the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate. On this basis, the value of P is further regulated to satisfy 3.1≤P≤4.2, which can continue to significantly reduce the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery.

[0142] In particular, the present application regulates the F1 value in the mass percentage content F1% of fluorobenzene in the electrolyte to satisfy 1.1≤F1≤4.3, which can make the secondary battery show a lower high-temperature cycle resistance growth rate and a fast-charge cycle resistance growth rate. Further, regulating the F2 value in the mass percentage content F2% of fluoroethylene carbonate in the electrolyte to satisfy 10.3≤F2≤19.8 can more significantly improve the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate. In particular, regulating the F2 value in the mass percentage content F3% of lithium difluorophosphate in the electrolyte to satisfy 0.01≤F3≤0.32 can further improve the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate.

[0143] In particular, the present application regulates the S value in the mass percentage content S% of dimethyl sulfone in the electrolyte to satisfy 1.1≤S≤3.4, which can further improve the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate. In particular, regulating the W value in the mass percentage content W% of 1,4-dioxane in the electrolyte to satisfy 2.3≤W≤4.6 can further improve the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate. In particular, when dimethyl sulfone and 1,4-dioxane are simultaneously included in the electrolyte for coordination, the high-temperature cycle resistance growth rate and the fast-charge cycle resistance growth rate of the secondary battery can be further significantly reduced.

[0144] Example 3-1 to Example 3-6

[0145] Except for adjusting the fluorobenzene content F1% and the silicon content C% parameters according to Table 3, the rest is the same as Example 1-27. The DEC content is adjusted according to the fluorobenzene content.

[0146] Table 3

[0147]

[0148] It can be seen from Table 3 that by adjusting C / F1 2 The value satisfies 3.4≤C / F1 2 ≤13.8, the high temperature cycle resistance growth rate and fast charge cycle resistance growth rate can be further improved. In particular, regulating C / F12 The value satisfies 5.5≤C / F1 2 ≤7.0, which can significantly improve the high-temperature cycle resistance growth rate and fast-charge cycle resistance growth rate of the secondary battery.

[0149] Although illustrative embodiments have been shown and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the principles and scope of the present application.

Claims

1. A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode comprises a current collector and a negative electrode mixture layer disposed on at least one surface of the current collector, characterized in that: The negative electrode mixture layer contains silicon-carbon composite particles and a conductive agent. The average particle size of the silicon-carbon composite particles is D μm. The silicon-carbon composite particles include silicon and carbon. Based on the sum of the mass of the silicon and carbon, the mass proportion of the silicon is C%, and 0.21≤C / D 2 ≤1.2; The electrolyte comprises propylene carbonate and ethylene carbonate, and based on the mass of the electrolyte, the sum of the mass percentages of the propylene carbonate and the ethylene carbonate is H%, 15≤H≤50; The electrolyte includes fluorobenzene, fluoroethylene carbonate and lithium difluorophosphate.

2. The secondary battery according to claim 1, characterized in that: 0.39≤C / D 2 ≤0.96。 3. The secondary battery according to claim 1, characterized in that: 7.1≤D≤10.9, 25≤C≤59; and / or, 0.58≤C / D 2 ≤0.

88.

4. The secondary battery according to claim 1, characterized in that: The electrolyte also includes propyl propionate and ethyl propionate. Based on the mass of the electrolyte, the sum of the mass percentages of the propyl propionate and the ethyl propionate is L%, 12≤L≤39, 18≤H≤44.

5. The secondary battery according to claim 4, characterized in that: The electrolyte satisfies at least one of the following: (1)18≤L≤34; (2)24≤H≤39。 6. The secondary battery according to claim 4 or 5, characterized in that: Based on the quality of the electrolyte, the electrolyte satisfies at least one of the following: (1) The mass percentage of the propyl propionate is L1%, the mass percentage of the ethyl propionate is L2%, and 1.3≤L1 / L2≤2.8; (2) The mass percentage of the propylene carbonate is H1%, the mass percentage of the ethylene carbonate is H2%, and 0.9≤H1 / H2≤2.

3.

7. The secondary battery according to claim 6, characterized in that: 1.7≤L1 / L2≤2.3; and / or, 1.1≤H1 / H2≤2.

0.

8. The secondary battery according to any one of claims 1 to 5, characterized in that: The electrolyte includes 1,3-propane sultone. Based on the mass of the electrolyte, the mass percentage of the 1,3-propane sultone is P%, and 2.6≤P≤4.

7.

9. The secondary battery according to claim 8, characterized in that: 3.1≤P≤4.2。 10. The secondary battery according to any one of claims 1 to 5, characterized in that: Based on the quality of the electrolyte, the electrolyte satisfies at least one of the following: (1) The mass percentage content of fluorobenzene is F1%, 1.1≤F1≤4.3; (2) The mass percentage of the fluoroethylene carbonate is F2%, 10.3≤F2≤19.8; (3) The mass percentage of the lithium difluorophosphate is F3%, 0.01≤F3≤0.

32.

11. The secondary battery according to any one of claims 1 to 5, characterized in that: The electrolyte includes dimethyl sulfone. Based on the mass of the electrolyte, the mass percentage of the dimethyl sulfone is S%, and 1.1≤S≤3.

4.

12. The secondary battery according to any one of claims 1 to 5, characterized in that: The electrolyte includes 1,4-dioxane. Based on the mass of the electrolyte, the mass percentage of the 1,4-dioxane is W%, and 2.3≤W≤4.

6.

13. The secondary battery according to claim 10, characterized in that: 3.4≤C / F1 2 ≤13.8。 14. The secondary battery according to any one of claims 1 to 5, characterized in that: The silicon-carbon composite particles include a carbon skeleton and a protective layer located on at least a portion of the surface of the carbon skeleton, the material of the protective layer includes amorphous carbon, and the material of the carbon skeleton includes at least one of artificial graphite, natural graphite, mesophase carbon microspheres, soft carbon or hard carbon.

15. The secondary battery according to any one of claims 1 to 5, characterized in that: The conductive agent includes carbon nanotubes.

16. An electronic device, characterized in that: It comprises the secondary battery according to any one of claims 1 to 15.