Gel electrolyte and preparation method and application thereof

By treating trifunctional triacrylate into trifunctional triacrylate and reacting with polyethylene glycol diacrylate, gel electrolytes that do not need to be cured are prepared, which solves the problem of long curing time of gel electrolytes , simplifies battery preparation process and improves battery performance and safety.

CN119029293AActive Publication Date: 2024-11-26XIAOGAN CORNEX NEW ENERGY INNOVATION TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411439981.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-11-26
Estimated Expiration
2044-10-15

AI Technical Summary

Technical Problem

The long curing time of existing gel electrolytes has affected its industrial production efficiency in new energy vehicle batteries.

Method used

By treating trifunctional triacrylate into difunctional triacrylate and reacting with polyethylene glycol diacrylate and alkyl mercaptan, a gel electrolyte that does not require curing is prepared to increase its ions Conductivity and wetting effect.

Benefits of technology

The preparation process of semi-solid state batteries is simplified, the curing completeness of gel electrolytes is improved, and the electrical performance and safety of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029293A_ABST
    Figure CN119029293A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of batteries, and particularly provides a gel electrolyte and a preparation method and application thereof, and the gel electrolyte comprises an electrolyte and a polymer as shown in a structural formula (I). The gel electrolyte has the beneficial effects that the gel electrolyte does not need to be cured when being used for preparing a semi-solid battery, and has relatively high ionic conductivity and safety performance; in the preparation process of the gel electrolyte, the trifunctional triacrylate is used as a polymer monomer, and the trifunctional triacrylate is treated into the difunctional triacrylate, so that the hardness of the product is reduced, and the conductivity of the product is further improved; and then the difunctional triacrylate reacts with polyethylene glycol diacrylate (PEGDA), so that the crosslinking density of the product can be reduced, the ionic conductivity can be improved, and the wettability of the electrolyte can be optimized. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries, and in particular relates to a gel electrolyte and a preparation method and application thereof. Background Art

[0002] With the rapid development of new energy vehicles, traditional power battery systems will find it difficult to meet the demand for energy density in 10 years. Moreover, the annual growth in sales of new energy vehicles is accompanied by an increase in safety accidents, among which battery spontaneous combustion accounts for 31% of the causes of accidents. The cause of spontaneous combustion is that after an internal or external short circuit in a lithium battery, the battery releases a large amount of heat in a short period of time, and the temperature rises sharply, leading to thermal runaway. The flammable liquid electrolyte will ignite at high temperatures, eventually causing the battery to catch fire or explode.

[0003] Solid-state batteries use non-flammable solid electrolytes to replace flammable organic liquid electrolytes, which greatly improves the safety of the battery system. At the same time, they can better adapt to high-energy positive and negative electrodes and reduce the weight of the system, achieving a simultaneous increase in energy density. Among various new battery systems, solid-state batteries are the next-generation technology closest to industrialization, which has become a consensus in the industry and scientific community. However, the existing gel electrolytes need to react at a certain temperature for a period of time before they can solidify. The curing time is relatively long, which seriously affects their industrial production. Therefore, it is necessary to study and improve the gel electrolyte. Summary of the invention

[0004] The present application provides a gel electrolyte and a preparation method and application thereof, aiming to solve the problems of long curing time and low production efficiency of existing gel electrolytes.

[0005] In a first aspect of the present application, a gel electrolyte is provided, comprising an electrolyte and a polymer represented by structural formula (I),

[0006]

[0007] Among them, 1≤x≤6, 5≤m≤500, 1≤n≤5.

[0008] According to some embodiments of the gel electrolyte described herein, the gel electrolyte further includes an initiator.

[0009] According to some embodiments of the gel electrolyte described herein, the electrolyte includes a ternary electrolyte.

[0010] According to some embodiments of the gel electrolyte described herein, the initiator includes one or both of dibenzoyl peroxide and dimethyl azobisisobutyrate.

[0011] According to some embodiments of the gel electrolyte described in the present application, the mass ratio of the polymer to the electrolyte is (0.03-0.05):1.

[0012] According to some embodiments of the gel electrolyte described in the present application, the mass ratio of the initiator to the electrolyte is (0.008-0.12):1.

[0013] The gel electrolyte described in the present application has high ionic conductivity, excellent wetting effect, and does not require curing when preparing a semi-solid battery.

[0014] The second aspect of the present application provides a method for preparing the gel electrolyte described in the first aspect of the present application, comprising the following steps:

[0015] (1) treating a trifunctional triacrylate to obtain a difunctional triacrylate;

[0016] (2) mixing and reacting the difunctional triacrylate, polyethylene glycol diacrylate and alkyl mercaptan to obtain a polymer represented by formula (I);

[0017] (3) Mixing the polymer represented by formula (I) and an electrolyte to obtain the gel electrolyte.

[0018] The preparation method described in the present application converts trifunctional triacrylate into difunctional triacrylate, which can reduce the hardness of the product and improve the ionic conductivity of the gel electrolyte. Then, reacting with polyethylene glycol diacrylate can further improve the ionic conductivity and optimize the wettability of the electrolyte.

[0019] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the trifunctional triacrylate includes trimethylolpropane triacrylate.

[0020] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the step of treating the trifunctional triacrylate includes: mixing the trifunctional triacrylate and alkylthiol for a first reaction to obtain a difunctional triacrylate.

[0021] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the alkyl mercaptan includes one or more of butanethiol, propanethiol and ethanethiol.

[0022] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the trifunctional triacrylate to the alkylthiol is 1:(0.1-2).

[0023] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the temperature of the first reaction is 15-35° C., and the time of the first reaction is 0.5-2 h.

[0024] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the first reaction is carried out in a first solvent.

[0025] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the first solvent includes one or more of dioxolane, dioxane and tetrahydrofuran.

[0026] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the trifunctional triacrylate to the first solvent is 1:(3-10).

[0027] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the first reaction is performed in the presence of a first catalyst.

[0028] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the first catalyst includes dimethylphenylphosphine.

[0029] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the trifunctional triacrylate to the first catalyst is 1:(0.005-0.05).

[0030] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the number average molecular weight of the polyethylene glycol diacrylate is 170-350.

[0031] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the difunctional triacrylate to the polyethylene glycol diacrylate is 1:(0.01-5).

[0032] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the difunctional triacrylate to the polyethylene glycol diacrylate is 1:(0.25-4).

[0033] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the difunctional triacrylate to the alkylthiol is 1:(0.5-1.5).

[0034] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the temperature of the mixing reaction is 15-35° C., and the time of the mixing reaction is 0.5-4 h.

[0035] According to some embodiments of the method for preparing the gel electrolyte described in the present application, in step (2), the mixing reaction is carried out in a second solvent.

[0036] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the second solvent includes DMF and / or dimethylacetamide.

[0037] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the difunctional triacrylate to the second solvent is 1:(5-15).

[0038] According to some embodiments of the method for preparing the gel electrolyte described in the present application, in step (2), the mixing reaction is carried out in the presence of a second catalyst.

[0039] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the second catalyst includes dimethylphenylphosphine.

[0040] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the molar ratio of the difunctional triacrylate to the second catalyst is 1:(0.005-0.05).

[0041] According to some embodiments of the method for preparing the gel electrolyte described in the present application, the preparation of the gel electrolyte includes the following steps:

[0042] The monomer M1 trimethylolpropane triacrylate (TMPTA) is reacted with alkyl mercaptan to generate monomer M2 (BS-TMPTA), thereby converting the trifunctional triacrylate into a difunctional triacrylate; the monomer M2, alkyl mercaptan and polyethylene glycol diacrylate are reacted to generate a linear polymer; the linear polymer is added to a ternary electrolyte to prepare a gel electrolyte.

[0043] The specific reaction formula is as follows:

[0044]

[0045] Among them, 1≤x≤6, 5≤m≤500, 1≤n≤5.

[0046] The third aspect of the present application provides a semi-solid battery, comprising the gel electrolyte described in the first aspect of the present application or the gel electrolyte obtained by the preparation method described in the second aspect of the present application.

[0047] The semi-solid battery described in the present application does not need to be cured because it contains the gel electrolyte, which simplifies the preparation process of the semi-solid battery. In addition, if there are monomers that do not participate in the gel during the static process, they can be further gelled during the battery formation process, thereby improving the curing completeness of the gel electrolyte and further improving the electrical performance and safety of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is an analysis chart of the capacity cycle retention rate of the semi-solid state batteries prepared in Example 1 and Comparative Example 3 of the present application. DETAILED DESCRIPTION

[0049] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0050] The technical solution of the present application is described in detail below in conjunction with specific embodiments and drawings.

[0051] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0052] The present application embodiment provides a gel electrolyte, comprising an electrolyte and a polymer represented by structural formula (I),

[0053]

[0054] Among them, 1≤x≤6, 5≤m≤500, 1≤n≤5.

[0055] In some embodiments, the gel electrolyte further includes an initiator.

[0056] In some embodiments, the electrolyte comprises a ternary electrolyte.

[0057] In some embodiments, the initiator includes one or both of dibenzoyl peroxide and dimethyl azobisisobutyrate.

[0058] In some embodiments, the mass ratio of the polymer to the electrolyte is (0.03-0.05):1, for example, 0.03:1, 0.04:1, 0.05:1, etc.

[0059] In some embodiments, the mass ratio of the initiator to the electrolyte is (0.008-0.12):1, for example, 0.008:1, 0.01:1, 0.12:1, etc.

[0060] The gel electrolyte described in the present application does not need to be solidified when preparing a semi-solid battery and has high ionic conductivity.

[0061] The present invention also provides a method for preparing a gel electrolyte, comprising the following steps:

[0062] (1) treating a trifunctional triacrylate to obtain a difunctional triacrylate;

[0063] (2) mixing and reacting the difunctional triacrylate, polyethylene glycol diacrylate and alkyl mercaptan to obtain a polymer represented by formula (I);

[0064] (3) Mixing the polymer represented by the linear formula (I) and an electrolyte to obtain the gel electrolyte.

[0065] Because trifunctional triacrylates have high reactivity, high crosslinking density, low volatility, low irritation, and good curing speed, using them as polymer monomers to process trifunctional triacrylates into difunctional triacrylates can reduce the hardness of the product and further improve the conductivity of the product. Then, reacting the difunctional triacrylate with polyethylene glycol diacrylate (PEGDA) can reduce the crosslinking density of the product, improve the ionic conductivity, and optimize the wetting properties of the electrolyte.

[0066] In some embodiments, the step of treating the trifunctional triacrylate comprises: mixing the trifunctional triacrylate and alkylthiol for a first reaction to obtain a difunctional triacrylate. Converting the trifunctional triacrylate to a difunctional triacrylate can reduce the hardness of the product and improve the ionic conductivity of the gel electrolyte.

[0067] In some embodiments, the trifunctional triacrylate includes trimethylolpropane triacrylate.

[0068] In some embodiments, the alkyl mercaptan includes one or more of butyl mercaptan, propyl mercaptan, and ethyl mercaptan.

[0069] In some embodiments, the molar ratio of the trifunctional triacrylate to the alkylthiol is 1:(0.1-2), for example, 1:0.1, 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:2, etc.

[0070] In some embodiments, the temperature of the first reaction is 15-35°C, for example 15°C, 20°C, 25°C, 30°C, 35°C, and the time of the first reaction is 0.5-2h, for example 0.5h, 0.8h, 1.2h, 1.8h, 2h, etc.

[0071] In some embodiments, the first reaction is performed in a first solvent.

[0072] In some embodiments, the first solvent includes one or more of dioxolane, dioxane, and tetrahydrofuran.

[0073] In some embodiments, the molar ratio of the trifunctional triacrylate to the first solvent is 1:(3-10), such as 1:3, 1:5, 1:8, 1:10, etc.

[0074] In some embodiments, the first reaction is performed in the presence of a first catalyst.

[0075] In some embodiments, the first catalyst includes dimethylphenylphosphine.

[0076] In some embodiments, the molar ratio of the trifunctional triacrylate to the first catalyst is 1:(0.005-0.05), for example, 1:0.005, 1:0.008, 1:0.01, 1:0.02, 1:0.04, 1:0.05.

[0077] In some embodiments, the number average molecular weight of the polyethylene glycol diacrylate is 170-350.

[0078] In some embodiments, the molar ratio of the difunctional triacrylate to the polyethylene glycol diacrylate is 1:(0.01-5), such as 1:0.01, 1:0.1, 1:1, 1:2, 1:3, 1:4, 1:5. Selecting this molar ratio can ensure that the prepared gel electrolyte has good ionic conductivity and good curing effect.

[0079] In some embodiments, the molar ratio of the difunctional triacrylate to the alkylthiol is 1:(0.5-1.5), for example, 1:0.5, 1:0.8, 1:1.2, 1:1.5, and the like.

[0080] In some embodiments, the temperature of the mixing reaction is 15-35°C, such as 15°C, 20°C, 25°C, 30°C, 35°C, etc., and the time of the mixing reaction is 0.5-4h, such as 0.5h, 0.8h, 1.2h, 1.5h, 2h, 3h, 3.5h, 4h, etc. If the temperature of the mixing reaction is too high, the reaction speed will be accelerated, resulting in the reaction occurring before the mixture has time to be mixed evenly. If the temperature is too low, the reaction time will be prolonged, which will affect the curing effect of the product.

[0081] In some embodiments, in step (2), the mixing reaction is carried out in a second solvent.

[0082] In some embodiments, the second solvent comprises DMF and / or dimethylacetamide.

[0083] In some embodiments, the molar ratio of the difunctional triacrylate to the second solvent is 1:(5-15), for example, 1:5, 1:8, 1:10, 1:12, 1:15, etc.

[0084] In some embodiments, in step (2), the mixing reaction is carried out in the presence of a second catalyst.

[0085] In some embodiments, the second catalyst includes dimethylphenylphosphine.

[0086] In some embodiments, the molar ratio of the difunctional triacrylate to the second catalyst is 1:(0.005-0.05), for example, 1:0.005, 1:0.008, 1:0.01, 1:0.02, 1:0.04, 1:0.05.

[0087] In some embodiments, in step (3), the polymer represented by formula (I) and the electrolyte generate a gel electrolyte under the action of an initiator.

[0088] The embodiment of the present application also provides a semi-solid-state battery, comprising the gel electrolyte described in the embodiment of the present application and the gel electrolyte obtained by the preparation method of the embodiment of the present application.

[0089] The semi-solid battery of the embodiment of the present application does not need to be cured because it contains the gel electrolyte, which simplifies the preparation process of the semi-solid battery. In addition, if there are monomers that do not participate in the gel during the static process, they can be further gelled during the battery formation process, thereby improving the curing completeness of the gel electrolyte and further improving the electrical performance and safety of the battery.

[0090] Example 1

[0091] (I) Preparation of gel electrolyte

[0092] The monomer M1 trimethylolpropane triacrylate (1 mol) and butanethiol (1 mol) were dissolved in 576 g of tetrahydrofuran (THF) solvent, and a catalyst dimethylphenylphosphine (0.03 mol) was added, and the mixture was stirred at 0°C until uniform, and then allowed to react at room temperature for 1 hour; the above product was then separated and purified by column chromatography to obtain the monomer M2;

[0093] The monomer M2 (0.5 mol), polyethylene glycol diacrylate (0.5 mol) with a number average molecular weight of 214 and butanethiol (1 mol) were dissolved in 730 g of dimethylacetamide (DMAc) solvent, dimethylphenylphosphine (0.01 mol) was added, and the mixture was stirred at 0°C until uniform, and then allowed to react at room temperature for 2 hours to obtain a linear polymer.

[0094] The linear polymer is added to the ternary electrolyte in an amount of 4% by mass of the ternary electrolyte, and a dibenzoyl peroxide initiator is added at the same time in an amount of 1% by mass of the ternary electrolyte, and the mixture is mixed to obtain a gel electrolyte.

[0095] Example 2

[0096] The only difference between Example 2 and Example 1 is that during the preparation of the gel electrolyte in Example 2, the amount of monomer M2 added is 0.2 mol, and the amount of polyethylene glycol diacrylate with a number average molecular weight of 214 added is 0.8 mol, that is, the molar ratio of monomer M2 to polyethylene glycol diacrylate is 1:4.

[0097] The specific steps are:

[0098] The monomer M1 trimethylolpropane triacrylate (1 mol) and butanethiol (1 mol) were dissolved in 576 g of tetrahydrofuran (THF) solvent, and a catalyst dimethylphenylphosphine (0.03 mol) was added, and the mixture was stirred at 0°C until uniform, and then allowed to react at room temperature for 1 hour; the above product was then passed through a column, separated, purified, and the monomer M2 was obtained;

[0099] The monomer M2 (0.2 mol), polyethylene glycol diacrylate (0.8 mol) and butanethiol (1 mol) were dissolved in 730 g of dimethylacetamide (DMAc) solvent, dimethylphenylphosphine (0.01 mol) was added, stirred at 0°C until uniform, and then allowed to react at room temperature for 2 hours to obtain a linear polymer.

[0100] The linear polymer is added to the ternary electrolyte in an amount of 4% by mass of the ternary electrolyte, and a dibenzoyl peroxide initiator is added at the same time in an amount of 1% by mass of the ternary electrolyte, and the mixture is mixed to obtain a gel electrolyte.

[0101] Example 3

[0102] The only difference between Example 3 and Example 1 is that in the preparation process of the gel electrolyte in Example 3, the amount of monomer M2 added is 0.8 mol, and the amount of polyethylene glycol diacrylate with a number average molecular weight of 214 added is 0.2 mol, that is, the molar ratio of monomer M2 to polyethylene glycol diacrylate is 1:0.25.

[0103] The specific steps are:

[0104] The monomer M1 trimethylolpropane triacrylate (1 mol) and butanethiol (1 mol) were dissolved in 576 g of tetrahydrofuran (THF) solvent, and a catalyst dimethylphenylphosphine (0.03 mol) was added, and the mixture was stirred at 0°C until uniform, and then allowed to react at room temperature for 1 hour; the above product was then passed through a column, separated, purified, and the monomer M2 was obtained;

[0105] The monomer M2 (0.8 mol), polyethylene glycol diacrylate (0.2 mol) and butanethiol (1 mol) were dissolved in 730 g of dimethylacetamide (DMAc) solvent, dimethylphenylphosphine (0.01 mol) was added, stirred at 0°C until uniform, and then allowed to react at room temperature for 2 hours to obtain a linear polymer.

[0106] The linear polymer is added to the ternary electrolyte in an amount of 4% by mass of the ternary electrolyte, and a dibenzoyl peroxide initiator is added at the same time in an amount of 1% by mass of the ternary electrolyte, and the mixture is mixed to obtain a gel electrolyte.

[0107] Comparative Example 1

[0108] The difference between Comparative Example 1 and Example 1 is that the raw material polyethylene glycol diacrylate is not added during the preparation process of Comparative Example 1, and the remaining operations are the same as those of Example 1.

[0109] The specific steps are:

[0110] The monomer M1 trimethylolpropane triacrylate (1 mol) and butanethiol (1 mol) were dissolved in 576 g of tetrahydrofuran (THF) solvent, and a catalyst dimethylphenylphosphine (0.03 mol) was added, and the mixture was stirred at 0°C until uniform, and then allowed to react at room temperature for 1 hour; the above product was then passed through a column, separated, purified, and the monomer M2 was obtained;

[0111] The monomer M2 (0.5 mol) and butanethiol (1 mol) were dissolved in 730 g of dimethylacetamide (DMAc) solvent, dimethylphenylphosphine (0.01 mol) was added, and the mixture was stirred at 0°C until uniform, and then allowed to react at room temperature for 2 h to obtain a linear polymer.

[0112] The linear polymer is added to the ternary electrolyte in an amount of 4% by mass of the ternary electrolyte, and a dibenzoyl peroxide initiator is added at the same time in an amount of 1% by mass of the ternary electrolyte, and the mixture is mixed to obtain a gel electrolyte.

[0113] Comparative Example 2

[0114] The difference between Comparative Example 2 and Example 1 is that no monomer M2 is added during the preparation process of Comparative Example 2.

[0115] The specific steps are:

[0116] Polyethylene glycol diacrylate (0.5 mol) and butanethiol (1 mol) were dissolved in 730 g of dimethylacetamide (DMAc) solvent, dimethylphenylphosphine (0.01 mol) was added, stirred at 0°C until uniform, and then allowed to react at room temperature for 2 hours to obtain a linear polymer.

[0117] The linear polymer is added to the ternary electrolyte in an amount of 4% by mass of the ternary electrolyte, and a dibenzoyl peroxide initiator is added at the same time in an amount of 1% by mass of the ternary electrolyte, and the mixture is mixed to obtain a gel electrolyte.

[0118] Comparative Example 3

[0119] A conventional ternary electrolyte is used as comparative example 3.

[0120] Comparative Example 4

[0121] The difference between Comparative Example 4 and Example 1 of the present application is that a trifunctional triacrylate is directly reacted with polyethylene glycol diacrylate to prepare a linear polymer.

[0122] Monomer M1 (0.5 mol), polyethylene glycol diacrylate (0.5 mol) and butanethiol (1 mol) were dissolved in 730 g of dimethylacetamide (DMAc) solvent, dimethylphenylphosphine (0.01 mol) was added, stirred at 0°C until uniform, and then allowed to react at room temperature for 2 hours to obtain a linear polymer.

[0123] The linear polymer is added to the ternary electrolyte in an amount of 4% by mass of the ternary electrolyte, and a dibenzoyl peroxide initiator is added at the same time in an amount of 1% by mass of the ternary electrolyte, and the mixture is mixed to obtain a gel electrolyte.

[0124] (II) Preparation of semi-solid batteries

[0125] S1. Preparation of positive electrode sheet: Preparation of positive electrode material layer: 97.5% of lithium nickel cobalt manganese oxide, 1.25% of binder polyvinylidene fluoride, 0.75% of conductive agent conductive carbon black and 0.5% of single-walled carbon nanotubes are weighed by mass, firstly polyvinylidene fluoride is added to N-methylpyrrolidone solvent to prepare a glue solution, then conductive carbon black and single-walled carbon nanotubes are added to the above glue solution, stirred until uniform, then lithium nickel cobalt manganese oxide is added to the above slurry, stirred until uniform; finally, the slurry is coated on the current collector, and the positive electrode sheet is prepared after drying; small positive electrode sheets are obtained by rolling and slitting;

[0126] S2. Preparation of negative electrode sheet: 85% of graphite negative electrode material, 10% of silicon dioxide negative electrode material, 2.25% of negative electrode binder polyacrylic acid, 0.75% of negative electrode conductive agent conductive carbon black and 0.5% of negative electrode conductive agent conductive carbon black, and 1.5% of styrene-butadiene rubber are weighed by mass, firstly polyacrylic acid is added to deionized water to prepare a glue solution, then conductive carbon black, graphite and silicon oxide are added to the above glue solution, stirred until uniform, then styrene-butadiene rubber is added, and finally the slurry is coated on the current collector, and the negative electrode sheet is prepared after drying; small negative electrode sheets are obtained by rolling and cutting;

[0127] S3. Prepare the battery cell: vacuum bake the positive and negative electrode sheets at a temperature of 85°C for 24 hours, stack them into a battery cell and encapsulate them in an aluminum-plastic film;

[0128] S4. The gel electrolytes prepared in this embodiment and the comparative example are respectively injected into the baked battery cells, and after formation, aging and capacity separation, a semi-solid battery is obtained.

[0129] The gel electrolytes and semi-solid batteries prepared in Examples 1-3 and Comparative Examples 1-4 of the present application were subjected to performance tests, and the test results are shown in Table 1.

[0130] The test method is as follows:

[0131] The divided capacitance internal resistance is tested using a voltage internal resistance tester;

[0132] Cycle performance: At 25°C, charge to 4.2V at 0.5C constant current and constant voltage, leave for 10 minutes, and then discharge to 2.75V at 1C constant current.

[0133] Acupuncture: The acupuncture test of this application shall be carried out in accordance with GB31485-2020 Safety requirements and test methods for power batteries for electric vehicles. The higher the acupuncture pass rate, the better the safety of the battery.

[0134] Table 1

[0135]

[0136]

[0137] It can be seen from Table 1 that the gel electrolyte obtained by the preparation method described in the present application has high safety; the higher the needle puncture pass rate, the better the safety of the battery prepared by the gel electrolyte prepared by the present application, and the performance of the gel electrolyte can be further optimized by adjusting the addition amount of monomer M2 and polyethylene glycol diacrylate.

[0138] The capacity cycle retention rate of the semi-solid-state battery prepared in Example 1 and Comparative Example 3 of the present application at 25°C, 0.5C charging and 1C discharging is as follows: Figure 1 As shown:

[0139] from Figure 1 It can be seen that the room-temperature cyclability of the semi-solid battery prepared by the gel electrolyte prepared in Example 1 of the present application is better than that prepared by the gel electrolyte described in Comparative Example 3, that is, the gel electrolyte obtained by the preparation method described in the present application can improve the cycle performance of the battery.

[0140] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A gel electrolyte, characterized in that: It comprises an electrolyte and a polymer represented by structural formula (I), Among them, 1≤x≤6, 5≤m≤500, 1≤n≤5.

2. The gel electrolyte according to claim 1, characterized in that The gel electrolyte also includes an initiator; And / or, the electrolyte comprises a ternary electrolyte; And / or, the initiator comprises one or both of dibenzoyl peroxide and dimethyl azobisisobutyrate; And / or, the mass ratio of the polymer to the electrolyte is (0.03-0.05):1; And / or, the mass ratio of the initiator to the electrolyte is (0.008-0.12):

1.

3. A method for preparing the gel electrolyte according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) treating a trifunctional triacrylate to obtain a difunctional triacrylate; (2) mixing and reacting the difunctional triacrylate, polyethylene glycol diacrylate and alkyl mercaptan to obtain a polymer represented by formula (I); (3) Mixing the polymer represented by the formula (I) and an electrolyte to obtain the gel electrolyte.

4. The method for preparing the gel electrolyte according to claim 3, characterized in that: The trifunctional triacrylate includes trimethylolpropane triacrylate; And / or, the step of treating the trifunctional triacrylate comprises: mixing the trifunctional triacrylate and alkylthiol for a first reaction to obtain a difunctional triacrylate; Preferably, the alkyl mercaptan comprises one or more of butyl mercaptan, propyl mercaptan and ethyl mercaptan; Preferably, the molar ratio of the trifunctional triacrylate to the alkylthiol is 1:(0.1-2); Preferably, the temperature of the first reaction is 15-35°C; the time of the first reaction is 0.5-2h.

5. The method for preparing the gel electrolyte according to claim 4, characterized in that: The first reaction is carried out in a first solvent, preferably, the first solvent comprises one or more of dioxolane, dioxane and tetrahydrofuran, more preferably, the molar ratio of the trifunctional triacrylate to the first solvent is 1:(3-10); And / or, the first reaction is carried out in the presence of a first catalyst, preferably, the first catalyst comprises dimethylphenylphosphine, more preferably, the molar ratio of the trifunctional triacrylate to the first catalyst is 1:(0.005-0.05).

6. The method for preparing the gel electrolyte according to claim 4, characterized in that: In the step (2), the number average molecular weight of the polyethylene glycol diacrylate is 170-350; and / or, the molar ratio of the difunctional triacrylate to the polyethylene glycol diacrylate is 1:(0.01-5), preferably 1:(0.25-4); and / or, the molar ratio of the difunctional triacrylate to the alkyl mercaptan is 1:(0.5-1.5); And / or, the temperature of the mixed reaction is 15-35° C., and the time of the mixed reaction is 0.5-4 h.

7. The method for preparing the gel electrolyte according to claim 4, characterized in that: In step (2), the mixing reaction is carried out in a second solvent. Preferably, the second solvent includes DMF and / or dimethylacetamide. More preferably, the molar ratio of the difunctional triacrylate to the second solvent is 1:(5-15).

8. The method for preparing the gel electrolyte according to claim 4, characterized in that: In step (2), the mixing reaction is carried out in the presence of a second catalyst, preferably, the second catalyst comprises dimethylphenylphosphine; more preferably, the molar ratio of the difunctional triacrylate to the second catalyst is 1:(0.005-0.05).

9. The method for preparing the gel electrolyte according to claim 3, characterized in that: In step (3), the polymer represented by formula (I) and the electrolyte generate a gel electrolyte under the action of an initiator.

10. A semi-solid battery, characterized in that: The invention comprises the gel electrolyte described in any one of claims 1 to 2 or the gel electrolyte obtained by the preparation method described in any one of claims 3 to 9.

Citation Information

Patent Citations

  • Preparation method for in-situ synthesis of high-performance gel electrolyte

    CN114824460A

  • Self-adaptive deformation elastomer electrolyte, electrode and battery

    CN115160233A

  • Viscoelastic conductor polymer electrolyte, preparation method thereof and lithium metal semi-solid-state battery

    CN117154213A

  • Electrolyte, gel electrolyte and preparation method thereof

    CN117174998A

  • Polymer electrolyte for lithium secondary battery and lithium secondary battery comprising the same